Zinc oxide resistor disc with high-stability power frequency reference voltage and preparation method of zinc oxide resistor disc

By adding MgO and AgNO3 to the zinc oxide resistor and performing high-temperature heat treatment, the problem of insufficient stability of the zinc oxide lightning arrester's power frequency reference voltage is solved, and higher resistance plate stability and longer service life are achieved.

CN119092232AInactive Publication Date: 2024-12-06XIANGFAN SANSAN ELECTRICAL APPLIANCE CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411288452.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing zinc oxide lightning arresters have insufficient stability in the power frequency reference voltage, resulting in frequent lightning failures, affecting power supply reliability, increasing maintenance costs, and shortening service life.

Method used

By optimizing the composition formula of zinc oxide resistor sheet, adding MgO and AgNO3 as dopants, and using high-temperature heat treatment process, the nonlinear voltage coefficient and microstructure stability of the resistor sheet are improved, and the stability of the industrial frequency reference voltage is improved.

Benefits of technology

The stability of the industrial frequency reference voltage of the zinc oxide resistor plate is significantly improved, ensuring that the industrial frequency reference voltage change rate is within ±5% after a large current impact, extending the service life of the lightning arrester and reducing maintenance costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
  • Figure SMS_4
    Figure SMS_4
Patent Text Reader

Abstract

The invention discloses a zinc oxide resistor disc with high stability and power frequency reference voltage and a preparation method of the zinc oxide resistor disc. The zinc oxide resistor disc is prepared from the following components in parts by mole: 93.4 to 96.8 parts of ZnO, 0.822 to 0.897 parts of Bi2O3, 0.807 to 0.866 parts of Co2O3, 0.09 to 0.16 parts of Cr2O3, 0.49 to 0.59 parts of MnCO3, 0.26 to 0.34 parts of Ni2O3, 0.62 to 0.98 parts of MgO, 0.072 to 0.12 parts of AgNO3, 0.042 to 0.69 parts of GF-86 silver glass powder, 0.0032 to 0.0049 parts of Al (NO3) 3.9 H2O, 0.51 to 0.68 parts of H3BO3 and 0.24 to 0.39 parts of BaCO3. According to the composition formula of the zinc oxide resistor disc, MgO and a small amount of AgNO3 are added into a traditional formula, so that the stability of the power frequency reference voltage of the zinc oxide resistor disc is greatly improved. The invention further provides a preparation method of the zinc oxide resistor disc, according to the preparation method, a heat treatment process with the highest temperature reaching 600-620 DEG C is added in a traditional preparation process, and the large current impact resistance and the power frequency reference voltage stability of the prepared zinc oxide resistor disc are further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lightning arrester varistors, and in particular to a zinc oxide resistor with a high-stability power frequency reference voltage and a preparation method thereof. Background Art

[0002] Lightning arrester, also known as overvoltage protector or surge protector, is an electrical device used to protect electrical equipment from damage caused by lightning overvoltage, operating overvoltage, and power frequency transient overvoltage. In recent years, with the advancement of lean operation and maintenance, the reliability of distribution network power supply has been significantly improved, but the number of households suffering power outages caused by lightning strikes remains high, which seriously restricts the improvement of power supply reliability. The quality problem of 10kv distribution lightning arrester products is the main cause of lightning strike failures.

[0003] The stability of lightning arrester performance can lead to the following consequences: (1) If the stability is poor, it may not provide adequate protection under overvoltage conditions, thus affecting the safe and stable operation of the power system; (2) Increased maintenance costs: Lightning arresters with poor stability may require more frequent inspections and replacements, which will increase the maintenance costs of the power system; (3) Shortened service life: The instability of the power frequency reference voltage may be a sign of aging or deterioration of the lightning arrester, which may shorten the service life of the lightning arrester and require early replacement; (4) May cause power system failure: If the lightning arrester cannot provide stable protection during an overvoltage event, it may cause power system failure and even cause a power outage. The power frequency reference voltage is an important parameter for measuring the stability of lightning arrester performance. It reflects the protection level of the lightning arrester under power frequency voltage. High lightning arrester performance stability means that the rate of change of the lightning arrester power frequency reference voltage is low, especially after being subjected to a large current shock, the rate of change of the lightning arrester power frequency reference voltage can still be maintained at a low level.

[0004] Arrester with zinc oxide resistor as core component, referred to as zinc oxide arrester, has been the focus of arrester research and development in countries around the world since its introduction due to its good nonlinear volt-ampere characteristics, and its application is also very common. However, so far, there are few research reports on how to improve the stability of the power frequency reference voltage of zinc oxide arresters. The Chinese patent "CN112694324A" discloses a zinc oxide nonlinear resistor and its preparation method. Although the public content proposes that the zinc oxide nonlinear resistor in the patent improves the stability of large current impact by adding Sb2O3, Cr2O3, Ni2O3, H3BO3, and Nb2O5, there is still a lot of room for improvement. In order to further manufacture zinc oxide arresters with high-stability power frequency reference voltage, the focus is on providing zinc oxide resistors with high-stability power frequency reference voltage.

[0005] Therefore, developing a zinc oxide resistor with high stability power frequency reference voltage has become a technical problem that needs to be solved urgently. Summary of the invention

[0006] In view of this, the purpose of this application is to provide a zinc oxide resistor with high stability power frequency reference voltage and a preparation method thereof, wherein the potential gradient of the resistor is C=220±5V / mm, and it is mainly used in the production of lightning arresters in 10KV power supply systems. The zinc oxide resistor is prepared by a special composition formula and process, and its power frequency reference voltage has high stability. The zinc oxide resistor is assembled into a lightning arrester, and after a 65KA / 100KA high current shock, the rate of change of the power frequency reference voltage of the lightning arrester is controlled within ±5%.

