Composite positive electrode material, preparation method thereof, positive electrode slurry, positive electrode plate and lithium ion battery

By introducing B2O3 and TeO3 into lithium iron phosphate and carbon nanotubes to prepare secondary balls and coat additives, the problems of density and preparation complexity of composite positive electrode materials are solved, the conductive performance and cycle stability are improved, and the process is simplified process.

CN119092667APending Publication Date: 2024-12-06JIANGSU TIANHE ENERGY STORAGE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411189995.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The simple physical mixing of existing lithium iron phosphate and carbon nanotubes leads to the incontinuous density of composite positive electrode materials, affecting the conductivity, mechanical properties and cycle stability, and the complex preparation process is not conducive to industrialization.

Method used

B2O3 and TeO3 were introduced into lithium iron phosphate and carbon nanotubes to prepare secondary spheres, and the liquid phase was formed by melting at lower temperatures, which prompted the lithium iron phosphate and carbon nanotubes to sinter them tightly at lower temperatures and wrapped them on the surface of the secondary spheres Covering additives to improve the degree of bonding and compaction density of materials.

Benefits of technology

The conductive performance and cyclic stability of the composite positive electrode material are improved, the sintering temperature is reduced, the high-temperature burnout of carbon nanotubes is reduced, the preparation process is simplified, and the pressure resistance of the material is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092667A_ABST
    Figure CN119092667A_ABST
Patent Text Reader

Abstract

The invention discloses a composite positive electrode material and a preparation method thereof, positive electrode slurry, a positive electrode plate and a lithium ion battery. The composite positive electrode material comprises a secondary ball and an auxiliary agent layer coating the surface of the secondary ball, the secondary balls are formed by aggregating primary particles; the secondary sphere is prepared from the following materials: lithium iron phosphate, a carbon nano tube, B2O3 and TeO3; and the material of the auxiliary agent layer is selected from one or more of LiNbO3, LiGaO3, LiGeO3 and LiTaO3. The prepared composite positive electrode material is high in compaction density, excellent in conductivity and cycling stability, simple in preparation process and low in sintering temperature in the preparation process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of lithium-ion batteries, and in particular relates to a composite positive electrode material, a preparation method thereof, a positive electrode slurry, a positive electrode sheet and a lithium-ion battery. Background Art

[0002] As one of the representatives of new energy, lithium-ion batteries have been booming in the fields of electric vehicles and large-scale energy storage in recent years. The cathode material accounts for more than 45% of the composition and cost of lithium-ion batteries, so the improvement of cathode materials is the focus of improving the performance of lithium-ion batteries. The olivine structure of lithium iron phosphate (LiFePO4) gives it good thermal stability, cycle stability and safety. Lithium iron phosphate has the advantages of stable charge and discharge performance, wide source, high specific capacity, and green environmental protection. These make lithium iron phosphate one of the most promising cathode materials for lithium-ion batteries. However, the low lithium ion diffusion coefficient (10-14cm 2 / s) and low electronic conductivity (about 10 -9 s / cm) inhibits the electrochemical performance of LiFePO4, so the improvement of lithium iron phosphate is the focus of improving the performance of lithium-ion batteries.

[0003] Existing improvement measures improve lithium iron phosphate materials by mixing and sintering lithium iron phosphate and carbon nanotubes. However, the simple physical mixing and sintering of lithium iron phosphate and carbon nanotubes will result in the composite positive electrode material being not dense, and thus unable to form an effective carbon nanotube conductive network, affecting the conductive properties, mechanical properties and cycle stability of the positive electrode material. In addition, this preparation process is difficult to operate and has strict equipment requirements, which is not conducive to industrialization.

[0004] Therefore, it is urgent to develop a composite positive electrode material with excellent conductivity, excellent mechanical properties, excellent cycle stability and simple preparation process. Summary of the invention

[0005] In order to solve the problems existing in the prior art, the present invention provides a composite positive electrode material, a preparation method thereof, a positive electrode slurry, a positive electrode sheet and a lithium ion battery.

[0006] B2O3 and TeO3 are introduced into the secondary balls, and B2O3 and TeO3 are melted at a relatively low temperature to generate a liquid phase, which promotes the primary ball particles containing lithium iron phosphate and carbon nanotubes to be sintered and compacted at a relatively low temperature, thereby improving the degree of bonding between the carbon nanotubes and the lithium iron phosphate, improving the compaction degree of the secondary balls, improving the conductivity of the composite positive electrode material, reducing the sintering temperature in the preparation process of the composite positive electrode material, and reducing the high-temperature burning of the carbon nanotubes; the invention is coated with an auxiliary agent, which plays a toughening role, increases the compaction density of the composite positive electrode material, and improves Cyclic stability of composite positive electrode materials; the improvements of the secondary balls and the additive layer coated on the surface of the secondary balls in the composite positive electrode material of the present invention have a synergistic effect. On the one hand, the present invention avoids the liquid phase formed when B2O3 and TeO3 reach the melting temperature from overflowing the secondary balls through the steps of first coating the additive and then sintering, thereby improving the compaction density of the composite positive electrode material. On the other hand, the addition of B2O3 and TeO3 enhances the compaction degree of a single secondary ball, and the addition of the additive further enhances the overall pressure resistance. The two synergistically promote the high compaction performance of the composite positive electrode material.

