Positive plate and lithium ion battery
By adding acid additives to the positive electrode active layer of the positive electrode sheet, the problems of binder failure and slurry stability caused by high alkalinity of the nickel-based positive electrode material are solved, and the circulation and storage performance of lithium-ion batteries are significantly improved.
Patent Information
- Application Number
- CN202411583481.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-07
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Due to its high alkalinity, the nickel-based positive electrode material leads to failure of the binder and poor slurry stability, which affects the cycle life and rate performance of lithium-ion batteries.
Add acidic additives, such as carboxylic acids, phosphoric acids, sulfonic acids or boric acid compounds to the positive electrode active layer of the positive electrode sheet, neutralize alkaline substances on the surface of the active material, reduce alkaline reactions, and improve the circulation of lithium-ion batteries and Storage performance.
It effectively solves the problems of binder failure and slurry stability caused by strong alkalinity of nickel-based positive electrode materials, reduces gas production caused by alkaline substances in the battery, and improves the circulation and storage performance of lithium-ion batteries.
Smart Images

Figure SMS_5 
Figure SMS_6 
Figure SMS_7
Abstract
Description
Technical Field
[0001] The present invention relates to the field of lithium batteries, and in particular to a positive electrode sheet and a lithium ion battery. Background Art
[0002] With the rapid development of lithium-ion batteries, nickel-based positive electrode materials have been favored due to their higher gram capacity and have become a commonly used positive electrode material in lithium-ion batteries. However, the alkali content of nickel-based positive electrode materials is relatively high, which brings a series of process and performance challenges. First, the alkaline substances in nickel-based positive electrode materials react with commonly used positive electrode binders PVDF (polyvinylidene fluoride), carboxymethyl cellulose, polyacrylic acid, and polyimide, which will affect the viscosity of the slurry and thus affect the normal coating process. Secondly, alkaline substances such as LiOH (lithium hydroxide) and Li2CO3 (lithium carbonate) on the surface of the positive electrode material will react with the electrolyte, which will not only produce gas during the storage and circulation of the battery, but also increase the impedance of the positive electrode interface, resulting in increased polarization, which in turn affects the cycle life and rate performance of the battery. In extreme cases, these problems may even cause a significant decrease in battery capacity. Summary of the invention
[0003] The embodiments of the present invention provide a positive electrode sheet and a lithium-ion battery to solve the problem that alkaline nickel-based positive electrode materials affect the battery production process and performance.
[0004] An embodiment of the present invention provides a positive electrode sheet, comprising a positive electrode current collector and a positive electrode active layer arranged on at least one side of the positive electrode current collector, wherein the positive electrode active layer comprises a positive electrode material and an acidic additive, wherein the positive electrode material comprises an active material, a conductive agent and a binder, and the active material comprises a nickel-containing compound; the acidic additive comprises an acidic compound A and / or a compound B whose decomposition product is acidic; the compound A comprises a carboxylic acid compound, a phosphoric acid compound, a sulfonic acid compound or a boric acid compound; the compound B comprises a carboxylic anhydride compound, a phosphoric anhydride compound, a sulfuric anhydride compound or a sulfonic anhydride compound.
[0005] Optionally, the mass ratio of the acidic additive to the active material is 0.01% to 1%.
[0006] Optionally, the mass ratio of the acidic additive to the active material is 0.1% to 0.5%.
[0007] Optionally, the carboxylic acid compound includes one or more of oxalic acid, citric acid, malic acid, benzoic acid, tartaric acid, lactic acid, adipic acid and acetic acid; Alternatively, the phosphate compound includes one or more of phosphoric acid, pyrophosphoric acid and acetyl phosphate; Alternatively, the sulfonic acid compound includes one or more of sulfonic acid, 2-naphthalenesulfonic acid, methanesulfonic acid and benzenesulfonic acid; Alternatively, the boric acid compound includes one or more of tetraboric acid, metaboric acid and orthoboric acid.
