Lithium-alloy composite negative electrode and preparation method and application thereof

By forming a Cu2Sb modification layer on the surface of the copper current collector and coating molten lithium, the lithium-alloy composite negative electrode is prepared, which solves the problem of lithium dendrites and thickness unevenness in the lithium metal negative electrode, and realizes the lithium-alloy composite negative electrode Adjustable thickness and improved electrochemical stability, suitable for high-energy density lithium metal batteries.

CN119092642APending Publication Date: 2024-12-06HUAZHONG UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411387069.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing lithium metal negative electrodes are prone to growth of lithium dendrites during charging and discharging, resulting in electrode structure damage and safety problems. The thickness is uneven and cost high, making it difficult to meet the needs of high-energy-density batteries.

Method used

By forming a Cu2Sb modification layer on the surface of the copper current collector and coating it with molten lithium, Li-Cu and Li3Sb layers are formed, and the lithium-alloy composite negative electrode is prepared by a scraper method to ensure uniform deposition of lithium metal and stability of the electrode structure.

Benefits of technology

The thickness adjustable, electrochemical stability and energy density of the lithium-alloy composite negative electrode are achieved, avoiding the growth of lithium dendrites, and enhancing the cycle stability and battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092642A_ABST
    Figure CN119092642A_ABST
Patent Text Reader

Abstract

The invention provides a lithium-alloy composite negative electrode and a preparation method and application thereof. The lithium-alloy composite negative electrode comprises a copper current collector, and a Li-Cu alloy layer and a Li-Li3Sb layer which are arranged on the surface of the copper current collector. The preparation method comprises the following steps: placing a copper foil in an antimony-containing solution for reaction to obtain a Cu2Sb modified copper foil; and placing a lithium sheet on the surface of the Cu2Sb layer, heating to 180-240 DEG C, and blade-coating molten lithium on the surface of the Cu2Sb layer to obtain the lithium-alloy composite negative electrode. And the molten lithium and the Cu2Sb react to form Li3Sb and LiCu in situ. Li3Sb is uniformly distributed in metal lithium, and a Li-Li3Sb composite electrode layer is formed on the surface of copper. And the Li-Li3Sb layer is connected with the copper foil through Li-Cu to form an electrode and current collector integrated structure. On one hand, the compounding of Li-Li3Sb and the copper foil is promoted, the contact internal resistance is reduced, and the cycling stability of the battery is improved; on the other hand, spreading of the Li-Li3Sb electrode on the copper surface is promoted to form an ultrathin negative electrode; and meanwhile, the uniformly compounded Li-Li3Sb accelerates Li < + > transmission, electrode pulverization in subsequent circulation is avoided, and lithium dendrite growth is inhibited. The negative electrode has an important application prospect in a high-specific-energy lithium battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium metal batteries, and specifically relates to a lithium-alloy composite negative electrode and a preparation method and application thereof. Background Art

[0002] In recent years, with the rapid development of electronic products and electric vehicles, the energy demand for batteries has continued to increase. Graphite anodes are the most widely used in lithium-ion batteries, but the capacity of commercial graphite anodes is close to its theoretical specific capacity, which is difficult to meet the application needs of high energy density batteries. Compared with traditional graphite anodes, lithium metal anodes have a capacity of up to 3860mAh g -1 The theoretical specific capacity is 10 times that of graphite anode. Therefore, lithium batteries based on lithium metal anodes have received widespread attention in recent years and are considered to be an important direction for the development of high energy density batteries in the future. However, lithium metal anodes are prone to the growth of lithium dendrites during the battery charging and discharging process, accompanied by huge volume changes, which leads to the destruction of the electrode structure and even safety issues. In addition, the thickness of the currently commonly used commercial lithium metal anode is about 450μm, while the thickness of the lithium anode that matches the positive electrode is only 15-50μm (area capacity: 3-10mAh cm -2 ), which results in a far-too-excess amount of lithium metal, which not only reduces the energy density of lithium metal batteries, but also increases the cost, hindering the practical application of lithium metal anodes.

