Nickel-zinc battery negative electrode material, nickel-zinc battery negative electrode, nickel-zinc battery negative electrode preparation method and nickel-zinc battery

By using additives such as magnesium oxide and zinc-containing substances in the negative electrode of nickel-zinc battery, a protective film is formed and Zn2+ is provided for charging and discharging. Combined with other additives, the problem of poor storage and circulation performance of nickel-zinc battery at high temperatures is solved, and achievable Good storage and cycle stability and extended battery life.

CN119092704APending Publication Date: 2024-12-06SHENZHEN HIGHPOWER TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411000027.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Nickel-zinc batteries have poor storage and circulation performance in high-temperature environments. The existing technology cannot improve storage and circulation performance at the same time, resulting in serious battery self-discharge.

Method used

Using nickel-zinc battery negative electrode materials, including negative electrode active materials and negative electrode additives, the negative electrode additives include magnesium oxide and zinc-containing substances, such as calcium zincate, zinc hydroxide, zinc sulfate, etc., to form a uniform magnesium-containing interface protective film to slow down alkalinity Corrosion and provide rich Zn2+ substances to speed up the charging and discharging process, increase conductive agents and other additives such as In2O3, Bi2O3, Al2O3, Ca(OH)2 to optimize battery performance.

Benefits of technology

Slow down battery self-discharge in high temperature environments, improve the storage performance and cycle stability of nickel-zinc batteries, extend battery life, and enhance battery charging and discharging efficiency and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092704A_ABST
    Figure CN119092704A_ABST
Patent Text Reader

Abstract

The invention provides a nickel-zinc battery negative electrode material, a nickel-zinc battery negative electrode, a nickel-zinc battery negative electrode preparation method and a nickel-zinc battery in order to solve the problem of poor storage and cycle performance of a nickel-zinc battery in the prior art. The nickel-zinc battery negative electrode material comprises a negative electrode active material and a negative electrode additive, the negative electrode additive comprises a first negative electrode additive, and the first negative electrode additive comprises magnesium oxide and a zinc-containing substance. According to the nickel-zinc battery negative electrode provided by the invention, magnesium oxide is added to form a uniform magnesium-containing protective film on the negative electrode, so that the corrosion to ZnO and Zn of the negative electrode is slowed down, and the nickel-zinc battery has good storage and cycle stability in a high-temperature environment; besides, in the charging and discharging process of the negative electrode of the nickel-zinc battery, Zn and ZnO need to be subjected to path conversion, various zinc intermediates are involved, zinc-containing substances in a water system environment contain rich Zn < 2 + >, rich Zn < 2 + > substances can be provided for path conversion, substance conversion in the charging and discharging process of the negative electrode is accelerated, Zn and ZnO losses are reduced, the service life of the nickel-zinc battery is prolonged, and the high-temperature storage performance of the nickel-zinc battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of electrode and battery manufacturing, and specifically relates to a negative electrode material for a nickel-zinc battery, a negative electrode for a nickel-zinc battery, a method for preparing a negative electrode for a nickel-zinc battery, and a nickel-zinc battery. Background Art

[0002] Nickel-zinc batteries have the advantages of long life, high voltage, and low internal resistance, but they have a high degree of self-discharge.

[0003] Furthermore, the storage performance of nickel-zinc batteries in high temperature environments is poor, and the self-discharge phenomenon of nickel-zinc batteries occurs because of the irreversible consumption of Zn or ZnO in a strong alkaline electrolyte. For the above problems of nickel-zinc batteries, the prior art adds lead and cellulose to the negative electrode of the nickel-zinc battery to reduce its self-discharge phenomenon and improve the storage performance, and adds bismuth oxide, indium oxide, tin oxide and other components to the negative electrode to improve the cycle performance of the nickel-zinc battery. The above improvements cannot balance the battery storage performance and cycle performance, and thus cannot simultaneously improve the storage performance and cycle performance of the nickel-zinc battery. Summary of the invention

[0004] In view of the problem of poor storage performance and cycle performance of nickel-zinc batteries in the prior art, a nickel-zinc battery negative electrode material, a nickel-zinc battery negative electrode, a method for preparing a nickel-zinc battery negative electrode and a nickel-zinc battery are provided.

[0005] The technical solution adopted by the present invention to solve the above technical problems is as follows:

[0006] On the one hand, the present invention provides a nickel-zinc battery negative electrode material, including a negative electrode active material and a negative electrode additive, wherein the negative electrode additive includes a first negative electrode additive, wherein the first negative electrode additive includes magnesium oxide and a zinc-containing substance, and the zinc-containing substance includes one or more of calcium zincate, zinc hydroxide, zinc sulfate and zinc gluconate.

[0007] Optionally, the mass ratio of the magnesium oxide to the zinc-containing substance is 1:3 to 3:1.

[0008] Optionally, the first negative electrode additive is added in an amount of 1 wt% to 10 wt% in the nickel-zinc battery negative electrode material.

