Solid-state electrolyte membrane, preparation method thereof and solid-state battery

By spraying glue liquid and solid electrolyte on the porous substrate layer, combined with oscillation and pressing steps, the problem of insufficient density of solid electrolyte membranes in traditional processes is solved, and efficient lithium ion transmission and battery circulation performance is achieved.

CN119092800APending Publication Date: 2024-12-06SUZHOU QINGTAO NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411438069.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-15
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The traditional solid electrolyte membrane preparation process cannot be both thin and dense, resulting in extended transmission path of lithium ions, increased internal resistance of the battery, deteriorated circulation performance, and insufficient utilization of active materials.

Method used

Spray glue liquid on one side of the porous substrate layer to form a glue layer, spray solid electrolyte, and combine the oscillation and pressing steps to form a dense solid electrolyte membrane with good ionic conductivity to avoid solid electrolyte breaking out and improve circulation performance.

Benefits of technology

The prepared solid-state electrolyte membrane is thin and dense, improving the transmission efficiency of lithium ions, extending battery life, and significantly improving the circulation performance of solid-state batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092800A_ABST
    Figure CN119092800A_ABST
Patent Text Reader

Abstract

The invention provides a solid electrolyte membrane, a preparation method thereof and a battery, and relates to the field of energy storage. The preparation method of the solid electrolyte membrane comprises the following steps: spraying a glue solution on the surface of one side of a base material layer to form a glue layer; wherein the base material layer is of a porous structure; spraying a solid electrolyte on the surface of one side, back to the adhesive layer, of the base material layer to form an electrolyte membrane precursor; and pressing to form the solid electrolyte membrane. The adhesive layer partially enters the holes of the base material layer to block the solid electrolyte, so that the solid electrolyte is prevented from being separated from the base material layer, the cycle performance of the solid electrolyte membrane in the operation of the battery is improved, and the service life of the battery is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of energy storage technology, and in particular to a solid electrolyte membrane and a preparation method thereof, and a solid-state battery. Background Art

[0002] Solid-state batteries are energy storage elements that can store electrical energy and release it when needed. Compared with traditional liquid batteries, solid-state batteries use solid electrolytes instead of liquid or gel electrolytes for ion transmission, which has higher safety, higher energy density, faster charging speed and longer cycle life. Solid-state electrolyte membranes play an important role in achieving lithium ion passage in solid-state batteries.

[0003] In traditional technology, solid electrolyte is pressed into membrane material to form solid electrolyte membrane, which requires the membrane material to have good pores to facilitate the entry of solid electrolyte. Multiple pressings are required to prepare solid electrolyte membrane with good density. As a result, the solid electrolyte membrane prepared by this process in traditional technology cannot have the advantages of being thin and dense. If the solid electrolyte membrane is too thick, the transmission path of lithium ions will be extended, which is not conducive to the transmission of lithium ions and the internal resistance of the battery will also increase. If the solid electrolyte membrane is not dense enough, the cycle performance will deteriorate and the active materials of the battery cannot be fully utilized, which is not conducive to the performance of the battery. Summary of the invention

[0004] Based on this, it is necessary to provide a preparation process that can avoid solid electrolyte membranes, so that the prepared solid electrolyte membranes have the advantages of being thin and dense.

[0005] In a first aspect, the present application provides a method for preparing a solid electrolyte membrane, comprising the following steps:

[0006] Spraying glue liquid on one side of the substrate layer to form a glue layer; wherein the substrate layer is a porous structure;

[0007] Spraying a solid electrolyte on the surface of the substrate layer facing away from the adhesive layer to form an electrolyte membrane precursor;

[0008] Press to form a solid electrolyte membrane.

[0009] In some embodiments, in the step of spraying the glue solution on one surface of the substrate layer, the porosity of the substrate layer is 65% to 95%.

[0010] In some embodiments, the step of spraying glue on one side of the substrate layer includes applying glue in a mesh or dot pattern on one side of the substrate layer so that the glue layer covers an area of ​​10% to 40% of the surface area of ​​the substrate layer.