[0008] Optionally, the carboxylic anhydride compound includes one or more of maleic anhydride, succinic anhydride, citraconic anhydride, nadic anhydride, phenyl maleic anhydride, methyl nadic anhydride, 2,3-pyridinedicarboxylic anhydride and 3,4-pyridinedicarboxylic anhydride; Alternatively, the phosphoric anhydride compound includes one or more of lithium hexafluorophosphate, phosphoric anhydride, 1-propyl phosphoric anhydride and 1-butyl phosphoric anhydride; Alternatively, the sulfuric anhydride compound includes vinyl sulfate; Alternatively, the sulfonic anhydride compound includes methylene methanedisulfonate.
[0009] Optionally, the nickel-containing compound includes one or more of lithium nickel cobalt manganese oxide, lithium nickel oxide, lithium nickel cobalt aluminum oxide, lithium nickel manganese oxide, lithium nickel cobalt oxide, aluminum nickel cobalt and nickel cobalt manganese.
[0010] Optionally, the molecular formula of the nickel-containing compound is , wherein M is selected from Mn and / or Al; Alternatively, the molecular formula of the nickel-containing compound is .
[0011] Optionally, the mass ratio of the conductive agent to the active material is 0.3% to 3%; And / or, the mass ratio of the binder to the active material is 0.3% to 5%.
[0012] Optionally, the conductive agent includes one or more of carbon nanotubes, carbon black and graphene; And / or, the binder includes one or more of polyvinylidene fluoride, carboxymethyl cellulose, polyacrylic acid, and polyimide.
[0013] The present invention also provides a lithium-ion battery, comprising a shell, a negative electrode sheet, a separator and a positive electrode sheet as described in any one of the above items, wherein the positive electrode sheet, the separator and one side of the negative electrode sheet are stacked or wound to form a battery core, and the battery core is arranged in the shell, and the shell is also injected with an electrolyte.
[0014] The beneficial effects of the present invention are: The present invention adds an acidic additive to the positive electrode active layer of the positive electrode sheet. On the one hand, the acidic additive reacts with the alkaline substance on the surface of the active material to eliminate the alkaline substance and avoid the alkaline substance from affecting the binder in the positive electrode active layer. Therefore, the problem of binder failure, jelly-like slurry and poor stability caused by the strong alkalinity of nickel-based positive electrode materials can be solved. On the other hand, the acidic additive neutralizes the alkaline substance on the surface of the positive electrode material, thereby reducing the gas production caused by the alkaline substance during the use of the battery cell. In addition, the acidic additive participates in the film formation on the surface of the active material, so that the lithium-ion battery obtains excellent electrical properties such as cycle and storage performance, discharge performance, etc. DETAILED DESCRIPTION
[0015] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention clearer, the present invention is further described in detail below in conjunction with embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. The present invention is further described below by embodiments.
[0016] In the prior art, the binders PVDF, carboxymethyl cellulose, polyacrylic acid, and polyimide will react with alkaline substances, affecting the viscosity of the slurry: polyvinylidene fluoride will undergo a dehydrofluorination reaction in high-temperature alkaline solution to generate carbon-carbon double bonds, which may be further oxidized into oxygen-containing groups, increasing the intermolecular forces of PVDF, resulting in a significant increase in the viscosity of the slurry, and even a jelly phenomenon; carboxymethyl cellulose may undergo a cross-linking reaction under alkaline conditions, increasing the viscosity of the slurry; the reaction of polyacrylic acid with alkali is an acid-base neutralization reaction, causing the carboxylic acid groups in the polymer molecules to be converted into ionic states, thereby affecting the viscosity of the slurry; polyimide may undergo a hydrolysis reaction under strong alkaline conditions, resulting in the degradation of the polymer chain, thereby affecting the viscosity of the slurry. Nickel-based positive electrode materials are easily reacted with carbon dioxide and moisture in the air during the manufacturing process, and will naturally form a certain amount of alkaline substances such as Li2CO3 and LiOH, which will react with the binder and electrolyte to affect the battery performance.
[0017] Based on the above problems, an embodiment of the present invention provides a positive electrode sheet, including a positive electrode current collector and a positive electrode active layer arranged on at least one side of the positive electrode current collector, the positive electrode active layer includes a positive electrode material and an acidic additive, the positive electrode material includes an active material, a conductive agent and a binder, and the active material includes a nickel-containing compound; the acidic additive includes an acidic compound A and / or a compound B whose decomposition product is acidic; the compound A includes a carboxylic acid compound, a phosphoric acid compound, a sulfonic acid compound or a boric acid compound; the compound B includes a carboxylic anhydride compound, a phosphoric anhydride compound, a sulfuric anhydride compound or a sulfonic anhydride compound.
