High-nickel ternary positive electrode material, preparation method thereof and lithium ion battery
By covering the metal carbon oxide layer on the high-nickel ternary positive electrode material, the problems of poor structural stability and alkaline impurities are solved, and better circulation performance and safety are achieved.
Patent Information
- Application Number
- CN202411199605.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The high-nickel ternary cathode material has poor structural stability and high alkaline impurities residues in lithium-ion batteries, resulting in serious gas production during charging and discharging, which affects the safety and cycle life of the battery.
The metal carbon oxide coating layer is used to coat the core of the high-nickel ternary positive electrode material. The oxygen-rich metal carbon oxide is formed through calcination and carburizing technology to capture the oxygen precipitated during the cycle, reduce the residue of alkaline impurities and improve the Structural stability.
It effectively reduces the residual alkaline impurities, reduces the gas production of the battery, improves the cycling performance and charging and discharge performance of the battery, and enhances the safety and stability of the battery.
Smart Images

Figure CN119092671A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium-ion battery materials, and in particular, to a high-nickel ternary cathode material, a preparation method thereof, and a lithium-ion battery. Background Art
[0002] Ternary cathode materials have the advantages of stable voltage, high capacity, large tap density, and large energy density, and are widely used in the field of new energy power batteries. At present, high-nickel ternary cathode materials with high specific capacity have become an important development direction of lithium-ion batteries. With the increase in nickel content, lithium-nickel mixing is relatively serious. At the same time, during the charge and discharge process of lithium-ion batteries, the surface structure of the high-nickel ternary cathode material will undergo a phase change from H2 to H3, resulting in the transformation of the surface structure from a layered structure to a rock salt phase structure, thereby affecting the structural stability of the cathode material and further leading to the deterioration of the performance of the cathode material. In addition, strong oxidizing high-valent transition metal ions on the surface of the high-nickel ternary cathode material will have a serious side reaction with the electrolyte, which will also cause problems such as increased polarization of the battery and rapid capacity decay. At the same time, the heat and oxygen generated during the reaction will cause safety problems. The increase in nickel content will lead to a significant increase in the residual alkaline impurities between the particles of the high-nickel cathode material, thereby causing serious gas generation problems during the charge and discharge process, further resulting in battery bulging and deformation, greatly shortening the cycle and shelf life, and generating safety hazards. At the same time, the problem of residual alkaline impurities in the high-nickel cathode material has become the key to restricting the application of high-nickel ternary cathode materials in high-energy-density power batteries for electric vehicles. Summary of the Invention
[0003] The main object of the present invention is to provide a high-nickel ternary cathode material, a preparation method thereof, and a lithium-ion battery, so as to solve the problems of poor structural stability of the high-nickel cathode material and high residual alkaline impurities leading to serious gas generation during the charge and discharge process in the prior art.
[0004] To achieve the above object, according to one aspect of the present invention, a high-nickel ternary cathode material is provided. The high-nickel ternary cathode material includes a high-nickel ternary cathode material core and a metal carbon oxide coating layer coated on the surface of the high-nickel ternary cathode material core; the chemical general formula of the high-nickel ternary cathode material is LiNi x Co y Mn 1-x-y O2@MO m C n , where 0.8 ≤ x ≤ 1.0, 0 ≤ y ≤ 0.2, 0 < m < 2, 0 < n < 2, and M is selected from any one or more of Nb, Ti, V, Mo, and W.
[0005] The metal carbon oxide coating layer in the high-nickel ternary cathode material of the present invention can not only form an effective and stable interface layer on the surface of the high-nickel ternary cathode material core, but also reduce the formation of Li2CO3 and LiOH by isolating moisture and carbon dioxide in the air, thereby reducing the residual alkaline impurities. In addition, the metal carbon oxide is rich in oxygen vacancies, which can capture the oxygen precipitated due to material phase change during the cycling of the high-nickel ternary cathode material, thereby reducing gas generation and further improving the cycling performance of the battery cell.
[0006] Further, 0.8 ≤ x ≤ 0.9, 0.05 ≤ y ≤ 0.1, 1 < m < 2, 0.5 < n < 1.5, and M is Nb and / or W.
[0007] To further improve the structural stability and cycling performance of the high-nickel cathode material, it is preferred that x, y, m, and n are within the above ranges and the type of M is preferably Nb and / or W.
[0008] Further, the mass ratio of the metal carbon oxide coating layer to the high-nickel ternary cathode material core is 1-5:100.
[0009] Preferably controlling the mass ratio of the metal carbon oxide coating layer to the high-nickel ternary cathode material core within the above range helps the metal carbon oxide coating layer to better coat the surface of the high-nickel ternary cathode material core, thereby contributing to further improving the structural stability of the high-nickel cathode material.