[0009] Optionally, the negative electrode additive further includes a second negative electrode additive, wherein the second negative electrode additive includes In 2 O 3 、Bi 2 O 3 、Al 2 O 3 and Ca(OH) 2 One or more of .

[0010] Optionally, in the nickel-zinc battery negative electrode material, the In 2 O 3 The added mass is 0.01% to 1%, the Bi 2 O 3 The added mass is 0.08% to 2.88%, the Al 2 O 3 The added mass is 3% to 5%, the Ca(OH) 2 The added mass is 1% to 3%.

[0011] Optionally, it also includes a conductive agent, a thickener, a dispersant and a binder; in the nickel-zinc battery negative electrode material, the added mass of the conductive agent is 1% to 2%, the added mass of the thickener is 0.3% to 0.5%, the added mass of the dispersant is 1% to 2%, and the added mass of the binder is 2% to 3%.

[0012] Optionally, the negative electrode active material includes zinc and zinc oxide, and the mass ratio of the zinc to the zinc oxide is 1:7 to 1:3.

[0013] On the one hand, the nickel-zinc battery negative electrode provided by the present invention comprises a current collector and a negative electrode material layer, wherein the negative electrode material layer is arranged on the current collector, and the negative electrode material layer comprises the nickel-zinc battery negative electrode material.

[0014] In one aspect, the present invention provides a method for preparing a negative electrode of a nickel-zinc battery, comprising the following operations:

[0015] S1: After mixing the conductive agent, thickener and dispersant, add the second negative electrode additive and mix well to obtain a mixture A;

[0016] S2: adding the first negative electrode additive to the mixture A, and then adding the negative electrode active material, and mixing again to obtain a mixture B;

[0017] S3: adding the binder to the mixture B and mixing well to obtain a negative electrode slurry;

[0018] S4: coating the negative electrode slurry onto the corresponding negative electrode current collector to obtain a negative electrode for a nickel-zinc battery.

[0019] In one aspect, the present invention provides a nickel-zinc battery, comprising a positive electrode, a separator, an electrolyte, and the nickel-zinc battery negative electrode or the nickel-zinc battery negative electrode prepared by the nickel-zinc battery negative electrode preparation method.

[0020] The beneficial effects of this application are:

[0021] The nickel-zinc battery negative electrode material provided in the present application includes a negative electrode active material and a negative electrode additive, wherein the negative electrode additive includes a first negative electrode additive, wherein the first negative electrode additive includes magnesium oxide and a zinc-containing substance. After the addition of magnesium oxide, the magnesium element forms a uniform, extremely thin magnesium-containing interface protective film at the negative electrode under weak alkaline conditions in the aqueous system, which slows down the corrosion of alkalinity on ZnO and Zn in the negative electrode, plays a role in slowing down self-discharge, and thus enables the nickel-zinc battery to exhibit good storage performance and cycle stability in a high temperature environment. In addition, during the negative electrode charge and discharge process of the nickel-zinc battery, Zn and ZnO need to undergo path conversion, involving a variety of zinc intermediates, and the above-mentioned zinc-containing substances in the aqueous environment are rich in Zn. 2+ , which can provide abundant Zn for the above conversion process 2+ The nickel-zinc battery negative electrode provided in the present application is conducive to slowing down the self-discharge of the battery, while improving the life and high-temperature storage performance of the nickel-zinc battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The invention discloses a process for preparing a negative electrode of a nickel-zinc battery. DETAILED DESCRIPTION

[0023] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0024] The present invention provides a negative electrode material for a nickel-zinc battery, comprising a negative electrode active material and a negative electrode additive, wherein the negative electrode additive comprises a first negative electrode additive, wherein the first negative electrode additive comprises magnesium oxide and a zinc-containing substance, and the zinc-containing substance comprises one or more of calcium zincate, zinc hydroxide, zinc sulfate and zinc gluconate.

[0025] Nickel-zinc batteries have serious self-discharge under strong alkaline conditions, which affects the long-term storage performance of the battery.

[0026] Specifically, the negative electrode of the nickel-zinc battery includes a negative electrode active material layer, including a negative electrode active material and a negative electrode additive. The negative electrode additive includes a first negative electrode additive. The first negative electrode additive includes magnesium oxide and a zinc-containing substance. After adding magnesium oxide, the magnesium element forms a uniform, extremely thin magnesium-containing interface protective film on the negative electrode under weak alkaline conditions in the water system, which slows down the corrosion of alkalinity on ZnO and Zn in the negative electrode, plays a role in slowing down self-discharge, and thus enables the nickel-zinc battery to exhibit good storage performance and cycle stability in a high temperature environment. In addition, during the charge and discharge process of the negative electrode of the nickel-zinc battery, Zn and ZnO need to undergo path conversion, involving a variety of zinc intermediates, and the above-mentioned zinc-containing substances in the water system environment are rich in Zn 2+ , which can provide abundant Zn for the above conversion process 2+ Material, accelerates the conversion of materials during the charge and discharge process of the negative electrode, and reduces the loss of Zn and ZnO; in addition, when the zinc-containing material is zinc hydroxide, the zinc hydroxide contains OH- which can improve the ion conductivity of the slurry, which is beneficial to the ion migration during the battery charging process; that is, the nickel-zinc battery negative electrode provided by the present application is beneficial to slowing down the self-discharge phenomenon of the battery, while improving the life and high-temperature storage performance of the nickel-zinc battery.

