Antimony-based composite negative electrode material and preparation method and application thereof

The antimony-based composite negative electrode material addresses volume changes in sodium-ion batteries by forming a three-dimensional conductive network and a ductile SEI film, enhancing the electrochemical performance and stability of sodium-ion batteries.

CN119092665AActive Publication Date: 2024-12-06NANCHANG UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411165914.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-12-06
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

The large radius of sodium ions and the volume changes of metal antimony during sodiumization and de-sodiumization in sodium-ion batteries lead to low specific capacity and rapid performance degradation, including capacity reduction and decreased cycle stability.

Method used

A method involving the preparation of an antimony-based composite negative electrode material by mixing antimony metal powder with amorphous carbon precursor, ball-milling, and calcining, followed by surface treatment of carbon nanotubes and spray-drying with organic sodium modification to form a three-dimensional conductive network, which inhibits volume expansion and enhances anchoring and conductivity.

Benefits of technology

The method effectively improves the electrochemical performance of sodium-ion batteries by reducing particle size, enhancing structural stability, and forming a ductile SEI film, resulting in improved capacity retention and cycle stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092665A_ABST
    Figure CN119092665A_ABST
Patent Text Reader

Abstract

The invention provides an antimony-based composite negative electrode material as well as a preparation method and application thereof, and relates to the technical field of new energy batteries. The preparation method provided by the invention comprises the following steps: mixing antimony metal powder and amorphous carbon, ball-milling, drying and calcining to obtain an antimony-based intermediate; the method comprises the following steps: acidizing the surface of a carbon nanotube to obtain an acidized carbon nanotube, dispersing the acidized carbon nanotube in an organic sodium modified solution, stirring, filtering and drying to obtain a modified carbon nanotube; and mixing and dispersing the antimony-based intermediate, sodium polyacrylate and the modified carbon nanotube to prepare a suspension, and performing spray drying to prepare the antimony-based composite negative electrode material. According to the preparation method provided by the invention, the problem of performance reduction such as capacity fading caused by huge volume expansion generated in the sodium ion de-intercalation process of metal antimony can be improved, and the electrochemical performance of the antimony-based negative electrode material is effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of new energy batteries, and in particular to an antimony-based composite negative electrode material and a preparation method and application thereof. Background Art

[0002] Energy and environment have always been the two most important issues that people all over the world are concerned about. Energy is the most important resource for human society to survive and develop, while the environment is the basic environment for human survival. In terms of the current development of energy, natural fossil energy is still the main source, and fossil energy is bound to cause environmental pollution and other environmental problems when used. Therefore, the development of renewable energy and energy storage technology has become particularly important. Among them, lithium batteries have become the focus of current energy storage technology research due to their excellent electrochemical properties, high energy density and green environmental protection.

[0003] At present, lithium-ion batteries are widely used in portable electronic devices. With the large-scale development and application of electric vehicles and electronic portable devices, the limited lithium resources on the earth may lead to an increase in the cost of lithium-ion batteries. Therefore, sodium-ion secondary batteries with electrochemical properties similar to those of lithium-ion batteries have become the most suitable substitute. Sodium-ion batteries use single substances or compounds that can reversibly embed and extract sodium ions as the positive and negative electrodes of the battery, and sodium is easy to obtain and has a higher half-cell potential. Therefore, sodium-ion batteries can use electrolytes with low decomposition voltages, and their safety is better than that of lithium-ion batteries.

[0004] However, due to the large radius of sodium ions, when the interlayer spacing of the negative electrode is smaller than the diameter of the sodium ions, it will cause the sodium ions to be difficult to embed into the negative electrode material, resulting in a very small amount of sodium ions embedded, which in turn leads to a low specific capacity of the sodium ion battery. Since metal antimony (Sb) can react with sodium ions to alloy, the amount of sodium ions embedded is increased, thereby increasing the theoretical specific capacity of the sodium ion battery. However, metal antimony undergoes drastic volume changes during the process of sodiumization and de-sodiumization, and may even cause the electrode to break and pulverize, causing the electrochemical performance of the sodium ion battery to decline rapidly, resulting in severe capacity reduction and decreased cycle stability. Therefore, it is urgent to provide a solution to improve the above problems. Summary of the invention

[0005] The purpose of the present invention is to provide an antimony-based composite negative electrode material and a preparation method and application thereof, which can improve the performance degradation problems such as capacity attenuation caused by the huge volume expansion of metal antimony during the process of sodium ion insertion and extraction, and effectively improve the electrochemical performance of antimony-based negative electrode materials.