[0011] In some embodiments, in the step of spraying glue on one side of the substrate layer, the glue is sprayed on one side of the substrate layer so that the relationship between the glue layer thickness d1 and the total thickness d0 of the substrate layer satisfies: d1=(1%~20%)d0.

[0012] In some embodiments, the step of spraying the glue solution on one side of the substrate layer includes drying the glue solution after spraying the glue solution on one side of the substrate layer.

[0013] In some embodiments, the step of spraying the glue solution on one side of the substrate layer further comprises: dissolving a binder and a lithium salt in a solvent to prepare the glue solution;

[0014] The binder includes at least one of polyvinylidene fluoride, polyacrylic acid, carboxymethyl cellulose, styrene-butadiene rubber and polyethylene oxide.

[0015] In some embodiments, after spraying the solid electrolyte on the surface of the substrate layer facing away from the adhesive layer to form an electrolyte membrane precursor, the step further includes:

[0016] oscillating the electrolyte membrane precursor;

[0017] In some embodiments, the number of oscillating the electrolyte membrane precursor is 1 or more times;

[0018] In some embodiments, the step of oscillating the electrolyte membrane precursor specifically includes: oscillating the electrolyte membrane precursor using a vibrating screen;

[0019] In some embodiments, the oscillation frequency of the vibrating screen is 20 kHz to 1000 kHz.

[0020] In some embodiments, in the pressing step, the pressing temperature is 60° C. to 100° C.; and / or,

[0021] The pressing pressure is 2t~3t; and / or,

[0022] The pressing time is 0.5 min ~5 min;

[0023] In some embodiments, the surface of the substrate layer sprayed with the solid electrolyte is pressed.

[0024] In a second aspect, the present application also provides a solid electrolyte membrane prepared by the solid electrolyte membrane preparation method.

[0025] In a third aspect, the present application also provides a solid-state battery, which includes a positive electrode sheet, a negative electrode sheet and the solid-state electrolyte membrane.

[0026] In the above-mentioned preparation method of the solid electrolyte membrane, a glue layer is formed on one side of the porous substrate layer, and the glue layer partially enters into the pores to form a barrier to the solid electrolyte, thereby preventing the solid electrolyte from escaping from the substrate layer during the pressing process. The preparation method of the present application is conducive to forming a highly dense solid electrolyte membrane with fewer pressing times, effectively avoiding the breakage of the solid electrolyte caused by multiple pressing.

[0027] The solid electrolyte membrane prepared in the present application is both thin and dense and has good ionic conductivity, so that the cycle performance of the solid-state battery prepared therefrom is significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] FIG. 1 is a schematic diagram of a method for preparing a solid electrolyte membrane according to an embodiment. DETAILED DESCRIPTION

[0029] References to embodiments of the present application will now be provided in detail, one or more examples of which are described below. Each example is provided as an explanation rather than a limitation of the present application. In fact, it will be apparent to those skilled in the art that various modifications and variations may be made to the present application without departing from the scope or spirit of the present application. For example, a feature described or described as part of one embodiment may be used in another embodiment to produce a further embodiment.

[0030] Therefore, it is intended that the present application covers such modifications and variations that fall within the scope of the appended claims and their equivalents. Other objects, features and aspects of the present application are disclosed in or are apparent from the following detailed description. It will be appreciated by those of ordinary skill in the art that this discussion is merely a description of exemplary embodiments and is not intended to limit the broader aspects of the present application.

[0031] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0032] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values ​​of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0033] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0034] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, it is mentioned that the method may also include step (c), which means that step (c) can be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0035] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0036] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0037] In the traditional technology, a solid electrolyte membrane is obtained by pressing a solid electrolyte into a non-woven fabric, and the solid electrolyte realizes the function of lithium ion transmission, and the non-woven fabric realizes the improvement of the mechanical strength of the solid electrolyte membrane. However, it is difficult to adjust the particle size of the solid electrolyte and the pore size of the non-woven fabric during pressing. When the particle size of the solid electrolyte is small and the pressure is small, it is not easy for the powder to form a continuous ion-conducting path in the pore structure. When the particle size is small and the pressure is high, the halide solid electrolyte powder is easy to escape, and more solid electrolyte powder is required, and the prepared solid electrolyte membrane is also thicker. When the particle size of the solid electrolyte is large and the pressure is small, it is difficult to press the powder particles into the non-woven fabric. The large particle size and high pressure can easily destroy the pore structure of the non-woven fabric, resulting in a decrease in the mechanical strength of the solid electrolyte membrane.