[0007] Specifically, the present invention provides a composite positive electrode material, which includes secondary balls and an auxiliary agent layer coated on the surface of the secondary balls; the secondary balls are formed by agglomeration of primary particles; the material of the secondary balls includes lithium iron phosphate, carbon nanotubes, B2O3 and TeO3; the material of the auxiliary agent layer is selected from one or more of LiNbO3, LiGaO3, LiGeO3 and LiTaO3.

[0008] In one or more embodiments, the particle size D50 of the composite positive electrode material is 5 to 25 μm, preferably 5 to 15 μm.

[0009] In one or more embodiments, in the composite positive electrode material, the mass fraction of the secondary spheres is 98 wt % to 99.5 wt %.

[0010] In one or more embodiments, in the composite positive electrode material, the mass fraction of the auxiliary agent layer is 0.5 wt % to 2 wt %.

[0011] In one or more embodiments, in the secondary sphere, the mass of the carbon nanotubes is 0.4 wt % to 1 wt % of the mass of the lithium iron phosphate.

[0012] In one or more embodiments, in the secondary ball, the mass of B2O3 is 0.5wt% to 3wt% of the mass of lithium iron phosphate.

[0013] In one or more embodiments, in the secondary ball, the mass of TeO3 is 0.1 wt% to 1 wt% of the mass of lithium iron phosphate.

[0015] The present invention provides a method for preparing the composite positive electrode material of the present invention, the method comprising the following steps:

[0016] (1) mixing a lithium source, an iron source, a phosphorus source, carbon nanotubes, B2O3 and TeO3 uniformly, grinding them in water to obtain a primary particle precursor, and then spraying and balling them to obtain a secondary ball precursor agglomerated from the primary particle precursor;

[0017] (2) using a fusion machine to coat the surface of the secondary ball precursor obtained in step (1) with an auxiliary agent to obtain a secondary ball precursor coated with the auxiliary agent;

[0018] (3) Sintering the secondary ball precursor with the surface coated with the auxiliary agent obtained in step (2) to form secondary balls formed by agglomeration of primary particles and an auxiliary agent layer coated on the surface of the secondary balls, thereby obtaining the composite positive electrode material.

[0019] In one or more embodiments, in step (1), the lithium source is selected from one or more of lithium carbonate, lithium hydroxide, lithium phosphate and lithium dihydrogen phosphate.

[0020] In one or more embodiments, in step (1), the iron source is selected from one or more of ferric phosphate, ferrous oxide and ferrous oxalate.

[0021] In one or more embodiments, in step (1), the phosphorus source is selected from one or more of ferric phosphate, lithium dihydrogen phosphate, phosphoric acid and monoammonium phosphate.

[0022] In one or more embodiments, in step (1), the molar ratio of the lithium element in the lithium source to the iron element in the iron source is 1:(0.9-1.05).

[0023] In one or more embodiments, in step (1), the molar ratio of the lithium element in the lithium source to the phosphorus element in the phosphorus source is 1:(1-1.05).

[0024] In one or more embodiments, in step (1), the particle size D50 of the primary particle precursor is 150 to 500 nm, preferably 150 to 250 nm.

[0025] In one or more embodiments, in step (1), the particle size D50 of the secondary sphere precursor is 5 to 25 μm, preferably 5 to 15 μm.

[0026] In one or more embodiments, in step (2), the operating temperature of the fusion machine is 15-50°C.

[0027] In one or more embodiments, in step (2), the rotation speed of the fusion machine is 200 to 1000 r / min.

[0028] In one or more embodiments, in step (3), the sintering is performed in a protective atmosphere, and the protective atmosphere is preferably nitrogen or argon.

[0030] In one or more embodiments, in step (3), the sintering temperature is 700-800°C.

[0031] In one or more embodiments, in step (3), the sintering time is 5 to 15 hours.

[0032] The present invention provides a positive electrode slurry comprising the composite positive electrode material of the present invention or the composite positive electrode material prepared by the method of the present invention.

[0033] The present invention provides a positive electrode sheet comprising the composite positive electrode material of the present invention or the composite positive electrode material prepared by the method of the present invention.

[0034] The present invention provides a lithium ion battery comprising the positive electrode plate of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is a 20K-fold scanning electron microscope (SEM) image of the spherical section of the composite positive electrode material prepared in Example 1 of the present invention.

[0036] Figure 2 This is a 20K-fold scanning electron microscope (SEM) image of a spherical section of the composite positive electrode material prepared in Comparative Example 1 of the present invention.

[0037] Figure 3 This is a 50K-fold scanning electron microscope (SEM) image of the surface of the sphere of the composite positive electrode material prepared in Example 1 of the present invention.

[0038] Figure 4 This is a 50K-fold scanning electron microscope (SEM) image of the spherical surface of the composite positive electrode material prepared in Comparative Example 1 of the present invention.

[0039] Figure 5 This is a 10K-fold scanning electron microscope (SEM) image of the spherical surface of the composite positive electrode material prepared in Example 1 of the present invention.

[0040] Figure 6 This is a 10K-fold scanning electron microscope (SEM) image of the spherical surface of the composite positive electrode material prepared in Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0041] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.

[0042] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.

[0043] Herein, “comprising”, “including”, “containing” and similar terms encompass the meanings of “consisting essentially of” and “consisting of”. For example, when “A comprises B and C” is disclosed herein, “A consists essentially of B and C” and “A consists of B and C” should be deemed to be disclosed herein.

[0044] In this article, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are only for brevity and convenience. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values ​​within the range (including integers and fractions).

[0045] In this document, unless otherwise specified, percentage refers to mass percentage and ratio refers to mass ratio.