[0006] In a first aspect, the present invention provides a method for preparing an antimony-based composite negative electrode material, comprising the following steps:

[0007] The antimony metal powder and the amorphous carbon precursor are mixed, ball-milled, dried and calcined to obtain an antimony-based intermediate;

[0008] Performing surface acidification treatment on carbon nanotubes to obtain acidified carbon nanotubes, dispersing the acidified carbon nanotubes in an organic sodium modification solution, stirring, filtering, and drying to obtain modified carbon nanotubes;

[0009] The antimony-based intermediate, sodium polyacrylate and modified carbon nanotubes are mixed and dispersed to obtain a suspension, which is then spray-dried to obtain an antimony-based composite negative electrode material.

[0010] The method for preparing the antimony-based composite negative electrode material provided by the present invention can effectively reduce the particle size of the antimony metal powder by ball milling the antimony metal powder with the amorphous carbon precursor, and can better and uniformly composite with the amorphous carbon precursor in the subsequent process, and can effectively inhibit the volume expansion of the metal antimony;

[0011] At the same time, the modification of carbon nanotubes is conducive to the cross-linking between carbon nanotubes, and can also improve the anchoring ability of antimony metal powder. Adding organic sodium to carbon nanotubes can improve the capacity and service life of sodium ion batteries. After being treated with spray drying technology, it is conducive to the formation of a three-dimensional conductive network by the modified carbon nanotubes, and the antimony-based intermediates are locked in the three-dimensional conductive network, which can further inhibit the volume expansion of metal antimony, and can also improve the overall conductivity and structural stability of the negative electrode material, and overall improve the electrochemical performance of the antimony-based composite negative electrode material;

[0012] In addition, organic sodium can form an organic SEI film in the negative electrode material, which has stronger ductility and weaker rigidity, so that the SEI film is not easy to break during the use of the negative electrode material, and can play a better protective role for the negative electrode material. At the same time, spray drying the antimony-based intermediate and the modified carbon nanotubes can avoid destroying the carbon structure coated on the surface of the antimony-based intermediate.

[0013] Optionally, during the process of mixing the antimony metal powder and the amorphous carbon precursor for ball milling, the mass ratio of the antimony metal powder to the amorphous carbon precursor is 0.5-1.

[0014] Optionally, during the process of mixing the antimony metal powder and the amorphous carbon precursor and ball milling, the ball-to-material ratio is 10-20.

[0015] Optionally, the process of mixing antimony metal powder and amorphous carbon precursor, ball-milling them, drying them and calcining them to obtain an antimony-based intermediate includes: mixing antimony metal powder and amorphous carbon precursor, ball-milling them, filtering and drying them to obtain an antimony-based precursor; and calcining the antimony-based precursor in an inert atmosphere at 1000-1300° C. for 2-4 hours to obtain an antimony-based intermediate.

[0016] Optionally, the process of mixing antimony metal powder and amorphous carbon precursor, ball-milling them, filtering and drying them to obtain an antimony-based precursor includes: mixing antimony metal powder and amorphous carbon precursor, ball-milling them, filtering them, and drying the filtered product at 50-80° C. for 10-14 hours to obtain an antimony-based precursor.

[0017] Optionally, when the antimony-based intermediate and the modified carbon nanotube are mixed and dispersed to prepare a suspension, the solid-liquid ratio in the suspension is 0.03-0.06.

[0018] Optionally, the process of subjecting the carbon nanotubes to surface acidification to obtain the acidified carbon nanotubes comprises: soaking the carbon nanotubes in nitric acid, filtering and drying to obtain the acidified carbon nanotubes.

[0019] Optionally, the process of subjecting the carbon nanotubes to surface acidification to obtain acidified carbon nanotubes includes: soaking the carbon nanotubes in nitric acid for 20-30 hours and then filtering, washing the filtered product with deionized water and drying it at 50-80° C. for 10-14 hours to obtain the acidified carbon nanotubes.

