Control panel and preparation method thereof
By introducing a surface hardness layer, infrared induction ink and character layer into the control panel, combining a PMMA semi-transmissive plate and diffusion film with a light transmittance of 8-10%, the poor light sensing effect and aesthetics in the prior art are solved. , achieving a higher-grade sensing effect and beautiful appearance.
Patent Information
- Application Number
- CN202311619134.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-30
- Publication Date
- 2024-12-06
AI Technical Summary
The existing control panel has poor light sensing effect, is not sensitive enough, has light string problems, is not beautiful on the surface, and print characters and ink are prone to fall off.
A control panel was designed, including a surface hardness layer, a thin film, an infrared induction ink and character layer, a PMMA semi-permeable plate, a diffusion film, a shading ink layer and an OCA followed by glue. The infrared induction ink and character layer are located inside, using UV hardening liquid and UV glue to cure and then, a PMMA semi-transmissive plate and diffusing film with a light transmittance of 8-10% were set to improve sensitivity and aesthetics.
It improves the sensitivity to infrared rays, prevents ink and characters from falling off, achieves color consistency after the lamp is turned off, and has a beautiful appearance. It is suitable for a variety of electrical equipment.
Smart Images

Figure CN119087564A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of operating panels, and in particular to a control panel and a preparation method thereof. Background Art
[0002] In the prior art, the control panel is usually prepared by printing characters, shading ink, and diffusion ink on the surface of a PMMA sheet. The control panel prepared in this way has poor light sensing effect, is not sensitive enough, and has a cross-light problem when the light is on. The screen printing can be seen on the surface, which is not very beautiful, and the color is inconsistent after the light is turned off. In addition, since the printed characters, shading ink, and diffusion ink are located on the outside of the PMMA sheet of the control panel, the characters and the ink located in the sensing area are easily rubbed off during use. Therefore, it is necessary to improve the control panel in the prior art. Summary of the invention
[0003] Based on this, it is necessary to provide a control panel and a preparation method thereof to address the current problems.
[0004] On the one hand, the present application provides a control panel, which comprises a surface hardness layer, a film, an infrared sensing ink and character layer, a first UV bonding layer, a PMMA semi-transparent plate, a second UV bonding layer, a diffusion film, a shading ink layer, and an OCA adhesive in sequence; wherein the infrared sensing ink and character layer comprises an infrared sensing ink layer and characters printed on one side of the infrared sensing ink layer; the transmittance of the PMMA semi-transparent plate is 8-10%; and a pattern area to be displayed is hollowed out in the shading ink layer.
[0005] Due to the provision of a surface hardness layer and a thin film, the infrared sensing ink and character layer are located inside the control panel and will not come into contact with the hands during use, which can prevent the ink and characters in the existing control panel from falling off due to long-term friction. In addition, by setting the ink as infrared sensing ink, the sensitivity to infrared rays can be enhanced, making the touch more sensitive. In addition, by selecting a PMMA semi-transparent plate with a transmittance of 8-10%, the penetration of light will not be hindered, and the consistency of the color of the control panel surface can be achieved after the lights are turned off, achieving an integrated black effect, making the control panel and the products to which it is applied more integrated, more upscale, and more atmospheric. In addition, through the provision of a diffusion film, the diffusion film diffuses the light to where it needs to be displayed, making the light transmission in the display pattern area more uniform, and the screen printing of the silk screen cannot be seen on the surface of the control panel, making the appearance more beautiful.
[0006] In one embodiment, the film is a PET film, and the thickness of the film is 0.07-0.25 mm.
[0007] In one embodiment, the diffusion membrane is a PET diffusion membrane, and the thickness of the diffusion membrane is 0.1-0.5 mm.
[0008] In one embodiment, the surface hardness layer has a thickness of 3-5 μm and a hardness of 1-4H; The thickness of the infrared sensing ink and character layer is 8-10 μm; The thickness of the first UV bonding layer and the second UV bonding layer are both 8-10 μm; The thickness of the PMMA semi-permeable plate is 0.5-4 mm; The thickness of the light-shielding ink layer is 10-15 μm; The thickness of the OCA adhesive is 0.1-0.3 mm.
[0009] In one embodiment, the light-shielding ink used to form the light-shielding ink layer is the XP-9259 model ultra-black ink produced by Shenzhen Chenrui Technology Co., Ltd.
[0010] On the other hand, the present application provides a method for preparing the above control panel, the method comprising the following steps: S1, coating a UV curing liquid on one side of the film, and UV curing the UV curing liquid to form a surface hardness layer; Among them, the UV curing liquid is a transparent liquid, which can be cured by UV equipment. The surface hardness after curing can be adjusted by adjusting the energy of the UV lamp of the UV equipment so that its hardness value is between 1-4H.