[0046] Herein, when describing embodiments or examples, it should be understood that they are not used to limit the present invention to these embodiments or examples. On the contrary, all substitutes, improvements and equivalents of the methods and materials described in the present invention can be included in the scope limited by the claims.

[0047] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.

[0048] The invention provides a composite positive electrode material, which comprises a secondary ball and an auxiliary agent layer coated on the surface of the secondary ball.

[0049] In the present invention, the secondary balls are formed by agglomeration of primary particles, and the materials of the secondary balls include lithium iron phosphate, carbon nanotubes, B2O3 and TeO3. In the present invention, B2O3 and TeO3 are introduced into lithium iron phosphate and carbon nanotubes to prepare secondary balls, and B2O3 and TeO3 are melted at a relatively low temperature to generate a liquid phase, thereby preventing the closure of pores caused by crystal growth during the sintering process, and promoting the sintering and compacting of lithium iron phosphate and carbon nanotubes at a relatively low temperature, thereby improving the degree of bonding between carbon nanotubes and lithium iron phosphate, improving the compactness of the secondary balls, improving the conductivity and cycle stability of the composite positive electrode material, reducing the sintering temperature during the preparation of the composite positive electrode material, and reducing the high-temperature burning of the carbon nanotubes.

[0051] In the present invention, B2O3 and TeO3 have a synergistic effect. When the two exist at the same time, the mechanical properties and cycle stability of the composite positive electrode material can be greatly improved, thereby improving the cycle performance of the lithium battery.

[0052] In the present invention, the material of the auxiliary agent layer can be one or more selected from LiNbO3, LiGaO3, LiGeO3 and LiTaO3. The auxiliary agent of the present invention is a piezoelectric ferroelectric material. When the crack is extended to the auxiliary agent, a part of the mechanical energy of the crack extension is dissipated by the electromechanical energy conversion of the piezoelectric material on the one hand, and on the other hand, the stress field at the crack tip will cause the electric domain to flip and consume energy. At the same time, the electric domain flipping changes the stress state of the crack from the tensile stress state to the compressive stress state, which has the effect of closing the crack and hindering the crack extension. Therefore, the addition of the auxiliary agent of the present invention can play a toughening role, which is conducive to the positive electrode sheet to withstand higher pressure during rolling, and increase the compaction density of the positive electrode sheet. At the same time, the auxiliary agent is uniformly coated outside the secondary ball, which can improve the cycle stability of the composite positive electrode material. In summary, by using the auxiliary agent for coating, the mechanical properties and cycle stability of the composite positive electrode material can be improved, thereby improving the cycle performance of the lithium battery.

[0053] In the present invention, the particle size D50 of the composite positive electrode material can be 5 to 25 μm, preferably 5 to 15 μm, such as 5 μm, 7 μm, 9 μm, 11 μm, 13 μm, 15 μm. The present invention controls the particle size D50 of the composite positive electrode material within the above range, which is beneficial to improving the processing performance of the composite positive electrode material during battery processing.

[0054] In the present invention, in the composite positive electrode material, the mass fraction of the secondary balls can be 98wt% to 99.5wt%, such as 98wt%, 98.2wt%, 98.4wt%, 98.6wt%, 98.8wt%, 99wt%, 99.2wt%, 99.4wt%. The present invention controls the mass fraction of the secondary balls in the composite positive electrode material within the above range, which is beneficial to improving the mechanical properties and cycle stability of the composite positive electrode material and improving the cycle performance of the corresponding lithium battery.

[0055] In the present invention, in the composite positive electrode material, the mass fraction of the auxiliary agent layer can be 0.5wt% to 2wt%, such as 0.6wt%, 0.8wt%, 1wt%, 1.2wt%, 1.4wt%, 1.6wt%, 1.8wt%, 2wt%. The present invention controls the mass fraction of the auxiliary agent layer in the composite positive electrode material within the above range, which is beneficial to improving the mechanical properties and cycle stability of the composite positive electrode material and improving the cycle performance of the corresponding lithium battery.

[0056] In the present invention, the mass of carbon nanotubes in the secondary balls can be 0.4wt% to 1wt% of the mass of lithium iron phosphate, such as 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt%, 1wt%. The present invention controls the mass of carbon nanotubes in the secondary balls within the above range, which is beneficial to improving the mechanical properties and cycle stability of the composite positive electrode material and improving the cycle performance of the corresponding lithium battery.

[0057] In the present invention, the mass of B2O3 in the secondary ball can be 0.5wt% to 3wt% of the mass of lithium iron phosphate, such as 0.5wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%. The present invention controls the mass of B2O3 in the secondary ball within the above range, which is beneficial to improving the mechanical properties and cycle stability of the composite positive electrode material and improving the cycle performance of the corresponding lithium battery.

[0058] In the present invention, the mass of TeO3 in the secondary ball can be 0.1wt% to 1wt% of the mass of lithium iron phosphate, such as 0.1wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt%, 1wt%. The present invention controls the mass of TeO3 in the secondary ball within the above range, which is beneficial to improving the mechanical properties and cycle stability of the composite positive electrode material and improving the cycle performance of the corresponding lithium battery.