[0007] In order to achieve or at least partially achieve the above objectives, the present application provides the following technical solutions:

[0008] In the first aspect, the present application provides a zinc oxide resistor with a high stability power frequency reference voltage, comprising the following components in molar proportions: ZnO: 93.4 to 96.8 parts, Bi2O3: 0.822 to 0.897 parts, Co2O3: 0.807 to 0.866 parts, Cr2O3: 0.09 to 0.16 parts, MnCO3: 0.49 to 0.59 parts, Ni2O3: 0.26 to 0.34 parts, MgO: 0.62 to 0.98 parts, AgNO3: 0.072 to 0.12 parts, GF-86 silver glass powder: 0.042 to 0.69 parts, Al(NO3)3·9H2O: 0.0032 to 0.0049 parts, H3BO3: 0.51 to 0.68 parts, and BaCO3: 0.24 to 0.39 parts.

[0009] Preferably, the zinc oxide resistor comprises the following components in molar proportions: ZnO: 95.2 parts, Bi2O3: 0.85 parts, Co2O3: 0.83 parts, Cr2O3: 0.14 parts, MnCO3: 0.5 parts, Ni2O3: 0.3 parts, MgO: 0.8 parts, AgNO3: 0.1 parts, GF-86 silver glass powder: 0.35 parts, Al(NO3)3·9H2O: 0.004 parts, H3BO3: 0.6 parts, and BaCO3: 0.325 parts.

[0010] In a second aspect, the present application also provides a method for preparing the aforementioned zinc oxide resistor, comprising the following steps:

[0011] Weigh the raw materials according to the molar fractions in the above zinc oxide resistor recipe and mix them evenly to obtain a mixed material;

[0012] preparing the mixed material into a slurry;

[0013] Drying to obtain dry powder;

[0014] The dried powder is granulated and then pressed, debonded and sintered to obtain a sintered resistor.

[0015] The sintered resistor is subjected to heat treatment to obtain a heat-treated resistor;

[0016] The heat-treated resistor is post-processed to obtain the aforementioned zinc oxide resistor.

[0017] The zinc oxide resistor with high stability power frequency reference voltage and its preparation method provided in the present application have at least the following beneficial effects compared with the prior art:

[0018] 1. The present application optimizes the composition formula of zinc oxide resistors, adding MgO and AgNO3 to the traditional formula. MgO, as a dopant, can improve the nonlinear voltage coefficient of zinc oxide resistors and enhance their stability under continuous operating voltage. MgO doping can also affect the microstructure of zinc oxide resistors, by optimizing the formation of grains and grain boundaries and reducing defects at grain boundaries, thereby improving the stability of the power frequency reference voltage of the resistor. At the same time, AgNO3 doping also improves the nonlinearity and stability of the resistor. + Ion doping can weaken the nonlinearity of varistor. A small amount of Ag + Ion doping can reduce the resistivity of the grains in the high current region, thereby reducing the residual voltage of the zinc oxide resistor and improving the nonlinearity and stability of the varistor. In addition, AgNO3, as a dopant, will affect the microstructure of the zinc oxide resistor, including the grain size and grain boundary characteristics. These microstructural changes will directly affect the electrical properties of the resistor. By doping MgO and AgNO3 in the traditional formula, the stability of the power frequency reference voltage of the zinc oxide resistor has been greatly improved.

[0019] 2. The present application provides a unique preparation process for zinc oxide resistors with high stability power frequency reference voltage. Through a heat treatment process with a maximum temperature of 600-620°C, the zinc oxide resistors' resistance to large current impacts and power frequency reference voltage stability are improved. DETAILED DESCRIPTION

[0020] In order to make the purpose, technical solution and advantages of the present application more clear, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described here are only used to explain the present application and are not used to limit the present application.

[0021] The embodiment of the present application optimizes the formula of the existing zinc oxide resistor by adding doping components that affect the conductivity characteristics and microstructure of the resistor, such as MgO and AgNO3, and at the same time optimizes the preparation process of the zinc oxide resistor, thereby greatly improving the stability of the power frequency reference voltage of the zinc oxide resistor.

[0022] Based on this, an embodiment of the present application provides a zinc oxide resistor with a high stability power frequency reference voltage, comprising the following components in molar fractions: ZnO: 93.4 to 96.8 parts, Bi2O3: 0.822 to 0.897 parts, Co2O3: 0.807 to 0.866 parts, Cr2O3: 0.09 to 0.16 parts, MnCO3: 0.49 to 0.59 parts, Ni2O3: 0.26 to 0.34 parts, MgO: 0.62 to 0.98 parts, AgNO3: 0.072 to 0.12 parts, GF-86 silver glass powder: 0.042 to 0.69 parts, Al(NO3)3·9H2O: 0.0032 to 0.0049 parts, H3BO3: 0.51 to 0.68 parts, and BaCO3: 0.24 to 0.39 parts.

[0023] In the composition formula of the zinc oxide resistor with high stability power frequency reference voltage, ZnO is the main raw material of zinc oxide varistor ceramics, and its microstructure is hexagonal white powder spherical or columnar, which is the main body of the final semiconductor structure. During the sintering process of zinc oxide nonlinear ceramics, a ZnO crystal phase will be formed, and the crystal phase has solid solution of Co, Mn, Cr, Al, Mg, B and other elements in the doping additives. Bi2O3 is an indispensable component for the high resistance grain boundary network skeleton structure of ZnO nonlinear resistor ceramics, and plays a very important role in improving the grain boundary barrier. H3BO3 and BaCO3 play a certain good role in promoting the sintering of ZnO, the growth of grains, and improving the stability of grain boundaries, thereby greatly improving the internal uniformity of the resistor. Co2O3 and MnCo3 are additives to improve the nonlinear function of ZnO ceramics, and play a very important role in improving the nonlinearity of ZnO ceramics and reducing leakage current. Sb2O3, Cr2O3 and Ni2O3 are additives that improve the stability of ZnO ceramics. They all help to improve the stability of ZnO ceramics in withstanding 2ms square waves, large current shocks and long-term operation under electric fields.