[0038] In order to solve the problem that solid electrolyte powder is difficult to mix with membrane materials during pressing, referring to Figure 1, the present application provides a method for preparing a solid electrolyte membrane. A method for preparing a solid electrolyte membrane includes the following steps S11 to S13.

[0039] S11, spraying glue liquid on one side surface of the substrate layer to form a glue layer; wherein the substrate layer has a porous structure.

[0040] Exemplarily, the substrate layer includes at least one of aramid, non-woven fabric, and PI (Polyimide). In this way, the solid electrolyte membrane has good lithium ion permeability, good mechanical strength, and good chemical stability, and can improve the battery performance of the solid-state battery.

[0041] Exemplarily, the glue has certain fluidity and adhesion. Optionally, the glue includes a binder and a solvent. The solvent is not limited in the present application, and it only needs to be able to dissolve the binder to form a uniform slurry.

[0042] Furthermore, the method further includes drying, wherein the solvent in the glue solution is removed by drying to form a glue layer.

[0043] S12, spraying a solid electrolyte on the surface of the substrate layer facing away from the adhesive layer to form an electrolyte membrane precursor.

[0044] Exemplarily, the solid electrolyte includes a halide solid electrolyte. The specific composition of the halide solid electrolyte is not limited in the present application. Optionally, the halide solid electrolyte may be Li a M b X6, wherein 1<a<5, M includes one or more metals, and X includes halogen elements such as Cl, Br, I, etc. Optionally, the halide solid electrolyte can be Li2ZrCl6, Li3InCl6, Li3YCl6, Li3ScCl6 and Li2HfCl6. The halide solid electrolyte has high ionic conductivity and low crystallinity, which helps to inhibit the dendrite growth of active materials such as metallic lithium, thereby improving the safety and cycle life of the solid-state battery.

[0045] Exemplarily, the spraying process can be performed by a powder spraying device, and the amount of the solid electrolyte can be adjusted according to the porosity of the substrate layer and the porosity of the target substrate layer.

[0046] S13, pressing to form a solid electrolyte membrane.

[0047] In the preparation method of the above-mentioned solid electrolyte membrane, a glue layer is formed on one side of the substrate layer. When the substrate layer is a porous structure, the glue layer partially flows into the pores, which can improve the density of the substrate layer on the one hand, and improve the bonding strength between the glue layer and the substrate layer on the other hand. After the glue layer enters some of the pores, it will form a barrier to the solid electrolyte, preventing the solid electrolyte from escaping from the substrate layer, improving the cycle performance of the solid electrolyte membrane in battery operation, and extending the battery life.

[0048] In some embodiments, in the step of spraying the glue on one side of the substrate layer, the porosity of the substrate layer is 65% to 95%. For example, the porosity of the substrate layer may be, but is not limited to, 65%, 70%, 75%, 80%, 85%, 90% or 95%. Within the above range, the substrate layer has good tensile strength and has a good accommodation effect on the solid electrolyte, reducing the probability of the solid electrolyte coming out, so as to improve the cycle performance of the battery.

[0049] Optionally, the adhesive layer is only located on one side of the substrate layer and penetrates into the substrate layer to a certain depth, but does not penetrate the entire pore structure of the substrate layer. Further, the adhesive layer is distributed in a dotted manner on one side of the substrate layer.

[0050] In some embodiments, the relationship between the coverage area S1 of the glue layer and the surface area S0 of the substrate layer satisfies: S1<S0. In this way, the glue layer does not completely cover the surface of the substrate layer, so as to avoid the glue layer causing the substrate layer and the electrode plate to be separated, thereby reducing the ionic conductivity of the solid electrolyte membrane.