[0059] The present invention provides a method for preparing a composite positive electrode material, the method comprising the following steps:

[0060] (1) mixing a lithium source, an iron source, a phosphorus source, carbon nanotubes, B2O3 and TeO3 uniformly, grinding them in water to obtain a primary particle precursor, and then spraying and balling them to obtain a secondary ball precursor agglomerated from the primary particle precursor;

[0061] (2) using a fusion machine to coat the surface of the secondary ball precursor obtained in step (1) with an auxiliary agent to obtain a secondary ball precursor coated with the auxiliary agent;

[0062] (3) Sintering the secondary ball precursor with the surface coated with the auxiliary agent obtained in step (2) to form secondary balls formed by agglomeration of primary particles and an auxiliary agent layer coated on the surface of the secondary balls, thereby obtaining a composite positive electrode material.

[0063] In the present invention, spray spheronization allows small-sized primary particle precursors to agglomerate into large-sized secondary spherical precursors.

[0064] In the present invention, during the preparation process of the composite positive electrode material, the auxiliary agent is first coated and then sintered, which avoids the liquid phase formed when B2O3 and TeO3 reach the melting temperature from overflowing the secondary balls, thereby improving the compaction density and cycle stability of the composite positive electrode material, and further improving the cycle stability of the corresponding lithium battery.

[0065] In step (1), the lithium source may be one or more selected from lithium carbonate, lithium hydroxide, lithium phosphate and lithium dihydrogen phosphate.

[0066] In step (1), the iron source may be one or more selected from ferric phosphate, ferrous oxide and ferrous oxalate.

[0068] In step (1), the phosphorus source may be one or more selected from the group consisting of iron phosphate, lithium dihydrogen phosphate, phosphoric acid and monoammonium phosphate.

[0069] In step (1), the molar ratio of lithium in the lithium source to iron in the iron source can be 1:(0.9-1.05), for example, 1:0.92, 1:0.94, 1:0.96, 1:0.98, 1:1, 1:1.02, 1:1.04, 1:1.05.

[0070] In step (1), the molar ratio of lithium in the lithium source to phosphorus in the phosphorus source can be 1:(1-1.05), for example, 1:1, 1:1.01, 1:1.02, 1:1.03, 1:1.04, 1:1.05.

[0071] In step (1), the particle size D50 of the primary particle precursor can be 150 to 500 nm, preferably 150 to 250 nm, for example, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, or 100 nm.

[0072] In step (1), the particle size D50 of the secondary sphere precursor can be 5 to 25 μm, preferably 5 to 15 μm, for example 5 μm, 7 μm, 9 μm, 11 μm, 13 μm, 15 μm.

[0073] In step (2), the operating temperature of the fusion machine can be 15-50°C, for example, 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C.

[0074] In step (2), the rotation speed of the fusion machine can be 200-1000 r / min, for example, 200 r / min, 300 r / min, 400 r / min, 500 r / min, 600 r / min, 700 r / min, 800 r / min, 900 r / min, 1000 r / min.

[0075] In step (3), sintering can be carried out in a protective atmosphere, and the protective atmosphere is preferably nitrogen or argon.

[0076] In step (3), the sintering temperature may be 700-800° C., for example, 700° C., 710° C., 720° C., 730° C., 740° C., 750° C., 760° C., 770° C., 780° C., 790° C., 800° C. The present invention controls the sintering temperature within the above range, which is beneficial to reducing the high-temperature burning of carbon nanotubes, improving the mechanical properties and cycle stability of the composite positive electrode material, improving the cycle performance of the corresponding lithium battery, and reducing energy loss.

[0077] In step (3), the sintering time can be 5 to 15 hours, for example, 5 hours, 7 hours, 9 hours, 11 hours, 13 hours, or 15 hours.

[0078] The present invention provides a positive electrode slurry comprising a composite positive electrode material of the present invention. The positive electrode slurry comprises a composite positive electrode material of the present invention, a conductive agent, a binder and a solvent. The conductive agent may be commonly used in the art, preferably selected from one or more of conductive carbon black (SP), carbon fiber (CF), acetylene black, Ketjen black, graphene and carbon nanotubes. The binder may be commonly used in the art, preferably selected from one or more of fluorine-containing resins, polypropylene resins, fiber-type binders and polyimide-type binders. In some embodiments, the fluorine-containing resin is polyvinylidene fluoride (PVDF). The solvent may be commonly used in the art, such as N-methylpyrrolidone. The mass ratio of each component in the positive electrode slurry may be conventional. The solid content of the positive electrode slurry may be conventional, for example, the solid content of the positive electrode slurry may be 55wt% to 65wt%. The viscosity of the positive electrode slurry may be conventional, for example, the viscosity of the positive electrode slurry may be 5000 to 15000 mPa·S, preferably 5000 to 10000 mPa·S or 10000 to 15000 mPa·S.

[0079] The present invention provides a positive electrode sheet comprising the composite positive electrode material of the present invention. Specifically, the positive electrode sheet generally includes a positive electrode current collector and a positive electrode material layer formed on the surface of the positive electrode current collector. The positive electrode current collector can be copper foil, aluminum foil, titanium foil, nickel foil, iron foil, zinc foil, etc., preferably aluminum foil. The positive electrode material layer includes the positive electrode material of the present invention, a conductive agent and a binder. The positive electrode slurry comprising the composite positive electrode material of the present invention, a conductive agent, a binder and a solvent is coated on the positive electrode current collector, and then rolled, die-cut and baked to obtain a positive electrode sheet. The mass ratio of each component in the positive electrode material layer can be conventional. For example, based on the total weight of the positive electrode material layer, the mass of the positive electrode active material can be 94wt% to 98wt%, preferably 96wt% to 98wt%, the content of the conductive agent can be 0.5wt% to 5wt%, preferably 1wt% to 3wt%, for example 1wt%, 1.5wt%, 2wt%, 2.5wt%, and the content of the binder can be 2wt% to 4wt%, preferably 1.5wt% to 3wt%, for example 2.5wt%, 3wt%, 3.5wt%.