[0024] In the above-mentioned high-stability power frequency reference voltage zinc oxide resistor formula, MgO as a dopant has a significant effect on the stability of the power frequency reference voltage. MgO doping can improve the nonlinear voltage coefficient of the zinc oxide resistor and enhance its stability under continuous operating voltage, thereby improving the power frequency reference voltage stability of the resistor. This is because MgO 2+ It can make equivalent substitutions for zinc ions at grain boundary segregation, and can also fill the gaps of Zn 2+The number of MgO is reduced, thereby improving the stability of grain boundaries. At the same time, MgO doping can reduce the charge carrier concentration on the grain boundary and reduce the grain boundary conductivity, thereby improving the stability and service life of the resistor. In addition, MgO doping can also affect the microstructure of the zinc oxide resistor, by optimizing the formation of grains and grain boundaries, reducing defects at the grain boundaries, and further improving the electrical performance of the resistor.

[0025] In the above-mentioned high-stability power frequency reference voltage zinc oxide resistor formula, AgNO3 is used as a dopant, which can affect the electrical properties of the resistor, mainly in the following aspects: (1) AgNO3 can improve the nonlinearity and stability of the zinc oxide resistor; + Ion doping can weaken the nonlinearity of varistor. 3+ and Ag + The combined doping of can improve the nonlinearity and stability of the varistor; (2) a small amount of Ag + While avoiding leakage current, it reduces the resistivity of the grains in the high current region, thereby reducing the residual voltage of the zinc oxide resistor; (3) AgNO3 affects the microstructure of the zinc oxide resistor, including the grain size and grain boundary characteristics, reduces grain boundary defects, and thus improves the electrical properties of the resistor, such as the increase in voltage gradient and current capacity; (4) Ag + Doping can increase the barrier height and suppress leakage current, thereby improving the working stability of zinc oxide resistors.

[0026] Therefore, by doping with MgO and AgNO3, the stability of the power frequency reference voltage of the zinc oxide resistor provided in the embodiment of the present application is greatly improved. After a large current shock, the power frequency reference voltage change rate of the zinc oxide resistor provided in the embodiment of the present application is low.

[0027] In certain preferred embodiments, the zinc oxide resistor comprises the following components in molar fractions: ZnO: 95.2 parts, Bi2O3: 0.85 parts, Co2O3: 0.83 parts, Cr2O3: 0.14 parts, MnCO3: 0.5 parts, Ni2O3: 0.3 parts, MgO: 0.8 parts, AgNO3: 0.1 parts, GF-86 silver glass powder: 0.35 parts, Al(NO3)3·9H2O: 0.004 parts, H3BO3: 0.6 parts, and BaCO3: 0.325 parts.

[0028] Based on this, the present application also provides a method for preparing the aforementioned zinc oxide resistor, comprising the following steps: (1) weighing the following raw materials by mole: ZnO, Bi2O3, Co2O3, Cr2O3, MnCO3, Ni2O3, MgO, AgNO3, GF-86 silver glass powder, Al(NO3)3·9H2O, H3BO3, BaCO3; mixing the raw materials uniformly to obtain a mixed material; (2) adding a dispersant and deionized water to the mixed material for ball milling to prepare a slurry, drying the slurry, and obtaining (3) adding a binder to the dry powder, mixing, and granulating; (4) pressing the granules obtained in step (3) to obtain a molded green sheet; (5) debinding the molded green sheet to remove the binder components in the green sheet; (6) sintering the molded green sheet obtained in step (5) to obtain a sintered resistor; (7) heat-treating the sintered resistor to obtain a heat-treated resistor; (8) spraying aluminum electrodes on the heat-treated resistor, glazing, and other processes to finally obtain the aforementioned zinc oxide resistor.

[0029] In some preferred embodiments, in step (2), the dispersant is polyacrylamide or tetradecyl acetate. The dispersant can make the resistor slurry have a higher solid content at a lower viscosity, thereby improving production efficiency and material utilization; at the same time, it can improve the uniformity of the resistor composition and microstructure.

[0030] In certain preferred embodiments, in step (3), the binder is polyvinyl alcohol. The binder can increase the adhesion of the powder, so that a uniform green body with sufficient strength can be formed during the tableting process, thereby improving the molding efficiency and the quality of the green body. The binder helps to form the desired microstructure during the sintering process, which is crucial to the electrical performance of the resistor.

[0031] In certain embodiments, in (2), the ball milling speed is 100-200 r / min, and the ball milling time is 12-24 h; the drying temperature is 120-150° C., and the drying time is 24-36 h.

[0032] In some preferred embodiments, in step (2), the average particle size of the powder obtained is 75 μm. Smaller powder particle size helps to obtain a more uniform microstructure and reduce defects at the grain boundaries, thereby improving the potential gradient and current carrying capacity of the resistor.

[0033] In certain preferred embodiments, in step (3), the particle size of the particles obtained by granulation is 80 to 110 μm.

[0034] In certain preferred embodiments, in step (4), the density of the obtained shaped green sheet is controlled at (3.2±0.05) g / cm3 .

