Homogeneous-phase high-temperature-resistant zinc-bromine flow battery electrolyte as well as preparation method and application thereof
By using ionic liquids to react with ZnBr2 in zinc bromine flow batteries to prepare homogeneous electrolytes, the dispersion of oil-phase polybromide complexes and easy decomplexing are solved, high energy density and thermal stability are achieved, and the Battery performance and efficiency.
Patent Information
- Application Number
- CN202411190099.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-08-23
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
AI Technical Summary
The uneven dispersion of oil-phase polybromide complex and aqueous electrolyte in zinc-bromide flow batteries leads to an increase in charge and discharge transfer resistance, reducing the overall performance of zinc-bromide flow batteries. The bromine complex is easy to decompress at high temperatures, which limits the The operating temperature of the battery.
The homogeneous electrolyte is prepared by reacting ionic liquid with ZnBr2 to form a homogeneous electrolyte with water and oil amphiphilicity, ensuring that the polybromide complex produced by the positive electrode is completely dissolved in the electrolyte, and the battery operating temperature is maintained in combination with the temperature control system. At 20-70°C, 1-methyl-1-ethylpyrrolidine bromide and 1-ethyl-3-methylimidazole bromide plasma liquid are selected as bromine complexing agents.
It achieves high energy density, good thermal stability and low viscosity, avoids the problem of easy decompression of bromine complexes at high temperatures, and maintains good battery efficiency and performance stability.
Smart Images

Figure CN119092770A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of zinc-bromine liquid flow batteries, and in particular relates to a homogeneous high-temperature resistant zinc-bromine liquid flow battery electrolyte, a preparation method thereof and an application thereof. Background Art
[0002] Under the stringent requirements of industrial development, flow batteries have shown great potential. Compared with other flow batteries, zinc-bromine flow batteries use the same aqueous electrolyte for positive and negative electrodes, have no cross-contamination, are low-cost, highly safe, and have a theoretical energy density of up to 430Wh / kg. They are considered to be one of the most promising large-scale energy storage technologies.
[0003] During the charging process of zinc-bromine flow battery, the positive electrode Br - Oxidation generates elemental bromine Br2, which is highly corrosive and volatile. In order to prevent Br2 from volatilizing and diffusing to the negative electrode to react with zinc to produce self-discharge and cause corrosion of related materials, a bromine complexing agent is usually added to the electrolyte to capture Br2 and prevent it from evaporating. 1-Methyl-1-ethylpyrrolidine bromide (MEP) is the most commonly used bromine complexing agent, which undergoes a reversible complexing reaction with bromine to form a dense, viscous oil-phase polybromine complex that is immiscible with the aqueous phase. Due to the uneven dispersion of the oily polybromine complex phase, the charge and discharge transfer resistance increases, which will rapidly reduce the overall performance of the zinc-bromine flow battery. In order to solve this problem, patent CN 116742092A discloses a new type of high-efficiency homogeneous bromine complexing agent, which is selected from cyclodextrin derivatives and improves the solubility of the bromine complex in the electrolyte through functional groups such as methyl, sulfate, and phosphate. On the other hand, the bromine complex is easy to decomplex at high temperatures, resulting in a low operating temperature of the zinc-bromine flow battery. Summary of the invention
[0004] In view of the technical problem of phase separation of oil-phase polybromine complex and aqueous electrolyte in zinc-bromine flow battery, the present invention proposes a homogeneous high-temperature resistant zinc-bromine flow battery electrolyte and a preparation method and application thereof. Homogeneous means that the polybromine complex produced by the positive electrode during battery charging will not become a separate phase, but will be completely dissolved in the electrolyte to become a homogeneous phase, thereby avoiding the reduction of the performance of the zinc-bromine flow battery due to the uneven dispersion of the polybromine complex phase in water.
[0005] In order to achieve the above object, the technical solution of the present invention is achieved as follows:
[0006] A method for preparing a homogeneous high-temperature resistant zinc-bromine flow battery electrolyte comprises the following steps: mixing an ionic liquid and ZnBr2 and reacting them to obtain a homogeneous electrolyte.