[0080] The present invention provides a lithium ion battery. The battery core of the lithium ion battery comprises the positive electrode sheet, the negative electrode sheet, a separator and an electrolyte.

[0081] The negative electrode sheet includes a negative electrode current collector and a negative electrode material layer disposed on the surface of the negative electrode current collector. The negative electrode current collector may be a material commonly used in the art with excellent conductivity, such as copper foil. The negative electrode material layer includes a negative electrode active material, a conductive agent and a binder. The negative electrode material layer is obtained by coating a negative electrode slurry containing a negative electrode active material, a conductive agent, a binder and a solvent onto the negative electrode current collector, and then drying and pressing. The negative electrode active material, the conductive agent and the binder may be added to a solvent to prepare the negative electrode slurry. The solvent of the negative electrode slurry may be a conventional solvent in the art, such as deionized water. The negative electrode active material may be one or more selected from graphite (including artificial graphite, natural graphite), silicon-carbon negative electrode, hard carbon and lithium titanate, the conductive agent is preferably selected from one or more of conductive carbon black (such as acetylene black, Ketjen black), carbon fiber, graphene and carbon nanotubes, and the binder is preferably selected from one or more of fluorine-containing resin, polypropylene resin, fiber-type binder, rubber-type binder and polyimide-type binder, such as styrene-butadiene rubber (SBR). The negative electrode material layer and the negative electrode slurry may further include a thickener such as sodium carboxymethylcellulose (CMC-Na).

[0082] The separator in the lithium ion battery of the present invention can be a polymer separator, a ceramic separator or a polymer / ceramic composite separator. The polymer separator includes a single-layer polymer separator and a multi-layer polymer separator. The single-layer polymer separator includes a polyethylene (PE) separator and a polypropylene (PP) separator.

[0083] The electrolyte in the lithium ion battery of the present invention generally comprises a solvent and a lithium salt. The electrolyte suitable for the present invention may be conventional, for example, the solvent may be selected from one or more of dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC) and propylene carbonate (PC); the lithium salt may be selected from one or more of lithium iron phosphate, lithium hexafluorophosphate (LiPF6), lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethylsulfonyl)imide, lithium bis(oxalatoborate), lithium difluorooxalatoborate and lithium tetrafluoroborate (LiBF4).

[0084] The present invention laminates and / or winds the positive electrode sheet, the negative electrode sheet and the separator, and packages them in a shell, and then undergoes drying, liquid injection (injection of electrolyte), packaging, standing, formation, and volume separation to obtain a lithium ion battery. The packaging process of the lithium ion battery of the present invention can be cylindrical, square or soft package. The cylindrical packaging generally adopts steel shell packaging, the square packaging generally adopts aluminum alloy and stainless steel packaging, and the soft package packaging generally adopts aluminum plastic film packaging. Therefore, the form of the lithium ion battery of the present invention is not particularly limited, and can be a cylindrical lithium ion battery, a soft package lithium ion battery or an aluminum shell lithium ion battery.

[0085] Compared with the prior art, the present invention has the following beneficial effects:

[0086] (1) The present invention introduces B2O3 and TeO3 into lithium iron phosphate and carbon nanotubes to prepare secondary balls. B2O3 and TeO3 melt at a relatively low temperature to generate a liquid phase, which promotes the sintering and compaction of primary ball particles containing lithium iron phosphate and carbon nanotubes at a relatively low temperature, thereby improving the degree of bonding between carbon nanotubes and lithium iron phosphate, increasing the compactness of secondary balls, improving the conductivity of the composite positive electrode material, reducing the sintering temperature in the preparation process of the composite positive electrode material, and reducing the high-temperature burning of carbon nanotubes;

[0087] (2) The present invention coats the secondary sphere surface with an additive, thereby improving the mechanical properties and cycle stability of the composite positive electrode material;

[0089] (3) The introduction of B2O3 and TeO3 into the composite positive electrode material of the present invention to prepare the secondary ball and the improvement of the coating auxiliary agent layer has a synergistic effect. On the one hand, the auxiliary agent is coated first and then sintered, which avoids the liquid phase formed when B2O3 and TeO3 reach the melting temperature from overflowing the secondary ball, thereby improving the compaction density of the composite positive electrode material. On the other hand, the addition of B2O3 and TeO3 enhances the compactness of the single secondary ball, and the addition of the auxiliary agent enhances the overall pressure resistance. The two synergistically promote the high compaction performance of the composite positive electrode material.

[0090] (4) The preparation method of the present invention is simple to operate and is easy to scale up for industrial production.

[0091] The present invention will be described below in the form of specific examples. It should be understood that these examples are merely illustrative and are not intended to limit the scope of the present invention. The methods, reagents and materials used in the examples are, unless otherwise stated, conventional methods, reagents and materials in the art. The raw material compounds in the examples can all be purchased through commercial routes.