[0010] According to another aspect of the present invention, there is provided a method for preparing the above-mentioned high-nickel ternary cathode material, the preparation method comprising: Step S1, mixing raw materials including a high-nickel ternary precursor and a lithium source and then calcining to obtain a high-nickel ternary cathode material core; Step S2, first stirring raw materials including an organometallic compound, a carbon source, and a solvent to obtain Solution A; and Step S3, sequentially second stirring, drying, and sintering raw materials including the high-nickel ternary cathode material core, Solution A, and a surfactant to obtain a high-nickel ternary cathode material; wherein the metal element in the organometallic compound is selected from any one or more of Nb, Ti, V, Mo, and W.
[0011] In Step S1, the high-nickel ternary precursor and the lithium source can quickly form the crystal structure of the high-nickel ternary cathode material core through calcination; in Step S2, the organometallic compound is carburized by the carbon source to form a metal carbon oxide MO m C n with oxygen vacancies, which can capture the oxygen precipitated due to material phase change during the cycling of the high-nickel ternary cathode material, thereby reducing gas generation and further improving the cycling performance of the battery cell; through Step S3, the metal carbon oxide can be more uniformly coated on the surface of the high-nickel ternary cathode material core to form a metal carbon oxide coating layer, thereby obtaining a high-nickel ternary cathode material with stable structure.
[0012] Furthermore, in the above step S1, the high nickel ternary precursor is Ni x Co y Mn 1-x-y (OH)2 and / or Ni x Co y Mn 1-x- y CO3, wherein 0.8≤x≤1.0, 0≤y≤0.2; and / or, the lithium source is selected from any one or more of Li2CO3, LiOH and CH3COOLi; and / or, the ratio of the amount of all metal ions in the high nickel ternary precursor to the amount of lithium ions in the lithium source is 1:1 to 1.1.
[0013] Preferably, the types of high-nickel ternary precursor, lithium source and the ratio of the amount of all metal ions in the high-nickel ternary precursor to the amount of lithium ions in the lithium source are within the above range, which helps the lithium source and the high-nickel ternary precursor to form a high-nickel ternary positive electrode material core with a stable crystal structure.
[0014] Furthermore, in the above step S1, the calcination temperature is 800-900° C., and / or the calcination time is 10-18 hours, and / or the calcination atmosphere is oxygen.
[0015] It is preferred to control the calcination temperature, time and atmosphere within the above ranges, which is conducive to the rapid formation of the crystal structure of the inner core of the high-nickel ternary positive electrode material.
[0016] Further, in the above step S2, the organic metal compound is selected from any one or more of niobium ethoxide, titanium ethoxide, vanadium ethoxide, molybdenum ethoxide, tungsten ethoxide, niobium isopropoxide, vanadium isopropoxide, molybdenum ethoxide, molybdenum isopropoxide, tungsten ethoxide and tungsten isopropoxide; and / or, the carbon source is selected from any one or more of urea, formamide, acetamide and dimethylamide; and / or, the solvent is selected from any one or more of ethanol, methanol and propanol; and / or, the molar ratio of the organic metal compound to the carbon source is 1:0.25-1, preferably 1:0.5-1; and / or, the molar concentration of the organic metal compound in solution A is 0.005-0.1 mol / L; and / or, the rotation speed of the first stirring is 300-600 r / min, and / or, the time of the first stirring is 60-120 min.
[0017] It is preferred that the types of the organometallic compound, the carbon source and the solvent, the molar ratio of the organometallic compound to the carbon source, the molar concentration of the organometallic compound in the solution A, and the speed and time of the first stirring are within the above ranges, which helps the organometallic compound to be better carburized by the carbon source to form a metal carbide MO rich in oxygen vacancies. m C n, which helps to reduce the gas production caused by oxygen evolution due to phase change of the material, which in turn helps to further improve the cycle performance of the battery cell.
[0018] Furthermore, in the above step S3, the mass concentration of the core of the high-nickel ternary positive electrode material is 100-200 g / L; and / or, the surfactant is selected from any one or more of dodecyl ammonium bromide, sodium dodecyl sulfonate and sodium dodecyl sulfate; and / or, the molar concentration of the surfactant is 0.01-0.05 mol / L.
[0019] It is preferred to control the mass concentration of the core of the high-nickel ternary positive electrode material, the type and molar concentration of the surfactant within the above range, which helps the core of the high-nickel ternary positive electrode material to be better dispersed in solution A, thereby helping the metal carbide to be better coated on the surface of the core of the high-nickel ternary positive electrode material, thereby forming a structurally stable high-nickel ternary positive electrode material.