[0027] In one embodiment, the mass ratio of the magnesium oxide to the zinc-containing substance is 1:3 to 3:1.

[0028] Specifically, the mass ratio of the magnesium oxide to the zinc-containing substance may be 1:3, 2:3 or 3:1.

[0029] In one embodiment, the first negative electrode additive is added in an amount of 1 wt % to 10 wt % in the negative electrode material of the nickel-zinc battery.

[0030] Specifically, adding the magnesium oxide and the zinc-containing substance to the negative electrode material of the nickel-zinc battery, and further adjusting the overall addition amount of the magnesium oxide and the zinc-containing substance, is beneficial to optimizing the overall storage and cycle performance of the nickel-zinc battery.

[0031] Specifically, the addition amount of the magnesium oxide and the zinc-containing substance in the negative electrode active material of the nickel-zinc battery can be 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt% or 10wt%.

[0032] In one embodiment, the amount of the magnesium oxide and the zinc-containing substance added to the nickel-zinc battery negative electrode active material is 1wt% to 5wt%; preferably, the total amount of the magnesium oxide and the zinc-containing substance added can be 1wt%, 2wt%, 3wt%, 4wt% or 5wt%, more preferably, the total amount of the magnesium oxide and the zinc-containing substance added is 3wt% or 5wt%.

[0033] In one embodiment, the negative electrode additive further includes a second negative electrode additive, wherein the second negative electrode additive includes In 2 O 3 、Bi 2 O 3 、Al 2 O 3 and Ca(OH) 2 One or more of .

[0034] Specifically, in 2 O 3 (Indium oxide) is mainly used as an electrolyte additive, separator material and positive electrode material modifier in batteries. 2 O 3 In the negative electrode of the battery, it mainly plays the role of improving conductivity and enhancing cycle stability, thereby significantly improving battery performance; specifically, when In 2 O 3 When used as an additive for battery negative electrode materials, it can effectively reduce the internal resistance of the battery, thereby improving the charge and discharge efficiency of the battery, and further significantly improve the overall conductivity of the electrode material. 2 O 3 The structural stability of In enables it to maintain a high capacity after multiple charge and discharge cycles. By combining with other negative electrode materials such as graphite or silicon, In 2 O 3 It helps to reduce the structural damage of these materials caused by volume changes during the charge and discharge process, thereby improving the cycle stability of the battery; Bi 2 O 3 (Bismuth oxide) plays a role in improving electrochemical performance, inhibiting dendrite formation and enhancing cycle life in the negative electrode material of nickel-zinc batteries; specifically, Bi 2 O 3 As an electrode material, it has a high theoretical capacity because bismuth can react reversibly with metals such as lithium and sodium to form alloys, thereby storing a large amount of energy. In addition, in secondary batteries such as nickel-zinc batteries, Bi 2 O 3 As an additive, it can effectively inhibit the formation of dendrites, thereby improving the safety and cycle stability of the battery. 2 O 3 , a dendrite-free zinc anode can be prepared, which is beneficial to improve the energy density and power of the battery; Bi 2 O 3 By combining with carbon or zinc materials, the volume expansion problem during charge and discharge can be alleviated, and the cycle stability of electrode materials can be improved. 2 O 3 With zinc oxide composite materials (such as ZnO / ZnO~Bi 2 O 3) showed stable performance in the cycle test; specifically, Al 2 O 3 In the negative electrode of nickel-zinc batteries, Al plays a role in inhibiting dendrite growth, improving electrochemical performance and increasing life. 2 O 3 It helps to maintain the activity and specific surface area of ​​the zinc electrode during the cycle, destroys the tight stacking of zinc oxide, and increases the reactive surface area of ​​zinc oxide, so that zinc oxide maintains a high electrochemical activity during the cycle; specifically, Ca(OH) 2 During the charging process, the hydrogen evolution overpotential of the zinc negative electrode can be increased, thereby enhancing the corrosion resistance of zinc metal. In addition, Ca(OH) 2 It can improve the charging efficiency of the zinc negative electrode, improve the electrochemical reaction conditions, and help to increase the overall cycle life of the zinc-nickel battery; in summary, adding a second negative electrode additive to the negative electrode of the nickel-zinc battery is beneficial to improving the overall electrical performance of the nickel-zinc battery.

[0035] In one embodiment, the In 2 O 3 The addition amount is 0.01% to 1%, the Bi 2 O 3 The addition amount is 0.08% to 2.88%, the Al 2 O 3 The addition amount is 3% to 5%, the Ca(OH) 2 The addition amount is 1% to 3%.