[0020] Optionally, the process of dispersing the acidified carbon nanotubes in the organic sodium modified solution, stirring, filtering and drying includes: stirring, filtering and drying the acidified carbon nanotubes in a siloxane solution to obtain activated carbon nanotubes; dispersing the activated carbon nanotubes in the organic sodium modified solution, stirring and dispersing at 50-60° C. for 5-6 hours, and then filtering and drying. By pre-activating the surface of the acidified carbon nanotubes in the siloxane solution, it is beneficial to the subsequent modification reaction between the acidified carbon nanotubes and the organic sodium modified solution and the anchoring of the antimony metal powder.

[0021] Optionally, when the acidified carbon nanotubes are stirred and filtered in a siloxane solution, the solute of the siloxane solution includes at least one of γ-aminopropyltrimethoxysilane and γ-glycidyloxypropyltrimethoxysilane.

[0022] Optionally, the acidified carbon nanotubes are dispersed in an organic sodium modified solution during stirring, filtering and drying, and the solute of the organic sodium modified solution includes at least one of disodium ethylenediaminetetraacetic acid and trisodium cyanurate.

[0023] In a second aspect, the present invention also provides an antimony-based composite negative electrode material prepared by any of the above optional preparation methods.

[0024] In a third aspect, the present invention also provides the use of the antimony-based composite negative electrode material prepared by any of the above optional preparation methods in a sodium ion battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 A flowchart of a method for preparing an antimony-based composite negative electrode material provided in an embodiment of the present invention;

[0026] Figure 2 A schematic structural diagram of an antimony-based composite negative electrode material provided in an embodiment of the present invention;

[0027] Figure 3 These are the cycle performance diagrams of Examples 1 to 3 and Comparative Examples 1 to 7 of the present invention. DETAILED DESCRIPTION

[0028] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Unless otherwise defined, the technical terms or scientific terms used herein should be the common meanings understood by people with general skills in the field to which the present invention belongs.

[0029] See also Figure 1 The present invention provides a method for preparing an antimony-based composite negative electrode material, comprising the following steps:

[0030] S1. preparing an antimony-based intermediate: mixing antimony metal powder and an amorphous carbon precursor, ball-milling the mixture, drying the mixture, and calcining the mixture to obtain an antimony-based intermediate;

[0031] S2, preparing modified carbon nanotubes: performing surface acidification treatment on carbon nanotubes to obtain acidified carbon nanotubes, dispersing the acidified carbon nanotubes in an organic sodium modification solution, stirring, filtering, and drying to obtain modified carbon nanotubes;

[0032] S3. Preparation of antimony-based composite negative electrode material: mixing and dispersing the antimony-based intermediate, sodium polyacrylate and modified carbon nanotubes to obtain a suspension, and then spray drying to obtain an antimony-based composite negative electrode material.

[0033] In some embodiments, the antimony metal powder used in step S1 is a micron-sized powder. Specifically, the particle size of the micron-sized antimony metal powder is 1-20 μm, and the purity of the metal antimony in the antimony metal powder is greater than or equal to 99%. In fact, the antimony metal powder can be selected from conventional commercial products, such as spherical antimony powder with a specification of 1-20 μm produced by Tianjin Liz Technology Co., Ltd.

[0034] In some embodiments, the amorphous carbon precursor selected when performing step S1 includes at least one of an oily phenolic resin and asphalt. Specifically, the oil-soluble phenolic resin and asphalt can be commercially available products or recycled waste. When the oily phenolic resin is a commercially available product, it can be an oil-soluble phenolic resin with a molecular weight of 80,000-100,000 purchased from Shaoxing Yitong Plastics Priority Company; when the asphalt is a commercially available product, it can be a coal tar powder with a particle size of 1-3 mm purchased from Hankai Energy.

[0035] In fact, the process of executing step S1 includes the following sub-steps:

[0036] S1.1, mixing antimony metal powder and amorphous carbon precursor, performing wet ball milling, filtering and drying to obtain an antimony-based precursor;

[0037] S1.2. The antimony-based precursor is calcined in an inert atmosphere at 1000-1300° C. for 2-4 hours to obtain an antimony-based intermediate.