[0018] The embodiment of the present invention adds an acidic additive to the positive active layer of the positive electrode sheet. On the one hand, the acidic additive reacts with the alkaline substances (LiOH, Li2CO3, etc.) on the surface of the active material to prevent the alkaline substances from affecting the binder in the positive active layer, thereby solving the problem of binder failure and poor stability of nickel-based positive electrode materials due to their strong alkalinity. On the other hand, the acidic additive neutralizes the alkaline substances on the surface of the positive electrode material, thereby reducing the gas production caused by the alkaline substances during the use of the battery cell. In addition, the acidic additive participates in the film formation on the surface of the active material, improves the film formation quality of the CEI film, and obtains a lithium-ion battery with excellent cycle performance, storage performance and discharge performance.
[0019] In one embodiment of the present invention, the mass ratio of the acidic additive to the active material is 0.01% to 1%. Specifically, the mass ratio of the acidic additive to the active material is any point value or a range value consisting of any two point values in 0.01%, 0.02%, 0.05%, 0.08%, 0.1%, 0.12%, 0.15%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9% or 1%. Preferably, the mass ratio of the acidic additive to the active material is 0.1% to 0.5%. If the mass ratio of the acidic additive to the positive electrode material is too low, the alkaline substances cannot be eliminated well; if the mass ratio of the acidic additive to the positive electrode material is too high, it is easy to cause a decrease in the proportion of active materials, thereby reducing the capacity of the battery, and too much acidic substances are also easy to cause the electrical performance of the battery to deteriorate.
[0020] In one embodiment of the present invention, the carboxylic acid compound includes one or more of oxalic acid, citric acid, malic acid, benzoic acid, tartaric acid, lactic acid, adipic acid and acetic acid. The phosphoric acid compound includes one or more of phosphoric acid, pyrophosphoric acid and acetylphosphoric acid. The sulfonic acid compound includes one or more of sulfonic acid, 2-naphthalenesulfonic acid, methanesulfonic acid and benzenesulfonic acid. The boric acid compound includes one or more of tetraboric acid, metaboric acid and orthoboric acid. The carboxylic anhydride compound includes one or more of maleic anhydride, succinic anhydride, citraconic anhydride, nadic anhydride, phenyl maleic anhydride, methyl nadic anhydride, 2,3-pyridinedicarboxylic anhydride and 3,4-pyridinedicarboxylic anhydride. The phosphoric anhydride compound includes one or more of lithium hexafluorophosphate, phosphoric anhydride, 1-propyl phosphoric anhydride and 1-butyl phosphoric anhydride. The sulfuric anhydride compound includes vinyl sulfate. The sulfonic anhydride compound includes methylene disulfonate.
[0021] These acidic additives in the positive electrode slurry can significantly inhibit the rapid increase in viscosity of the positive electrode slurry during the storage process, while maintaining the stability of the solid content of the upper and lower layers of the positive electrode slurry, improving the peeling force of the electrode sheet after rolling, and significantly improving the stability of the positive electrode slurry and the mechanical properties of the positive electrode sheet. Secondly, after being assembled into a battery, the acidic additives react with the residual lithium on the surface of the active material, reducing the alkalinity and water absorption of the slurry, while reducing the damage of the alkaline substance to the binder, significantly improving the stability of the slurry and the mechanical properties of the positive electrode sheet. In addition, the reduction of residual lithium is conducive to the formation of a good CEI film on the positive electrode surface, and also effectively inhibits the gas production caused by residual lithium and the side reaction of the electrolyte and the positive electrode active layer. Therefore, the capacity retention rate during the battery cycle is significantly improved, and the gas production and hard expansion of the battery during storage, circulation, and floating charge are suppressed.