[0036] Specifically, the In 2 O 3 The addition amount of can be 0.01%, 0.05%, 0.10%, 0.20%, 0.30%, 0.40%, 0.50%, 0.60%, 0.70%, 0.80%, 0.90% or 1%; the addition amount of Bi2O3 can be 0.08%, 0.15%, 0.20%, 0.30%, 0.40%, 0.50%, 0.60%, 0.70%, 0.80%, 0.90%, 1%, 1.5%, 1.8%, 2.3%, 2.5%, 2.7%, 2.8% or 2.88%; the Al 2 O 3 The addition amount can be 3%, 3.2%, 3.5%, 4%, 4.5% or 5%; the addition amount of Ca(OH)2 can be 1%, 1.5%, 2%, 2.5%, 2.8% or 3%; by adding the above substances in appropriate amounts, the storage performance of the nickel-zinc battery under high temperature cycle can be improved.

[0037] In one embodiment, the negative electrode active material layer further includes a conductive agent, a thickener, a dispersant and a binder;

[0038] In the nickel-zinc battery negative electrode material, the added mass of the conductive agent is 1% to 2%, the added mass of the thickener is 0.3% to 0.5%, the added mass of the dispersant is 1% to 2%, and the added mass of the binder is 2% to 3%.

[0039] Specifically, the conductive agent includes one or more of nickel powder, carbonyl nickel powder, cobalt oxide, graphene, graphite, acetylene black and carbon powder; the thickener includes carboxymethyl cellulose (CMC); the dispersant includes any one of sodium polyacrylate (PAANa), potassium polyacrylate (PAAK), polyacrylamide (PAM) and polyacrylic acid (PAA); selecting a polymer with high ionic conductivity as a dispersant can reduce the internal resistance of the negative electrode, increase the conductivity, and improve the storage and life of the battery. In a preferred embodiment, the dispersant is selected from polyacrylic acid; the binder includes styrene-butadiene rubber (SBR) and polytetrafluoroethylene (PTFE), and the mass ratio of the styrene-butadiene rubber to the polytetrafluoroethylene is 4:1.

[0040] The added amount of the conductive agent can be 1%, 1.3%, 1.5%, 1.8% or 2.0%; the added amount of the thickener can be 0.3%, 0.4% or 0.5%; the added amount of the dispersant can be 1%, 1.3%, 1.5%, 1.8% or 1.2%; the added amount of the binder can be 2%, 2.3%, 2.5%, 2.8% or 3%.

[0041] In one embodiment, the negative electrode active material includes zinc and zinc oxide, and the mass ratio of the zinc to the zinc oxide is 1:7 to 1:3.

[0042] Another embodiment of the present invention provides a nickel-zinc battery negative electrode, comprising a current collector and a negative electrode material layer, wherein the negative electrode material layer is disposed on the current collector, and the negative electrode material layer comprises the nickel-zinc battery negative electrode material described in any of the above embodiments. Another embodiment of the present invention provides a method for preparing a nickel-zinc battery negative electrode, comprising the following operations:

[0043] S1: After mixing the conductive agent, thickener and dispersant, add the second negative electrode additive and mix well to obtain a mixture A;

[0044] S2: adding the first negative electrode additive to the mixture A, and then adding the negative electrode active material, and mixing again to obtain a mixture B;

[0045] S3: adding the binder to the mixture B and mixing well to obtain a negative electrode slurry;

[0046] S4: coating the negative electrode slurry onto the corresponding negative electrode current collector to obtain a negative electrode for a nickel-zinc battery.

[0047] When calcium hydroxide is included as the second negative electrode additive of the nickel-zinc battery, attention should be paid to the order of adding the materials. Specifically, the negative electrode active materials can be added in batches to improve the degree of mixed dispersion. In addition, before adding calcium hydroxide, the conductive agent (such as nickel powder, graphite, etc.) can be mixed with the negative electrode material, and then the calcium hydroxide can be added to the negative electrode material containing the conductive agent to promote the dispersion of the mixture. A reasonable order of addition can not only maximize the performance advantages of calcium hydroxide, but also utilize its stable chemical properties to ensure that the nickel-zinc battery exhibits excellent electrochemical performance and stability in practical applications.

[0048] Specifically, the negative electrode slurry prepared in S3 is coated on the negative electrode current collector, and the negative electrode sheet is obtained after rolling and drying; the negative electrode current collector is any one of a diagonally drawn copper mesh, a tinned diagonally drawn copper mesh, a galvanized diagonally drawn copper mesh, a copper foil, and a tinned copper foil, wherein the thickness of the diagonally drawn copper mesh is 0.17 mm, the porosity is 60% to 85%, and the specification is 20 to 500 meshes, wherein the tinned diagonally drawn copper mesh and the galvanized diagonally drawn copper mesh have a coating thickness of 2 to 10 μm,

[0049] The thickness of the copper foil is 0.17 mm, the porosity is 40% to 60%, and the coating thickness of the tin-plated copper foil is 3 to 5 μm.