[0035] In certain preferred embodiments, in step (5), a stainless steel mesh is used to hold the formed green sheets during debinding, a distance of 2 to 3 mm is maintained between the green sheets, and the green sheets are placed in a single layer for debinding to ensure complete volatilization of the binder components inside the green sheets.

[0036] In some embodiments, the preparation method of the aforementioned zinc oxide resistor also includes a high resistance layer coating process before the debinding process, that is, coating a composite high resistance layer of Zn-Bi-Sb-Si-Mn-Ni-Li system on the surface of the formed green sheet to ensure a high degree of matching of the shrinkage ratio after subsequent sintering.

[0037] In certain preferred embodiments, in step (6), the formed green sheet is placed in a corundum mullite sagger for sintering during sintering, and the inside and outside of the corundum mullite sagger are brushed with the slurry in step (2), and the slurry is dried; a pad is placed at the bottom of the corundum mullite sagger, which is obtained by crushing and sieving the formed green sheet obtained in step (5), and its thickness is 4 to 5 mm. The pad is doped with Bi2O3 to compensate for the volatilization of bismuth under high-temperature sintering, thereby suppressing the leakage current of the product.

[0038] The technical solution of the present application and the technical effects achieved are described in detail below through more specific embodiments.

[0039] Example 1

[0040] This embodiment provides a method for preparing a zinc oxide resistor with a high-stability power frequency reference voltage, comprising the following steps:

[0041] (1) Ingredients: Ingredients are prepared according to the molar fraction of the raw materials, and the raw materials listed in Table 1 are weighed respectively. After weighing, the raw materials are mixed to obtain a mixed material;

[0042] Table 1 (unit: mol)

[0043]

[0044]

[0045] (2) Ball milling: deionized water and dispersant polyacrylamide are added to the above-mentioned mixture (wherein the amount of deionized water added is 50% of the total weight of the mixture, and the amount of polyacrylamide added is 1% of the total weight of the mixture), and the mixture is ground using a high-speed stirring ball mill (the high-speed stirring ball mill contains zirconium oxide grinding balls with a diameter of 5 mm) to obtain a slurry after ball milling. The ball milling speed of the high-speed stirring ball mill is 150 r / min, and the ball milling time is 12 h. The dried block material is passed through a 200-mesh sieve to remove coarser particles to obtain a powder with a particle size of about 75 μm. Polyvinyl alcohol is added to the powder (the amount added is 10% of the total weight of the powder).

[0046] (3) Granulation: The slurry after ball milling is dried at a temperature of 150° C. for 24 h. The dried block material is sieved through a 200-mesh sieve to remove coarser particles. The particle size of the obtained powder is about 75 μm. Polyvinyl alcohol (the amount added is 10% of the total weight of the powder) is added to the powder, and the mixture is stirred and mixed to obtain a mixed granular material.

[0047] (4) Forming: The granular material obtained in the previous step is pressed into tablets using a tablet press, and the tablet pressing pressure is 8 MPa / cm 2 The tableting time is 3 min, and the obtained tablet has a density of 3.2 ± 0.05 g / cm 3 ;

[0048] (5) High resistance layer coating: coating a composite high resistance layer of a special formula Zn-Bi-Sb-Si-Mn-Ni-Li system on the surface of the formed green sheet;

[0049] (6) Debinding: Use a stainless steel screen to hold the formed blanks, keep a distance of 2 to 3 mm between the blanks, and place them in a single layer for debinding;

[0050] (7) Sintering: The molded green sheet after debinding is placed in a corundum mullite sagger for sintering. The inside and outside of the corundum mullite sagger are brushed with the slurry in step (2), and the slurry is dried; a pad is placed at the bottom of the corundum mullite sagger, which is obtained by crushing and sieving the molded green sheet obtained in step (5), and its thickness is 4-5 mm. The pad is doped with 50g Bi2O3; the whole sintering time is 12h, and the sintered resistor is obtained. The specific change of sintering temperature with time is shown in Table 2 below:

[0051] Table 2

[0052]

[0053] (8) Heat treatment: The resistor obtained in step (7) is placed in a heat treatment furnace for heat treatment at a temperature of 600 to 620° C. for 3 hours, and then cooled to room temperature at a cooling rate of 15 to 25° C. to obtain a resistor after heat treatment;

[0054] (9) Spraying aluminum electrode and glazing: The resistor obtained in step (8) is sprayed with a 100 μm thick aluminum electrode by plasma spraying, and a glass glaze is coated on the side of the resistor as a side insulating layer with a thickness of 0.5 mm, and finally a finished zinc oxide resistor A with a high-stability power frequency reference voltage is obtained.

[0055] Example 2

[0056] This embodiment provides a method for preparing a zinc oxide resistor with a high-stability power frequency reference voltage, comprising the following steps:

[0057] (1) Ingredients: Ingredients are prepared according to the molar fraction of the raw materials, and the raw materials listed in Table 3 are weighed respectively. After weighing, the raw materials are mixed to obtain a mixed material;

[0058] Table 3 (unit: mol)

[0059]

[0060] (2) Ball milling: deionized water and dispersant polyacrylamide are added to the above-mentioned mixture (wherein the amount of deionized water added is 50% of the total weight of the mixture, and the amount of polyacrylamide added is 1% of the total weight of the mixture), and the mixture is ground using a high-speed stirring ball mill (the high-speed stirring ball mill contains zirconium oxide grinding balls with a diameter of 5 mm) to obtain a slurry after ball milling. The ball milling speed of the high-speed stirring ball mill is 150 r / min, and the ball milling time is 12 h. The dried block material is passed through a 200-mesh sieve to remove coarser particles to obtain a powder with a particle size of about 75 μm. Polyvinyl alcohol is added to the powder (the amount added is 10% of the total weight of the powder).

