Surface acoustic wave enhanced Ga2O3 solar blind ultraviolet detector and preparation method thereof
By using ε-Ga2O3 as the piezoelectric semiconductor layer and active layer in Ga2O3 daily blind UV detector, and generating surface acoustic waves through the design of interdigit transducer, the problems of low responsiveness and process complexity of traditional detectors are solved. , realizes a high-performance and low-cost Ga2O3 daily blind ultraviolet photodetector.
Patent Information
- Application Number
- CN202411192367.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
AI Technical Summary
Traditional MSM-type ultraviolet detectors have problems with low responsiveness and low detection rate in weak signal detection, and the material selection of existing surface acoustic wave-enhanced detectors leads to cumbersome process steps and performance degradation.
ε-Ga2O3 is used as the piezoelectric semiconductor layer and active layer, and surface acoustic waves are generated through the interdigit transducer design, which regulates the Ga2O3 energy band and suppresses carrier recombination, thereby improving the detector performance.
It improves the performance of Ga2O3 daily blind ultraviolet photodetector, reduces process complexity and production cost, and has high sensitivity and wide application potential.
Smart Images

Figure CN119092582A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of optoelectronic devices, and in particular relates to a surface acoustic wave-enhanced Ga2O3 solar-blind ultraviolet detector and a preparation method thereof. Background Art
[0002] In recent years, solar-blind UV detectors have been used in many fields due to their weak background interference and low warning rate. Metal-semiconductor-metal (MSM) photoconductive UV detectors have the advantages of simple structure and easy manufacturing, which make them potential for the preparation of large-scale detector arrays. However, traditional MSM detectors face the problems of low responsivity and low detection rate, which seriously hinder their application in weak signal detection. Surface acoustic waves (SAW) can periodically modulate the energy band of semiconductors, promote the separation of photogenerated carriers, and suppress the recombination of electrons and holes, thereby improving the performance of photodetectors.
[0003] CN113725314A applied by Beijing University of Posts and Telecommunications in 2021 proposed a surface acoustic wave enhanced deep ultraviolet detector and its preparation method, including a lithium niobate piezoelectric substrate, a semiconductor film and two pairs of ohmic electrodes placed on the surface of the semiconductor film and the substrate stacked in sequence, and the scheme is to use one of the two pairs of electrodes to receive and propagate surface acoustic waves to modulate the band structure of the film and the substrate to increase the number of photogenerated carriers and transmission efficiency. However, it is achieved by using one material as a piezoelectric substrate and another material as an active layer, which increases the difficulty of preparation and makes the process steps cumbersome and time-consuming.
[0004] ACS Nano 2023 (17), 24033-24041, published by Beijing University of Posts and Telecommunications in 2023, prepared a gallium oxide solar-blind ultraviolet detector enhanced by acoustic-photoelectric coupling, including a lithium niobate piezoelectric substrate, an α-Ga2O3 active layer, and metal electrodes on the substrate and the active layer arranged from bottom to top. It uses surface acoustic waves to achieve periodic modulation of the gallium oxide energy band, suppressing carrier recombination, thereby enhancing the detector performance. However, the lattice mismatch between Ga2O3 and lithium niobate usually introduces defects and interfaces that are not conducive to light detection, reducing device performance.