[0050] The nickel-zinc battery negative electrode also includes auxiliary adhesive tape, and the auxiliary adhesive tape is selected from any one of masking adhesive and insulating adhesive.

[0051] Another embodiment of the present invention provides a nickel-zinc battery, comprising a positive electrode, a separator, an electrolyte, and the nickel-zinc battery negative electrode or the nickel-zinc battery negative electrode prepared by the nickel-zinc battery negative electrode preparation method.

[0052] The diaphragm is placed between the positive electrode and the negative electrode to form a battery cell, and then the battery cell and the battery casing are assembled and injected to obtain a nickel-zinc battery; in the negative electrode material of the nickel-zinc battery described in the present application, the first negative electrode additive includes magnesium oxide and a zinc-containing substance. After adding magnesium oxide, the magnesium element forms a uniform, extremely thin magnesium-containing interface protective film at the negative electrode under weak alkaline conditions in the aqueous system, which slows down the corrosion of alkaline to ZnO and Zn in the negative electrode, plays a role in slowing down self-discharge, and thus enables the nickel-zinc battery to exhibit good storage performance and cycle stability in a high temperature environment. In addition, during the charge and discharge process of the negative electrode of the nickel-zinc battery, Zn and ZnO need to undergo path conversion, involving a variety of zinc intermediates, and the above-mentioned zinc-containing substances are rich in Zn in the aqueous environment. 2+ , which can provide abundant Zn for the above conversion process 2+ The nickel-zinc battery negative electrode provided in the present application is conducive to slowing down the self-discharge of the battery, while improving the life and high-temperature storage performance of the nickel-zinc battery.

[0053] The positive electrode comprises a positive electrode current collector and a positive electrode active material layer, wherein the positive electrode active material layer comprises a positive electrode active material, and the positive electrode active material is selected from Ni(OH) 2 (nickel hydroxide), ZnO, CoO (cobalt oxide), Ni powder, Y 2 O 3 (yttrium trioxide) and Yb 2 O 3 (ytterbium trioxide) or one or more thereof.

[0054] The positive electrode current collector has a surface density of 300 to 400 g / m 2 Nickel foam.

[0055] The positive electrode active material layer further includes a positive electrode binder and a positive electrode conductor. The positive electrode active material, the positive electrode binder and the positive electrode conductor are blended to obtain the positive electrode active material layer.

[0056] The positive electrode binder can be polyvinylidene fluoride, a copolymer of vinylidene fluoride, polytetrafluoroethylene, a copolymer of vinylidene fluoride-hexafluoropropylene, a copolymer of tetrafluoroethylene-hexafluoropropylene, a copolymer of tetrafluoroethylene-perfluoroalkyl vinyl ether, a copolymer of ethylene-tetrafluoroethylene, a copolymer of vinylidene fluoride-tetrafluoroethylene, a copolymer of vinylidene fluoride-trifluoroethylene, a copolymer of vinylidene fluoride-trichloroethylene, a copolymer of vinylidene fluoride-fluoroethylene, a copolymer of vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene, a thermoplastic resin such as thermoplastic polyimide, polyethylene and polypropylene; at least one of acrylic resin, carboxymethyl cellulose and styrene butadiene rubber.

[0057] The positive electrode conductive agent may be at least one of conductive carbon black, conductive carbon balls, conductive graphite, conductive carbon fibers, carbon nanotubes, graphene, or reduced graphene oxide.

[0058] The diaphragm can be an existing conventional diaphragm, which can be a ceramic diaphragm, a polymer diaphragm, a non-woven fabric, a non-woven

[0059] Organic-organic composite membranes, including but not limited to single-layer PP (polypropylene), single-layer PE (polyethylene),

[0060] Double-layer PP / PE, double-layer PP / PP and triple-layer PP / PE / PP diaphragms.

[0061] The pH value of the electrolyte is 13-15, the specific gravity is 1.2-1.5 g / mL, and the conductivity at 25° C. is 350-500 mS / cm.

[0062] In one embodiment, the electrolyte includes solution A and solution B, wherein solution A includes an alkaline solution and a zinc oxide solution, and solution B includes a phosphate solution and a boric acid solution;

[0063] The mass ratio of solution A to solution B is 8-9:1.