[0007] The anion of the ionic liquid is a bromide ion, and the cation is a pyrrole cation or an imidazole cation. The ionic liquid has non-volatility, non-flammability, and excellent electrochemical and thermal stability. The preferred ionic liquids are 1-methyl-1-ethylpyrrolidine bromide, 1-ethyl-3-methylimidazolium bromide, and 1-butyl-3-methylimidazolium bromide, all of which are solid at room temperature. It can be used as a bromine complexing agent in zinc-bromine flow batteries.
[0008] Select ZnBr2 to react with the preferred ionic liquid, and the product can provide Zn 2+ Supply negative electrode reaction and provide Br - Provides positive electrode reaction.
[0009] The molar ratio of the ionic liquid to ZnBr2 is 1:(0.5-1.5), preferably 1:(0.5~1).
[0010] The reaction temperature is 70-110°C, and the reaction temperature is different depending on the selected ionic liquid. The reaction temperature of 1-ethyl-3-methyl imidazole bromide and 1-butyl-3-methyl imidazole bromide is preferably 70-80°C, and the reaction temperature of 1-methyl-1-ethyl pyrrolidine bromide is preferably 100-110°C;
[0011] The reaction time is 24 to 72 hours, preferably 46 to 50 hours.
[0012] The reaction product of the partial ionic liquid and ZnBr2 is liquid at room temperature and can be directly used as an electrolyte at room temperature; if it is solid at room temperature, it needs to be heated and used as an electrolyte at high temperature.
[0013] The homogeneous electrolyte is the reaction product of the ionic liquid and ZnBr2, which is a kind of ionic liquid, easily soluble in the oil phase, with limited solubility in water, but completely soluble in a large amount of water phase, and has water-oil amphiphilicity. The principle that the positive electrode electrolyte always remains homogeneous is that the polybromine anions generated by the positive electrode and the cations of the ionic liquid produce electrostatic adsorption, and the formed oil-phase polybromine complex can be dissolved in the prepared homogeneous electrolyte.
[0014] A zinc-bromine flow battery, comprising a battery module, a positive electrode electrolyte storage tank, a negative electrode electrolyte storage tank, a circulation pump and a circulation pipeline; the battery module comprises a positive electrode, a negative electrode, a diaphragm and an electrolyte; it is characterized in that it also comprises a temperature control system, the temperature control system comprises a temperature control box for controlling the temperature of the entire battery system and a temperature controller for separately controlling the temperature of the battery stack and the electrolyte; the electrolyte is the homogeneous high temperature resistant zinc-bromine flow battery electrolyte as described in claim 7.
[0015] When the zinc-bromine flow battery is in operation, the temperature of the electrolyte of the homogeneous high-temperature resistant zinc-bromine flow battery is controlled to be 20-70° C. by a temperature control system.
[0016] The positive electrode and the negative electrode are both selected from carbon felt or carbon cloth.
[0017] Beneficial effects of the present invention:
[0018] (1) High energy density: The homogeneous electrolyte provided by the present invention is both an electrolyte and an active substance. It has a high energy density and is higher than 2M ZnBr2 aqueous solution (energy density of about 195Wh·L) under the same energy density conditions. -1 ) Small dosage and small footprint;
[0019] (2) High temperature resistance: The homogeneous electrolyte provided by the present invention is a type of ionic liquid, which has good thermal stability and non-flammability, and avoids the problem of easy decomplexation of bromine complexes at high temperatures. At the same time, the homogeneous electrolyte provided by the present invention is non-volatile and has low viscosity at high temperatures, and has better battery performance than that at room temperature;
[0020] (3) Homogeneous phase: Br2 generated at the positive electrode during the charging process. The ionic liquid used in the present invention contains bromide ions, which can form polybromine anions with bromine molecules, thereby having bromine complexing ability; at the same time, the synthesized homogeneous electrolyte has strong lipophilicity and can dissolve the generated polybromine complex, without causing two-phase problems and maintaining good battery efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0022] Figure 1 This is an application effect diagram of the present invention.