[0003] Due to its low mechanical strength and no "host" characteristics, lithium metal often needs to be adhered to copper foil in practical applications. The ultra-thin lithium negative electrode is formed on the surface of the copper foil by the melting method, which has stronger practicality and feasibility. However, the wettability of molten lithium on the surface of the copper current collector is poor, and its high surface tension makes it difficult to spread on the surface of the copper foil, resulting in the thickness and uniformity of the metallic lithium being difficult to control. By increasing the reaction temperature, the molten lithium and the copper foil undergo an alloying reaction to increase its affinity with the copper foil surface. For example, Li et al. (Energy Storage Mater. 2023, 63, 103067) directly wet-coated the molten lithium liquid on the heated copper foil at a heating temperature of 275-350°C. Due to the in-situ alloying of the molten lithium and the copper foil, the molten lithium is easily evenly distributed on the surface of the heated copper foil. However, this composite electrode still has the problem of lithium dendrites caused by uneven deposition of lithium metal. Therefore, by introducing lithium-philic materials, such as metal particles or alloys, it is not only beneficial to increase the wettability of copper foil with lithium, but also the abundant lithium-philic sites provided can adjust the uniform deposition of lithium metal and inhibit the growth of lithium dendrites. For example, Chinese invention patent CN116344746A discloses an ultra-thin lithium metal negative electrode and its preparation method and application, in which a molten lithium-zinc mixture is evenly coated on the surface of copper foil by a scraper to obtain a lithium metal composite negative electrode. Since the molten lithium reacts chemically with the zinc metal particles, the surface tension of the metallic lithium is spontaneously reduced, which promotes its rapid diffusion on the surface of the copper foil. However, the means of lithium-zinc mixture composite copper foil is only a simple coating, and the bonding force between it and the copper foil is often insufficient, which will lead to insufficient firmness of lithium-zinc adhesion on the copper foil. In the process of continuous lithium plating / stripping, cracks or powders are prone to appear on the electrode, and even the lithium-zinc mixture layer may fall off from the copper foil, resulting in an unstable electrode structure, thereby affecting the performance of the battery.

[0004] Therefore, how to develop a dendrite-free lithium-alloy composite negative electrode with a simple preparation process, stable electrode structure and excellent electrochemical performance has become a technical problem that needs to be solved urgently. Summary of the invention

[0005] The main purpose of the present invention is to provide a lithium-alloy composite negative electrode and a preparation method and application thereof in view of the problems and shortcomings of the prior art.

[0006] The technical solution of the present invention is:

[0007] A lithium-alloy composite negative electrode comprises a copper current collector and a Li-Cu alloy layer and a Li-Li3Sb layer sequentially arranged on the surface of the copper current collector, wherein the thickness of the Li-Li3Sb layer is 13-300 microns.

[0008] The method for preparing the lithium-alloy composite negative electrode comprises the following steps:

[0009] The copper foil is placed in an antimony-containing solution for reaction, and the surface Cu atoms react with the antimony ions to form a Cu2Sb modification layer on the surface of the copper current collector;

[0010] A metal lithium sheet is placed on the surface of a copper current collector containing a Cu2Sb modified layer and heated on a heating plate. The lithium sheet is molten at 180-240°C and the molten lithium is coated on the Cu2Sb modified copper current collector with a scraper to obtain a lithium-alloy composite negative electrode.

[0011] Preferably, the concentration of the antimony-containing solution is 0.02-0.08 mol / L.

[0012] Preferably, the copper foil is first placed in anhydrous ethanol for ultrasonic cleaning, and then dried to obtain a clean copper foil.

[0013] Preferably, the temperature for reacting the copper foil in the antimony-containing solution is 30-100° C., and the reaction time is 10-45 min.