[0022] Although fatty acids, sodium sulfonate, quaternary ammonium salts, polyvinyl pyrrolidone and other substances can also react with alkaline substances, the introduction of these surfactants will bring impurities into the lithium-ion battery, easily causing battery self-discharge and causing the high-temperature cycle performance of the lithium-ion battery to decay, which does more harm than good. Therefore, they are not suitable for neutralizing alkaline substances in lithium-ion batteries.
[0023] Specifically, the nickel-containing compound includes one or more of lithium nickel cobalt manganese oxide, lithium nickel oxide, lithium nickel cobalt aluminum oxide, lithium nickel manganese oxide, lithium nickel cobalt oxide, aluminum nickel cobalt and nickel cobalt manganese.
[0024] Preferably, the molecular formula of the nickel-containing compound is , wherein M is selected from Mn and / or Al; or, the molecular formula of the nickel-containing compound is .
[0025] In one embodiment of the present invention, the mass ratio of the conductive agent to the active material is 0.3% to 3%; the mass ratio of the binder to the active material is 0.3% to 5%. Specifically, the conductive agent includes one or more of carbon nanotubes, carbon black and graphene; the binder includes one or more of polyvinylidene fluoride (PVDF), carboxymethyl cellulose (CMC), polyacrylic acid (PAA), and polyimide (PI).
[0026] An embodiment of the present invention also provides a lithium-ion battery, comprising a shell, a negative electrode sheet, a separator and a positive electrode sheet as in any of the above embodiments, wherein the positive electrode sheet, the separator and one side of the negative electrode sheet are stacked or wound to form a battery cell, and the battery cell is arranged in the shell, and the shell is also injected with an electrolyte.
[0027] The present invention is further described below by way of examples. However, the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.
[0028] Example 1 Production of positive electrode: High voltage 4.45V nickel-cobalt-manganese is used as the active material. 0.68 Co 0.1 Mn 0.22 (active material), carbon nanotubes (conductive agent), PVDF (binder) and in a weight ratio of 97:1.5:1.5 are fully stirred and mixed in N-methylpyrrolidone solvent, and then 0.01% oxalic acid (acidic additive, based on the mass of active material) is added to form a uniform positive electrode slurry, which is coated on the positive electrode current collector aluminum foil, dried, and rolled to obtain a pole piece. The rolled pole piece is divided into strips to obtain a positive electrode sheet.
[0029] Preparation of negative electrode sheet: Graphite (active material), acetylene black (conductive agent), sodium carboxymethyl cellulose (thickener) are fully stirred and mixed in a deionized water solvent at a mass ratio of 95:2:2:1 to form a uniform negative electrode slurry. The slurry is coated on the negative electrode current collector copper foil, dried, and cold pressed to obtain a negative electrode sheet.
[0030] Preparation of electrolyte: The preparation steps of electrolyte are as follows: Ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) were mixed in a mass ratio of 15:15:20:50 (the solvent was normalized to 100%) as an organic solvent. Additives 3% PS (polystyrene), 0.5% VC (vinylene carbonate), 2% FEC (fluoroethylene carbonate), 1% LiPO2F2, 0.5% LiDFOB, and 0.2% LiBF4 were added to the organic solvent and mixed evenly, and then LiPF6 was added to obtain an electrolyte; wherein the concentration of LiPF6 was 1.15 mol / L.
[0031] Production of lithium-ion batteries: stack the positive electrode sheet, separator and negative electrode sheet in order, so that the separator is in the middle of the positive and negative electrode sheets to play an isolating role, and then wind them to obtain a bare cell. Put the bare cell in an outer packaging bag, dry it at high temperature until the water content of the electrode sheet is less than 100ppm, inject electrolyte, and complete the preparation of lithium-ion batteries through vacuum packaging, static, formation, capacity division, shaping and other processes.
[0032] As shown in Table 1, the difference between Examples 2 to 14 and Example 1 is that the type or content of the acidic additive is changed.
[0033] As shown in Table 2, Examples 15 to 32 differ from Example 1 in that the type of active material and the type and content of the acidic additive are changed.
[0034] Comparative Examples 1 to 4 differ from Example 1 in that no acidic additive is contained.