[0038] In some embodiments, during the step S1.1, the mass ratio of antimony metal powder to amorphous carbon precursor is 0.5-1, and during the mixed ball milling, the ball-to-material ratio is 10-20.

[0039] In some embodiments, during the execution of step S1.1, the antimony metal powder and the amorphous carbon precursor are mixed and ball-milled and then filtered, and the solid obtained by filtration is placed at 50-80° C. and dried for 10-14 hours to obtain an antimony-based precursor.

[0040] In some embodiments, during the execution of step S1.2, the antimony-based precursor is placed in an inert atmosphere environment in advance, and the antimony-based precursor is gradually heated from room temperature to 1000-1300° C., and then calcined at 1000-1300° C. for 2-4 hours to obtain an antimony-based intermediate. Specifically, the inert atmosphere environment can be an atmosphere furnace, and the inert atmosphere used can be an argon atmosphere, and the heating rate can be 2-10° C. / min.

[0041] In some embodiments, in the process of performing step S2 to prepare the acidified carbon nanotubes, the carbon nanotubes are immersed in nitric acid and then filtered and dried to prepare the acidified carbon nanotubes. In fact, the concentration of the nitric acid used is in the range of 70-80%, and the carbon nanotubes used can be at least one of single-walled carbon nanotubes and multi-walled carbon nanotubes.

[0042] Specifically, in the process of preparing the acidified carbon nanotubes in step S2, the carbon nanotubes are immersed in nitric acid for 20-30 hours and then filtered, the filtered product is repeatedly rinsed with deionized water, and the washed filtered product is dried at 50-80° C. for 10-14 hours to prepare the acidified carbon nanotubes.

[0043] In some embodiments, the process of preparing modified carbon nanotubes in step S2 includes:

[0044] The acidified carbon nanotubes are stirred, filtered and dried in a siloxane solution to obtain activated carbon nanotubes;

[0045] The activated carbon nanotubes are dispersed in an organic sodium modification solution, stirred and dispersed at 50-60° C. for 5-6 hours, and then filtered and dried to obtain modified carbon nanotubes.

[0046] In fact, when the acidified carbon nanotubes are stirred, filtered and dried in a siloxane solution, the solute of the siloxane solution used includes at least one of γ-aminopropyltrimethoxysilane (γ-APS) and γ-glycidyloxypropyltrimethoxysilane (KH560).

[0047] Specifically, when the acidified carbon nanotubes are stirred, filtered and dried in the siloxane solution, the solid-to-liquid ratio of the acidified carbon nanotubes to the siloxane solution is 0.05-0.07, and the solute concentration in the siloxane solution is 80-90% of the saturated concentration.

[0048] In fact, when the activated carbon nanotubes are dispersed in the organic sodium modified solution, the solute of the organic sodium modified solution used includes at least one of disodium ethylenediaminetetraacetic acid and trisodium cyanurate, and the solid-liquid ratio of the activated carbon nanotubes to the organic sodium modified solution is 0.05-0.08, and the solute concentration in the organic sodium modified solution is 70-90% of the saturated concentration.

[0049] In some embodiments, when performing step S3, when the antimony-based intermediate, sodium polyacrylate and modified carbon nanotubes are dispersed to prepare a suspension, the liquid environment used for the suspension is deionized water, and the solid-liquid ratio of the suspension is 0.03-0.06.

[0050] See also Figure 2 The present invention also provides an antimony-based composite negative electrode material prepared by any of the above embodiments, wherein the antimony metal powder 1 is adsorbed on the surface defect position of the amorphous carbon 2, and after being composited with the modified carbon nanotubes 3, the three-dimensional conductive network formed by the modified carbon nanotubes 3 is wrapped in the outermost layer of the antimony metal powder 1 and the amorphous carbon 2. The carbon skeleton formed by the amorphous carbon 2 and the three-dimensional conductive network formed by the modified carbon nanotubes are intertwined with each other, and the antimony-based metal powder 1 is locked in the skeleton gap, thereby effectively suppressing the antimony-based expansion effect of the antimony metal powder 1 in the process of sodium ion insertion and extraction, and improving the overall conductivity and electrochemical performance of the negative electrode material.