[0061] (3) Granulation: The slurry after ball milling is dried at a temperature of 150° C. for 24 h. The dried block material is sieved through a 200-mesh sieve to remove coarser particles. The particle size of the obtained powder is about 75 μm. Polyvinyl alcohol (the amount added is 10% of the total weight of the powder) is added to the powder, and the mixture is stirred and mixed to obtain a mixed granular material.

[0062] (4) Forming: The granular material obtained in the previous step is pressed into tablets using a tablet press, and the tablet pressing pressure is 8 MPa / cm 2 The tableting time is 3 min, and the obtained tablet has a density of 3.2 ± 0.05 g / cm 3 ;

[0063] (5) High resistance layer coating: coating a composite high resistance layer of a special formula Zn-Bi-Sb-Si-Mn-Ni-Li system on the surface of the formed green sheet;

[0064] (6) Debinding: Use a stainless steel screen to hold the formed blanks, keep a distance of 2 to 3 mm between the blanks, and place them in a single layer for debinding;

[0065] (7) Sintering: The molded green sheet after debinding is placed in a corundum mullite sagger for sintering. The inside and outside of the corundum mullite sagger are brushed with the slurry in step (2), and the slurry is dried; a pad is placed at the bottom of the corundum mullite sagger, which is obtained by crushing and sieving the molded green sheet obtained in step (5), and its thickness is 4-5 mm. The pad is doped with 50g Bi2O3; the whole sintering time is 12h, and the sintered resistor is obtained. The specific change of sintering temperature with time is shown in Table 4 below:

[0066] Table 4

[0067]

[0068]

[0069] (8) Heat treatment: The resistor obtained in step (7) is placed in a heat treatment furnace for heat treatment at a temperature of 600 to 620° C. for 3 hours, and then cooled to room temperature at a cooling rate of 15 to 25° C. to obtain a resistor after heat treatment;

[0070] (9) Spraying aluminum electrode and glazing: The resistor obtained in step (8) is sprayed with a 100 μm thick aluminum electrode by plasma spraying, and a glass glaze is coated on the side of the resistor as a side insulating layer with a thickness of 0.5 mm, and finally a zinc oxide resistor product B with a high-stability power frequency reference voltage is obtained.

[0071] Example 3

[0072] This embodiment provides a method for preparing a zinc oxide resistor with a high-stability power frequency reference voltage, comprising the following steps:

[0073] (1) Ingredients: Ingredients are prepared according to the molar fractions of the raw materials, and the raw materials listed in Table 5 are weighed respectively. After weighing, the raw materials are mixed to obtain a mixed material;

[0074] Table 5 (unit: mol)

[0075]

[0076] (2) Ball milling: deionized water and dispersant polyacrylamide are added to the above-mentioned mixture (wherein the amount of deionized water added is 50% of the total weight of the mixture, and the amount of polyacrylamide added is 1% of the total weight of the mixture), and the mixture is ground using a high-speed stirring ball mill (the high-speed stirring ball mill contains zirconium oxide grinding balls with a diameter of 5 mm) to obtain a slurry after ball milling. The ball milling speed of the high-speed stirring ball mill is 150 r / min, and the ball milling time is 12 h. The dried block material is passed through a 200-mesh sieve to remove coarser particles to obtain a powder with a particle size of about 75 μm. Polyvinyl alcohol is added to the powder (the amount added is 10% of the total weight of the powder).

[0077] (3) Granulation: The slurry after ball milling is dried at a temperature of 150° C. for 24 h. The dried block material is sieved through a 200-mesh sieve to remove coarser particles. The particle size of the obtained powder is about 75 μm. Polyvinyl alcohol (the amount added is 10% of the total weight of the powder) is added to the powder, and the mixture is stirred and mixed to obtain a mixed granular material.

[0078] (4) Forming: The granular material obtained in the previous step is pressed into tablets using a tablet press, and the tablet pressing pressure is 8 MPa / cm 2 The tableting time is 3 min, and the obtained tablet has a density of 3.2 ± 0.05 g / cm 3 ;

[0079] (5) High resistance layer coating: coating a composite high resistance layer of a special formula Zn-Bi-Sb-Si-Mn-Ni-Li system on the surface of the formed green sheet;

[0080] (6) Debinding: Use a stainless steel screen to hold the formed blanks, keep a distance of 2 to 3 mm between the blanks, and place them in a single layer for debinding;

[0081] (7) Sintering: The molded green sheet after debinding is placed in a corundum mullite sagger for sintering. The inside and outside of the corundum mullite sagger are brushed with the slurry in step (2), and the slurry is dried; a pad is placed at the bottom of the corundum mullite sagger, which is obtained by crushing and sieving the molded green sheet obtained in step (5), and its thickness is 4-5 mm. The pad is doped with 50g Bi2O3; the whole sintering time is 12h, and the sintered resistor is obtained. The specific change of sintering temperature with time is shown in Table 6 below:

[0082] Table 6

[0083]

[0084] (8) Heat treatment: The resistor obtained in step (7) is placed in a heat treatment furnace for heat treatment at a temperature of 600 to 620° C. for 3 hours, and then cooled to room temperature at a cooling rate of 15 to 25° C. to obtain a resistor after heat treatment;

[0085] (9) Spraying aluminum electrode and glazing: The resistor obtained in step (8) is sprayed with a 100 μm thick aluminum electrode by plasma spraying, and a glass glaze is coated on the side of the resistor as a side insulating layer with a thickness of 0.5 mm. Finally, a finished zinc oxide resistor C with a high-stability power frequency reference voltage is obtained.