[0051] In some embodiments, the step of spraying glue on one side of the substrate layer includes applying glue in a mesh or dot pattern on one side of the substrate layer so that the coverage area of ​​the glue layer accounts for 10% to 40% of the surface area of ​​the substrate layer. The relationship between the coverage area S1 of the glue layer and the surface area S0 of the substrate layer satisfies: S1=(10% to 40%)S0. Optionally, the relationship between the coverage area S1 of the glue layer and the surface area S0 of the substrate layer can be, but is not limited to, S1=10%S0, S1=15%S0, S1=20%S0, S1=25%S0, S1=30%S0, S1=35%S0 or S1=40%S0. In this way, the glue layer can block the solid electrolyte while avoiding reducing the ionic conductivity of the solid electrolyte membrane. Furthermore, the relationship between the coverage area S1 of the glue layer and the surface area S0 of the substrate layer can be S1=(20% to 30%)S0.

[0052] In some embodiments, the thickness d0 of the substrate layer is 5 μm to 40 μm. Optionally, the thickness of the substrate layer may be, but is not limited to, 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm or 40 μm. In this way, the substrate layer has good mechanical strength and has a good accommodation effect on the solid electrolyte, thereby improving ionic conductivity.

[0053] In some embodiments, in the step of spraying the glue on one side of the substrate layer, the glue is sprayed on one side of the substrate layer so that the relationship between the thickness of the glue layer d1 and the total thickness of the substrate layer d0 satisfies: d1 = (1%~20%) d0. Within the above range, the first glue layer has good bonding strength with the substrate layer, and effectively blocks the solid electrolyte and prevents the solid electrolyte from escaping, thereby improving the ionic conductivity of the solid electrolyte membrane. Exemplarily, the thickness of the glue layer can be adjusted by the particle size of the atomized droplets and the distance between the spraying device and the surface of the substrate layer, and can also be adjusted by the ratio of the glue binder and the solvent.

[0054] In some embodiments, the step of spraying the glue on one side of the substrate layer includes drying the glue after spraying the glue on one side of the substrate layer. Exemplarily, the glue is a liquid substance with certain fluidity and adhesion. After spraying the glue, based on its flow characteristics, it will partially enter the pores of the substrate layer, and remain in the pores after drying, thereby improving the bonding effect with the substrate layer.

[0055] In some embodiments, the step of spraying the glue solution on one side of the substrate layer further comprises: dissolving the binder and the lithium salt in a solvent to prepare the glue solution. Exemplarily, the glue layer is prepared by dissolving the binder and then curing it.

[0056] Exemplarily, the binder includes at least one of polyvinylidene fluoride, polyacrylic acid, carboxymethyl cellulose, styrene-butadiene rubber, and polyethylene oxide. Such binders have good chemical resistance to prevent the solid electrolyte membrane from falling off during the long-term charge and discharge process of the battery.

[0057] Illustratively, the lithium salt may include any one or a mixture of LiPF6, LiFSI, LiPO2F2, LiTFSI, LiBF4, LiBOB, LiDFOB, and LiCF3SO3.

[0058] In some embodiments, the particle size of the solid electrolyte is 1 μm to 10 μm. Optionally, the particle size of the solid electrolyte may be, but is not limited to, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm or 10 μm. Further, it may be 3 μm to 8 μm. In this way, the solid electrolyte can be effectively embedded in the pores of the substrate layer, reducing the probability of falling off, improving the stability of the solid electrolyte membrane, and avoiding the excessive contact area of ​​the solid electrolyte powder, which leads to a decrease in conductivity. Optionally, the above particle size is the value of particle size D50.

[0059] In some embodiments, the porosity of the solid electrolyte membrane is 0.1% to 10%. Optionally, the porosity of the solid electrolyte membrane can be but not limited to 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%. Further, the porosity of the solid electrolyte membrane can be 3% to 7%. After the substrate layer is filled with the solid electrolyte, the overall porosity of the solid electrolyte membrane decreases. Within the above porosity range, the solid electrolyte membrane has good mechanical strength and good lithium ion pass rate, which improves the cycle performance of the solid-state battery.