[0005] Traditional piezoelectric substrate materials used include AlN and ZnO. ZnO has a high piezoelectric coefficient (12.4pm / V), but a band gap of 3.37eV, which will cause serious losses in sound wave propagation, and the band gap width is not wide enough for use in day-blind ultraviolet detection. Although AlN has a wider band gap (6.2eV), a wide band gap will also lead to stronger chemical bonds between atoms, making the material's elastic constant and hardness higher, so the piezoelectric constant is relatively small (5pm / V). Summary of the invention
[0006] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a surface acoustic wave enhanced Ga2O3 day-blind ultraviolet detector and a preparation method thereof, deeply couple the surface acoustic wave with the detector photoelectric mechanism, generate surface acoustic waves through the physical mechanism of sound-light-electricity and by optimizing the design of the interdigital transducer, effectively regulate the Ga2O3 energy band and suppress carrier recombination, thereby achieving the improvement of the performance of the Ga2O3 detector, thereby promoting the development of high-performance Ga2O3 day-blind ultraviolet photoelectric detectors.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is:
[0008] A surface acoustic wave enhanced Ga2O3 day-blind ultraviolet detector, comprising a substrate, a piezoelectric semiconductor layer, a metal electrode and an interdigital transducer, wherein the piezoelectric semiconductor layer is arranged on the surface of the substrate; the metal electrode and the interdigital transducer are arranged on the surface of the piezoelectric semiconductor layer;
[0009] The interdigital transducer is used as the input end of the SAW to generate surface acoustic waves; the metal electrode is used as the electrode of the detector to collect carriers.
[0010] The piezoelectric semiconductor layer adopts ε-Ga2O3 material.
[0011] The metal electrode and the IDT are respectively placed on both sides of the surface of the piezoelectric semiconductor layer. The IDT and the metal electrode are parallel, and the distance between them is l.
[0012] The interdigital transducer and metal electrodes form a parallel structure from left to right. The width of a single electrode of the interdigital transducer is w, and they are arranged with a period p on the piezoelectric semiconductor layer to generate Rayleigh waves. The period p is the center distance between adjacent interdigital electrodes. There is no specific restriction on the width and period of the metal electrode, which are adjusted according to actual conditions.
[0013] The interdigital transducer adopts a metal Ti / Al laminated structure; the metal electrode is selected from one of Ti / Au laminated metal, Ti / Ni / Au laminated metal, and Ti / Al / Ni / Au laminated metal;
[0014] The substrate is made of Al2O3 material, and the piezoelectric semiconductor layer is made of ε-Ga2O3 material.
[0015] The interdigital transducer is arranged in the shape of interdigital electrodes; the metal electrodes are arranged in the shape of interdigital fingers and pads.
[0016] The SAW generated by applying electricity to the IDT propagates along the two ends of the piezoelectric semiconductor surface; the input signal of the IDT is a positive voltage applied to one end of the IDT electrode and a negative voltage applied to the other end of the IDT electrode, which is an AC signal, and its parameters such as frequency and amplitude are adjusted according to actual needs;
[0017] The metal electrode is used as the electrode of the detector to collect carriers. It can be an interdigital structure or a pad structure, and there is no specific shape or structure restriction.
[0018] When an AC voltage signal is applied to the IDT, the surface of the piezoelectric semiconductor layer vibrates and excites surface acoustic waves with the same frequency as the external signal. The piezoelectric field formed by the surface acoustic wave periodically modulates the energy band of Ga2O3 to form a ratchet-shaped energy band. When irradiated with ultraviolet light, the generated photogenerated carriers are effectively separated, thereby suppressing the recombination of photogenerated carriers, and more carriers are collected by the metal electrodes of the detector.
[0019] When the interdigital transducer is powered, the inverse piezoelectric effect converts the input electrical signal into an acoustic signal, generating a surface acoustic wave (SAW) that propagates along the surface of the piezoelectric semiconductor layer and localizes the energy on the surface. The metal electrode is used as the electrode of the detector part to collect photogenerated carriers, and the interdigital shape is used to increase the carrier collection efficiency.
[0020] The piezoelectric field generated by surface acoustic waves is used to periodically regulate the energy band of Ga2O3, promote the separation of photogenerated carriers and suppress the recombination of electrons and holes, thereby improving the performance of the detector.
[0021] The piezoelectric field formed by the surface acoustic wave (SAW) generated by the interdigital transducer periodically modulates the energy band of Ga2O3, and the ratchet-shaped conduction band (E c ) and valence band (E v ) effectively promotes the separation of photogenerated carriers and shifts their equilibrium positions. The spatial separation reduces the overlap of electron wave functions and hole wave functions, thereby suppressing their recombination and enhancing the photoresponse of the detector.
