Method for determining basalt grid concrete carbonization diffusion coefficient under unsteady state condition
By analyzing the influence of temperature and humidity on carbonization depth in basalt mesh concrete, and establishing and correcting the prediction model, the inaccurate problem of carbonization process under non-steady state conditions is solved, and the accurate prediction of the carbonization depth of basalt mesh concrete is achieved. Optimized structural design and maintenance strategies, extend the life of the structure and reduce maintenance costs.
Patent Information
- Application Number
- CN202411115259.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-12-06
AI Technical Summary
The prior art is difficult to effectively characterize the quantification and carbonization process of basalt grid concrete in non-steady state conditions, especially under repeated loads, which leads to insufficient establishment of carbonization models, affecting the durability and maintenance strategies of the structure.
By obtaining concrete samples, the carbonization test is carried out, the influence of temperature and humidity on carbonization depth is analyzed, the chemical reaction coefficient and temperature relationship based on Arrhenius's law is established, the humidity influence coefficient is established using a quadratic polynomial, and the prediction model is corrected through the Levenberg-Marquart algorithm, and accurate Predict the carbonization depth and verify the accuracy of the model.
It realizes more accurately predicting the carbonization depth of basalt mesh concrete under non-steady state conditions, optimizes structural design and maintenance strategies, extends the service life of the structure and reduces maintenance costs.
Smart Images

Figure CN119086409A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of highway bridge construction and detection, and specifically relates to a method for determining the carbonization diffusion coefficient of basalt grid concrete under non-steady-state conditions. Background Art
[0002] In practical applications, basalt grid concrete not only needs to withstand repeated vehicle loads, but also faces the erosion of external carbon dioxide. The repeated action of such vehicle loads will cause the microcracks and pores inside the basalt grid concrete to continuously occur or develop, providing a convenient channel for carbon dioxide to enter the interior of the basalt grid concrete, thereby accelerating the carbonization process of the basalt grid concrete. However, the quantitative characterization of fatigue damage in basalt grid concrete is still an immature field, especially after the basalt grid concrete beam is subjected to repeated bending tensile stress.
[0003] At present, the carbonization research of basalt grid concrete structure under static load has been relatively sufficient, but the carbonization research under fatigue damage caused by repeated load is relatively less. In actual operation, basalt grid concrete is not only eroded by carbon dioxide, but also subjected to stress cycles caused by vehicle loads. Even repeated loads at low stress levels will lead to fatigue growth of microcracks and pores in basalt grid concrete, which will further accelerate the carbonization of basalt grid concrete.
[0004] Therefore, for the durability study of basalt grid concrete, it is very important to reliably characterize the fatigue damage degree of concrete, comprehensively consider the effect of fatigue damage on carbonization, and carefully establish the carbonization model of basalt grid concrete under fatigue damage. Summary of the invention
[0005] Purpose of the invention: To provide a method for determining the carbonation diffusion coefficient of basalt grid concrete under non-steady-state conditions, thereby solving the above-mentioned problems existing in the prior art.
[0006] Technical solution: A method for determining the carbonization diffusion coefficient of basalt grid concrete under non-steady-state conditions, comprising the following steps:
[0007] Step S1, obtaining a concrete sample, and performing a carbonization test on the concrete sample;
[0008] Step S2, obtaining the carbonization test result of the concrete sample in step S1, and analyzing the change of the actual carbonization depth of the concrete sample according to the change of temperature and relative humidity;
[0009] Step S3, building a preliminary prediction model for carbonization depth based on concrete compressive strength, obtaining the relationship between chemical reaction coefficient and temperature according to Arrhenius law, establishing a temperature influence coefficient formula, and using a quadratic polynomial to establish a humidity influence coefficient formula;
[0010] Step S4, obtaining the nonlinear relationship between the preliminary prediction model and the temperature and humidity, and using the Levenberg-Marquart algorithm to obtain a revised prediction model;
[0011] Step S5, obtaining the actual carbonization depth in step S2, using the revised prediction model in step S4 to calculate the predicted carbonization depth of concrete under temperature and relative humidity conditions, verifying the relative error between the actual carbonization depth and the predicted carbonization depth, and verifying the revised prediction model.