[0023] Figure 2 This is a diagram of the battery cycle performance of Example 2. DETAILED DESCRIPTION
[0024] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] Example 1
[0026] A method for preparing a homogeneous high temperature resistant zinc-bromine flow battery electrolyte comprises the following steps:
[0027] Take 0.2 mol 1-butyl-3-methylimidazole bromide and 0.1 mol ZnBr2 and add them into a 250 mL single-necked round-bottom flask. Use an oil bath to heat and stir the round-bottom flask. Stir and react at 70 °C for 48 h to obtain a light yellow ionic liquid electrolyte A1. Take 30 mL respectively and add them into the positive and negative electrolyte storage tanks for standby use.
[0028] Example 2
[0029] A method for preparing a homogeneous high temperature resistant zinc-bromine flow battery electrolyte comprises the following steps:
[0030] Take 0.2 mol 1-butyl-3-methylimidazole bromide and 0.2 mol ZnBr2 and add them into a 250 mL single-necked round-bottom flask. Use an oil bath to heat and stir the round-bottom flask. Stir and react at 70 °C for 72 h to obtain a light yellow ionic liquid electrolyte A2. Take 30 mL respectively and add them into the positive and negative electrolyte storage tanks for standby use.
[0031] Example 3
[0032] A method for preparing a homogeneous high temperature resistant zinc-bromine flow battery electrolyte comprises the following steps:
[0033] Take 0.2 mol 1-butyl-3-methylimidazole bromide and 0.3 mol ZnBr2 and add them into a 250 mL single-necked round-bottom flask. Use an oil bath to heat and stir the round-bottom flask. Stir and react at 75 °C for 48 h to obtain a light yellow ionic liquid electrolyte A3. Take 30 mL respectively and add them into the positive and negative electrolyte storage tanks for standby use.
[0034] Example 4
[0035] A method for preparing a homogeneous high temperature resistant zinc-bromine flow battery electrolyte comprises the following steps:
[0036] Take 0.3 mol 1-ethyl-3-methylimidazole bromide and 0.3 mol ZnBr2 and add them into a 250 mL single-necked round-bottom flask. Use an oil bath to heat and stir the round-bottom flask. Stir and react at 70 °C for 24 h to obtain a light yellow ionic liquid electrolyte A4. Take 30 mL respectively and add them into the positive and negative electrolyte storage tanks for standby use.
[0037] Example 5
[0038] A method for preparing a homogeneous high temperature resistant zinc-bromine flow battery electrolyte comprises the following steps:
[0039] Take 0.3 mol 1-methyl-1-ethylpyrrolidine bromide and 0.3 mol ZnBr2 and add them into a 250 mL single-necked round-bottom flask. Use an oil bath to heat and stir the round-bottom flask. Stir and react at 105 °C for 48 h to obtain a reddish-brown ionic liquid electrolyte A5. Take 30 mL respectively and add them into the positive and negative electrolyte storage tanks for standby use.
[0040] Comparative Example 1
[0041] Prepare 2M ZnBr2, 3M KCl, and 2M 1-methyl-1-ethylpyrrolidine bromide aqueous solution B1, take 30mL respectively and add them to the positive and negative electrode electrolyte storage tanks for later use.
[0042] Application Examples
[0043] A zinc-bromine flow battery comprises a battery module, a positive electrode electrolyte storage tank, a negative electrode electrolyte storage tank, a circulation pump and a circulation pipeline; the battery module comprises a positive electrode, a negative electrode, a diaphragm and an electrolyte; it is characterized in that it also comprises a temperature control system, the temperature control system comprises a temperature control box for controlling the temperature of the entire battery system and a temperature controller for separately controlling the temperature of the battery stack and the electrolyte; the electrolyte is a homogeneous high temperature resistant zinc-bromine flow battery electrolyte.