[0014] Preferably, the antimony-containing solution is prepared by placing an antimony-containing reagent in a solvent and stirring until the antimony-containing reagent is uniformly dissolved to obtain the antimony-containing solution.

[0015] Preferably, the dissolving temperature is 20-30° C., and the stirring time is 15 to 120 min, preferably 15 to 30 min.

[0016] Preferably, the antimony-containing reagent is antimony trichloride, and the solvent is tetrahydrofuran.

[0017] The lithium-alloy composite negative electrode is used in lithium metal batteries.

[0018] The beneficial effects of the present invention are as follows: the present invention first forms a lithium-philic alloy layer (Cu2Sb@Cu) in situ on the surface of a copper current collector through a simple chemical replacement reaction, and further scrapes molten lithium metal onto the surface of the Cu2Sb@Cu substrate with the lithium-philic layer through a scraper coating method. As the molten lithium reacts with the Cu2Sb alloy, lithium-philic Li-Cu and Li3Sb are formed on the Cu surface. The lithium metal in the Li-Cu layer formed in situ on the Cu surface spontaneously spreads out on the surface of the current collector, and the generated Li3Sb also spontaneously mixes evenly with the molten lithium to form a lithium-alloy composite negative electrode (Li-Li3Sb@Cu) with adjustable thickness on the copper surface. The lithium-alloy composite negative electrode prepared by the present invention has a thickness as thin as 13 μm. In addition, the Li-Li3Sb composite electrode layer and the Cu current collector in the composite negative electrode are connected by a Li-Cu bond, which ensures the continuity and structural integrity of the electrode and the current collector, forming a complete electrode and current collector integrated structure, avoiding the occurrence of electrode pulverization or cracking in the subsequent repeated deposition / stripping process of the battery, and enhancing the electrochemical stability of the battery; in addition, Li3Sb is evenly distributed in the metallic lithium, effectively inhibiting the growth of lithium dendrites. When used as an ultra-thin lithium negative electrode for lithium metal batteries, the cycle stability and energy density of lithium metal batteries can be significantly improved, and the preparation method is simple, the lithium thickness is adjustable, and the sheet area is controllable, which is suitable for mass and rapid production. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 It is a schematic diagram of the process of preparing an ultra-thin lithium-alloy composite negative electrode (Li-Li3Sb@Cu) according to the present invention;

[0020] Figure 2 Characterization diagrams of the morphology, thickness and chemical composition of the ultra-thin Li-Li3Sb@Cu composite negative electrode prepared in Example 1 of the present invention and the pure thin lithium prepared in Comparative Example 1;

[0021] (a) Optical photograph of the lithium affinity test of pure Cu current collector and molten lithium; (b) Optical photograph of the lithium affinity test of Cu2Sb@Cu current collector and molten lithium; (c) Optical photograph of large-area preparation of ultra-thin Li-Li3Sb@Cu composite negative electrode sheets; (d) SEM image of the cross-sectional thickness of the ultra-thin Li-Li3Sb@Cu composite negative electrode (about 30μm); (e) SEM image of the cross-sectional thickness of the ultra-thin Li-Li3Sb@Cu composite negative electrode (about 13μm); (f) SEM image of cross-sectional thickness (about 125 μm); (g) Constant current charging test of the assembled battery of ultrathin Li-Li3Sb@Cu composite negative electrode; (h) Constant current charging test of the assembled battery of pure thin lithium; (i) XRD diffraction pattern of pure thin lithium and ultrathin Li-Li3Sb@Cu composite negative electrode; (j) EPMA spectrum of Sb element of ultrathin Li-Li3Sb@Cu composite negative electrode; (k) Schematic diagram of the layered structure of ultrathin Li-Li3Sb@Cu composite negative electrode;