[0035] Table 1 Condition variables table of Examples 1-14 and Comparative Example 1
[0036] Table 2 Condition variables table of Example 4, Examples 9-32 and Comparative Examples 1-4
[0037] The positive electrode slurries, positive electrode sheets and lithium-ion batteries prepared in the above examples and comparative examples were subjected to the following performance tests: 1. Static viscosity of positive electrode slurry The prepared positive electrode slurry was set aside for 72 hours, and the static viscosity at 0h, 24h, 48h, and 72h was tested and recorded using a viscometer, and the stability of the slurry was observed.
[0038] 2. Static solid content of positive electrode slurry The prepared positive electrode slurry was set aside for 72 hours, and the static solid content of the upper and lower layers of the slurry at 0h, 24h, 48h, and 72h was tested and recorded with a moisture tester, and the stability of the slurry was observed.
[0039] 3. Peeling force of positive electrode The electrode sheets after rolling are processed as follows: A. The electrode sheets are divided into strips to obtain positive electrode sheets with a size of 19mm*70mm; B. Fix the positive electrode sheets on the stainless steel plate using pressure-sensitive 3M-VHB double-sided tape; C. Test: Fix the stainless steel plate and the positive current collector on the two fixtures of the peeling force tester, and then perform a 180-degree peeling test at a speed of 10mm / min and a load of 10N. The force detected when the positive current collector is completely peeled off is the peeling force (three data are tested in each group and the average value is taken).
[0040] 4. 45℃ cycle test Place the lithium-ion battery in a 45±2℃ environment, and follow the standard charge and discharge cycle, with a charge rate of 3C, a discharge rate of 1C, and a charge voltage of 3.0-4.45V. Calculate the battery capacity retention rate and battery thickness expansion rate after the cycle (the thickness test uses a PPG battery thickness gauge, and the weight is set to 700g). Repeat the above charge and discharge process n times. The calculation formula is as follows: The capacity retention rate of the nth cycle (%) = (discharge capacity of the nth cycle) / (discharge capacity of the first cycle) * 100%; the thickness expansion rate of the nth cycle (%) = (cell thickness after the nth cycle) / (test thickness before the cycle) * 100%; 5. 45℃ intermittent cycle test Test method: Place the battery in a 45±2℃ environment, charge at 1C constant current to 4.45V (charge at constant voltage to 0.05C), let stand at 4.45V for 24 hours, discharge at 1C constant current to 3.0V, let stand for 5 minutes, repeat the above charge and discharge process n times (voltage window 3.0-4.45V), calculate the capacity retention rate and thickness expansion rate of the battery after the cycle (PPG battery thickness gauge is used for thickness test, and the weight is set to 700g). The calculation formula is as follows: The capacity retention rate of the nth cycle (%) = (discharge capacity of the nth cycle) / (discharge capacity of the first cycle) * 100%; the thickness expansion rate of the nth cycle (%) = (cell thickness after the nth cycle) / (test thickness before the cycle) * 100%; 6. 45℃ floating charge test Test method: Place the battery cell in a constant temperature box at 45±2℃, charge the battery at room temperature at 1C constant current to 4.45V (constant voltage to 0.05C), and continue charging at 4.45V for 45D, and record the thickness of the battery cell, and calculate the thickness expansion rate of the battery after continuous charging (the thickness test uses a PPG battery thickness gauge, and the weight is set to 700g). The calculation formula is as follows: Thickness expansion rate (%) = (cell thickness after continuous charging for 45D - cell thickness before test) / (cell thickness before test) * 100%; 7. 85℃ storage performance test Test method: Charge the battery at room temperature with a constant current of 1C to 4.45V (constant voltage charge to 0.05C), leave it at 4.45V for 5 minutes, then place the battery cell in an environment of 85±2℃ for 48 hours, record the thickness of the battery cell, and calculate the thickness expansion rate of the battery after storage (the thickness test uses a PPG battery thickness gauge, and the weight is set to 700g). The calculation formula is as follows: Thickness expansion rate (%) = (cell thickness after storage - test thickness before storage) / (test thickness before storage) * 100%; The above test results are shown in Table 3 and Table 4.