[0064] Specifically, the solution A is a 5-7 mol / L alkaline solution and a saturated ZnO solution, and the solution B is 2 wt % phosphate and 2 wt % boric acid;

[0065] The alkaline solution in the solution A includes one or more of nickel hydroxide, potassium hydroxide and sodium hydroxide; the nickel hydroxide, potassium hydroxide and sodium hydroxide are key components in the electrolyte of alkaline batteries and play an important role in improving battery performance;

[0066] The electrolyte containing nickel hydroxide can improve the energy density of the battery, so that the battery has a higher capacity under the same volume. The stability of nickel hydroxide in the electrochemical reaction helps to extend the cycle life of the battery and reduce the battery performance degradation. Potassium hydroxide, as a strong base, can produce a large amount of OH- ions after dissolving in water, thereby improving the conductivity of the electrolyte. In high or low temperature environments, sodium hydroxide electrolytes of appropriate concentrations can maintain good performance. In addition, compared with potassium hydroxide, the cost of sodium hydroxide is lower, which is conducive to reducing battery manufacturing costs. In summary, the ions formed after the above-mentioned alkaline compounds (nickel hydroxide, potassium hydroxide, sodium hydroxide) are dissolved in water can effectively improve the ionic conductivity of the electrolyte, thereby enhancing the overall performance of the battery.

[0067] In a specific embodiment, the alkaline solution of solution A is selected from potassium hydroxide.

[0068] The present invention is further described below by way of examples.

[0069] Example 1

[0070] This embodiment is used to illustrate a nickel-zinc battery negative electrode, a negative electrode preparation method and a nickel-zinc battery disclosed in the present invention, and includes the following steps:

[0071] Preparation of negative electrode:

[0072] S1: Mix 1.5% conductive material, 0.32% thickener, and 1.5% dispersant, and add 0.05% In 2 O 3 、2.8% Bi 2 O 3 、4% Al 2 O 3 , stirring for 30 min, and mixing well to obtain mixture A;

[0073] S2: Add magnesium oxide, zinc hydroxide (the mass ratio of the two is 1:3, and the total content of the two is 3%) and 1.5% Ca(OH) 2 , stirring for 30 min, after mixing, adding 60% ZnO and 27% Zn three times, mixing again, to obtain mixture B;

[0074] S3: adding the binder to the mixture B and mixing well to obtain a negative electrode slurry;

[0075] S4: coating the negative electrode slurry onto the obliquely drawn tin-plated copper mesh current collector, rolling, softening and cutting to obtain the negative electrode of the nickel-zinc battery.

[0076] Preparation of positive electrode:

[0077] Ni(OH) 2 , ZnO, CoO, Ni powder, Ca(OH) 2 , Y 2 O 3 , Yb 2 O 3 , graphite, CMC, and PTFE are mixed in a weight ratio of 80-90:1:3:2:1:2-3:2:1:5:0.5:3, stirred evenly, coated on the positive electrode collector, and then rolled, softened, and cut to make the nickel-zinc battery positive electrode.

[0078] Prepare electrolyte:

[0079] The electrolyte is a mixture of 5-5.5 mol / L KOH, 0.5 mol / L ZnO, 2 wt% disodium hydrogen phosphate and 2 wt% boric acid.

[0080] Preparation of nickel-zinc battery:

[0081] Assemble the positive electrode, negative electrode and separator into a battery cell. After injection, the zinc-nickel battery has an electrolyte of 25%.

[0082] A mixture of KOH and 1.5% LiOH

[0083] The positive electrode, the separator and the negative electrode are stacked in order so that the separator is between the positive and negative electrodes to prepare a battery cell. The battery cell is dried in an outer packaging bag, injected with the above-mentioned electrolyte, and subjected to vacuum packaging, standing, forming, shaping and other processes to obtain a nickel-zinc battery.

[0084] Example 2

[0085] This embodiment is used to illustrate a nickel-zinc battery negative electrode, a method for preparing a negative electrode, and a nickel-zinc battery disclosed in the present invention, and includes most of the steps in Example 1, except that:

[0086] During the preparation of the negative electrode: the first negative electrode additive is magnesium oxide and calcium zincate, with a mass ratio of 1:3, and the total content of the two is 3%.

[0087] Example 3

[0088] This embodiment is used to illustrate a nickel-zinc battery negative electrode, a method for preparing a negative electrode, and a nickel-zinc battery disclosed in the present invention, and includes most of the steps in Example 1, except that:

[0089] During the preparation of the negative electrode: the first negative electrode additive is magnesium oxide and zinc sulfate, the mass ratio is 1:3, and the total content of the two is 3%.

[0090] Example 4

[0091] This embodiment is used to illustrate a nickel-zinc battery negative electrode, a method for preparing a negative electrode, and a nickel-zinc battery disclosed in the present invention, and includes most of the steps in Example 1, except that:

[0092] During the preparation of the negative electrode: the first negative electrode additive is magnesium oxide and zinc gluconate, the mass ratio is 1:3, and the total content of the two is 3%.

[0093] Example 5

[0094] This embodiment is used to illustrate a nickel-zinc battery negative electrode, a method for preparing a negative electrode, and a nickel-zinc battery disclosed in the present invention, and includes most of the steps in Example 1, except that:

[0095] During the preparation of the negative electrode: the first negative electrode additive is magnesium oxide and zinc hydroxide, with a mass ratio of 2:3, and the total content of the two is 3%.