[0020] Furthermore, in the above step S3, the second stirring speed is 100-300 r / min, and / or the second stirring time is 60-120 min; and / or drying is performed under a vacuum environment; and / or the drying temperature is 100-120°C, and / or the drying time is 12-24 h; and / or the sintering temperature is 300-500°C, and / or the sintering time is 4-8 h, and / or the sintering atmosphere is argon and / or nitrogen.
[0021] It is preferred to control the rotation speed and time of the second stirring within the above range, which helps to further improve the dispersion uniformity of the high-nickel ternary positive electrode material core in solution A; it is preferred to control the drying environment, temperature and time within the above range, which helps to form a metal carbide coating layer and improve the structural stability of the metal carbide coating layer, so that it can be better coated on the surface of the high-nickel ternary positive electrode material core, thereby helping to improve the charge and discharge performance and cycle stability of the high-nickel ternary positive electrode material; it is preferred to control the sintering temperature, time and atmosphere within the above range, which helps to effectively form amorphous metal carbide.
[0022] According to another aspect of the present invention, a lithium-ion battery is provided, comprising a positive electrode sheet, a negative electrode sheet and a separator, wherein the positive electrode sheet comprises a positive electrode material, and the positive electrode material comprises the above-mentioned high-nickel ternary positive electrode material.
[0023] The lithium-ion battery including the above-mentioned high-nickel ternary positive electrode material has excellent charge and discharge performance and cycle performance.
[0024] Applying the technical solution of the present invention, in this application, through the metal carbon oxide coating layer coated on the surface of the high-nickel ternary cathode material core, on the one hand, the metal carbon oxide coating layer can form an effective and stable interfacial layer on the surface of the high-nickel ternary cathode material core, thereby reducing the interfacial reaction between the electrode and the electrolyte, and further improving the cycling performance of the high-nickel ternary cathode material; on the other hand, the metal carbon oxide coating layer has good moisture-proof performance and can reduce the formation of Li2CO3 and LiOH by isolating moisture and carbon dioxide in the air, thereby reducing the residual alkaline impurities and further enhancing the stability of the high-nickel ternary cathode material in the atmosphere. In addition, the metal carbon oxide in the high-nickel ternary cathode material of the present invention is rich in oxygen vacancies, which can capture the oxygen precipitated due to material phase change during the cycling of the high-nickel ternary cathode material, thereby reducing gas generation and further improving the cycling performance of the battery cell. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The accompanying drawings forming a part of this application are used to provide a further understanding of the present invention. The schematic embodiments and descriptions thereof of the present invention are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0026] Figure 1 The SEM image of the high-nickel ternary cathode material in Example 1 of this application is shown. DETAILED DESCRIPTION OF THE EMBODIMENTS
[0027] It should be noted that, without conflict, the embodiments in this application and the features in the embodiments can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.
[0028] As analyzed in the background art of this application, in the prior art, there are problems such as poor structural stability of the high-nickel cathode material and high residual alkaline impurities, resulting in serious gas generation during charge and discharge. To solve the above problems, this application provides a high-nickel ternary cathode material, its preparation method, and a lithium-ion battery.
[0029] In a typical embodiment of this application, a high-nickel ternary cathode material is provided. The high-nickel ternary cathode material includes a high-nickel ternary cathode material core and a metal carbon oxide coating layer coated on the surface of the high-nickel ternary cathode material core; the high-nickel ternary cathode material has a chemical general formula of LiNi x Co y Mn 1-x-y O2@MO m C n , where 0.8 ≤ x ≤ 1.0, 0 ≤ y ≤ 0.2, 0 < m < 2, 0 < n < 2, and M is selected from any one or more of Nb, Ti, V, Mo, and W.
[0030] In this application, a metal carbon oxide coating layer is coated on the surface of the high-nickel ternary cathode material core. On the one hand, the metal carbon oxide coating layer can form an effective and stable interfacial layer on the surface of the high-nickel ternary cathode material core, thereby reducing the interface reaction between the electrode and the electrolyte, and further improving the cycling performance of the high-nickel ternary cathode material. On the other hand, the metal carbon oxide coating layer has good moisture-proof performance, and can reduce the formation of Li2CO3 and LiOH by isolating moisture and carbon dioxide in the air, thereby reducing the residual alkaline impurities, and further enhancing the stability of the high-nickel ternary cathode material in the atmosphere. In addition, the metal carbon oxide in the high-nickel ternary cathode material of the present invention is rich in oxygen vacancies, which can capture the oxygen precipitated due to material phase change during the cycling process of the high-nickel ternary cathode material, thereby reducing gas generation and further improving the cycling performance of the battery cell.