[0092] Example 1

[0093] This embodiment prepares the composite positive electrode material according to the following steps:

[0094] (1) mixing iron phosphate, lithium carbonate, carbon nanotubes, B2O3 and TeO3 uniformly, wherein the molar ratio of lithium in the lithium source, iron in the iron source and phosphorus in the phosphorus source is 1:1:1; calculating the mass of lithium iron phosphate according to the iron source, the mass of carbon nanotubes is 0.5wt% of the mass of lithium iron phosphate, the mass of B2O3 is 1wt% of the mass of lithium iron phosphate, and the mass of TeO3 is 0.5wt% of the mass of lithium iron phosphate; grinding in water to obtain a primary particle precursor with a particle size D50 of 157nm, and then spraying and balling to obtain a secondary ball precursor agglomerated from the primary particle precursor, wherein the particle size D50 of the secondary ball precursor obtained by spraying and balling is 10μm;

[0095] (2) using a fusion machine to coat the surface of the secondary ball precursor obtained in step (1) with an auxiliary agent LiNbO3, thereby obtaining a secondary ball precursor with the surface coated with the auxiliary agent, wherein the mass of the auxiliary agent is 1wt% of the total mass of the auxiliary agent and the secondary ball precursor; the working temperature of the fusion machine is 25°C, and the speed of the fusion machine is 500r / min;

[0096] (3) Sintering the secondary ball precursor with the surface coating additive obtained in step (2) to obtain a composite positive electrode material (such as Figure 1 , Figure 3 , Figure 5 As shown), wherein the sintering atmosphere is nitrogen, the sintering temperature is 750°C, the sintering time is 10h, and the particle size D50 of the sintered composite positive electrode material is 9.6μm.

[0098] Example 2

[0099] This embodiment prepares the composite positive electrode material according to the following steps:

[0100] (1) mixing ferrous oxalate, lithium dihydrogen phosphate, monoammonium phosphate, carbon nanotubes, B2O3 and TeO3 uniformly, wherein the molar ratio of lithium in the lithium source, iron in the iron source and phosphorus in the phosphorus source is 1:0.9:1; calculating the mass of lithium iron phosphate according to the iron source, the mass of carbon nanotubes is 0.8wt% of the mass of lithium iron phosphate, the mass of B2O3 is 0.8wt% of the mass of lithium iron phosphate, and the mass of TeO3 is 0.8wt% of the mass of lithium iron phosphate; grinding in water to obtain a primary particle precursor with a particle size D50 of 184nm, and then spraying and balling to obtain a secondary ball precursor agglomerated from the primary particle precursor, wherein the particle size D50 of the secondary ball precursor obtained by spraying and balling is 8μm;

[0101] (2) using a fusion machine to coat the surface of the secondary ball precursor obtained in step (1) with an auxiliary agent LiNbO3, thereby obtaining a secondary ball precursor with the surface coated with the auxiliary agent, wherein the mass of the auxiliary agent is 1wt% of the total mass of the auxiliary agent and the secondary ball precursor; the working temperature of the fusion machine is 25°C, and the speed of the fusion machine is 500r / min;

[0102] (3) Sintering the secondary spherical precursor with the surface coating additive obtained in step (2) to obtain a composite positive electrode material, wherein the sintering atmosphere is nitrogen, the sintering temperature is 780° C., the sintering time is 8 h, and the particle size D50 of the sintered composite positive electrode material is 7.2 μm.

[0103] Example 3

[0104] This embodiment prepares the composite positive electrode material according to the following steps:

[0105] (1) mixing iron phosphate, lithium carbonate, carbon nanotubes, B2O3 and TeO3 uniformly, wherein the molar ratio of lithium in the lithium source, iron in the iron source and phosphorus in the phosphorus source is 1:1:1; calculating the mass of lithium iron phosphate according to the iron source, the mass of carbon nanotubes is 0.5wt% of the mass of lithium iron phosphate, the mass of B2O3 is 1wt% of the mass of lithium iron phosphate, and the mass of TeO3 is 0.5wt% of the mass of lithium iron phosphate; grinding in water to obtain a primary particle precursor with a particle size D50 of 166nm, and then spraying and balling to obtain a secondary ball precursor agglomerated from the primary particle precursor, wherein the particle size D50 of the secondary ball precursor obtained by spraying and balling is 13μm;

[0106] (2) using a fusion machine to coat the surface of the secondary ball precursor obtained in step (1) with an additive LiGaO3 to obtain a secondary ball precursor with the surface coated with the additive, wherein the mass of the additive is 1.5wt% of the total mass of the additive and the secondary ball precursor; the working temperature of the fusion machine is 40°C, and the speed of the fusion machine is 700r / min;

[0108] (3) Sintering the secondary spherical precursor with the surface coating additive obtained in step (2) to obtain a composite positive electrode material, wherein the sintering atmosphere is nitrogen, the sintering temperature is 720° C., the sintering time is 14 h, and the particle size D50 of the sintered composite positive electrode material is 11.8 μm.

[0109] Comparative Example 1

[0110] The other conditions of this comparative example are the same as those of Example 1, except that B2O3 and TeO3 are not added in this comparative example.

[0111] Comparative Example 2

[0112] The other conditions of this comparative example are the same as those of Example 1, except that B2O3 is not added in this comparative example.

[0113] Comparative Example 3

[0114] The other conditions of this comparative example are the same as those of Example 1, except that TeO3 is not added in this comparative example.

[0115] Comparative Example 4

[0116] The other conditions of this comparative example are the same as those of Example 1, except that this comparative example does not include a coating additive, that is, this comparative example does not include step (2), and the secondary spherical precursor agglomerated from the primary particle precursor obtained in step (1) is directly sintered.

[0117] Comparative Example 5

[0118] The other conditions of this comparative example are the same as those of Example 1, except that in this comparative example, the secondary sphere precursor agglomerated from the primary particle precursor is first sintered, and then the sintered secondary sphere precursor is coated with an additive.