[0012] Preferably, the carbonization test process of step S1 is as follows:
[0013] Step S11, placing the obtained concrete sample specimen in a drying oven for drying, taking it out, sealing the non-carbonized surface with heated paraffin, placing the sealed specimen in a carbonization box, and performing a carbonization test according to temperature, relative humidity and carbon dioxide concentration;
[0014] Step S12, after carbonization for a predetermined number of days, cut the half of the test piece into a pressure testing machine for carbonization depth testing to obtain a short carbonized test piece;
[0015] Step S13, after the cut surfaces of the remaining test pieces are sealed again with paraffin, the carbonization test is performed again;
[0016] Step S14, after carbonization for a predetermined number of days, the remaining specimens are placed in a pressure testing machine for carbonization depth testing to obtain long carbonized specimens;
[0017] Step S15: After respectively obtaining the carbonization depths of the short carbonized specimen and the long carbonized specimen, the average carbonization depths of the short carbonized specimen and the long carbonized specimen are obtained.
[0018] Preferably, in step S2, the change process of temperature and relative humidity on the actual carbonization depth is as follows:
[0019] Step S21, controlling the temperature to change from low to high during the carbonization process, and obtaining the carbonization depth change of the short carbonized specimen or the long carbonized specimen at different temperatures;
[0020] Step S22, during the carbonization process, the carbonization humidity is controlled to change from low to high, so as to obtain the change of the carbonization depth of the short carbonized specimen or the long carbonized specimen under different humidity.
[0021] Preferably, in step S3, the initial calculation formula of the preliminary prediction model is as follows:
[0022]
[0023] Where: A is the carbonation depth of concrete, H is the relative humidity, is the water-cement ratio, c is the cement dosage, The concentration of carbon dioxide in the environment, is the hydration degree correction factor, is the cement correction coefficient, and t is the carbonation time.
[0024] Preferably, in step S3, the temperature influence coefficient is proportional to the carbonation depth of concrete and the carbonation reaction coefficient, and the temperature influence coefficient equation is established as follows:
[0025]
[0026] In the formula: e represents the chemical reaction coefficient, a represents the pre-factor, e a represents the apparent activation energy of the carbonization reaction, r represents the molar gas constant, and T represents the ambient temperature.
[0027] Preferably, according to the temperature influence coefficient equation, the temperature influence coefficient formula is established as follows:
[0028]
[0029] In the formula: x and d represent the unknown coefficients, and f represents the Euler number;
[0030] Step S34: Based on the influence of relative humidity on carbonization depth, a humidity influence coefficient formula is established as follows:
[0031]
[0032] Where: y, z represent unknown coefficients.
[0033] Preferably, the initial calculation formula of the preliminary prediction model is modified by introducing the temperature and humidity influence coefficients, and the modified formula is as follows:
[0034]
[0035] Preferably, in step S4, an improvement is made on the basis of the Gauss-Newton method, a gradient evaluation algorithm is used, and a damping factor is introduced to adjust the algorithm. When the damping factor is greater than zero, the descending direction of the iteration is determined, and the formulas for the temperature influence coefficient and the humidity influence coefficient are obtained by using the Levenberg-Marquart algorithm as follows:
[0036]
[0037] By substituting formula (6) and (7) into formula (5), we get the modified prediction model:
[0038]
[0039] Preferably, the predicted value of concrete carbonization depth is calculated by the modified prediction model of formula (8), the experimental value of the actual carbonization depth of the concrete sample in step S2 is obtained, the predicted value of carbonization depth is compared with the experimental value of the actual carbonization depth, and the modified prediction model is verified.