[0060] In some embodiments, after spraying the solid electrolyte on the surface of the substrate layer facing away from the adhesive layer to form an electrolyte membrane precursor, the step further includes: oscillating the electrolyte membrane precursor. Oscillating the electrolyte membrane precursor can improve the uniformity of solid electrolyte dispersion.

[0061] In some embodiments, the electrolyte membrane precursor is oscillated once or more times. For example, the electrolyte membrane precursor is oscillated once, twice, three times, four times, five times, etc., but not limited thereto.

[0062] In some embodiments, the step of shaking the electrolyte membrane precursor specifically includes: shaking the electrolyte membrane precursor using a shaker. Exemplarily, the shaker method can be performed by placing the electrolyte membrane intermediate in a shaker.

[0063] In some embodiments, the oscillation frequency of the vibrating screen is 20kHz to 1000kHz. Exemplarily, the oscillation frequency of the vibrating screen can be, but is not limited to, 20kHz, 50kHz, 80kHz, 100kHz, 150kHz, 200kHz, 250kHz, 300kHz, 350kHz, 400kHz, 450kHz, 500kHz, 550kHz, 600kHz, 650kHz, 700kHz, 750kHz, 800kHz, 850kHz, 900kHz, 950kHz or 1000kHz, etc.

[0064] In some embodiments, in the pressing step, the pressing temperature is 60° C. to 100° C. In some embodiments, the pressing pressure is 2t to 3t. In some embodiments, the pressing time is 0.5 min to 5 min.

[0065] For example, the pressing temperature may be, but is not limited to, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, or 100°C. For example, the pressure of the pressing process may be, but is not limited to, 2t, 2.2t, 2.4t, 2.5t, 2.6t, 2.8t, or 3t. For example, the time of the pressing process may be, but is not limited to, 0.5min, 1min, 2min, 5min, 8min, 10min, 12min, 15min, 18min, or 20min. For example, the pressing method may be flat plate pressing or roller pressing.

[0066] In some embodiments, the surface of the substrate layer sprayed with the solid electrolyte is pressed. Exemplarily, these embodiments refer to unidirectional pressing, that is, the pressing side is the side sprayed with the solid electrolyte powder.

[0067] In some embodiments, the present application also provides a solid electrolyte membrane prepared by the method for preparing a solid electrolyte membrane provided in any of the above embodiments.

[0068] In some embodiments, the present application also provides a solid-state battery, which includes a positive electrode plate, a negative electrode plate and the above-mentioned solid electrolyte membrane.

[0069] Positive electrode:

[0070] In some embodiments, the secondary battery provided by the present invention includes a positive electrode, the positive electrode includes a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector, the positive electrode active material layer having a thickness of greater than or equal to about 1 μm to less than or equal to about 1,000 μm. The positive electrode active material layer includes a positive electrode active material, and the positive electrode active material includes a compound that reversibly intercalates and deintercalates lithium ions.

[0071] In some embodiments, the positive electrode active material comprises one or more transition metal cations, such as manganese (Mn), nickel (Ni), cobalt (Co), chromium (Cr), iron (Fe), vanadium (V), and combinations thereof.

[0072] In some embodiments, the positive electrode active material is one of a layered oxide, a spinel, and a polyanion. For example, the layered oxide (e.g., a rock salt layered oxide) comprises one or more lithium-based positive electrode active materials selected from the group consisting of LiCoO2 (LCO), LiNi x Mn y Co 1-x-y O2 (where 0≤x≤1 and 0≤y≤1), LiNi 1-x-y Co x Al y O2 (where 0≤x≤1 and 0≤y≤1), LiNi x Mn1-x O2 (where 0≤x≤1), and Li 1+x MO2 (wherein M is one of Mn, Ni, Co and Al and 0≤x≤1). The spinel comprises one or more lithium-based positive active materials selected from the group consisting of LiMn2O4 (LMO) and LiNi x Mn 1.5 O4. The olivine type contains one or more lithium-based positive electrode active materials LiMPO4 (wherein M is at least one of Fe, Ni, Co and Mn). The polyanion cation contains, for example, phosphates such as LiV2(PO4)3 and / or silicates such as LiFeSiO4.