[0022] Figure 3 The ultra-thin Li-Li3Sb@Cu composite negative electrode prepared in Example 1 of the present invention and the pure thin lithium prepared in Comparative Example 1 were assembled into a Li-Li3Sb@Cu||Li-Li3Sb@Cu symmetric battery and a Li||Li symmetric battery, and the cycle stability tests and corresponding electrochemical impedance spectra at different current densities were performed;

[0023] (a) Li-Li3Sb@Cu||Li-Li3Sb@Cu and Li||Li symmetric cells at 1.0 mA cm -2 Cyclic stability test under current density; (b) Li-Li3Sb@Cu||Li-Li3Sb@Cu and Li||Li symmetric cells at 1.0 mA cm-2 and 3.0 mA cm-2 -2 Different test time-polarization potential curves at different current densities; (c) Li-Li3Sb@Cu||Li-Li3Sb@Cu and Li||Li symmetric batteries at 3.0 mA cm -2 Cyclic stability test under current density; (d) Electrochemical impedance spectroscopy of Li-Li3Sb@Cu||Li-Li3Sb@Cu and Li||Li symmetric batteries before cycling;

[0024] Figure 4 The ultra-thin Li-Li3Sb@Cu composite negative electrode prepared in Example 1 of the present invention and the pure thin lithium prepared in Comparative Example 1 were assembled into a Li-Li3Sb@Cu||Li-Li3Sb@Cu symmetric battery and a Li||Li symmetric battery, and the deposition morphology of lithium and the growth of lithium dendrites were tested by an in-situ microscopic observation instrument;

[0025] (a) Pure thin Li||Li symmetric battery at 1.0 mA cm-2 Lithium deposition morphology test under current density; (b) Ultrathin Li-Li3Sb@Cu||Li-Li3Sb@Cu symmetric battery at 1.0 mA cm -2 Lithium deposition morphology test under current density;

[0026] Figure 5 The ultra-thin Li-Li3Sb@Cu composite anode prepared in Example 1 of the present invention and the pure thin lithium anode prepared in Comparative Example 1 are matched with commercial lithium iron phosphate (LFP) to assemble a lithium metal full battery with rate performance test and 0.5C and 1C cycle stability test, as well as the corresponding electrochemical impedance test graph and SEM morphology graph;

[0027] (a) Rate performance test of LFP||Li-Li3Sb@Cu and LFP||Li full cells at 0.5-3C; (b) Corresponding polarization potential bar graphs of LFP||Li-Li3Sb@Cu and LFP||Li full cells at different rates; (c) Cycle stability test of LFP||Li-Li3Sb@Cu and LFP||Li full cells at 0.5C rate; (d) Cycle stability test of LFP||Li-Li3Sb@Cu and LFP||Li full cells at 1C rate; (e) Electrochemical impedance spectra of LFP||Li-Li3Sb@Cu and LFP||Li full cells before cycling; (f) Electrochemical impedance spectra of LFP||Li-Li3Sb@Cu and LFP||Li full cells after cycling; (g) SEM surface morphology of LFP||Li-Li3Sb@Cu full cells after cycling; (h) SEM surface morphology of LFP||Li full cells after cycling. DETAILED DESCRIPTION

[0028] The principles and features of the present invention are described below in conjunction with examples, which are only used to explain the present invention and are not intended to limit the scope of the present invention. In addition, it is worth noting that the raw materials involved in the present invention are all common commercial products unless otherwise specified.

[0029] Example 1

[0030] like Figure 1 As shown, a method for preparing an ultra-thin lithium-alloy (Li-Li3Sb@Cu) composite negative electrode comprises the following steps:

[0031] (1) 3.0 mmol of antimony trichloride reagent was placed in 100 ml of tetrahydrofuran solvent and magnetically stirred at 25° C. for 20 min to obtain a uniformly dissolved antimony trichloride solution;

[0032] (2) The area is 125cm 2The commercial copper foil was placed in anhydrous ethanol, ultrasonically cleaned for 30 minutes, and dried in a 60°C forced air oven for 30 minutes for standby use;