[0022] A method for preparing a surface acoustic wave enhanced Ga2O3 solar-blind ultraviolet detector comprises the following steps:
[0023] Step 1): using a metal organic chemical vapor deposition (MOCVD) process, a layer of ε-Ga2O3 thin film is grown on a substrate to form a piezoelectric semiconductor layer;
[0024] Step 2); using electron beam lithography to form a mask layer of a metal electrode pattern on one end of the piezoelectric semiconductor layer;
[0025] Step 3): Depositing Ti / Al electrodes by magnetron sputtering process;
[0026] Step 4): using a stripping process to remove excess photoresist and metal to form a metal electrode;
[0027] Step 5): using an electron beam lithography process to form a mask layer of an IDT pattern on the other end of the piezoelectric semiconductor layer;
[0028] Step 6): Depositing Ti / Al electrodes by magnetron sputtering process;
[0029] Step 7): Using a stripping process, excess photoresist and metal are removed to form an IDT at the other end, thereby obtaining a complete metal electrode and IDT.
[0030] Beneficial effects of the present invention:
[0031] The present invention selects the performance of SAW by adjusting the geometric parameters of the interdigital transducer and ε-Ga2O3, thereby improving the performance of the device, having high flexibility and wide application. The present invention proposes a Ga2O3 solar-blind ultraviolet photodetector enhanced by surface acoustic wave, which has the following advantages:
[0032] 1) The surface acoustic wave is generated by the interdigital transducer, and the acoustic-electric effect introduced by it periodically modulates the Ga2O3 energy band to generate acoustic current;
[0033] 2) It can effectively promote the separation of photogenerated carriers;
[0034] 3) Reduce the overlap of electron wave functions and hole wave functions, inhibit their recombination, and thus enhance the performance of the detector.
[0035] The present invention realizes surface acoustic wave enhancement of the performance of the traditional Ga2O3 day-blind ultraviolet detector by using ε-Ga2O3 as both the device active layer and the piezoelectric substrate. The use of ε-Ga2O3 piezoelectric semiconductor material reduces the process complexity and reduces the production cost. Compared with surface acoustic wave enhanced detectors made of other piezoelectric materials, it has higher resonance frequency and sensitivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 It is a three-dimensional schematic diagram and a cross-sectional diagram of a surface acoustic wave enhanced Ga2O3 solar-blind ultraviolet detector of the present invention.
[0037] Figure 2 The present invention is a schematic diagram of the manufacturing process of a surface acoustic wave enhanced Ga2O3 solar-blind ultraviolet detector.
[0038] Figure 3 Energy band diagrams under illumination (a) with SAW and (b) without SAW. DETAILED DESCRIPTION
[0039] The present invention will be further described in detail below in conjunction with the accompanying drawings.
[0040] Reference Figure 1The present invention discloses a surface acoustic wave enhanced Ga2O3 day-blind ultraviolet detector, comprising: a substrate 1, a piezoelectric semiconductor layer 2, a metal electrode 3 and an interdigital transducer 4.
[0041] The thickness of the substrate 1 is 8-10 μm.
[0042] The piezoelectric semiconductor layer 2 is arranged on one side of the substrate 1 and has a thickness of 0.8-1.4 μm.
[0043] The IDT 4 and the metal electrode 3 are arranged at both ends of the piezoelectric semiconductor layer 2 to form a parallel structure from left to right, wherein the metal electrode 3 and the IDT 4 have a width of 1.2 to 1.4 μm and are arranged on the ε-Ga2O3 piezoelectric semiconductor layer with a period of 2.4 to 3.2 μm to generate Rayleigh waves.