[0073] In some embodiments, the positive electrode active material layer includes a binder, which improves the bonding between the positive electrode active material particles and also improves the bonding between the positive electrode active material layer and the positive electrode current collector.

[0074] In some embodiments, non-limiting examples of binders include polyvinyl alcohol, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, nylon, and the like.

[0075] In some embodiments of the present invention, the mass of the binder accounts for 1%-20% of the mass of the positive electrode material layer.

[0076] In some embodiments of the present invention, the positive electrode active material layer includes a conductive agent to impart conductivity to the electrode. The conductive agent may include any conductive material as long as it does not cause chemical changes. Non-limiting examples of conductive materials include carbon-based materials (e.g., natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, carbon fiber, etc.), metal-based materials (e.g., metal powder, metal fiber, etc., including, for example, copper, nickel, aluminum, silver, etc.), conductive polymers (e.g., polyphenylene derivatives) and mixtures thereof.

[0077] In some embodiments, the mass of the conductive agent accounts for 1%-20% of the mass of the positive electrode material layer.

[0078] In some embodiments, the positive electrode plate provided by the present invention further includes a fast ion conductor for improving the ionic conductivity of the positive electrode. The present invention does not limit the type of fast ion conductor, which can be an oxide solid electrolyte, a sulfide solid electrolyte, a halide solid electrolyte, a lithium salt, etc. Optionally, the mass of the fast ion conductor accounts for 1%-20% of the mass of the positive electrode plate; preferably 5%-20%.

[0079] In some embodiments, the positive electrode sheet includes a positive electrode current collector. Exemplarily, the positive electrode current collector may be aluminum (Al), but is not limited thereto.

[0080] It is understood that the above examples of positive electrode active materials, binders, and conductive materials are only illustrative, and any known positive electrode active materials, binders, and conductive materials can be used in this application without violating the inventive concept of this application. And the addition of known additives based on actual use requirements should also be considered within the scope of protection of this application.

[0081] Negative electrode:

[0082] In some embodiments of the present invention, the negative electrode sheet includes a current collector and a negative electrode active material layer disposed on the current collector.

[0083] In the present invention, the specific types of negative electrode active materials are not subject to specific restrictions and can be selected according to needs. Specifically, the negative electrode active material is selected from natural graphite, artificial graphite, mesophase microcarbon beads (MCMB for short), hard carbon, soft carbon, silicon, silicon-carbon composites, Li-Sn alloys, Li-Sn-O alloys, Sn, SnO, SnO2, spinel-structured lithiated TiO2-Li4Ti5O 12 , Li-Al alloy. Non-limiting examples of carbon materials include crystalline carbon, amorphous carbon and mixtures thereof. Crystalline carbon can be amorphous or flake-shaped, platelet-shaped, spherical or fibrous natural graphite or artificial graphite. Amorphous carbon can be soft carbon, hard carbon, mesophase pitch carbide, calcined coke, etc.

[0084] In some embodiments, metal elements and metal compounds can also be selected as negative electrode active materials, such as compounds containing metals or metalloids such as Li, Ag, Al, Bi, Cu, Ga, Ge, In, Ni, Pb, Sb, Si, Sn, Sr, and Zn.

[0085] In some embodiments, the mass percentage of the negative electrode active material contained in the negative electrode active material layer may be 80%-99%, for example, 80%, 85%, 90%, 95%, 97%, 99%, etc., preferably 95%-97%.

[0086] In some embodiments, the negative electrode material layer may include a binder; the binder improves bonding of negative electrode active material particles to each other and bonding of the negative electrode active material to the current collector.

[0087] In some embodiments, non-limiting examples of binders include polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene butadiene rubber, acrylated styrene butadiene rubber, epoxy resin, nylon, and the like.