[0119] Comparative Example 6

[0120] The other conditions of this comparative example are the same as those of Example 1, except that in step 245256

[0121] The sintering temperature in step (3) was set to 850°C.

[0122] Test Case

[0123] Compacted density test

[0124] The compaction density test of the composite positive electrode materials prepared in Examples 1-3 and Comparative Examples 1-6 was performed, and the specific operation was as follows:

[0125] Weigh 0.7g (d=0.0001) of the sample to be tested with an electronic balance, and enter the weight into the corresponding "mass" box on the panel of the compaction density meter. Pour the sample completely into the mold with the base installed, cover it gently to prevent the sample powder from spraying out of the mold, put the mold with the sample into the test position, press the start key, and when the pressure reaches 4800kg, read the value on the side instrument and enter it into the corresponding "height" box on the panel, and the density value will be automatically displayed. The test results of the compaction density of the composite positive electrode materials prepared in Examples 1-3 and Comparative Examples 1-6 are shown in Table 1.

[0126] Cyclic performance test

[0127] The lithium batteries assembled with the composite positive electrode materials prepared in Examples 1-3 and Comparative Examples 1-6 were subjected to cycle performance tests, and the specific operations were as follows:

[0128] (1) Preparation of positive electrode sheets: The composite positive electrode materials prepared in Examples 1-3 and Comparative Examples 1-6, the conductive agent acetylene black and the binder PVDF were mixed in a solvent N-methylpyrrolidone at a mass ratio of 94:3:3 to prepare a positive electrode slurry with a solid content of 65 wt %. The positive electrode slurry was evenly coated on the positive electrode current collector aluminum foil, and vacuum dried to obtain the corresponding positive electrode sheets;

[0129] (2) Preparing a negative electrode sheet: Graphite, thickener CMC, binder SBR, and conductive carbon black were mixed in water at a mass ratio of 95:1:2:2 to prepare a negative electrode slurry with a solid content of 50 wt%, and the negative electrode slurry was evenly coated on a negative electrode current collector Cu foil and cooled to obtain a negative electrode sheet;

[0130] (3) Assembling a lithium battery: Assemble the positive electrode sheet prepared in step (1), the negative electrode sheet prepared in step (2), a Celgard 2400 separator, and an electrolyte solution containing 1 mol / L solute of LiPF6 and a mixture of dimethyl carbonate and ethyl methyl carbonate in a volume ratio of 1:1 as solvent into a 18650 cylindrical lithium single cell;

[0131] (4) 2000 cycle capacity retention test: The prepared 18650 cylindrical lithium monomer battery was tested on the LAND battery test system of Wuhan Jinnuo Electronics Co., Ltd. at 25°C, with a charge and discharge voltage range of 2.0-3.65V and a current density of 1C. The first discharge specific capacity and the 2000th cycle discharge specific capacity of the battery were tested, and the 2000 cycle capacity retention rate was calculated. The 2000 cycle capacity retention rate = 2000th cycle discharge specific capacity / first discharge specific capacity. The test results of the cycle performance of the lithium batteries assembled with the composite positive electrode materials prepared in Examples 1-3 and Comparative Examples 1-6 are shown in Table 2.

[0132] Table 1: Compacted density of composite positive electrode materials prepared in Examples 1-3 and Comparative Examples 1-6

[0133] <![CDATA[Compaction density (g / cm 3 )]]> Example 1 2.69 Example 2 2.68 Example 3 2.68 Comparative Example 1 2.48 Comparative Example 2 2.54 Comparative Example 3 2.51 Comparative Example 4 2.47 Comparative Example 5 2.51 Comparative Example 6 2.60

[0134] Table 2: Cycling performance of lithium batteries assembled with composite positive electrode materials prepared in Examples 1-3 and Comparative Examples 1-6

[0135]

[0136]

[0137] It can be seen from Tables 1 and 2 that the compaction density of the composite positive electrode material prepared by adding B2O3 and TeO3 in Example 1 and the 2000 cycle capacity retention rate of the corresponding lithium battery are 0.21 g / cm higher than the compaction density of the composite positive electrode material prepared by adding no B2O3 and TeO3 in Comparative Example 1 and the 2000 cycle capacity retention rate of the corresponding lithium battery. 3 The compaction density of the composite positive electrode material prepared without adding B2O3 in Comparative Example 2 and the 2000 cycle capacity retention rate of the corresponding lithium battery are 0.06 g / cm higher than the compaction density of the composite positive electrode material prepared without adding B2O3 and TeO3 in Comparative Example 1 and the 2000 cycle capacity retention rate of the corresponding lithium battery. 3 The compaction density of the composite positive electrode material prepared without adding TeO3 in Comparative Example 3 and the 2000 cycle capacity retention rate of the corresponding lithium battery are 0.03 g / cm higher than the compaction density of the composite positive electrode material prepared without adding B2O3 and TeO3 in Comparative Example 1 and the 2000 cycle capacity retention rate of the corresponding lithium battery. 3 and 4.8%, from which it can be further known that the compaction density of the composite positive electrode material prepared by adding B2O3 and TeO3 in Example 1 and the 2000 cycle capacity retention rate of the corresponding lithium battery relative to the compaction density of the composite positive electrode material prepared without adding B2O3 and TeO3 in Comparative Example 1 and the increase in the compaction density of the corresponding lithium battery 2000 cycle capacity retention rate are much greater than the compaction density of the composite positive electrode material prepared without adding B2O3 in Comparative Example 2 and the 2000 cycle capacity retention rate of the corresponding lithium battery and the increase in the compaction density of the composite positive electrode material prepared without adding TeO3 in Comparative Example 3 relative to the composite positive electrode material prepared without adding B2O3 and TeO3 in Comparative Example 1 and the 2000 cycle capacity retention rate of the corresponding lithium battery, which illustrates that there is a synergistic effect between B2O3 and TeO3. When both exist at the same time, the mechanical properties and cycle stability of the composite positive electrode material can be greatly improved.