[0031] In order to further improve the structural stability and cycling performance of the high-nickel cathode material, in one embodiment of this application, 0.8 ≤ x ≤ 0.9, 0.05 ≤ y ≤ 0.1, 1 < m < 2, 0.5 < n < 1.5, and M is Nb and / or W.
[0032] In one embodiment of this application, the mass ratio of the metal carbon oxide coating layer to the high-nickel ternary cathode material core is 1-5:100.
[0033] Preferably controlling the mass ratio of the metal carbon oxide coating layer to the high-nickel ternary cathode material core within the above range helps the metal carbon oxide coating layer to better coat on the surface of the high-nickel ternary cathode material core, thereby helping to further improve the structural stability of the high-nickel cathode material.
[0034] In another typical embodiment of this application, a preparation method of the above high-nickel ternary cathode material is provided. The preparation method includes: Step S1, mixing raw materials including a high-nickel ternary precursor and a lithium source and then calcining to obtain a high-nickel ternary cathode material core; Step S2, first stirring raw materials including an organometallic compound, a carbon source and a solvent to obtain solution A; and Step S3, sequentially performing second stirring, drying and sintering on raw materials including the high-nickel ternary cathode material core, solution A and a surfactant to obtain the high-nickel ternary cathode material; wherein, the metal element in the organometallic compound is selected from any one or more of Nb, Ti, V, Mo, and W.
[0035] The present application forms a metal carbide coating layer coated on the core of the high-nickel ternary positive electrode material through the above-mentioned organic metal compound and carbon source. The metal carbide coating layer can not only form an effective and stable interface layer on the surface of the core of the high-nickel ternary positive electrode material, but also reduce the residual alkaline impurities by isolating the moisture and carbon dioxide in the air, thereby enhancing the stability of the high-nickel ternary positive electrode material in the atmosphere. Specifically, in step S1, the high-nickel ternary precursor and the lithium source are calcined to quickly form the crystal structure of the core of the high-nickel ternary positive electrode material; in step S2, the organic metal compound is carburized by the carbon source to form a metal carbide MO rich in oxygen vacancies. m C n , whose oxygen vacancies can capture oxygen released by the phase change of the high-nickel ternary positive electrode material during the cycle, thereby reducing gas production and improving the cycle performance of the battery cell; in step S3, the raw materials including the high-nickel ternary positive electrode material core, solution A and surfactant are sequentially subjected to a second stirring, drying and sintering, which can make the metal carbide more evenly coated on the surface of the high-nickel ternary positive electrode material core to form a metal carbide coating layer, thereby obtaining a high-nickel ternary positive electrode material with a stable structure.
[0036] In one embodiment of the present application, in the above step S1, the high nickel ternary precursor is Ni x Co y Mn 1-x-y (OH)2 and / or Ni x Co y Mn 1-x-y CO3, wherein 0.8≤x≤1.0, 0≤y≤0.2; and / or, the lithium source is selected from any one or more of Li2CO3, LiOH and CH3COOLi; and / or, the ratio of the amount of all metal ions in the high nickel ternary precursor to the amount of lithium ions in the lithium source is 1:1 to 1.1.
[0037] Preferably, the types of high-nickel ternary precursor, lithium source and the ratio of the amount of all metal ions in the high-nickel ternary precursor to the amount of lithium ions in the lithium source are within the above range, which helps the lithium source and the high-nickel ternary precursor to form a high-nickel ternary positive electrode material core with a stable crystal structure.
[0038] In one embodiment of the present application, in the above step S1, the calcination temperature is 800-900° C., and / or the calcination time is 10-18 hours, and / or the calcination atmosphere is oxygen.
[0039] It is preferred to control the calcination temperature, time and atmosphere within the above ranges, which is conducive to the rapid formation of the crystal structure of the inner core of the high-nickel ternary positive electrode material.
[0040] In one embodiment of the present application, in the above step S2, the organic metal compound is selected from any one or more of niobium ethoxide, titanium ethoxide, vanadium ethoxide, molybdenum ethoxide, tungsten ethoxide, niobium isopropoxide, vanadium isopropoxide, molybdenum ethoxide, molybdenum isopropoxide, tungsten ethoxide and tungsten isopropoxide, preferably niobium ethoxide and / or tungsten ethoxide; and / or, the carbon source is selected from any one or more of urea, formamide, acetamide and dimethylamide; and / or, the solvent is selected from any one or more of ethanol, methanol and propanol; and / or, the molar ratio of the organic metal compound to the carbon source is 1:0.25-1, preferably 1:0.5-1; and / or, the molar concentration of the organic metal compound in solution A is 0.01-0.1 mol / L; and / or, the rotation speed of the first stirring is 300-600 r / min, and / or, the time of the first stirring is 60-120 min.