[0044] The substrate 1 may be made of sapphire (Al2O3) or other substrate materials, such as silicon dioxide (SiO2); the piezoelectric semiconductor layer 2 may be made of ε-Ga2O3; the metal electrode 3 may be made of one of Ti / Au laminated metal, Ti / Ni / Au laminated metal, and Ti / Al / Ni / Au laminated metal;
[0045] The metal electrode 3 is arranged in the form of a fork finger or a pad on one end of the piezoelectric semiconductor layer 2 to form a detector electrode;
[0046] The interdigital transducer 4 and the metal electrode 3 are arranged in the shape of interdigital electrodes. By applying power to the interdigital transducer 4, the inverse piezoelectric effect converts the input electrical signal into an acoustic signal, thereby generating a SAW that propagates along the surface of the piezoelectric semiconductor material 2 and localizes energy on the surface. The metal electrode 3 is used as an electrode of the detector part to collect photogenerated carriers, and the interdigital shape can increase the carrier collection efficiency.
[0047] ε-Ga2O3 has a strong piezoelectric polarization effect, and its piezoelectric coefficient is d 33 =10.8~11.2pm / V, which is significantly higher than the piezoelectric coefficient of AlN (1~5pm / V). Theoretically, the electromechanical coupling coefficient of the bulk acoustic wave RF filter based on ε-Ga2O3 thin film can be 4 times that of AlN. In addition, ε-Ga2O3 is an ideal new piezoelectric semiconductor material due to its wide bandgap (4.9eV), high breakdown electric field (8MV / cm), and good thermal and chemical stability. Using it as the active layer of the detector, an interdigital transducer can be set on its surface to generate surface acoustic waves. By periodically modulating the gallium oxide energy band, the recombination of photogenerated carriers can be suppressed, thereby enhancing performance. The principle is as follows Figure 3 At the same time, the piezoelectric potential field generated by the surface acoustic wave can effectively separate the photogenerated carriers without external bias voltage and realize self-driving.
[0048] The research on the characteristics of Ga2O3 day-blind ultraviolet detector enhanced by surface acoustic wave shows that the input end interdigital transducer 4 can convert the input electrical signal into an acoustic signal through the inverse piezoelectric effect. This acoustic signal propagates along the surface of the piezoelectric semiconductor material 2, thereby generating a surface acoustic wave with energy localized on the surface.
[0049] like Figure 3 As shown, the piezoelectric field formed by the SAW generated by the interdigital transducer 4 can periodically modulate the energy band of Ga2O3 (this modulation does not cause changes in the structure or composition of the semiconductor material), and the ratchet-shaped conduction band (E c ) and valence band (E v ) can effectively promote the separation of photogenerated carriers and shift their equilibrium positions. The spatial separation reduces the overlap of electron wave functions and hole wave functions, thereby suppressing their recombination and enhancing the photoresponse of the detector.
[0050] When an AC voltage signal is applied to the IDT 4, the surface of the piezoelectric semiconductor layer 2 vibrates and excites a surface acoustic wave with the same frequency as the external signal. The piezoelectric field formed by the surface acoustic wave periodically modulates the energy band of Ga2O3 to form a ratchet-shaped energy band, such as Figure 3 As shown in the left figure, when ultraviolet light is irradiated, the photogenerated carriers generated are effectively separated, suppressing the recombination of photogenerated carriers, so that more carriers are collected by the metal electrodes of the detector.
[0051] Reference Figure 2 The present invention provides a method for making a surface acoustic wave enhanced Ga2O3 day-blind ultraviolet detector, and gives the following embodiments.
[0052] Embodiment: A surface acoustic wave enhanced Ga2O3 solar-blind ultraviolet detector is manufactured.
[0053] Reference Figure 2 , the implementation steps of this example are as follows:
[0054] Step 1: Deposition of ε-Ga2O3 layer
[0055] The metal organic chemical vapor deposition process was used, using deionized water (H2O), triethylgallium (TEGa) and pure oxygen (O2) as Ga and O sources respectively, and Ar as carrier gas;
[0056] Due to the large lattice mismatch between ε-Ga2O3 and the sapphire substrate 1, a two-step growth method is adopted: first, a nucleation layer with a thickness of about 100 nm is deposited at a temperature of about 560°C, then an epitaxial layer with a thickness of about 1100 nm is grown at a temperature of about 640°C, and finally, an ε-Ga2O3 film is grown to form a piezoelectric semiconductor layer 2, as shown in FIG. Figure 2 (a) shown.