[0040] Beneficial effects: The present invention relates to a method for determining the carbonation diffusion coefficient of basalt grid concrete under non-steady-state conditions. The relationship between the chemical reaction coefficient and the temperature is obtained according to the Arrhenius law, a temperature influence coefficient formula is established, and a humidity influence coefficient formula is established using a quadratic polynomial. The preliminary prediction model is corrected to more accurately predict the carbonation depth of basalt grid concrete under different environmental conditions, making the model more in line with actual engineering applications. By accurately predicting the carbonation depth of basalt grid concrete, it is helpful to optimize structural design and formulate more effective maintenance strategies, thereby extending the service life of the structure and reducing maintenance costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 It is a system block diagram of the present invention. DETAILED DESCRIPTION
[0042] like Figure 1 As shown, the present invention provides a technical solution: a method for determining the carbonization diffusion coefficient of basalt grid concrete under non-steady state conditions, comprising the following steps:
[0043] Step S1, obtaining a concrete sample, and performing a carbonization test on the concrete sample, wherein the carbonization test process of the concrete sample is as follows:
[0044] Step S11: The obtained concrete sample specimen is placed in a drying oven for drying. In this embodiment, the drying oven is dried at a temperature of 50° C. for 24 hours. The dried concrete sample is taken out, and the non-carbonized surface is sealed with heated paraffin wax. The sealed specimen is placed in a carbonization box, and a carbonization test is performed according to temperature, relative humidity and carbon dioxide concentration.
[0045] Step S12, after carbonization for 10 days, the carbonized concrete is cut in half, and the general concrete is put into a pressure testing machine for carbonization depth test to obtain a short carbonized specimen;
[0046] Step S13, after the remaining cut surface of the concrete is sealed again with paraffin, the carbonization test is performed again;
[0047] Step S14: After 10 days of carbonization, the remaining concrete is placed in a pressure testing machine for carbonization depth testing to obtain a long carbonized specimen;
[0048] Step S15: After respectively obtaining the carbonization depths of the short carbonized specimen and the long carbonized specimen, the average carbonization depths of the short carbonized specimen and the long carbonized specimen are obtained.
[0049] Step S2, obtaining the carbonization test result of the concrete sample in step S1, and analyzing the change of the actual carbonization depth of the concrete sample according to the change of temperature and relative humidity. The change process of the actual carbonization depth due to the change of temperature and relative humidity is as follows:
[0050] Step S21, controlling the temperature to change from low to high during the carbonization process, and obtaining the carbonization depth change of the short carbonized specimen or the long carbonized specimen at different temperatures;
[0051] Step S22, during the carbonization process, the carbonization humidity is controlled to change from low to high, and the carbonization depth of the short carbonized specimen or the long carbonized specimen under different humidity is obtained, and the change is shown in Table 1.
[0052] Table 1: Carbonization depth changes at different temperatures
[0053] Carbonization depth (mm) Carbonization time (days) Temperature(℃) 0.42 10 10 0.45 10 20 0.5 10 30 3.45 10 40 0.58 20 10 0.82 20 20 0.24 20 30 6.28 20 40
[0054] Step S3: construct a preliminary prediction model for carbonization depth based on the compressive strength of concrete. The initial calculation formula of the preliminary prediction model is as follows:
[0055]
[0056] Where: A is the carbonation depth of concrete, H is the relative humidity, is the water-cement ratio, c is the cement dosage, The concentration of carbon dioxide in the environment, is the hydration degree correction factor, is the cement correction factor, t is the carbonation time;
[0057] The relationship between the chemical reaction coefficient and temperature is obtained according to the Arrhenius law, and the temperature influence coefficient formula is established. The humidity influence coefficient formula is established using a quadratic polynomial. The temperature influence coefficient is proportional to the carbonation depth of concrete and the carbonation reaction coefficient. The temperature influence coefficient equation is established as follows:
[0058]
[0059] In the formula: e represents the chemical reaction coefficient, a represents the pre-factor, e a represents the apparent activation energy of the carbonization reaction, r represents the molar gas constant, and T represents the ambient temperature.