[0041] It is preferred that the types of the organometallic compound, the carbon source and the solvent, the molar ratio of the organometallic compound to the carbon source, the molar concentration of the organometallic compound in the solution A, and the speed and time of the first stirring are within the above ranges, which helps the organometallic compound to be better carburized by the carbon source to form a metal carbide MO rich in oxygen vacancies. m C n , which helps to reduce the gas generation caused by the release of oxygen due to the phase change of the material, and further helps to further improve the cycle performance of the battery. It is further preferred that the organic metal compound is niobium ethoxide and / or tungsten ethoxide, which helps to better form metal carbon oxide MO rich in oxygen vacancies m C n .
[0042] In one embodiment of the present application, in the above step S3, the mass concentration of the core of the high-nickel ternary positive electrode material is 100-200 g / L; and / or, the surfactant is selected from any one or more of dodecyl ammonium bromide, sodium dodecyl sulfonate and sodium dodecyl sulfate; and / or, the molar concentration of the surfactant is 0.01-0.05 mol / L.
[0043] It is preferred to control the mass concentration of the core of the high-nickel ternary positive electrode material, the type and molar concentration of the surfactant within the above range, which helps the core of the high-nickel ternary positive electrode material to be better dispersed in solution A, thereby helping the metal carbide to be better coated on the surface of the core of the high-nickel ternary positive electrode material, thereby forming a structurally stable high-nickel ternary positive electrode material.
[0044] In one embodiment of the present application, in the above-mentioned step S3, the rotation speed of the second stirring is 100-300 r / min, and / or, the time of the second stirring is 60-120 min; and / or, drying is performed under a vacuum environment; and / or, the drying temperature is 100-120°C, and / or, the drying time is 12-24h; and / or, the sintering temperature is 300-500°C, and / or, the sintering time is 4-8h, and / or, the sintering atmosphere is argon and / or nitrogen.
[0045] It is preferred to control the rotation speed and time of the second stirring within the above range, which helps to further improve the dispersion uniformity of the high-nickel ternary positive electrode material core in solution A; it is preferred to control the drying environment, temperature and time within the above range, which helps to form a metal carbide coating layer and improve the structural stability of the metal carbide coating layer, so that it can be better coated on the surface of the high-nickel ternary positive electrode material core, thereby helping to improve the charge and discharge performance and cycle stability of the high-nickel ternary positive electrode material; it is preferred to control the sintering temperature, time and atmosphere within the above range, which helps to form amorphous metal carbide. If the temperature is too high, the amorphous metal carbide may be converted into metal oxide and metal carbide. If the temperature is too low, carburization cannot be achieved, and thus metal carbide cannot be formed. Therefore, the present application controls the sintering temperature to 300-500°C, which helps to effectively form amorphous metal carbide.
[0046] In another typical embodiment of the present application, a lithium-ion battery is provided, including a positive electrode sheet, a negative electrode sheet and a separator, wherein the positive electrode sheet includes a positive electrode material, and the positive electrode material includes the above-mentioned high-nickel ternary positive electrode material.
[0047] The lithium-ion battery including the above-mentioned high-nickel ternary positive electrode material has excellent charge and discharge performance and cycle performance.
[0048] The beneficial effects of the present application will be further illustrated below in conjunction with embodiments.
[0049] Example 1
[0050] The high nickel ternary precursor Ni 0.8 Co 0.1 Mn 0.1 The raw materials of (OH)2 and LiOH are mixed and calcined in an oxygen atmosphere to obtain the core of the high-nickel ternary positive electrode material, wherein the high-nickel ternary precursor Ni 0.8 Co 0.1 Mn 0.1The ratio of the amount of all metal ions in (OH)2 to the amount of lithium ions in LiOH is 1:1.03, the calcination temperature is 900°C, and the calcination time is 14h. A raw material including 0.0025 mol of organic metal compound ethanol niobium, 0.0025 mol of carbon source urea and 100 mL of ethanol solution is first stirred to obtain solution A, wherein the first stirring speed is 500 r / min and the first stirring time is 120 min; a raw material including 10 g of a high-nickel ternary positive electrode material core, solution A and 0.1 g of a surfactant dodecylammonium bromide is sequentially second stirred, vacuum dried and sintered under an argon atmosphere, and finally ground and sieved to obtain a high-nickel ternary positive electrode material, wherein the second stirring speed is 200 r / min, the second stirring time is 60 min, the drying temperature is 100°C, the drying time is 12 h, the sintering temperature is 300°C, the sintering time is 8 h, and the mass ratio of the metal carbon oxide coating layer to the high-nickel ternary positive electrode material core in the high-nickel ternary positive electrode material is 3:100.