[0096] Example 6

[0097] This embodiment is used to illustrate a nickel-zinc battery negative electrode, a method for preparing a negative electrode, and a nickel-zinc battery disclosed in the present invention, and includes most of the steps in Example 1, except that:

[0098] During the preparation of the negative electrode: the first negative electrode additive is magnesium oxide and zinc hydroxide, with a mass ratio of 3:1, and the total content of the two is 3%.

[0099] Example 7

[0100] This embodiment is used to illustrate a nickel-zinc battery negative electrode, a method for preparing a negative electrode, and a nickel-zinc battery disclosed in the present invention, and includes most of the steps in Example 1, except that:

[0101] During the preparation of the negative electrode: the first negative electrode additive is magnesium oxide and zinc hydroxide, with a mass ratio of 3:1, and the total content of the two is 5%.

[0102] Example 8

[0103] This embodiment is used to illustrate a nickel-zinc battery negative electrode, a method for preparing a negative electrode, and a nickel-zinc battery disclosed in the present invention, and includes most of the steps in Example 1, except that:

[0104] During the preparation of the negative electrode: the first negative electrode additive is magnesium oxide and zinc hydroxide, with a mass ratio of 3:1, and the total content of the two is 10%.

[0105] Example 9

[0106] This embodiment is used to illustrate a nickel-zinc battery negative electrode, a method for preparing a negative electrode, and a nickel-zinc battery disclosed in the present invention, and includes most of the steps in Example 1, except that:

[0107] During the preparation of the negative electrode: the first negative electrode additive is magnesium oxide and zinc hydroxide, with a mass ratio of 3:1, and the total content of the two is 1%.

[0108] Example 10

[0109] This embodiment is used to illustrate a nickel-zinc battery negative electrode, a method for preparing a negative electrode, and a nickel-zinc battery disclosed in the present invention, and includes most of the steps in Example 1, except that:

[0110] Negative electrode preparation: the Ca(OH) 2 The addition amount is 2%.

[0111] Embodiment 11

[0112] This embodiment is used to illustrate a nickel-zinc battery negative electrode, a method for preparing a negative electrode, and a nickel-zinc battery disclosed in the present invention, and includes most of the steps in Example 1, except that:

[0113] Negative electrode preparation: the Ca(OH) 2 The addition amount is 3%.

[0114] Comparative Example 1

[0115] This comparative example is used to illustrate a nickel-zinc battery negative electrode, a method for preparing a negative electrode, and a nickel-zinc battery disclosed in the present invention, and includes most of the steps in Example 1, except that:

[0116] No magnesium oxide and zinc-containing substances are added in the preparation of the negative electrode.

[0117] Comparative Example 2

[0118] This comparative example is used to illustrate a nickel-zinc battery negative electrode, a method for preparing a negative electrode, and a nickel-zinc battery disclosed in the present invention, and includes most of the steps in Example 1, except that:

[0119] During the preparation of the negative electrode, no zinc-containing substance is added to the first negative electrode additive.

[0120] Comparative Example 3

[0121] This comparative example is used to illustrate a nickel-zinc battery negative electrode, a method for preparing a negative electrode, and a nickel-zinc battery disclosed in the present invention, and includes most of the steps in Example 1, except that:

[0122] During the preparation of the negative electrode, magnesium oxide is not added to the first negative electrode additive.

[0123] Performance Testing

[0124] The following performance tests were performed on Examples 1 to 11 and Comparative Examples 1 to 3 prepared as above:

[0125] Life test: The condition is 1C charge to 1.9V, 1C discharge to 1.3V.

[0126] Storage performance test: 60℃, 7 days.

[0127] Storage performance capacity test conditions: 0.2C discharge to 1.3V, 0.2C charge to 1.9V, stand for 10 minutes, and the above operation is repeated three times.

[0128] The test results obtained are entered in Table 1.

[0129] Table 1

[0130]

[0131] It can be seen from the test results in Table 1 that the cycle performance and storage performance of the nickel-zinc battery prepared in Examples 1 to 7 are better than those of the nickel-zinc battery in Comparative Examples 1 to 3; wherein, compared with Examples 2 to 3, Example 1 has the best cycle performance and storage performance, because magnesium oxide and zinc hydroxide in the zinc-containing substance are added in Example 1, and OH- in the zinc hydroxide can further improve the ionic conductivity of the negative electrode slurry of the nickel-zinc battery, thereby optimizing the discharge performance of the nickel-zinc battery; in addition, compared with Examples 1 and Examples 6 to 7, Examples 8 to 9 have overall test performances slightly lower than those of Examples 1 and Examples 6 to 7, because the total content of magnesium oxide and zinc hydroxide in the first negative electrode additive in Example 8 is 10%, and the total content of magnesium oxide and zinc hydroxide in the first negative electrode additive in Example 9 is 1%, relative to Examples 1 and 6 to 7, there is a problem that the first negative electrode additive is too high or too low, thereby affecting the overall cycle performance and storage performance of the nickel-hydrogen battery; compared with Examples 10 to 11, Ca(OH) in Example 1 2 The addition amount of Ca(OH) in Examples 10 to 11 is 1.5%. 2 The addition amount is 2% and 3% respectively. It can be seen that the Ca(OH) in the negative electrode of the nickel-zinc battery provided in this application is 2The amount of Ca(OH) added will also affect the cycle performance and storage performance of the final prepared NiMH battery. 2 When the addition amount is 1%, the cycle performance and storage performance are relatively good; in Comparative Example 1, the first negative electrode additive described in the present application is not added. Therefore, compared with Comparative Examples 2 to 3, the overall test results of the cycle performance and storage performance of the nickel-hydrogen battery in Comparative Example 1 are lower than those in Comparative Examples 2 to 3.