[0033] (3) placing the copper foil obtained in step (2) in the antimony trichloride solution obtained in step (1), reacting at 80° C. for 20 min, washing away the residual reaction solution with tetrahydrofuran, and then vacuum drying at 60° C. for 12 h to obtain a Cu2Sb-modified copper current collector (Cu2Sb@Cu);

[0034] (4) The Cu2Sb@Cu current collector obtained in step (3) is placed on a heating plate, and a lithium sheet is placed on the surface of the current collector. After heating at 220°C, the lithium sheet is in a molten state and is coated onto the Cu2Sb@Cu current collector by a scraper. By adjusting the thickness of the scraper, an ultra-thin Li-Li3Sb@Cu composite negative electrode with a thickness of 30 μm is obtained.

[0035] Example 2

[0036] This example uses the same experimental raw materials and conditions as Example 1, except that the amount of antimony trichloride is changed in step (1), specifically:

[0037] (1) 2.0 mmol of antimony trichloride reagent was placed in 100 ml of tetrahydrofuran solvent and magnetically stirred at 25° C. for 20 min to obtain a uniformly dissolved antimony trichloride solution;

[0038] Steps (2) to (4) are the same as those in Example 1 and will not be repeated here.

[0039] Example 3

[0040] This example uses the same experimental raw materials and conditions as Example 1, except that the amount of antimony trichloride is changed in step (1), specifically:

[0041] (1) 4.0 mmol of antimony trichloride reagent was placed in 100 ml of tetrahydrofuran solvent and magnetically stirred at 25° C. for 20 min to obtain a uniformly dissolved antimony trichloride solution;

[0042] Steps (2) to (4) are the same as those in Example 1 and will not be repeated here.

[0043] Example 4

[0044] This example uses the same experimental raw materials and conditions as Example 1, except that the amount of antimony trichloride is changed in step (1), specifically:

[0045] (1) 5.0 mmol of antimony trichloride reagent was placed in 100 ml of tetrahydrofuran solvent and magnetically stirred at 25° C. for 20 min to obtain a uniformly dissolved antimony trichloride solution;

[0046] Steps (2) to (4) are the same as those in Example 1 and will not be repeated here.

[0047] Example 5

[0048] This example uses the same experimental raw materials and conditions as Example 1, and only changes the reaction temperature in step (4), specifically:

[0049] Steps (1) and (3) are the same as those in Example 1 and will not be repeated here;

[0050] (4) The Cu2Sb@Cu current collector obtained in step (3) is placed on a heating plate, and a lithium sheet is placed on the surface of the current collector. After heating at 180°C, the lithium sheet is in a molten state and is coated onto the Cu2Sb@Cu current collector by a scraper. By adjusting the thickness of the scraper, an ultra-thin Li-Li3Sb@Cu composite negative electrode with a thickness of 30 μm is obtained.

[0051] Example 6

[0052] This example uses the same experimental raw materials and conditions as Example 1, and only changes the reaction temperature in step (4), specifically:

[0053] Steps (1) and (3) are the same as those in Example 1 and will not be repeated here;

[0054] (4) The Cu2Sb@Cu current collector obtained in step (3) is placed on a heating plate, and a lithium sheet is placed on its surface. After heating at 200°C, the lithium sheet is in a molten state and is coated onto the Cu2Sb@Cu current collector by a scraper. By adjusting the thickness of the scraper, an ultra-thin Li-Li3Sb@Cu composite negative electrode with a thickness of 30 μm is obtained.

[0055] Example 7

[0056] This example uses the same experimental raw materials and conditions as Example 1, and only changes the reaction temperature in step (4), specifically:

[0057] Steps (1) and (3) are the same as those in Example 1 and will not be repeated here;

[0058] (4) The Cu2Sb@Cu current collector obtained in step (3) is placed on a heating plate, and a lithium sheet is placed on its surface. After heating at 200°C, the lithium sheet is in a molten state and is coated onto the Cu2Sb@Cu current collector by a scraper. By adjusting the thickness of the scraper, an ultra-thin Li-Li3Sb@Cu composite negative electrode with a thickness of 30 μm is obtained.