[0051] Example 2
[0052] The difference from Example 1 is that the raw materials including 0.0025 mol of organic metal compound niobium ethoxide, 0.002 mol of carbon source urea and 100 mL of ethanol solution are first stirred to finally obtain a high-nickel ternary positive electrode material.
[0053] Example 3
[0054] The difference from Example 1 is that the raw materials including 0.0025 mol of organic metal compound niobium ethoxide, 0.00125 mol of carbon source urea and 100 mL of ethanol solution are first stirred to finally obtain a high-nickel ternary positive electrode material.
[0055] Example 4
[0056] The difference from Example 1 is that the raw materials including 0.0025 mol of organic metal compound niobium ethoxide, 0.000625 mol of carbon source urea and 100 mL of ethanol solution are first stirred to finally obtain a high-nickel ternary positive electrode material.
[0057] Example 5
[0058] The high nickel ternary precursor Ni 0.85 Co 0.1 Mn 0.1 The raw materials of (OH)2 and LiOH are mixed and calcined in an oxygen atmosphere to obtain the core of the high-nickel ternary positive electrode material, wherein the high-nickel ternary precursor Ni 0.8 Co 0.1 Mn 0.1The ratio of the amount of all metal ions in (OH)2 to the amount of lithium ions in LiOH is 1:1.04, the calcination temperature is 850°C, and the calcination time is 18h. The raw materials including 0.008mol of organic metal compound ethanol niobium, 0.008mol of carbon source urea and 100mL of ethanol solution are first stirred to obtain solution A, wherein the speed of the first stirring is 500r / min, and the time of the first stirring is 120min; the raw materials including 20g of high-nickel ternary positive electrode material core, solution A and 0.3g of surfactant dodecyl ammonium bromide are sequentially second stirred, vacuum dried and sintered in an argon atmosphere, and finally the high-nickel ternary positive electrode material is obtained after grinding and sieving, wherein the speed of the second stirring is 200r / min, the time of the second stirring is 60min, the drying temperature is 100°C, the drying time is 12h, the sintering temperature is 400°C, and the sintering time is 6h.
[0059] Example 6
[0060] The difference from Example 5 is that the raw materials including 0.0005 mol of organic metal compound niobium ethoxide, 0.0005 mol of carbon source urea and 100 mL of ethanol solution are first stirred to finally obtain a high-nickel ternary positive electrode material.
[0061] Example 7
[0062] The difference from Example 5 is that the raw materials including 0.0015 mol of organic metal compound niobium ethoxide, 0.0015 mol of carbon source urea and 100 mL of ethanol solution are first stirred to finally obtain a high-nickel ternary positive electrode material.
[0063] Example 8
[0064] The difference from Example 1 is that the mass ratio of the metal carbide coating layer to the core of the high-nickel ternary positive electrode material is 1:100, and a high-nickel ternary positive electrode material is finally obtained.
[0065] Example 9
[0066] The difference from Example 1 is that the mass ratio of the metal carbide coating layer to the core of the high-nickel ternary positive electrode material is 5:100, and a high-nickel ternary positive electrode material is finally obtained.
[0067] Example 10
[0068] The difference from Example 1 is that the mass ratio of the metal carbide coating layer to the core of the high-nickel ternary positive electrode material is 6:100, and a high-nickel ternary positive electrode material is finally obtained.
[0069] Embodiment 11
[0070] The difference from Example 1 is that the organic metal compound is tungsten ethoxide, and a high-nickel ternary positive electrode material is finally obtained.
[0071] Example 12
[0072] The difference from Example 1 is that the high nickel ternary precursor Ni 0.8 Co 0.1 Mn 0.1 The ratio of the amount of all metal ions in (OH)2 to the amount of lithium ions in LiOH is 1:1, and a high-nickel ternary positive electrode material is finally obtained.
[0073] Embodiment 13
[0074] The difference from Example 1 is that the high nickel ternary precursor Ni 0.8 Co 0.1 Mn 0.1 The ratio of the amount of all metal ions in (OH)2 to the amount of lithium ions in LiOH is 1:1.1, and a high-nickel ternary positive electrode material is finally obtained.
[0075] Embodiment 14
[0076] The difference from Example 1 is that the high nickel ternary precursor Ni 0.8 Co 0.1 Mn 0.1 The ratio of the amount of all metal ions in (OH)2 to the amount of lithium ions in LiOH is 1:1.5, and a high-nickel ternary positive electrode material is finally obtained.