[0051] Example 1

[0052] This embodiment 1 provides a method for preparing an antimony-based composite negative electrode material, comprising the following steps:

[0053] S1. Preparation of antimony-based intermediate: 4 g of micron-sized antimony metal powder and 5.5 g of oil-soluble phenolic resin were mixed and placed in a ball mill, with a ball-to-material ratio of 15 and a rotation speed of 500 rpm. After ball milling for 8 h, the solids obtained by filtration were transferred to a drying oven and dried at 70° C. for 12 h to obtain an antimony-based precursor. The antimony-based precursor was transferred to a tubular furnace filled with argon gas, heated from room temperature to 1200° C. at a rate of 5° C. / min, and then kept warm and calcined for 3 h to obtain an antimony-based intermediate.

[0054] S2, preparation of modified carbon nanotubes: multi-walled carbon nanotubes were soaked in 75% nitric acid for 25 hours and then filtered, the filtered product was rinsed three times with deionized water, and the washed filtered product was placed in a drying oven at 70°C for 12 hours to obtain acidified carbon nanotubes; the acidified carbon nanotubes were added to a siloxane solution (85% of the saturated concentration of KH560) at a solid-liquid ratio of 0.06, and the filtered product was washed after being dispersed for 3 hours with mechanical stirring at 200 rpm, and the washed filtered product was placed in a drying oven at 60°C for 8 hours to obtain activated carbon nanotubes; the activated carbon nanotubes were dispersed in an organic sodium modification solution (80% of the saturated concentration of disodium salt of ethylenediaminetetraacetic acid) at a solid-liquid ratio of 0.06, and the filtered product was washed after being dispersed for 3 hours with mechanical stirring at 200 rpm, and the washed filtered product was placed in a drying oven at 60°C for 8 hours to obtain modified carbon nanotubes;

[0055] S3. Preparation of antimony-based composite negative electrode material: 4.0 g of antimony-based intermediate and 0.5 g of modified carbon nanotubes were added into 78 g of deionized water and magnetically stirred to form a suspension. A spray drying device was used and the inlet air temperature was set to 160° C. to spray dry the suspension to obtain a powdered antimony-based composite negative electrode material.

[0056] Example 2

[0057] This embodiment 2 provides a method for preparing an antimony-based composite negative electrode material, which is different from the embodiment 1 in that 5.5 g of asphalt is selected as an amorphous carbon precursor in step S1.

[0058] Example 3

[0059] This embodiment 3 provides a method for preparing an antimony-based composite negative electrode material, which is different from embodiment 1 in that in step S3, 4.0 g of antimony-based intermediate, 0.5 g of sodium polyacrylate and 0.5 g of modified carbon nanotubes are added to 78 g of deionized water and magnetically stirred to form a suspension.

[0060] Comparative Example 1

[0061] This comparative example 1 provides a method for preparing an antimony-based composite negative electrode material, which is different from Example 1 in that: S3, 4.0 g of antimony-based intermediate and 0.5 g of modified carbon nanotubes are added to 78 g of deionized water and magnetically stirred to form a suspension, then allowed to settle, and filtered and dried to obtain a powdered antimony-based composite negative electrode material.

[0062] Comparative Example 2

[0063] This comparative example 2 provides a method for preparing an antimony-based composite negative electrode material, which is different from Example 1 in that step S2 and step S3 are not performed, and the antimony-based intermediate obtained after completing step S1 is the antimony-based composite negative electrode material.

[0064] Comparative Example 3

[0065] This comparative example 3 provides a method for preparing an antimony-based composite negative electrode material, which is different from that of example 1 in that step S2 is not performed, and multi-walled carbon nanotubes are directly used in step S3.

[0066] Comparative Example 4

[0067] Comparative Example 4 provides a method for preparing an antimony-based composite negative electrode material, which is different from Example 1 in that: in step S2, activated carbon nanotubes are dispersed in a saturated solution of sodium dodecyl sulfate at a solid-to-liquid ratio of 0.06.