[0011] S2, printing infrared sensing ink and characters on the other side of the film in sequence, and curing the infrared sensing ink and characters by heating to obtain an infrared sensing ink and character layer; S3, bonding the side of the plate obtained in step S2 with the infrared sensing ink and the character layer to the PMMA semi-transparent plate by UV glue, pressing them together, and UV curing the UV glue to form a first UV bonding layer; S4, bonding one side of the PMMA semi-transparent plate of the plate obtained in step S3 to the diffusion film by UV glue, pressing them together, and UV curing the UV glue to form a second UV bonding layer; S5, printing light-shielding ink on the surface of the diffusion film of the plate obtained in step S4, and curing the light-shielding ink by heating to obtain a light-shielding ink layer; Among them, the light-shielding ink is the XP-9259 extra black ink produced by Shenzhen Chenrui Technology Co., Ltd., which has good adhesion to the diffusion film and has good light-shielding effect.
[0012] S6, attaching OCA adhesive to the surface of the light-shielding ink layer of the plate obtained in step S5; Among them, OCA adhesive is a double-sided adhesive. When attaching OCA adhesive, all bubbles between OCA adhesive and the board need to be discharged to prevent bubbles from expanding when heated and affecting product quality.
[0013] S7, cutting the plate obtained in step S6 to obtain a control panel.
[0014] During cutting, the plate is cut according to the shape of the required product.
[0015] In one embodiment, during UV curing in step S1, step S3, and step S4, the energy density of the UV lamp is 1200-1500 mJ / cm 2 , curing time is 5s.
[0016] In one embodiment, the temperature of heating and curing in step S2 is 80-85° C., and the curing time is 80-100 min.
[0017] In one embodiment, the temperature of heating and curing in step S5 is 90-95° C., and the curing time is 60-80 min.
[0018] Compared with the prior art, the present invention has the following beneficial effects: A control panel of the present invention comprises, in sequence, a surface hardness layer, a film, an infrared sensing ink and character layer, a first UV bonding layer, a PMMA semi-transparent plate, a second UV bonding layer, a diffusion film, a shading ink layer, and an OCA adhesive. The infrared sensing ink and character layer comprises an infrared sensing ink layer and characters printed on one side of the infrared sensing ink layer. The PMMA semi-transparent plate has a light transmittance of 8-10%. A pattern area to be displayed is hollowed out in the shading ink layer. The control panel of the present invention has a good infrared sensing effect, a more uniform light display, no silk screen printing can be seen on the surface, the appearance is more beautiful, the surface color is consistent after the light is turned off, and the characters can be prevented from falling off due to friction. The control panel of the present invention has a wide range of applications and can be applied to various electrical appliances such as air conditioners, refrigerators, water heaters, water dispensers, and respirators. The preparation method of the control panel of the present invention has a simple preparation process and a low preparation cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 It is a structural schematic diagram of the control panel of the present invention; Figure 2 A photo of a control panel prepared for an embodiment of the present invention in a lighted state; Figure 3 A partially enlarged photo of the control panel prepared in an embodiment of the present invention in a lighted state; Figure 4 A photo of a control panel prepared in an embodiment of the present invention in a light-off state; Figure 5 This is a photo of a control panel prepared in a comparative example of the present invention in a lighted state; Figure 6 This is a partial enlarged photo of the control panel prepared in the comparative example of the present invention in a lighted state; Figure 7 This is a photo of a control panel prepared in a comparative example of the present invention in a light-off state; Among them, there are a surface hardness layer 11, a film 2, an infrared sensing ink and character layer 3, a first UV bonding layer 4, a PMMA semi-transparent plate 5, a second UV bonding layer 6, a diffusion film 7, a light-shielding ink layer 8, and an OCA adhesive 9. DETAILED DESCRIPTION
[0020] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.
[0021] It should be noted that when an element is referred to as being "fixed to" another element, it may be directly on the other element or there may also be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. On the contrary, when an element is referred to as being "directly on" another element, there is no intermediate element. The terms "vertical", "horizontal", "left", "right", "one side", "other side", "one end", "other end" and similar expressions used herein are for illustrative purposes only and are not intended to limit the specific orientation of components in a product or device.