[0044] Specifically, the positive terminal plate, current collector, graphite plate, carbon felt / carbon cloth, separator, carbon felt / carbon cloth, graphite plate, current collector, and negative terminal plate are arranged in sequence to assemble the battery. The effective area of the carbon felt electrode is 4 cm 2 (2cm×2cm). A thermostat is used to control the temperature of the battery and electrolyte. The electrolyte is circulated in the battery and storage tank by a pump. The structure is as follows Figure 1 As shown, the positive electrode electrolyte is brown-red, uniform and transparent, without phase separation. The battery test charge and discharge current is set to 20mA / cm 2 , the charge cut-off condition is set to 1mAh / cm 2 The discharge cut-off condition sets the voltage to 0.1 V. The test results of the electrolytes prepared in Examples 1-5 and Comparative Example 1 are shown in Table 1. The battery cycle performance of Example 2 is shown in Table 1. Figure 2 shown.
[0045] Table 1 Battery test results corresponding to the electrolytes obtained in the examples and comparative examples
[0046]
[0047] As shown in Table 1, when using A1 at different temperatures, the battery efficiency reaches a peak at 60°C, so the optimal test temperature is 60°C. The amount of active substance zinc bromide in A1, A2 and A3 gradually increases, and accordingly, the energy density also gradually increases. At the same temperature, equimolar amounts of ionic liquid and ZnBr2 show the best battery efficiency, so the molar amount of ionic liquid and zinc bromide is fixed to 1:1 in A4 and A5, which also shows good battery efficiency.
[0048] Example 6
[0049] A method for preparing a homogeneous high temperature resistant zinc-bromine flow battery electrolyte comprises the following steps:
[0050] Take 0.2 mol 1-ethyl-3-methylimidazole bromide and 0.1 mol ZnBr2 and add them into a 250 mL single-necked round-bottom flask. Use an oil bath to heat and stir the round-bottom flask. Stir and react at 70 °C for 48 h to obtain a light yellow ionic liquid electrolyte. Take 30 mL respectively and add them into the positive and negative electrolyte storage tanks for later use.
[0051] Example 7
[0052] A method for preparing a homogeneous high temperature resistant zinc-bromine flow battery electrolyte comprises the following steps:
[0053] Take 0.2 mol 1-ethyl-3-methylimidazole bromide and 0.1 mol ZnBr2 and add them into a 250 mL single-necked round-bottom flask. Use an oil bath to heat and stir the round-bottom flask. Stir and react at 75 °C for 48 h to obtain a light yellow ionic liquid electrolyte. Take 30 mL respectively and add them into the positive and negative electrolyte storage tanks for standby use.
[0054] Example 8
[0055] A method for preparing a homogeneous high temperature resistant zinc-bromine flow battery electrolyte comprises the following steps:
[0056] Take 0.2 mol 1-ethyl-3-methylimidazole bromide and 0.1 mol ZnBr2 and add them into a 250 mL single-necked round-bottom flask. Use an oil bath to heat and stir the round-bottom flask. Stir and react at 80 °C for 48 h to obtain a light yellow ionic liquid electrolyte. Take 30 mL respectively and add them into the positive and negative electrolyte storage tanks for standby use.
[0057] Example 9
[0058] A method for preparing a homogeneous high temperature resistant zinc-bromine flow battery electrolyte comprises the following steps:
[0059] Take 0.2 mol 1-butyl-3-methylimidazole bromide and 0.1 mol ZnBr2 and add them into a 250 mL single-necked round-bottom flask. Use an oil bath to heat and stir the round-bottom flask. Stir and react at 70 °C for 48 h to obtain a light yellow ionic liquid electrolyte. Take 30 mL respectively and add them into the positive and negative electrolyte storage tanks for later use.
[0060] Example 10
[0061] A method for preparing a homogeneous high temperature resistant zinc-bromine flow battery electrolyte comprises the following steps:
[0062] Take 0.2 mol 1-butyl-3-methylimidazole bromide and 0.1 mol ZnBr2 and add them into a 250 mL single-necked round-bottom flask. Use an oil bath to heat and stir the round-bottom flask. Stir and react at 80 °C for 48 h to obtain a light yellow ionic liquid electrolyte. Take 30 mL respectively and add them into the positive and negative electrolyte storage tanks for later use.