[0077] Embodiment 15
[0078] The difference from Example 1 is that the molar ratio of the organic metal compound niobium ethoxide to the carbon source urea is 1:1.5, and a high-nickel ternary positive electrode material is finally obtained.
[0079] Example 16
[0080] The difference from Example 1 is that the molar concentration of the organic metal compound niobium ethoxide in solution A is 0.01 mol / L, and a high-nickel ternary positive electrode material is finally obtained.
[0081] Embodiment 17
[0082] The difference from Example 1 is that the molar concentration of the organic metal compound niobium ethoxide in solution A is 0.1 mol / L, and a high-nickel ternary positive electrode material is finally obtained.
[0083] Embodiment 18
[0084] The difference from Example 1 is that the molar concentration of the organic metal compound niobium ethoxide in solution A is 0.2 mol / L, and a high-nickel ternary positive electrode material is finally obtained.
[0085] Embodiment 19
[0086] The difference from Example 1 is that the mass concentration of the inner core of the high-nickel ternary positive electrode material is 200 g / L, and a high-nickel ternary positive electrode material is finally obtained.
[0087] Embodiment 20
[0088] The difference from Example 1 is that the mass concentration of the inner core of the high-nickel ternary positive electrode material is 220 g / L, and a high-nickel ternary positive electrode material is finally obtained.
[0089] Embodiment 21
[0090] The difference from Example 1 is that the sintering temperature is 500° C., the sintering time is 4 h, and finally a high-nickel ternary positive electrode material is obtained.
[0091] Embodiment 22
[0092] The difference from Example 1 is that the sintering temperature is 600° C., the sintering time is 3 h, and finally a high-nickel ternary positive electrode material is obtained.
[0093] Comparative Example 1
[0094] The difference from Example 1 is that the high nickel ternary precursor Ni 0.8 Co 0.1 Mn 0.1 The raw materials of (OH)2 and LiOH are mixed and calcined in an oxygen atmosphere to finally obtain a high-nickel ternary positive electrode material, wherein the ratio of the amount of all metal ions in the high-nickel ternary precursor to the amount of lithium ions in the lithium source is 1:1.03, the calcination temperature is 900°C, and the calcination time is 14h.
[0095] Comparative Example 2
[0096] The difference from Example 1 is that the raw materials of 0.0025 mol of carbon source urea and 100 mL of ethanol solution are first stirred to finally obtain a high-nickel ternary positive electrode material.
[0097] Comparative Example 3
[0098] The difference from Example 1 is that the raw materials of 0.0025 mol of organic metal compound niobium ethoxide and 100 mL of ethanol solution are first stirred to finally obtain a high-nickel ternary positive electrode material.
[0099] Test Method
[0100] The high nickel ternary positive electrode materials of the above embodiments and comparative examples were subjected to electrochemical tests. The test method was as follows: the high nickel ternary positive electrode material, the conductive agent acetylene black and the binder PVDF were mixed in 10 mL of N-methylpyrrolidone in a mass ratio of 9:0.5:0.5, and the slurry was fully stirred to form a slurry. The slurry was applied to the surface of the aluminum foil by a coating machine, and then dried and cut. The lithium sheet was used as the negative electrode, the lithium hexafluorophosphate solution was used as the electrolyte, and the button battery was assembled in an argon-protected glove box using a 2032-type button battery shell. The normal temperature electrochemical performance test was carried out in the voltage range of 2.8 to 4.3 V at 25°C. The test results are shown in Table 1.
[0101] Table 1
[0102]
[0103]
[0104] in, Figure 1 This is a SEM image of the high nickel ternary positive electrode material in Example 1. Figure 1 It can be seen that the metal carbide coating layer is evenly coated on the surface of the core of the high nickel ternary positive electrode material.
[0105] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects:
[0106] The present application is a metal carbide coating layer coated on the surface of the core of the high-nickel ternary positive electrode material. On the one hand, the metal carbide coating layer can form an effective and stable interface layer on the surface of the core of the high-nickel ternary positive electrode material, thereby reducing the interface reaction of the electrode / electrolyte, thereby improving the cycle performance of the high-nickel ternary positive electrode material; on the other hand, the metal carbide coating layer has good moisture resistance, and can reduce the formation of Li2CO3 and LiOH by isolating moisture and carbon dioxide in the air, thereby reducing the residual alkaline impurities, thereby enhancing the stability of the high-nickel ternary positive electrode material in the atmosphere. In addition, the metal carbide in the high-nickel ternary positive electrode material of the present invention is rich in oxygen vacancies, which can capture the oxygen precipitated by the phase change of the material during the cycle of the high-nickel ternary positive electrode material, thereby reducing gas production, thereby improving the cycle performance of the battery cell.