[0041] Table 3 Test results of positive electrode slurries and positive electrode sheets in Examples 1-32 and Comparative Examples 1-4
[0042] Table 4 Test results of lithium-ion batteries in Examples 1-32 and Comparative Examples 1-4
[0043] From the test results in Table 3 and Table 4, we can see that: The viscosity increase of the positive electrode slurry in each embodiment is significantly lower than that in the comparative example, indicating that the addition of the acidic additive has a significant inhibitory effect on the rapid increase in viscosity of the positive electrode slurry during the storage process; and, in each comparative example, the positive electrode slurry is easy to stratify during the storage process, resulting in a large difference in the solid content of the upper and lower layers, while the difference in the solid content of the upper and lower layers of the positive electrode slurry during the storage process in each embodiment is small, and no obvious stratification occurs, indicating that the acidic additive can effectively maintain the stability of the positive electrode slurry; at the same time, the peeling force of the positive electrode sheet in each embodiment is far greater than the peeling force of the positive electrode sheet in the corresponding comparative example, indicating that the acidic additive in the positive electrode sheet can improve the anti-peeling performance of the positive electrode sheet after rolling. This is mainly due to the fact that the acidic additive reacts with the residual lithium on the surface of the active material, reducing the alkalinity and water absorption of the slurry, while reducing the damage of the alkaline substance to the binder PVDF, and significantly improving the slurry stability and the mechanical properties of the electrode sheet.
[0044] In addition, after being assembled into lithium-ion batteries, the capacity retention rate during the battery cycle is significantly improved, and the thickness expansion rate of the battery during storage, circulation, and floating charge is significantly reduced. The reasons are: first, the acidic additive eliminates the alkaline substances on the surface of the positive electrode material during the slurry preparation / storage process, reducing the gas production caused by alkaline substances during the use of the battery cell; secondly, the reduction of alkaline substances is not only conducive to the formation of a good CEI film on the surface of the positive electrode active layer, but also has a good inhibitory effect on the side reactions between the electrolyte and the electrode, so the electrical performance of the lithium-ion battery is also significantly improved.
[0045] By comparing the test results of Examples 1-6 and Comparative Example 1, it can be seen that as the proportion of the acidic additive increases, the viscosity increase of the positive electrode slurry is significantly reduced, the difference in solid content between the upper and lower layers is gradually reduced, and the peeling force of the positive electrode sheet, the capacity retention rate and the thickness expansion rate of the lithium-ion battery are all improved, indicating that the addition of the acidic additive has a significant inhibitory effect on the rapid increase in viscosity of the positive electrode slurry during the storage process; and the acidic additive can effectively maintain the stability of the positive electrode slurry, so the difference in solid content between the upper and lower layers is gradually reduced, and the stratification phenomenon is alleviated; In addition, after the proportion of acidic additives exceeds 0.3%, various performances no longer improve significantly, and the capacity decreases. This shows that too much acidic additives not only fail to further improve the electrical performance of lithium-ion batteries, but also reduce the proportion of active materials, thereby reducing the capacity of the battery.
[0046] By comparing the test results of Example 4, Examples 7-14 and Comparative Example 1, it can be seen that after changing the type of acidic additive, the viscosity increase of the positive electrode slurry, the stratification phenomenon and the peeling force of the positive electrode sheet, the capacity retention rate and the thickness expansion rate of the lithium ion battery in each embodiment have changed, but they are all better than Comparative Example 1, indicating that the improvement of the performance of the positive electrode slurry, the positive electrode sheet and even the lithium ion battery by adding the acidic additive proposed in the present invention has been verified, so changing the type of acidic additive can still significantly improve the performance of the positive electrode slurry, the positive electrode sheet and even the lithium ion battery.
[0047] As shown in Table 2, the types of active materials were changed in Examples 15-32 and Comparative Examples 2-4. Comparison of the test results in Table 3 and Table 4 shows that the viscosity increase of the positive electrode slurry, the delamination phenomenon and the peeling force of the positive electrode sheet, the capacity retention rate and the thickness expansion rate of the lithium ion battery in each embodiment have changed, but they are all better than the comparative examples with the same active materials, indicating that the addition of acidic additives can improve the performance of nickel-based positive electrode slurry, positive electrode sheet and even lithium ion battery.
[0048] The embodiments described above are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention, and should all be included in the protection scope of the present invention.