[0063] Embodiment 11
[0064] A method for preparing a homogeneous high temperature resistant zinc-bromine flow battery electrolyte comprises the following steps:
[0065] Take 0.2 mol of 1-methyl-1-ethylpyrrole bromide and 0.1 mol of ZnBr2 and add them into a 250 mL single-necked round-bottom flask. Use an oil bath to heat and stir the round-bottom flask. Stir and react at 100 °C for 48 h to obtain a reddish-brown ionic liquid electrolyte. Take 30 mL of each and add them into the positive and negative electrolyte storage tanks for later use.
[0066] Example 12
[0067] A method for preparing a homogeneous high temperature resistant zinc-bromine flow battery electrolyte comprises the following steps:
[0068] Take 0.2 mol of 1-methyl-1-ethylpyrrole bromide and 0.1 mol of ZnBr2 and add them into a 250 mL single-necked round-bottom flask. Use an oil bath to heat and stir the round-bottom flask. Stir and react at 105 °C for 48 h to obtain a reddish-brown ionic liquid electrolyte. Take 30 mL respectively and add them into the positive and negative electrolyte storage tanks for later use.
[0069] Embodiment 13
[0070] A method for preparing a homogeneous high temperature resistant zinc-bromine flow battery electrolyte comprises the following steps:
[0071] Take 0.2 mol of 1-methyl-1-ethylpyrrole bromide and 0.1 mol of ZnBr2 and add them into a 250 mL single-necked round-bottom flask. Use an oil bath to heat and stir the round-bottom flask. Stir and react at 110 °C for 48 h to obtain a reddish-brown ionic liquid electrolyte. Take 30 mL respectively and add them into the positive and negative electrolyte storage tanks for later use.
[0072] Embodiment 14
[0073] A method for preparing a homogeneous high temperature resistant zinc-bromine flow battery electrolyte comprises the following steps:
[0074] Take 0.2 mol 1-ethyl-3-methylimidazole bromide and 0.3 mol ZnBr2 and add them into a 250 mL single-necked round-bottom flask. Use an oil bath to heat and stir the round-bottom flask. Stir and react at 70 °C for 24 h to obtain a light yellow ionic liquid electrolyte. Take 30 mL respectively and add them into the positive and negative electrolyte storage tanks for standby use.
[0075] Embodiment 15
[0076] A method for preparing a homogeneous high temperature resistant zinc-bromine flow battery electrolyte comprises the following steps:
[0077] Take 0.2 mol 1-ethyl-3-methylimidazole bromide and 0.3 mol ZnBr2 and add them into a 250 mL single-necked round-bottom flask. Use an oil bath to heat and stir the round-bottom flask. Stir and react at 75 °C for 46 h to obtain a light yellow ionic liquid electrolyte. Take 30 mL respectively and add them into the positive and negative electrolyte storage tanks for later use.
[0078] Example 16
[0079] A method for preparing a homogeneous high temperature resistant zinc-bromine flow battery electrolyte comprises the following steps:
[0080] Take 0.2 mol 1-ethyl-3-methylimidazole bromide and 0.3 mol ZnBr2 and add them into a 250 mL single-necked round-bottom flask. Use an oil bath to heat and stir the round-bottom flask. Stir and react at 75 °C for 50 h to obtain a light yellow ionic liquid electrolyte. Take 30 mL respectively and add them into the positive and negative electrolyte storage tanks for later use.
[0081] Embodiment 17
[0082] A method for preparing a homogeneous high temperature resistant zinc-bromine flow battery electrolyte comprises the following steps:
[0083] Take 0.2 mol 1-ethyl-3-methylimidazole bromide and 0.3 mol ZnBr2 and add them into a 250 mL single-necked round-bottom flask. Use an oil bath to heat and stir the round-bottom flask. Stir and react at 75 °C for 72 h to obtain a light yellow ionic liquid electrolyte. Take 30 mL respectively and add them into the positive and negative electrolyte storage tanks for later use.
[0084] Embodiment 18
[0085] A method for preparing a homogeneous high temperature resistant zinc-bromine flow battery electrolyte comprises the following steps:
[0086] Take 0.2 mol 1-methyl-1-ethylpyrrolidine bromide and 0.3 mol ZnBr2 and add them into a 250 mL single-necked round-bottom flask. Use an oil bath to heat and stir the round-bottom flask. Stir and react at 105 °C for 48 h to obtain a reddish-brown ionic liquid electrolyte. Take 30 mL respectively and add them into the positive and negative electrolyte storage tanks for later use.