[0138] It can be seen from Tables 1 and 2 that compared with the composite positive electrode material prepared without coating additives in Comparative Example 4, the composite positive electrode material prepared with coating additives in Example 1 has higher compaction density and 2000 cycle capacity retention rate of the corresponding lithium battery, which indicates that coating additives on the surface of the secondary spheres is beneficial to improving the mechanical properties and cycle stability of the composite positive electrode material.

[0139] As can be seen from Table 1 and Table 2, compared with the composite positive electrode material prepared by first sintering the secondary ball precursor and then coating the sintered secondary ball precursor with an additive in Comparative Example 5, the secondary ball precursor is first coated with an additive and then the surface of the secondary ball precursor coated with the additive is coated with an additive.

[0140] The composite positive electrode material prepared by sintering the secondary spherical precursor has a higher compaction density and 2000 cycle capacity retention rate, which indicates that first coating the secondary spherical precursor with an additive and then sintering the secondary spherical precursor with the additive coated on the surface is beneficial to improving the mechanical properties and cycle stability of the composite positive electrode material.

Claims

1. A composite positive electrode material, characterized in that: The composite positive electrode material includes secondary balls and an additive layer coated on the surface of the secondary balls; the secondary balls are formed by agglomeration of primary particles; the material of the secondary balls includes lithium iron phosphate, carbon nanotubes, B2O3 and TeO3; the material of the additive layer is selected from one or more of LiNbO3, LiGaO3, LiGeO3 and LiTaO3.

2. The composite positive electrode material according to claim 1, characterized in that The composite positive electrode material has one or more of the following characteristics: The particle size D50 of the composite positive electrode material is 5 to 25 μm, preferably 5 to 15 μm; In the composite positive electrode material, the mass fraction of the secondary balls is 98wt% to 99.5wt%; In the composite positive electrode material, the mass fraction of the auxiliary agent layer is 0.5wt% to 2wt%.

3. The composite positive electrode material according to claim 1, characterized in that The composite positive electrode material has one or more of the following characteristics: In the secondary ball, the mass of the carbon nanotubes is 0.4wt% to 1wt% of the mass of the lithium iron phosphate; In the secondary ball, the mass of B2O3 is 0.5wt% to 3wt% of the mass of lithium iron phosphate; In the secondary ball, the mass of TeO3 is 0.1wt% to 1wt% of the mass of lithium iron phosphate.

4. A method for preparing the composite positive electrode material according to any one of claims 1 to 3, characterized in that: The method comprises the following steps: (1) mixing a lithium source, an iron source, a phosphorus source, carbon nanotubes, B2O3 and TeO3 uniformly, grinding them in water to form a primary particle precursor, and then spraying them to form a ball to obtain a secondary ball precursor agglomerated from the primary particle precursor; (2) using a fusion machine to coat the surface of the secondary ball precursor obtained in step (1) with an auxiliary agent to obtain a secondary ball precursor coated with the auxiliary agent; (3) Sintering the secondary ball precursor with the surface coated with the auxiliary agent obtained in step (2) to form secondary balls formed by agglomeration of primary particles and an auxiliary agent layer coated on the surface of the secondary balls, thereby obtaining the composite positive electrode material.

5. The method according to claim 4, characterized in that The method has one or more of the following features: In step (1), the lithium source is selected from one or more of lithium carbonate, lithium hydroxide, lithium phosphate and lithium dihydrogen phosphate; In step (1), the iron source is selected from one or more of ferric phosphate, ferrous oxide and ferrous oxalate; In step (1), the phosphorus source is selected from one or more of iron phosphate, lithium dihydrogen phosphate, phosphoric acid and monoammonium phosphate; In step (1), the molar ratio of the lithium element in the lithium source to the iron element in the iron source is 1:(0.9-1.05); In step (1), the molar ratio of the lithium element in the lithium source to the phosphorus element in the phosphorus source is 1:(1-1.05); In step (1), the particle size D50 of the primary particle precursor is 150 to 500 nm, preferably 150 to 250 nm; In step (1), the particle size D50 of the secondary sphere precursor is 5 to 25 μm, preferably 5 to 15 μm.

6. The method according to claim 4, characterized in that In step (2), the operating temperature of the fusion machine is 15 to 50° C.; and / or In step (2), the rotation speed of the fusion machine is 200 to 1000 r / min.

7. The method according to claim 4, characterized in that The method has one or more of the following features: In step (3), the sintering is carried out in a protective atmosphere, and the protective atmosphere is preferably nitrogen or argon; In step (3), the sintering temperature is 700-800°C; In step (3), the sintering time is 5 to 15 hours.

8. A positive electrode slurry comprising the composite positive electrode material according to any one of claims 1 to 3 or the composite positive electrode material prepared by the method according to any one of claims 4 to 7.

9. A positive electrode sheet comprising the composite positive electrode material according to any one of claims 1 to 3 or the composite positive electrode material prepared by the method according to any one of claims 4 to 7.

10. A lithium ion battery, characterized in that: The lithium-ion battery comprises the positive electrode sheet according to claim 9.