Claims
1. A positive electrode sheet, characterized in that: It comprises a positive electrode current collector and a positive electrode active layer disposed on at least one side of the positive electrode current collector, wherein the positive electrode active layer comprises a positive electrode material and an acidic additive, wherein the positive electrode material comprises an active material, a conductive agent and a binder, and wherein the active material comprises a nickel-containing compound; The acidic additive includes an acidic compound A and / or a compound B whose decomposition product is acidic; the compound A includes a carboxylic acid compound, a phosphoric acid compound, a sulfonic acid compound or a boric acid compound; the compound B includes a carboxylic anhydride compound, a phosphoric anhydride compound, a sulfuric anhydride compound or a sulfonic anhydride compound.
2. The positive electrode sheet according to claim 1, characterized in that: The mass ratio of the acidic additive to the active material is 0.01% to 1%.
3. The positive electrode sheet according to claim 2, characterized in that: The mass ratio of the acidic additive to the active material is 0.1% to 0.5%.
4. The positive electrode sheet according to claim 1, characterized in that: The carboxylic acid compound includes one or more of oxalic acid, citric acid, malic acid, benzoic acid, tartaric acid, lactic acid, adipic acid and acetic acid; Alternatively, the phosphate compound includes one or more of phosphoric acid, pyrophosphoric acid and acetyl phosphate; Alternatively, the sulfonic acid compound includes one or more of sulfonic acid, 2-naphthalenesulfonic acid, methanesulfonic acid and benzenesulfonic acid; Alternatively, the boric acid compound includes one or more of tetraboric acid, metaboric acid and orthoboric acid.
5. The positive electrode sheet according to claim 1, characterized in that: The carboxylic anhydride compound includes one or more of maleic anhydride, succinic anhydride, citraconic anhydride, nadic anhydride, phenyl maleic anhydride, methyl nadic anhydride, 2,3-pyridinedicarboxylic anhydride and 3,4-pyridinedicarboxylic anhydride; Alternatively, the phosphoric anhydride compound includes one or more of lithium hexafluorophosphate, phosphoric anhydride, 1-propyl phosphoric anhydride and 1-butyl phosphoric anhydride; Alternatively, the sulfuric anhydride compound includes vinyl sulfate; Alternatively, the sulfonic anhydride compound includes methylene methanedisulfonate.
6. The positive electrode sheet according to claim 1, characterized in that: The nickel-containing compound includes one or more of lithium nickel cobalt manganese oxide, lithium nickel oxide, lithium nickel cobalt aluminum oxide, lithium nickel manganese oxide, lithium nickel cobalt oxide, aluminum nickel cobalt and nickel cobalt manganese.
7. The positive electrode sheet according to claim 1, characterized in that: The molecular formula of the nickel-containing compound is , wherein M is selected from Mn and / or Al; Alternatively, the molecular formula of the nickel-containing compound is .
8. The positive electrode sheet according to claim 1, characterized in that: The mass ratio of the conductive agent to the active material is 0.3% to 3%; And / or, the mass ratio of the binder to the active material is 0.3% to 5%.
9. The positive electrode sheet according to claim 8, characterized in that: The conductive agent includes one or more of carbon nanotubes, carbon black and graphene; And / or, the binder includes one or more of polyvinylidene fluoride, carboxymethyl cellulose, polyacrylic acid, and polyimide.
10. A lithium ion battery, characterized in that: It comprises a shell, a negative electrode sheet, a separator and the positive electrode sheet as claimed in any one of claims 1 to 9, wherein the positive electrode sheet, the separator and the negative electrode sheet are stacked or wound to form a battery core, and the battery core is arranged in the shell, and the shell is also injected with an electrolyte.
Citation Information
Patent Citations
Slurry for positive electrode of lithium ion secondary cell, positive electrode obtained using said slurry, method for manufacturing said positive electrode, lithium ion secondary cell formed using said positive electrode, and method for manufacturing said cell
CN105940530A
Positive electrode slurry, positive electrode sheet and lithium ion battery
CN109119632A
Positive electrode for nonaqueous electrolyte secondary batteries, nonaqueous electrolyte secondary battery using same, and positive electrode slurry for positive electrodes of nonaqueous electrolyte secondary batteries
WO2024070704A1