[0059] Example 8

[0060] This example uses the same experimental raw materials and conditions as Example 1, and only changes the reaction temperature in step (4), specifically:

[0061] Steps (1) and (3) are the same as those in Example 1 and will not be repeated here;

[0062] (4) The Cu2Sb@Cu current collector obtained in step (3) is placed on a heating plate, and a lithium sheet is placed on the surface of the current collector. After heating at 240°C, the lithium sheet is in a molten state and is coated onto the Cu2Sb@Cu current collector by a scraper. By adjusting the thickness of the scraper, an ultra-thin Li-Li3Sb@Cu composite negative electrode with a thickness of 30 μm is obtained.

[0063] Example 9

[0064] This embodiment uses the same experimental materials and conditions as in embodiment 1, except that the scraper height is changed in step (4), specifically:

[0065] Steps (1) and (3) are the same as those in Example 1 and will not be repeated here;

[0066] (4) The Cu2Sb@Cu current collector obtained in step (3) is placed on a heating plate, and a lithium sheet is placed on the surface of the current collector. After heating at 220°C, the lithium sheet is in a molten state and is coated onto the Cu2Sb@Cu current collector by a scraper. By adjusting the thickness of the scraper, an ultra-thin Li-Li3Sb@Cu composite negative electrode with a thickness of 13 μm is obtained.

[0067] Example 10

[0068] This embodiment uses the same experimental materials and conditions as in embodiment 1, except that the scraper height is changed in step (4), specifically:

[0069] Steps (1) and (3) are the same as those in Example 1 and will not be repeated here;

[0070] (4) The Cu2Sb@Cu current collector obtained in step (3) is placed on a heating plate, and a lithium sheet is placed on the surface of the current collector. After heating at 220°C, the lithium sheet is in a molten state and is coated onto the Cu2Sb@Cu current collector by a scraper. By adjusting the thickness of the scraper, an ultra-thin Li-Li3Sb@Cu composite negative electrode with a thickness of 18 μm is obtained.

[0071] Embodiment 11

[0072] This embodiment uses the same experimental materials and conditions as in embodiment 1, except that the scraper height is changed in step (4), specifically:

[0073] Steps (1) and (3) are the same as those in Example 1 and will not be repeated here;

[0074] (4) The Cu2Sb@Cu current collector obtained in step (3) is placed on a heating plate, and a lithium sheet is placed on the surface of the current collector. After heating at 220°C, the lithium sheet is in a molten state and is coated onto the Cu2Sb@Cu current collector by a scraper. By adjusting the thickness of the scraper, an ultra-thin Li-Li3Sb@Cu composite negative electrode with a thickness of 50 μm is obtained.

[0075] Example 12

[0076] This embodiment uses the same experimental materials and conditions as in embodiment 1, except that the scraper height is changed in step (4), specifically:

[0077] Steps (1) and (3) are the same as those in Example 1 and will not be repeated here;

[0078] (4) The Cu2Sb@Cu current collector obtained in step (3) is placed on a heating plate, and a lithium sheet is placed on its surface. After heating at 220°C, the lithium sheet is in a molten state and is coated onto the Cu2Sb@Cu current collector by a scraper. By adjusting the thickness of the scraper, a Li-Li3Sb@Cu composite negative electrode with a thickness of 100 μm is obtained.

[0079] Example 13

[0080] This embodiment uses the same experimental materials and conditions as in embodiment 1, except that the scraper height is changed in step (4), specifically:

[0081] Steps (1) and (3) are the same as those in Example 1 and will not be repeated here;

[0082] (4) The Cu2Sb@Cu current collector obtained in step (3) is placed on a heating plate, and a lithium sheet is placed on its surface. After heating at 220°C, the lithium sheet is in a molten state and is coated onto the Cu2Sb@Cu current collector by a scraper. By adjusting the thickness of the scraper, a Li-Li3Sb@Cu composite negative electrode with a thickness of 300 μm is obtained.