[0068] Comparative Example 5

[0069] This comparative example 5 provides a method for preparing an antimony-based composite negative electrode material, which is different from that of Example 1 in that: in step S3, the antimony-based intermediate and the modified carbon nanotubes are fully ground and then calcined at 500° C. in an argon atmosphere for 3 hours to obtain an antimony-based composite negative electrode material.

[0070] Comparative Example 6

[0071] This comparative example 6 provides a method for preparing an antimony-based composite negative electrode material, which is different from Example 1 in that: in step S3, after a powdered material is obtained using a spray drying device, the powdered material is calcined for 3 hours in an argon atmosphere at 300°C to obtain an antimony-based composite negative electrode material.

[0072] Comparative Example 7

[0073] This comparative example 7 provides a method for preparing an antimony-based composite negative electrode material, which is different from Example 1 in that step S2 is not performed, and in step S3, 0.5 g of multi-walled carbon nanotubes, 4.0 g of antimony-based intermediates, and 0.5 g of sodium polyacrylate are directly used to prepare a suspension.

[0074] Performance Testing

[0075] The antimony-based composite negative electrode materials prepared in Examples 1 to 3 and Comparative Examples 1 to 7 were assembled into sodium ion button half-cells, and a mixed solution of 1M NaClO4 (sodium perchlorate) / EC (ethylene carbonate):DEC (diethyl carbonate) in a volume ratio of 1:1 was used as an electrolyte. A cycle performance test was carried out under the test conditions of 0.01-2.5V and a current density of 100mA / g. The test results are shown in FIG. Figure 3 shown.

[0076] from Figure 3 It can be seen that Example 1 and Example 2 provided by the present invention have good initial charge specific capacity, and at the same time, the capacity retention rate is good during a long cycle. Therefore, it can be explained that the negative electrode material prepared by the method provided by the present invention has good cycle stability and capacity retention performance. At the same time, it can be seen that sodium polyacrylate is added in Example 3 to improve the cycle stability of the negative electrode material by promoting the dispersion uniformity of the antimony-based intermediate and the modified carbon nanotubes. At the same time, sodium polyacrylate can also be organically combined with the organic sodium on the surface of the modified carbon nanotubes, which is conducive to the formation of an SEI film on the surface of the negative electrode material, thereby providing better protection for the negative electrode material.

[0077] from Figure 3 It can also be seen that in Example 1, since spray drying was not performed, the bonding performance between the antimony-based intermediate and the modified carbon nanotubes was poor, resulting in a serious decrease in capacity during the cycle. In Example 2, since the antimony-based intermediate was directly used as the negative electrode material, it was difficult to suppress the antimony-based antimony-based expansion effect. In Example 3, directly using multi-arm carbon nanotubes can also improve the cycle stability of the negative electrode material. However, compared with Examples 1 and 2, it can be explained that the present invention has an obvious positive effect by modifying the multi-arm carbon nanotubes.

[0078] And from Figure 2 It can also be seen that in Comparative Example 4, the use of sodium dodecyl sulfate as organic sodium and the composite with activated carbon nanotubes cannot significantly improve the cycle performance and rate performance of the negative electrode material. This is because sodium dodecyl sulfate is only used as a dispersant, and improving the dispersion performance of the antimony-based intermediate and the carbon nanotubes can only slightly improve the cycle performance of the battery.

[0079] In Comparative Example 5, after the antimony-based intermediate and the modified carbon nanotubes are ground, the carbon coating structure formed on the surface of the antimony-based intermediate is destroyed, resulting in the exposure of the antimony metal powder in the antimony-based intermediate. Figure 3 As shown, the cycle performance of the negative electrode material in Comparative Example 5 is significantly reduced.

[0080] In Example 6, spray drying is performed followed by high-temperature calcination, so that the internal organic sodium is carbonized into an inorganic carbon network structure. Although this can improve the anchoring ability of the antimony metal powder in the antimony-based composite material and the density of the carbon network structure, the SEI film structure formed by the organic sodium is lacking, and the cycle performance still shows a significant decline.

[0081] In Comparative Example 7, after spray drying with multi-arm carbon nanotubes, antimony-based intermediates and sodium polyacrylate, sodium polyacrylate can only have an effect similar to that of sodium dodecyl sulfate, and has no obvious effect on the cycle performance of the negative electrode material. In addition, sodium polyacrylate is also difficult to form an SEI film structure when used as a negative electrode material.