[0086] Comparative Example 1

[0087] This comparative example provides a method for preparing a zinc oxide resistor, comprising the following steps:

[0088] (1) Ingredients: Ingredients are prepared according to the molar fraction of the raw materials. The raw materials listed in Table 7 are weighed respectively. After weighing, the raw materials are mixed to obtain a mixed material;

[0089] Table 7 (unit: mol)

[0090]

[0091] (2) Ball milling: deionized water and dispersant polyacrylamide are added to the above-mentioned mixture (wherein the amount of deionized water added is 50% of the total weight of the mixture, and the amount of polyacrylamide added is 1% of the total weight of the mixture), and the mixture is ground using a high-speed stirring ball mill (the high-speed stirring ball mill contains zirconium oxide grinding balls with a diameter of 5 mm) to obtain a slurry after ball milling. The ball milling speed of the high-speed stirring ball mill is 150 r / min, and the ball milling time is 12 h. The dried block material is passed through a 200-mesh sieve to remove coarser particles to obtain a powder with a particle size of about 75 μm. Polyvinyl alcohol is added to the powder (the amount added is 10% of the total weight of the powder).

[0092] (3) Granulation: The slurry after ball milling is dried at a temperature of 150° C. for 24 h. The dried block material is sieved through a 200-mesh sieve to remove coarser particles. The particle size of the obtained powder is about 75 μm. Polyvinyl alcohol (the amount added is 10% of the total weight of the powder) is added to the powder, and the mixture is stirred and mixed to obtain a mixed granular material.

[0093] (4) Forming: The granular material obtained in the previous step is pressed into tablets using a tablet press, and the tablet pressing pressure is 8 MPa / cm 2 The tableting time is 3 min, and the obtained tablet has a density of 3.2 ± 0.05 g / cm 3 ;

[0094] (5) High resistance layer coating: coating a composite high resistance layer of a special formula Zn-Bi-Sb-Si-Mn-Ni-Li system on the surface of the formed green sheet;

[0095] (6) Debinding: Use a stainless steel screen to hold the formed blanks, keep a distance of 2 to 3 mm between the blanks, and place them in a single layer for debinding;

[0096] (7) Sintering: The molded green sheet after debinding is placed in a corundum mullite sagger for sintering. The inside and outside of the corundum mullite sagger are brushed with the slurry in step (2), and the slurry is dried; a pad is placed at the bottom of the corundum mullite sagger, which is obtained by crushing and sieving the molded green sheet obtained in step (5), and its thickness is 4-5 mm. The pad is doped with 50g Bi2O3; the whole sintering time is 12h, and the sintered resistor is obtained. The specific change of sintering temperature with time is shown in Table 8 below:

[0097] Table 8

[0098]

[0099] (8) Heat treatment: The resistor obtained in step (7) is placed in a heat treatment furnace for heat treatment at a temperature of 600 to 620° C. for 3 hours, and then cooled to room temperature at a cooling rate of 15 to 25° C. to obtain a resistor after heat treatment;

[0100] (9) Spraying aluminum electrode and glazing: The resistor obtained in step (8) is sprayed with a 100 μm thick aluminum electrode by plasma spraying, and a glass glaze is coated on the side of the resistor as a side insulating layer with a thickness of 0.5 mm to finally obtain a zinc oxide resistor product D.

[0101] Comparative Example 2

[0102] This comparative example provides a method for preparing a zinc oxide resistor, comprising the following steps:

[0103] (1) Ingredients: Ingredients are prepared according to the molar fractions of the raw materials. The raw materials listed in Table 9 are weighed respectively. After weighing, the raw materials are mixed to obtain a mixed material;

[0104] Table 9 (unit: mol)

[0105]

[0106] (2) Ball milling: deionized water and dispersant polyacrylamide are added to the above-mentioned mixture (wherein the amount of deionized water added is 50% of the total weight of the mixture, and the amount of polyacrylamide added is 1% of the total weight of the mixture), and the mixture is ground using a high-speed stirring ball mill (the high-speed stirring ball mill contains zirconium oxide grinding balls with a diameter of 5 mm) to obtain a slurry after ball milling. The ball milling speed of the high-speed stirring ball mill is 150 r / min, and the ball milling time is 12 h. The dried block material is passed through a 200-mesh sieve to remove coarser particles to obtain a powder with a particle size of about 75 μm. Polyvinyl alcohol is added to the powder (the amount added is 10% of the total weight of the powder).

[0107] (3) Granulation: The slurry after ball milling is dried at a temperature of 150° C. for 24 h. The dried block material is sieved through a 200-mesh sieve to remove coarser particles. The particle size of the obtained powder is about 75 μm. Polyvinyl alcohol (the amount added is 10% of the total weight of the powder) is added to the powder, and the mixture is stirred and mixed to obtain a mixed granular material.

[0108] (4) Forming: The granular material obtained in the previous step is pressed into tablets using a tablet press, and the tablet pressing pressure is 8 MPa / cm 2 The tableting time is 3 min, and the obtained tablet has a density of 3.2 ± 0.05 g / cm 3 ;

[0109] (5) High resistance layer coating: coating a composite high resistance layer of a special formula Zn-Bi-Sb-Si-Mn-Ni-Li system on the surface of the formed green sheet;

[0110] (6) Debinding: Use a stainless steel screen to hold the formed blanks, keep a distance of 2 to 3 mm between the blanks, and place them in a single layer for debinding;

[0111] (7) Sintering: The molded green sheet after debinding is placed in a corundum mullite sagger for sintering. The inside and outside of the corundum mullite sagger are brushed with the slurry in step (2), and the slurry is dried; a pad is placed at the bottom of the corundum mullite sagger, which is obtained by crushing and sieving the molded green sheet obtained in step (5), and its thickness is 4-5 mm. The pad is doped with 50g Bi2O3; the whole sintering time is 12h, and the sintered resistor is obtained. The specific change of sintering temperature with time is shown in Table 10 below:

[0112] Table 10

[0113]

[0114] (8) Spraying aluminum electrode and glazing: The resistor obtained in step (7) is sprayed with a 100 μm thick aluminum electrode by plasma spraying, and a glass glaze is coated on the side of the resistor as a side insulating layer with a thickness of 0.5 mm to finally obtain a zinc oxide resistor product E.