[0132] By comparing the test results of Examples 1 to 11 with Comparative Examples 1 to 3, it can be seen that the magnesium oxide and the zinc-containing substance in the negative electrode material of the nickel-zinc battery provided by the present application form a magnesium-containing interface protective film at the negative electrode under weak alkaline conditions in the aqueous system, which slows down the corrosion of the alkaline to ZnO and Zn in the negative electrode, plays a role in slowing down the self-discharge, and thus enables the nickel-zinc battery to exhibit good storage performance and cycle stability in a high temperature environment. In addition, the zinc-containing substance is rich in Zn 2+ In the process of charging and discharging the negative electrode of nickel-zinc batteries, a variety of zinc intermediates are involved. In the aqueous environment, the above can provide rich Zn for the conversion process of Zn and ZnO. 2+ It accelerates the conversion of materials during the charge and discharge process of the negative electrode, reduces the loss of Zn and ZnO, helps to slow down the self-discharge of the battery, and at the same time improves the life and high-temperature storage performance of the nickel-zinc battery.

[0133] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A nickel-zinc battery negative electrode material, characterized in that: The invention comprises a negative electrode active material and a negative electrode additive, wherein the negative electrode additive comprises a first negative electrode additive, wherein the first negative electrode additive comprises magnesium oxide and a zinc-containing substance, and the zinc-containing substance comprises one or more of calcium zincate, zinc hydroxide, zinc sulfate and zinc gluconate.

2. The negative electrode material for nickel-zinc batteries according to claim 1, characterized in that: The mass ratio of the magnesium oxide to the zinc-containing substance is 1:3 to 3:

1.

3. The negative electrode material for nickel-zinc batteries according to claim 1, characterized in that: The first negative electrode additive is added in an amount of 1 wt % to 10 wt % in the negative electrode material of the nickel-zinc battery.

4. The negative electrode material for nickel-zinc batteries according to claim 1, characterized in that: The negative electrode additive further includes a second negative electrode additive, and the second negative electrode additive includes one or more of In2O3, Bi2O3, Al2O3 and Ca(OH)2.

5. The negative electrode material for nickel-zinc batteries according to claim 4, characterized in that: In the nickel-zinc battery negative electrode material, the added mass of In2O3 is 0.01% to 1%, the added mass of Bi2O3 is 0.08% to 2.88%, the added mass of Al2O3 is 3% to 5%, and the added mass of Ca(OH)2 is 1% to 3%.

6. The negative electrode material for nickel-zinc batteries according to claim 1, characterized in that: It also includes a conductive agent, a thickener, a dispersant and a binder; in the nickel-zinc battery negative electrode material, the added mass of the conductive agent is 1% to 2%, the added mass of the thickener is 0.3% to 0.5%, the added mass of the dispersant is 1% to 2%, and the added mass of the binder is 2% to 3%.

7. The negative electrode material for nickel-zinc batteries according to claim 1, characterized in that: The negative electrode active material includes zinc and zinc oxide, and the mass ratio of the zinc to the zinc oxide is 1:7 to 1:

3.

8. A nickel-zinc battery negative electrode, characterized in that: It comprises a current collector and a negative electrode material layer, wherein the negative electrode material layer is arranged on the current collector, and the negative electrode material layer comprises the nickel-zinc battery negative electrode material according to any one of claims 1 to 7.

9. The method for preparing a negative electrode of a nickel-zinc battery according to claim 8, characterized in that: The following operations are included: S1: After mixing the conductive agent, thickener and dispersant, add the second negative electrode additive and mix well to obtain a mixture A; S2: adding the first negative electrode additive to the mixture A, and then adding the negative electrode active material, and mixing again to obtain a mixture B; S3: adding the binder to the mixture B and mixing well to obtain a negative electrode slurry; S4: coating the negative electrode slurry onto the corresponding negative electrode current collector to obtain a negative electrode for a nickel-zinc battery.

10. A nickel-zinc battery, characterized in that: The invention comprises a positive electrode, a separator, an electrolyte and the negative electrode of the nickel-zinc battery according to any one of claims 1 to 8 or the negative electrode of the nickel-zinc battery prepared by the method for preparing the negative electrode of the nickel-zinc battery according to claim 9.