[0060] According to the temperature influence coefficient equation, the temperature influence coefficient formula is established as follows:
[0061]
[0062] In the formula: x and d represent the unknown coefficients, and f represents the Euler number;
[0063] Step S34: Based on the influence of relative humidity on carbonization depth, a humidity influence coefficient formula is established as follows:
[0064]
[0065] Where: y, z represent unknown coefficients.
[0066] Preferably, the initial calculation formula of the preliminary prediction model is modified by introducing the temperature and humidity influence coefficients, and the modified formula is as follows:
[0067]
[0068] Step S4, obtaining the nonlinear relationship between the preliminary prediction model and temperature and humidity, using the Levenberg-Marquart algorithm to obtain a modified prediction model, improving the Gauss-Newton method, using the gradient evaluation algorithm, introducing a damping factor to adjust the algorithm, and determining the descending direction of the iteration when the damping factor is greater than zero, using the Levenberg-Marquart algorithm to obtain the temperature influence coefficient and the humidity influence coefficient formulas as follows:
[0069]
[0070] By substituting formula (6) and (7) into formula (5), we get the modified prediction model:
[0071]
[0072] Step S5, obtaining the actual carbonization depth in step S2, using the corrected prediction model in step S4 to calculate the predicted carbonization depth of concrete under temperature and relative humidity conditions, verifying the relative error between the actual carbonization depth and the predicted carbonization depth, and verifying the corrected prediction model, wherein the comparison data of the actual carbonization depth and the predicted carbonization depth are shown in Table 2.
[0073] Table 2: Comparison data of actual carbonization depth and predicted carbonization depth
[0074] Water-cement ratio <![CDATA[Cement consumption (kg / m 3 )]]> Temperature / ℃ Relative humidity / % Test value / mm Predicted value / mm Relative error / % 0.45 450 45 40 20.1 19.8 1.5 0.6 550 55 70 19.3 18.7 2.9 0.55 480 48 52 17.5 17.2 1.7 0.4 380 35 38 21.9 22.3 1.8 0.7 600 60 80 15.8 15.5 1.9 0.3 320 30 65 23.7 24.1 1.6
[0075] The preferred embodiments of the present invention are described in detail above; however, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, various equivalent transformations can be made to the technical solutions of the present invention, and these equivalent transformations all belong to the protection scope of the present invention.
Claims
1. A method for determining the carbonization diffusion coefficient of basalt grid concrete under non-steady-state conditions, characterized in that: The following steps are involved: Step S1, obtaining a concrete sample, and performing a carbonization test on the concrete sample; Step S2, obtaining the carbonization test result of the concrete sample in step S1, and analyzing the change of the actual carbonization depth of the concrete sample according to the change of temperature and relative humidity; Step S3, building a preliminary prediction model for carbonization depth based on concrete compressive strength, obtaining the relationship between chemical reaction coefficient and temperature according to Arrhenius law, establishing a temperature influence coefficient formula, and using a quadratic polynomial to establish a humidity influence coefficient formula; Step S4, obtaining the nonlinear relationship between the preliminary prediction model and the temperature and humidity, and using the Levenberg-Marquart algorithm to obtain a revised prediction model; Step S5, obtaining the actual carbonization depth in step S2, using the revised prediction model in step S4 to calculate the predicted carbonization depth of concrete under temperature and relative humidity conditions, verifying the relative error between the actual carbonization depth and the predicted carbonization depth, and verifying the revised prediction model.