[0115] Comparative Example 3

[0116] This comparative example provides a method for preparing a zinc oxide resistor, comprising the following steps:

[0117] (1) Ingredients: Ingredients are prepared according to the molar fraction of the raw materials, and the raw materials listed in Table 11 are weighed respectively. After weighing, the raw materials are mixed to obtain a mixed material;

[0118] Table 11 (Unit: mol)

[0119]

[0120] (2) Ball milling: deionized water and dispersant polyacrylamide are added to the above-mentioned mixture (wherein the amount of deionized water added is 50% of the total weight of the mixture, and the amount of polyacrylamide added is 1% of the total weight of the mixture), and the mixture is ground using a high-speed stirring ball mill (the high-speed stirring ball mill contains zirconium oxide grinding balls with a diameter of 5 mm) to obtain a slurry after ball milling. The ball milling speed of the high-speed stirring ball mill is 150 r / min, and the ball milling time is 12 h. The dried block material is passed through a 200-mesh sieve to remove coarser particles to obtain a powder with a particle size of about 75 μm. Polyvinyl alcohol is added to the powder (the amount added is 10% of the total weight of the powder).

[0121] (3) Granulation: The slurry after ball milling is dried at a temperature of 150° C. for 24 h. The dried block material is sieved through a 200-mesh sieve to remove coarser particles. The particle size of the obtained powder is about 75 μm. Polyvinyl alcohol (the amount added is 10% of the total weight of the powder) is added to the powder, and the mixture is stirred and mixed to obtain a mixed granular material.

[0122] (4) Forming: The granular material obtained in the previous step is pressed into tablets using a tablet press, and the tablet pressing pressure is 8 MPa / cm 2 The tableting time is 3 min, and the obtained tablet has a density of 3.2 ± 0.05 g / cm 3 ;

[0123] (5) High resistance layer coating: coating a composite high resistance layer of a special formula Zn-Bi-Sb-Si-Mn-Ni-Li system on the surface of the formed green sheet;

[0124] (6) Debinding: Use a stainless steel screen to hold the formed blanks, keep a distance of 2 to 3 mm between the blanks, and place them in a single layer for debinding;

[0125] (7) Sintering: The molded green sheet after debinding is placed in a corundum mullite sagger for sintering. The inside and outside of the corundum mullite sagger are brushed with the slurry in step (2), and the slurry is dried; a pad is placed at the bottom of the corundum mullite sagger, which is obtained by crushing and sieving the molded green sheet obtained in step (5), and its thickness is 4-5 mm. The pad is doped with 50g Bi2O3; the whole sintering time is 12h, and the sintered resistor is obtained. The specific change of sintering temperature with time is shown in Table 12 below:

[0126] Table 12

[0127]

[0128] (8) Spraying aluminum electrode and glazing: The resistor obtained in step (7) is sprayed with a 100 μm thick aluminum electrode by plasma spraying, and a glass glaze is coated on the side of the resistor as a side insulating layer with a thickness of 0.5 mm to finally obtain a finished zinc oxide resistor F.

[0129] The zinc oxide resistors A, B, C, D, E, and F prepared in the above embodiments and comparative examples are all cylindrical resistors with a diameter of 34 mm and a thickness of 24 mm. Referring to the test method in the standard GB / T 11032-2020 AC gapless metal oxide arrester, the zinc oxide resistors A, B, C, D, E, and F are subjected to 65KA and 100KA high current impact tests respectively, and the power frequency reference voltages before and after the current impact are recorded. The rate of change of the power frequency reference voltage of each zinc oxide resistor after the high current impact is calculated to measure the stability of the power frequency reference voltage of each zinc oxide resistor. The calculation formula is:

[0130] Change rate = (power frequency reference voltage after impact - power frequency reference voltage before impact) / power frequency reference voltage after impact × 100% The test results are shown in Table 13 below.

[0131] Table 13

[0132]

[0133] From the results in Table 13, it can be seen that the power frequency reference voltage change rate of the zinc oxide resistors A, B, and C prepared in Examples 1 to 3 after being subjected to large current shocks of 65KA and 100KA is lower than that of the comparative example, indicating that the power frequency reference voltage stability of the zinc oxide resistors A, B, and C prepared in the examples is high.

[0134] In the results of Table 13 above, the zinc oxide resistor A prepared in Example 1 has the lowest power frequency reference voltage change rate and the highest stability. The zinc oxide resistor D prepared in Comparative Example 1 has the same preparation process as Example 1, but its formula components lack MgO and AgNO3 compared with Example 1, and are replaced by Ni2O3 and TiO2 respectively. After being subjected to high current shocks of 65KA and 100KA, it finally shows a higher power frequency reference voltage change rate.

[0135] Compared with Example 1, the zinc oxide resistor E prepared in Comparative Example 2 has the same formula components, but lacks the last step of heat treatment process in the preparation process. Compared with Example 1, the final resistor product has a larger rate of change of the power frequency reference voltage after being subjected to large current shocks of 65KA and 100KA, indicating that heat treatment promotes the stability of the power frequency reference voltage of the zinc oxide resistor.