[0107] The above are only embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A high-nickel ternary cathode material, characterized in that, the high-nickel ternary cathode material comprises a high-nickel ternary cathode material core and a metal carbon oxide coating layer coated on the surface of the high-nickel ternary cathode material core; The chemical general formula of the high-nickel ternary cathode material is LiNi x Co y Mn 1-x-y O 2 @MO m C n , where 0.8 ≤ x ≤ 1.0, 0 ≤ y ≤ 0.2, 0 < m < 2, 0 < n < 2, and M is selected from any one or more of Nb, Ti, V, Mo, and W.
2. The high-nickel ternary cathode material according to claim 1, characterized in that, 0.8 ≤ x ≤ 0.9, 0.05 ≤ y ≤ 0.1, 1 < m < 2, 0.5 < n < 1.5, where M is Nb and / or W.
3. The high-nickel ternary cathode material according to claim 1 or 2, characterized in that, the mass ratio of the metal carbon oxide coating layer to the high-nickel ternary cathode material core is 1-5:
100.
4. A preparation method of the high-nickel ternary cathode material according to any one of claims 1 to 3, characterized in that, the preparation method comprises: Step S1, mixing raw materials including a high-nickel ternary precursor and a lithium source and then calcining to obtain a high-nickel ternary cathode material core; Step S2, first stirring raw materials including an organometallic compound, a carbon source and a solvent to obtain solution A; and Step S3, sequentially performing second stirring, drying and sintering on raw materials including the high-nickel ternary cathode material core, the solution A and a surfactant to obtain the high-nickel ternary cathode material; wherein, the metal element in the organometallic compound is selected from any one or more of Nb, Ti, V, Mo, and W.
5. The preparation method according to claim 4, characterized in that, In step S1, the high nickel ternary precursor is Ni x Co y Mn 1-x-y (OH) 2 and / or Ni x Co y Mn 1-x-y CO 3 , wherein 0.8≤x≤1.0, 0≤y≤0.2; and / or, the lithium source is selected from Li 2 CO 3 , LiOH and CH 3 Any one or more of COOLi; and / or, the ratio of the amount of all metal ions in the high-nickel ternary precursor to the amount of lithium ions in the lithium source is 1:1 to 1.
1.
6. The preparation method according to claim 4 or 5, characterized in that, in step S1, the calcination temperature is 800-900 °C, and / or the calcination time is 10-18 h, and / or the calcination atmosphere is oxygen.
7. The preparation method according to any one of claims 4 to 6, characterized in that, in step S2, the organometallic compound is selected from any one or more of niobium ethoxide, titanium ethoxide, vanadium ethoxide, molybdenum ethoxide, tungsten ethoxide, niobium isopropoxide, vanadium isopropoxide, molybdenum ethoxide, molybdenum isopropoxide, tungsten ethoxide and tungsten isopropoxide; and / or the carbon source is selected from any one or more of urea, formamide, acetamide and dimethylformamide; and / or the solvent is selected from any one or more of ethanol, methanol and propanol; and / or the molar ratio of the organometallic compound to the carbon source is 1:0.25-1, preferably 1:0.5-1; and / or the molar concentration of the organometallic compound in solution A is 0.005-0.1 mol / L; and / or the rotation speed of the first stirring is 300-600 r / min, and / or the time of the first stirring is 60-120 min.
8. The preparation method according to any one of claims 4 to 7, characterized in that, in step S3, the mass concentration of the high-nickel ternary cathode material core is 100-200 g / L; and / or the surfactant is selected from any one or more of ammonium dodecyl bromide, sodium dodecyl sulfonate and sodium dodecyl sulfate; and / or the molar concentration of the surfactant is 0.01-0.05 mol / L.
9. The preparation method according to any one of claims 4 to 8, It is characterized in that In the step S3, the rotation speed of the second stirring is 100 to 300 r / min, and / or the time of the second stirring is 60 to 120 min; and / or the drying is performed under a vacuum environment; and / or the drying temperature is 100 to 120° C., and / or the drying time is 12 to 24 h; and / or the sintering temperature is 300 to 500° C., and / or the sintering time is 4 to 8 h, and / or the sintering atmosphere is argon and / or nitrogen.
10. A lithium ion battery comprising a positive electrode sheet, a negative electrode sheet and a separator, wherein the positive electrode sheet comprises a positive electrode material, It is characterized in that The positive electrode material comprises the high-nickel ternary positive electrode material according to any one of claims 1 to 3.
Citation Information
Patent Citations
High-nickel ternary positive electrode material containing active oxygen removing agent and preparation method thereof
CN110071278A