[0057] Step 2: Photolithography of metal electrode mask
[0058] Electron beam photoresist is spin-coated on the ε-Ga2O3 piezoelectric semiconductor layer 2 and pre-baked on a hot plate. A metal electrode pattern is formed using an electron beam exposure system, which is placed in a developer for development and then placed in isopropyl alcohol for fixing to form a metal electrode pattern, such as Figure 2 (b) as shown.
[0059] Step 3: Sputtering Ti / Al layer
[0060] Using the magnetron sputtering process, the sample was placed in a magnetron sputtering reaction chamber and Ar was introduced, and the gas pressure was maintained at 20mTorr, so that a layer of Ti / Al material was grown on the ε-Ga2O3 piezoelectric semiconductor layer. The electrode growth was optimized by adjusting the RF power, such as Figure 2 (c) as shown.
[0061] Step 4: Forming Metal Electrodes
[0062] The sample after the metal layer is sputtered is immersed in an acetone solution and allowed to stand for 4 hours, and then placed in an isopropanol solution for cleaning for 1 minute to form a Ti / Al metal electrode 3, as shown in FIG. Figure 2 (d) as shown.
[0063] Step 5: Photolithography of IDT mask
[0064] Spin-coat the ε-Ga2O3 piezoelectric semiconductor layer with electron beam photoresist and pre-bake it on a hot plate. Use an electron beam exposure system to overlay to form an IDT pattern, place it in a developer for development, and then place it in isopropyl alcohol for fixing to form an IDT pattern, such as Figure 2 (e) as shown.
[0065] Step 6: Sputtering Ti / Al layer
[0066] Using the magnetron sputtering process, the sample was placed in a magnetron sputtering reaction chamber and Ar was introduced. The gas pressure was maintained at 20mTorr and the sputtering power was 30 to 80W, so that a layer of Ti / Al material was grown on the ε-Ga2O3 piezoelectric semiconductor layer. The electrode growth was optimized by adjusting the RF power, such as Figure 2 (f) as shown.
[0067] Step 7: Forming the IDT
[0068] The sample after the metal layer is sputtered is immersed in an acetone solution and allowed to stand for 4 hours, and then placed in an isopropanol solution for cleaning for 1 minute to form an IDT 4, thereby obtaining a complete metal electrode 3 and an IDT 4. Figure 2 (g) as shown.
[0069] The etching process may be one of ion beam etching, reactive ion etching (RIE), inductively coupled plasma etching (ICP), and capacitively coupled plasma etching (CCP);
[0070] The electrode manufacturing process can adopt one of magnetron sputtering and electron beam evaporation.
[0071] The above are only several preferred embodiments of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A surface acoustic wave enhanced Ga2O3 solar-blind ultraviolet detector, characterized in that: It comprises a substrate (1), a piezoelectric semiconductor layer (2), a metal electrode (3) and an interdigital transducer (4), wherein the piezoelectric semiconductor layer (2) is arranged on the surface of the substrate (1); the metal electrode (3) and the interdigital transducer (4) are arranged on the surface of the piezoelectric semiconductor layer (2); The interdigital transducer (4) serves as an input end of a surface acoustic wave (SAW) to generate a surface acoustic wave; the metal electrode (3) serves as an electrode of a detector to collect carriers; The piezoelectric semiconductor layer (2) is made of ε-Ga2O3 material.
2. The surface acoustic wave enhanced Ga2O3 solar-blind ultraviolet detector according to claim 1, characterized in that: The metal electrode (3) and the interdigital transducer (4) are respectively placed on both sides of the surface of the piezoelectric semiconductor layer (2); the interdigital transducer (4) and the metal electrode (3) are parallel, and the distance between them is l.