[0022] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0023] In order to illustrate the problem, the present invention designs an embodiment and a comparative example. Example:
[0024] like Figure 1As shown, a control panel of the present invention comprises a surface hardness layer 1, a film 2, an infrared sensing ink and character layer 3, a first UV bonding layer 4, a PMMA semi-transparent plate 5, a second UV bonding layer 6, a diffusion film 7, a shading ink layer 8, and an OCA adhesive 9 in sequence; wherein, the infrared sensing ink and character layer 3 comprises an infrared sensing ink layer and characters printed on one side of the infrared sensing ink layer; the transmittance of the PMMA semi-transparent plate 5 is 8-10%; and a pattern area to be displayed is hollowed out in the shading ink layer 8.
[0025] The method for preparing the control panel in this embodiment includes the following steps: S1, coating a UV curing liquid on one side of the film 2, and UV curing the UV curing liquid to form a surface hardness layer; The plate obtained in step S1 of this embodiment is purchased directly from Shenzhen Jiayuanfu Technology Co., Ltd., wherein film 2 is a PET film with a thickness of 0.125 mm, and the energy density of the UV lamp during UV curing is 1500 mJ / cm 2 , the curing time is 5s, and the hardness value of the surface hardness layer is 4H.
[0026] S2, printing infrared sensing ink and characters on the other side of the film 2 in sequence, and curing the infrared sensing ink and characters by heating to obtain an infrared sensing ink and character layer 3; Among them, the infrared sensing ink in step S2 of this embodiment is the CR-IR-6611 model infrared sensing ink of Zhongshan Hengmei Ink and Coating Co., Ltd., and the ink used for the character layer is the CR-XP-120 model ink of Shenzhen Chenrui Technology Co., Ltd. The heating and curing temperature in step S2 is 80°C and the curing time is 90 minutes.
[0027] S3, bonding the side of the plate obtained in step S2 with the infrared sensing ink and the character layer 3 to the PMMA semi-transparent plate 5 by UV glue, pressing them together, and UV curing the UV glue to form a first UV bonding layer 4; In this embodiment, the thickness of the PMMA semi-transparent plate 5 is 3 mm, and the light transmittance is 8%; the UV glue is the B02-1UV acrylic adhesive produced by Zhihe Environmental Protection Materials Co., Ltd.; during UV curing in step S3 of this embodiment, the energy density of the UV lamp is 1200 mJ / cm 2 , curing time is 5s.
[0028] S4, bonding one side of the PMMA semi-transparent plate 5 of the plate obtained in step S3 to the diffusion film 7 by UV glue, pressing them together, and UV curing the UV glue to form a second UV bonding layer 6; The diffusion film 7 in this embodiment is a PET diffusion film of model TC-0.125 produced by Shenzhen Changshiwang Optoelectronic Materials Co., Ltd., with a thickness of 0.125 mm; the UV glue is an acrylic adhesive of model B02-1UV produced by Zhihe Environmental Protection Materials Co., Ltd.; during UV curing in step S4 of this embodiment, the energy density of the UV lamp is 1200 mJ / cm 2 , curing time is 5s.
[0029] S5, printing light-shielding ink on the surface of the diffusion film 7 of the plate obtained in step S4, and curing the light-shielding ink by heating to obtain a light-shielding ink layer 8; The light-shielding ink in this embodiment is the XP-9259 model extra black ink produced by Shenzhen Chenrui Technology Co., Ltd.; the heating and curing temperature in step S5 of this embodiment is 90° C., and the curing time is 80 min.
[0030] S6, attaching OCA adhesive 9 to the surface of the light-shielding ink layer 8 of the plate obtained in step S5; Among them, OCA adhesive 9 is a double-sided adhesive, which is the EB18175 model double-sided adhesive of Dongguan Zhengxian New Materials Co., Ltd. When attaching OCA adhesive 9, a film pressing roller machine is used. When attaching, the bubbles between OCA adhesive 9 and the plate are completely discharged by the rolling of the pressing roller.
[0031] S7, cutting the plate obtained in step S6 to obtain a control panel.
[0032] In step S7, a CNC (numerical control machine) is used to cut the plate according to the shape of the actual product.
[0033] See also Figure 2-Figure 4 , Figure 2 and Figure 4 The following are photos of the control panel prepared in the embodiment of the present invention in the light-on state and the light-off state, Figure 3 This is a partial enlarged photo of a control panel prepared in an embodiment of the present invention in a lighted state. The control panel can be applied to a medical ventilator, wherein the area where a row of characters is located at the bottom of the control panel is a control area for controlling the control panel, and other patterns except the above characters are pattern areas to be displayed; Figure 2 and Figure 3 It can be seen that when the light is on, the area to be displayed on the control panel has uniform light transmission, clear display content, no light crosstalk, and no silk screen printing on the surface of the control panel, making the appearance more beautiful. Figure 4 It can be seen that after the light is turned off, the color of the pattern area to be displayed on the control panel is consistent, and an integrated black effect can be achieved. Comparative Example:
[0034] This comparative example is an existing preparation method for a control panel, which comprises the following steps: printing characters on one side of a fully transparent PMMA plate, and heating and curing the characters at 80°C for 90 minutes; then printing shading ink on the side where the characters are located, and heating and curing the characters at 90°C for 80 minutes; then printing diffusion ink on the side where the shading ink is located, and heating and curing the characters at 90°C for 80 minutes; cutting the obtained plate, and affixing adhesive to the side without characters and ink to obtain a control panel.