[0082] Although the embodiments of the present invention are described in detail above, it is obvious to those skilled in the art that various modifications and variations can be made to these embodiments. However, it should be understood that such modifications and variations are within the scope and spirit of the present invention as described in the claims. Moreover, the present invention described herein may have other embodiments and may be implemented or realized in a variety of ways.

Claims

1. A method for preparing an antimony-based composite negative electrode material, characterized in that: The following steps are involved: The antimony metal powder and the amorphous carbon precursor are mixed, ball-milled, dried and calcined to obtain an antimony-based intermediate; The surface of the carbon nanotubes is subjected to acidification treatment to obtain acidified carbon nanotubes, and the acidified carbon nanotubes are dispersed in an organic sodium modification solution, stirred, filtered, and dried to obtain modified carbon nanotubes; the solute of the organic sodium modification solution is disodium ethylenediaminetetraacetic acid; The antimony-based intermediate, sodium polyacrylate and the modified carbon nanotubes are mixed and dispersed to obtain a suspension, and then spray-dried to obtain an antimony-based composite negative electrode material.

2. The preparation method according to claim 1, characterized in that: The process of mixing antimony metal powder and amorphous carbon precursor, ball-milling, drying and calcining to obtain an antimony-based intermediate includes: mixing antimony metal powder and amorphous carbon precursor in a mass ratio of 0.5-1, ball-milling, filtering and drying to obtain an antimony-based precursor; and calcining the antimony-based precursor in an inert atmosphere at 1000-1300° C. for 2-4 hours to obtain an antimony-based intermediate.

3. The preparation method according to claim 2, characterized in that: The process of mixing antimony metal powder and amorphous carbon precursor, ball-milling and then filtering and drying to obtain an antimony-based precursor includes: mixing antimony metal powder and amorphous carbon precursor in a mass ratio of 0.5-1, ball-milling and then filtering, and placing the filtered product at 50-80° C. for 10-14 hours to obtain an antimony-based precursor.

4. The preparation method according to claim 1, characterized in that: The process of performing surface acidification treatment on carbon nanotubes to obtain acidified carbon nanotubes comprises: soaking the carbon nanotubes in nitric acid, then filtering and drying to obtain the acidified carbon nanotubes.

5. The preparation method according to claim 4, characterized in that: The process of surface acidifying carbon nanotubes to obtain acidified carbon nanotubes includes: soaking the carbon nanotubes in nitric acid for 20-30 hours and then filtering, washing the filtered product with deionized water and drying it at 50-80° C. for 10-14 hours to obtain the acidified carbon nanotubes.

6. The preparation method according to claim 1, characterized in that: The process of dispersing the acidified carbon nanotubes in an organic sodium modified solution, stirring, filtering and drying comprises: Stirring, filtering and drying the acidified carbon nanotubes in a siloxane solution to obtain activated carbon nanotubes; The activated carbon nanotubes are dispersed in an organic sodium modification solution, stirred and dispersed at 50-60° C. for 5-6 hours, and then filtered and dried.

7. The preparation method according to claim 6, characterized in that: When the acidified carbon nanotubes are stirred and filtered in a siloxane solution, the solute of the siloxane solution includes at least one of γ-aminopropyltrimethoxysilane and γ-glycidyloxypropyltrimethoxysilane.

8. An antimony-based composite negative electrode material prepared by the preparation method according to any one of claims 1 to 7.

9. Use of the antimony-based composite negative electrode material prepared by the preparation method according to any one of claims 1 to 7 in a sodium ion battery.

Citation Information

Patent Citations

  • Negative pole made of nanometer antimony / graphite nanosheet composite material of lithium ion battery and preparation method thereof

    CN101593825A

  • Antimony-carbon nano-tube-carbon composite material, as well as preparation method and application thereof

    CN108899504A

  • Three-dimensional porous titanium-antimony-doped hard carbon composite material and preparation method thereof

    CN117497729A

  • Negative electrode material, negative electrode using the same, and lithium ion secondary battery using the negative electrode

    JP2004303613A