[0136] The zinc oxide resistor F prepared in Comparative Example 3 lacks MgO and AgNO3 in the composition formula compared with Example 1, and is replaced by Ni2O3 and TiO2 respectively. At the same time, the final heat treatment process is omitted in the preparation process. Therefore, the power frequency reference voltage change rate of the zinc oxide resistor F after the high current impact of 65KA and 100KA is the highest, indicating that the power frequency reference voltage stability of the zinc oxide resistor F is the worst.

[0137] In summary, the composition formula and the heat treatment process in the preparation process have a decisive influence on the stability of the power frequency reference voltage of the final zinc oxide resistor product. In the technical solution provided in the embodiment of the present application, the traditional formula is optimized, MgO and AgNO3 are added, and a special heat treatment process is added to the preparation process. Through the superposition of these two, the stability of the power frequency reference voltage of the prepared zinc oxide resistor is ultimately greatly improved.

[0138] The present application is described in detail above. Specific examples are used in this article to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the present application and its core ideas. It should be pointed out that for ordinary technicians in this technical field, without departing from the principles of the present application, several improvements and modifications can be made to the present application, and these improvements and modifications also fall within the scope of protection of the claims of the present application.

Claims

1. A zinc oxide resistor with high stability power frequency reference voltage, characterized in that: The following components are included in molar proportions: ZnO: 93.4~96.8 parts, Bi2O3: 0.822~0.897 parts, Co2O3: 0.807~0.866 parts, Cr2O3: 0.09~0.16 parts, MnCO3: 0.49~0.59 parts, Ni2O3: 0.26~0.34 parts, MgO: 0.62~0.98 parts, AgNO3: 0.072~0.12 parts, GF-86 silver glass powder: 0.042~0.69 parts, Al(NO3)3·9H2O: 0.0032~0.0049 parts, H3BO3: 0.51~0.68 parts, BaCO3: 0.24~0.39 parts.

2. The zinc oxide resistor with high stability power frequency reference voltage according to claim 1, characterized in that: The following components are included in mole fractions: ZnO: 95.2 parts, Bi2O3: 0.85 parts, Co2O3: 0.83 parts, Cr2O3: 0.14 parts, MnCO3: 0.5 parts, Ni2O3: 0.3 parts, MgO: 0.8 parts, AgNO3: 0.1 parts, GF-86 silver glass powder: 0.35 parts, Al(NO3)3·9H2O: 0.004 parts, H3BO3: 0.6 parts, BaCO3: 0.325 parts.

3. The method for preparing the zinc oxide resistor with high stability power frequency reference voltage according to claim 1, characterized in that: The following steps are involved: Weigh the raw materials according to the molar fractions in claim 1 and mix them evenly to obtain a mixed material; preparing the mixed material into a slurry; Drying to obtain dry powder; The dried powder is granulated and then pressed, debonded and sintered to obtain a sintered resistor. The sintered resistor is subjected to heat treatment to obtain a heat-treated resistor; The heat-treated resistor is post-processed to obtain the aforementioned zinc oxide resistor.

4. The preparation method according to claim 3, characterized in that: The process of preparing the slurry is as follows: adding a dispersant and deionized water to the mixed material for ball milling to prepare the slurry, wherein the dispersant is polyacrylamide or tetradecyl acetate amine; the ball milling speed is 100-200 r / min, and the ball milling time is 12-24 hours.

5. The preparation method according to claim 3, characterized in that: The drying temperature is 120-150° C., and the drying time is 24-36 hours. The average particle size of the obtained powder is 75 μm.

6. The preparation method according to claim 3, characterized in that: A binder is added during the granulation process, wherein the binder is polyvinyl alcohol, and the particle size of the particles obtained by the granulation is 80 to 110 μm.

7. The preparation method according to claim 3, characterized in that: During the compression molding process, the density of the obtained molded green sheet is controlled at (3.2±0.05) g / cm 3 .

8. The preparation method according to claim 3, characterized in that: Before the debinding process, a high resistance layer coating process is also included, that is, a composite high resistance layer of Zn-Bi-Sb-Si-Mn-Ni-Li system is coated on the surface of the formed green sheet.

9. The preparation method according to claim 3, characterized in that: The sintering process comprises: placing the formed green sheet in a corundum mullite sagger for sintering, brushing the slurry on the inside and outside of the corundum mullite sagger, and drying the slurry; placing a pad at the bottom of the corundum mullite sagger, the pad is obtained by crushing and sieving the formed green sheet, the thickness is 4 to 5 mm, and the pad is doped with Bi2O3.

10. The preparation method according to claim 3, characterized in that: The heat treatment process is as follows: placing the obtained sintered resistor into a heat treatment furnace, the heat treatment temperature is 600-620°C, the heat treatment time is 3 hours, cooling to room temperature, and the cooling rate is controlled at 15-25°C to obtain the resistor after heat treatment.

Citation Information

Patent Citations

  • Preparation method of nonlinear resistance piece for miniaturization GIS lightning arrestor

    CN101140821A

  • Chip multi-layer ZnO piezoresistor ceramic powder

    CN106554200A

  • Method for improving through-current capability of zinc oxide piezoresistor by regulating and controlling bismuth oxide crystal form, zinc oxide resistor disc and preparation method for zinc oxide resistor disc

    CN111362689A

  • Zinc oxide nonlinear resistor disc and preparation method thereof

    CN112694324A

  • Manufacturing method of zinc oxide resistor disc with high through-flow density

    CN114400121A