2. The method for determining the carbonization diffusion coefficient of basalt grid concrete under non-steady state conditions according to claim 1 is characterized in that: The carbonization test process of step S1 is as follows: Step S11, the obtained concrete sample specimen is placed in a drying oven for drying, and after being taken out, the non-carbonized surface is sealed with heated paraffin wax, and the sealed specimen is placed in a carbonization box to perform a carbonization test according to temperature, relative humidity and carbon dioxide concentration; Step S12, after carbonization for a predetermined number of days, cut the half of the test piece into a pressure testing machine for carbonization depth testing to obtain a short carbonized test piece; Step S13, after the cut surfaces of the remaining test pieces are sealed again with paraffin, the carbonization test is performed again; Step S14, after carbonization for a predetermined number of days, the remaining specimens are placed in a pressure testing machine for carbonization depth testing to obtain long carbonized specimens; Step S15: After respectively obtaining the carbonization depths of the short carbonized specimen and the long carbonized specimen, the average carbonization depths of the short carbonized specimen and the long carbonized specimen are obtained.
3. The method for determining the carbonization diffusion coefficient of basalt grid concrete under non-steady state conditions according to claim 2 is characterized in that: In step S2, the change process of temperature and relative humidity on the actual carbonization depth is as follows: Step S21, controlling the temperature to change from low to high during the carbonization process, and obtaining the carbonization depth change of the short carbonized specimen or the long carbonized specimen at different temperatures; Step S22, during the carbonization process, the carbonization humidity is controlled to change from low to high, so as to obtain the change of the carbonization depth of the short carbonized specimen or the long carbonized specimen under different humidity.
4. The method for determining the carbonization diffusion coefficient of basalt grid concrete under non-steady state conditions according to claim 1 is characterized in that: In step S3, the initial calculation formula of the preliminary prediction model is as follows: Where: A is the carbonation depth of concrete, H is the relative humidity, is the water-cement ratio, c is the cement dosage, The concentration of carbon dioxide in the environment, is the hydration degree correction factor, is the cement correction coefficient, and t is the carbonation time.
5. The method for determining the carbonization diffusion coefficient of basalt grid concrete under non-steady state conditions according to claim 4 is characterized in that: In step S3, the temperature influence coefficient is established based on the relationship that the carbonization depth of concrete is proportional to the carbonization reaction coefficient. The temperature influence coefficient equation is as follows: In the formula: e represents the chemical reaction coefficient, a represents the pre-factor, e a represents the apparent activation energy of the carbonization reaction, r represents the molar gas constant, and T represents the ambient temperature.
6. The method for determining the carbonization diffusion coefficient of basalt grid concrete under non-steady state conditions according to claim 5 is characterized in that: According to the temperature influence coefficient equation, the temperature influence coefficient formula is established as follows: In the formula: x and d represent the unknown coefficients, and f represents the Euler number; Step S34: Based on the influence of relative humidity on carbonization depth, a humidity influence coefficient formula is established as follows: Where: y, z represent unknown coefficients.
7. The method for determining the carbonization diffusion coefficient of basalt grid concrete under non-steady state conditions according to claim 6 is characterized in that: The initial calculation formula of the preliminary prediction model is modified by introducing the temperature and humidity influence coefficients. The modified formula is as follows:
8. The method for determining the carbonization diffusion coefficient of basalt grid concrete under non-steady state conditions according to claim 7, characterized in that: In step S4, the Gauss-Newton method is improved by using a gradient evaluation algorithm and introducing a damping factor to adjust the algorithm. When the damping factor is greater than zero, the descending direction of the iteration is determined, and the formulas for the temperature influence coefficient and the humidity influence coefficient are obtained by using the Levenberg-Marquart algorithm as follows: By substituting formula (6) and (7) into formula (5), we get the modified prediction model:
9. The method for determining the carbonization diffusion coefficient of basalt grid concrete under non-steady state conditions according to claim 8, characterized in that: The predicted value of concrete carbonization depth is calculated by the modified prediction model of formula (8), the experimental value of the actual carbonization depth of the concrete sample in step S2 is obtained, the predicted value of carbonization depth is compared with the experimental value of the actual carbonization depth, and the modified prediction model is verified.