3. The surface acoustic wave enhanced Ga2O3 solar-blind ultraviolet detector according to claim 1, characterized in that: The width of a single electrode of the interdigital transducer (4) is w, and they are arranged with a period p on the piezoelectric semiconductor layer (2) to generate Rayleigh waves, where the period p is the distance between the centers of adjacent interdigital electrodes.
4. The surface acoustic wave enhanced Ga2O3 solar-blind ultraviolet detector according to claim 1, characterized in that: The interdigital transducer (4) adopts a metal Ti / Al laminated structure; the metal electrode (3) is selected from one of Ti / Au laminated metal, Ti / Ni / Au laminated metal, and Ti / Al / Ni / Au laminated metal; and the substrate (1) is made of Al2O3 material.
5. The surface acoustic wave enhanced Ga2O3 solar-blind ultraviolet detector according to claim 1, characterized in that: The interdigital transducer (4) is arranged in the shape of an interdigital electrode; and the metal electrode (3) is arranged in the shape of an interdigital pad.
6. The surface acoustic wave enhanced Ga2O3 solar-blind ultraviolet detector according to claim 5, characterized in that: The SAW generated by applying electricity to the interdigital transducer (4) propagates along the two ends of the surface of the piezoelectric semiconductor (2); the input signal of the interdigital transducer (4) is a positive voltage applied to one end of the electrode of the interdigital transducer (4) and a negative voltage applied to the other end of the electrode, which is an AC signal.
7. The surface acoustic wave enhanced Ga2O3 solar-blind ultraviolet detector according to claim 5, characterized in that: The metal electrode (3) is used as an electrode of the detector to collect carriers and has an interdigital structure or a Pad structure.
8. The surface acoustic wave enhanced Ga2O3 solar-blind ultraviolet detector according to claim 5, characterized in that: When an AC voltage signal is applied to the interdigital transducer (4), the surface of the piezoelectric semiconductor layer (2) vibrates and excites a surface acoustic wave with the same frequency as the external signal. The piezoelectric field formed by the surface acoustic wave periodically modulates the energy band of Ga2O3 to form a ratchet-shaped energy band. When irradiated with ultraviolet light, the generated photogenerated carriers are effectively separated, thereby suppressing the recombination of the photogenerated carriers, and more carriers are collected by the metal electrode of the detector.
9. The surface acoustic wave enhanced Ga2O3 solar-blind ultraviolet detector according to claim 5, characterized in that: When the interdigital transducer (4) is powered, the inverse piezoelectric effect converts the input electrical signal into an acoustic signal, generating a surface acoustic wave (SAW) that propagates along the surface of the piezoelectric semiconductor layer (2) and has energy localized on the surface. The metal electrode (3) is used as an electrode of the detector part to collect photogenerated carriers, and the interdigital shape is used to increase the carrier collection efficiency.
10. The method for preparing a surface acoustic wave enhanced Ga2O3 solar-blind ultraviolet detector according to claim 1, characterized in that: The steps include: Step 1): using a metal organic chemical vapor deposition (MOCVD) process, a layer of ε-Ga2O3 thin film is grown on a substrate (1) to form a piezoelectric semiconductor layer (2); Step 2); using electron beam lithography technology, a mask layer of a metal electrode pattern is formed on one end of the piezoelectric semiconductor layer (2); Step 3): Depositing Ti / Al electrodes by magnetron sputtering process; Step 4): using a stripping process to remove excess photoresist and metal to form a metal electrode (3); Step 5): using an electron beam lithography process to form a mask layer with an IDT pattern on the other end of the piezoelectric semiconductor layer (2); Step 6): Depositing Ti / Al electrodes by magnetron sputtering process; Step 7): Using a stripping process, excess photoresist and metal are removed to form an IDT (4) at the other end, thereby obtaining a complete metal electrode (3) and IDT (4).