[0035] See also Figure 5-Figure 7 , Figure 5 and Figure 7 These are photos of the control panel prepared in the comparative example of the present invention in the light-on state and the light-off state, Figure 6 This is a partial enlarged photo of the control panel prepared in the comparative example of the present invention in the lighted state. The control panel can be applied to a medical ventilator, wherein the area where a row of characters is located at the bottom of the control panel is the control area for controlling the control panel, and other patterns except the above characters are the pattern area to be displayed; Figure 5 and Figure 6 It can be seen that when the light is on, the light transmission of the pattern area to be displayed on the control panel is uneven. In addition to the parts that need to be displayed (such as 96 and 73), gray-white traces can be seen on the parts that do not need to be displayed, indicating that there is a cross-light problem. In addition, the silk-screen screen print (the background part of "Working") can be seen on the surface of the control panel, and the display effect is not good. Figure 7 It can be seen that after the lights are turned off, unclear patterns can still be seen in the pattern area to be displayed on the control panel, and the effect of integrated black cannot be achieved.
[0036] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0037] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A control panel, characterized in that: The control panel includes a surface hardness layer, a film, an infrared sensing ink and character layer, a first UV bonding layer, a PMMA semi-transparent plate, a second UV bonding layer, a diffusion film, a shading ink layer, and an OCA adhesive in sequence; wherein the infrared sensing ink and character layer includes an infrared sensing ink layer and characters printed on one side of the infrared sensing ink layer; the transmittance of the PMMA semi-transparent plate is 8-10%; and a pattern area to be displayed is hollowed out in the shading ink layer.
2. The control panel according to claim 1, characterized in that: The film is a PET film, and the thickness of the film is 0.07-0.25 mm.
3. The control panel according to claim 1, characterized in that: The diffusion film is a PET diffusion film, and the thickness of the diffusion film is 0.1-0.5 mm.
4. The control panel according to claim 1, characterized in that: The surface hardness layer has a thickness of 3-5 μm and a hardness of 1-4H; The thickness of the infrared sensing ink and character layer is 8-10 μm; The thickness of the first UV bonding layer and the second UV bonding layer are both 8-10 μm; The thickness of the PMMA semi-permeable plate is 0.5-4 mm; The thickness of the light-shielding ink layer is 10-15 μm; The thickness of the OCA adhesive is 0.1-0.3 mm.
5. The control panel according to claim 1, characterized in that: The light-shielding ink used to form the light-shielding ink layer is the XP-9259 model extra black ink produced by Shenzhen Chenrui Technology Co., Ltd.
6. A method for preparing a control panel according to any one of claims 1 to 5, characterized in that: The preparation method comprises the following steps: S1, coating a UV curing liquid on one side of the film, and UV curing the UV curing liquid to form a surface hardness layer; S2, printing infrared sensing ink and characters on the other side of the film in sequence, and curing the infrared sensing ink and characters by heating to obtain an infrared sensing ink and character layer; S3, bonding the side of the plate obtained in step S2 with the infrared sensing ink and the character layer to the PMMA semi-transparent plate by UV glue, pressing them together, and UV curing the UV glue to form a first UV bonding layer; S4, bonding one side of the PMMA semi-transparent plate of the plate obtained in step S3 to the diffusion film by UV glue, pressing them together, and UV curing the UV glue to form a second UV bonding layer; S5, printing light-shielding ink on the surface of the diffusion film of the plate obtained in step S4, and curing the light-shielding ink by heating to obtain a light-shielding ink layer; S6, attaching OCA adhesive to the surface of the light-shielding ink layer of the plate obtained in step S5; S7, cutting the plate obtained in step S6 to obtain a control panel.
7. The preparation method according to claim 6, characterized in that During UV curing in step S1, step S3 and step S4, the energy density of the UV lamp is 1200-1500 mJ / cm 2 , curing time is 5s.
8. The preparation method according to claim 6, characterized in that: The temperature of heating and curing in step S2 is 80-85° C., and the curing time is 80-100 min.