[0083] In order to compare the excellent functions of the ultra-thin Li-Li3Sb@Cu composite negative electrode of the present invention, such as stable electrode structure, inhibition of lithium dendrite growth and adjustable thickness, the following comparative examples are set:

[0084] Comparative Example 1

[0085] A commercial lithium metal sheet with a thickness of 450 μm was mechanically rolled to obtain a pure thin lithium sheet with a thickness of 125 μm, which was then cut into thin lithium metal discs with a diameter of 12 mm for later use.

[0086] The following is a description of the detection and analysis of the above embodiments and comparative examples:

[0087] The ultra-thin Li-Li3Sb@Cu composite negative electrode prepared in Examples 1-13 of the present invention can control the thickness of the ultra-thin Li-Li3Sb@Cu composite negative electrode by controlling the height of the scraper, and the thickness is adjustable. At the same time, the synthesis process is simple to operate, the sheet area is controllable, and dendrite-free lithium deposition can be achieved.

[0088] The ultra-thin Li-Li3Sb@Cu composite negative electrode prepared in Example 1 of the present invention and the pure thin lithium prepared in Comparative Example 1 were analyzed for lithium affinity, morphology, thickness and chemical composition. The results are as follows: Figure 2 As shown, it was found through optical photographs that the lithium affinity of the Cu2Sb@Cu current collector is much stronger than that of the pure Cu current collector, which provides a basis for the subsequent preparation of a large-area ultra-thin Li-Li3Sb@Cu composite negative electrode; the results of the SEM cross-sectional view, constant current charging test, XRD spectrum and EPMA characterization diagram show that an ultra-thin Li-Li3Sb@Cu composite negative electrode with a thickness of 13-30μm was successfully prepared, and the Li3Sb alloy and lithium metal were uniformly mixed in the ultra-thin Li-Li3Sb@Cu composite negative electrode prepared in Example 1, and the uppermost Li-Li3Sb composite layer and the copper foil layer were connected in the form of a Li-Cu bond, which ensured the structural stability of the entire electrode and avoided cracking and pulverization of the subsequent lithium metal negative electrode during the cycle.

[0089] The ultra-thin Li-Li3Sb@Cu composite negative electrode prepared in Example 1 of the present invention and the pure thin lithium prepared in Comparative Example 1 were assembled into Li-Li3Sb@Cu||Li-Li3Sb@Cu symmetric cells and Li||Li symmetric cells, respectively. The cycle stability tests and corresponding electrochemical impedance spectra at different current densities were performed. The results are as follows Figure 3 As shown, whether it is 1.0 or 3.0mAcm -2 At a current density of , the Li-Li3Sb@Cu||Li-Li3Sb@Cu symmetric batteries exhibited longer cycle stability and lower polarization potential, indicating that the Li-Li3Sb@Cu composite electrode has good reversibility and a more stable structure; through electrochemical impedance spectroscopy, the results showed that the Li-Li3Sb@Cu||Li-Li3Sb@Cu symmetric battery had a lower charge transfer resistance, indicating that the composite negative electrode has higher lithium ion transfer kinetics.

[0090] The ultra-thin Li-Li3Sb@Cu composite negative electrode prepared in Example 1 of the present invention and the pure thin lithium prepared in Comparative Example 1 were assembled into a Li-Li3Sb@Cu||Li-Li3Sb@Cu symmetric battery and a Li||Li symmetric battery, respectively. The deposition morphology of lithium and the growth of lithium dendrites were tested by an in-situ microscopic observation instrument. The results are as follows Figure 4As shown, compared with the uneven lithium deposition and growth of lithium dendrites of pure thin lithium, the ultrathin Li-Li3Sb@Cu||Li-Li3Sb@Cu symmetric battery exhibits more uniform and smooth lithium deposition without the formation of lithium dendrites.