[0087] Embodiment 19
[0088] A method for preparing a homogeneous high temperature resistant zinc-bromine flow battery electrolyte comprises the following steps:
[0089] Take 0.2 mol 1-methyl-1-ethylpyrrolidine bromide and 0.3 mol ZnBr2 and add them into a 250 mL single-necked round-bottom flask. Use an oil bath to heat and stir the round-bottom flask. Stir and react at 105 °C for 50 h to obtain a reddish-brown ionic liquid electrolyte. Take 30 mL respectively and add them into the positive and negative electrolyte storage tanks for later use.
[0090] Embodiment 20
[0091] A method for preparing a homogeneous high temperature resistant zinc-bromine flow battery electrolyte comprises the following steps:
[0092] Take 0.2 mol 1-methyl-1-ethylpyrrolidine bromide and 0.3 mol ZnBr2 and add them into a 250 mL single-necked round-bottom flask. Use an oil bath to heat and stir the round-bottom flask. Stir and react at 105 °C for 72 h to obtain a reddish-brown ionic liquid electrolyte. Take 30 mL respectively and add them into the positive and negative electrolyte storage tanks for later use.
[0093] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a homogeneous high temperature resistant zinc-bromine flow battery electrolyte, It is characterized in that The following steps are involved: The ionic liquid and ZnBr 2 After mixing, the mixture is reacted to obtain a homogeneous electrolyte.
2. The method for preparing the homogeneous high temperature resistant zinc-bromine flow battery electrolyte according to claim 1, It is characterized in that The anion of the ionic liquid is a bromide ion, and the cation is a pyrrole cation or an imidazole cation.
3. The method for preparing the homogeneous high temperature resistant zinc-bromine flow battery electrolyte according to claim 2, It is characterized in that The ionic liquid is 1-methyl-1-ethylpyrrolidine bromide, 1-ethyl-3-methylimidazole bromide, and 1-butyl-3-methylimidazole bromide.
4. A method for preparing a homogeneous high temperature resistant zinc-bromine flow battery electrolyte according to any one of claims 1 to 3, It is characterized in that The ionic liquid and ZnBr 2 The molar ratio is 1:(0.5~1.5).
5. The method for preparing the homogeneous high temperature resistant zinc-bromine flow battery electrolyte according to claim 4, It is characterized in that The ionic liquid and ZnBr 2 The molar ratio is 1:(0.5~1).
6. The method for preparing the homogeneous high temperature resistant zinc-bromine flow battery electrolyte according to claim 1, It is characterized in that The reaction temperature is 70-110° C., and the reaction time is 24-72 hours.
7. A homogeneous high temperature resistant zinc-bromine flow battery electrolyte prepared by the method according to any one of claims 1 to 6.
8. A zinc-bromine flow battery, It is characterized in that It comprises a battery module, a positive electrode electrolyte storage tank, a negative electrode electrolyte storage tank, a circulation pump and a circulation pipeline; the battery module comprises a positive electrode, a negative electrode, a diaphragm and an electrolyte; it is characterized in that it also comprises a temperature control system, the temperature control system comprises a temperature control box for controlling the temperature of the entire battery system and a temperature controller for controlling the temperature of the battery stack and the electrolyte separately; the electrolyte is the homogeneous high temperature resistant zinc-bromine flow battery electrolyte as described in claim 7.
9. The zinc-bromine flow battery according to claim 8, It is characterized in that When the zinc-bromine flow battery is in operation, the temperature of the electrolyte of the homogeneous high-temperature resistant zinc-bromine flow battery is controlled to be 20-70° C. by a temperature control system.
10. The zinc-bromine flow battery according to claim 8, It is characterized in that The positive electrode and the negative electrode are both selected from carbon felt or carbon cloth.
Citation Information
Cited By
Biphase diaphragm-free zinc-bromine battery electrolyte, preparation method and application
CN120637552A