[0091] The ultra-thin Li-Li3Sb@Cu composite anode prepared in Example 1 of the present invention and the pure thin lithium anode prepared in Comparative Example 1 were matched with commercial lithium iron phosphate (LFP) to assemble LFP||Li-Li3Sb@Cu and LFP||Li full batteries, and the 0.5-3C rate performance test and 0.5C and 1C cycle stability test were performed on them. The results are as follows Figure 5 As shown, the LFP||Li-Li3Sb@Cu full battery exhibits higher rate performance and longer cycle stability at both 0.5C and 1C; through the electrochemical impedance test graphs before and after cycling and the SEM morphology graphs after cycling, it can be seen that the LFP||Li-Li3Sb@Cu full battery exhibits lower charge transfer resistance and flatter SEM morphology, proving the cycle reversibility and structural stability of the ultra-thin Li-Li3Sb@Cu composite negative electrode.

[0092] It can be seen that the ultra-thin Li-Li3Sb@Cu composite negative electrode synthesized by the present invention through a simple method, due to the lithium affinity of the Cu2Sb modified layer and its spontaneous alloying reaction with molten lithium, a uniformly mixed Li-Li3Sb composite negative electrode is prepared. The thickness of the composite negative electrode is adjustable and the area of ​​the thin sheet is controllable, which is convenient for large-scale production. In addition, the Li-Li3Sb composite layer is connected to the copper foil layer in the form of a Li-Cu bond, which maintains the structural stability of the entire electrode during subsequent cycles. At the same time, the uniformly mixed Li-Li3Sb composite negative electrode can guide uniform lithium deposition, and finally obtain a dendrite-free lithium metal battery with long cycle stability.

[0093] It should be noted that, for those skilled in the art, several modifications and improvements can be made without departing from the concept of the present invention, and these modifications and improvements all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A lithium-alloy composite negative electrode, characterized in that: The lithium-alloy composite negative electrode comprises a copper current collector and a Li-Cu alloy layer and a Li-Li3Sb layer formed in situ on the surface thereof, and the thickness of the Li-Li3Sb layer is 13-300 microns.

2. The method for preparing a lithium-alloy composite negative electrode according to claim 1, characterized in that: The following steps are involved: The copper foil is placed in an antimony-containing solution for reaction, and the surface Cu atoms react with the antimony ions to form a Cu2Sb modification layer on the surface of the copper current collector; A metal lithium sheet is placed on the surface of a copper current collector containing a Cu2Sb modified layer and heated on a heating plate. The lithium sheet is molten at 180-240°C and the molten lithium is coated on the Cu2Sb modified copper current collector with a scraper to obtain a lithium-alloy composite negative electrode.

3. The preparation method according to claim 2, characterized in that: The concentration of the antimony-containing solution is 0.02-0.08 mol / L.

4. The preparation method according to claim 2, characterized in that: The copper foil is first placed in anhydrous ethanol for ultrasonic cleaning, and then dried to obtain the cleaned copper foil.

5. The preparation method according to claim 2, characterized in that: The temperature for reacting the copper foil in the antimony-containing solution is 30-100° C., and the reaction time is 10-45 minutes.

6. The preparation method according to claim 2, characterized in that: The antimony-containing solution is prepared by placing an antimony-containing reagent in a solvent and stirring until the antimony-containing reagent is uniformly dissolved to obtain the antimony-containing solution.

7. The preparation method according to claim 6, characterized in that: The dissolving temperature is 20-30° C., and the stirring time is 15-30 min.

8. The preparation method according to claim 6, characterized in that: The antimony-containing reagent is antimony trichloride, and the solvent is tetrahydrofuran.

9. Use of the lithium-alloy composite negative electrode as claimed in claim 1 in a lithium metal battery.