[0088] In some embodiments, the negative electrode active material layer can be obtained by coating a negative electrode slurry on a negative electrode current collector and then drying the negative electrode slurry, wherein the negative electrode slurry includes at least a negative electrode active material and a negative electrode binder. When an aqueous solvent is used as a liquid medium for forming the negative electrode slurry, a thickener is preferably used for slurrying, and the thickener can generally be used to adjust the viscosity of the slurry.

[0089] In some embodiments, the aforementioned viscosity enhancer may be one or more of the following: carboxymethyl cellulose, methyl cellulose, hydroxymethyl cellulose, ethyl cellulose, polyvinyl alcohol, oxidized starch, phosphorylated starch, casein, and salts thereof.

[0090] In some embodiments, the mass proportion of the thickener in the negative electrode slurry can be 0.1%-5%, for example, 0.1%, 0.2%, 0.5%, 0.6%, 1%, 2%, 3%, 4%, 5%, etc., preferably 0.5%-3%, and more preferably 0.6%-2%.

[0091] In some embodiments, the negative electrode active material layer includes a conductive material so that the electrode has conductivity. The conductive material may include any conductive material as long as it does not cause chemical changes. Non-limiting examples of conductive materials include carbon-based materials (e.g., natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, etc.), metal-based materials (e.g., metal powder, metal fiber, etc., such as copper, nickel, aluminum, silver, etc.), conductive polymers (e.g., polyphenylene derivatives) and mixtures thereof.

[0092] In some embodiments of the present invention, the negative electrode current collector may be selected from copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, and combinations thereof.

[0093] Secondary battery:

[0094] In some embodiments, the secondary battery of the present invention comprises the above-mentioned positive electrode sheet, negative electrode sheet, separator, electrolyte, etc., but is not limited thereto.

[0095] In some embodiments, the secondary battery according to the present invention is made by stacking the above-mentioned positive and negative electrode sheets.

[0096] In some embodiments, the secondary battery of the present invention may include an outer package, which may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer package of the secondary battery may also be a soft package, such as a bag-type soft package. The material of the soft package may be plastic, such as one or more of polypropylene (PP), polybutylene terephthalate (PBT), polybutylene succinate (PBS), etc.

[0097] The following are specific embodiments.

[0098] Example 1

[0099] Preparation of solid electrolyte membrane:

[0100] (1) Spray glue liquid on one side of the substrate layer and dry it to form a glue layer.

[0101] The substrate layer is a nonwoven fabric with a porosity of 85% and a thickness of 30 μm.

[0102] The glue solution includes a binder and a solvent, the binder is polyvinylidene fluoride, the lithium salt is LiPF6, and the solvent is N,N-dimethylformamide.

[0103] (2) Spraying a solid electrolyte on the side of the substrate layer facing away from the adhesive layer to form an electrolyte membrane precursor.

[0104] The electrolyte membrane precursor was oscillated once using a screen shaker, and the oscillation frequency of the screen shaker was 600 kHz.

[0105] The solid electrolyte is Li2ZrCl6 with a particle size D50 of 5 μm.

[0106] (3) The surface of the substrate layer sprayed with the solid electrolyte is pressed to form a solid electrolyte membrane.

[0107] The pressing temperature was 65 °C, the pressing pressure was 2t, and the pressing time was 10 min.

[0108] After testing, the coverage area S1 of the formed adhesive layer accounts for 20% of the area S0 of the substrate layer, and the relationship between the thickness d1 of the substrate layer containing the adhesive layer and the total thickness d0 of the substrate layer satisfies: d1=10%d0

[0109] Preparation of lithium-ion batteries:

[0110] The positive electrode sheets are aligned and stacked on the side of the substrate layer in the solid electrolyte membrane facing away from the glue layer, and then the negative electrode sheets are attached to the side of the glue layer after rolling. After assembling with the shell, a button-type lithium-ion battery is obtained. The positive electrode composition is 95wt% NCM622, 3wt% PTFE and 2wt% super-P; the negative electrode composition is 95wt% graphite, 3wt% (CMC+SBR) and 2wt% super-P.

[0111] Example 2

[0112] The preparation method of Example 2 is substantially the same as that of Example 1, except that:

[0113] The coverage area S1 of the formed adhesive layer accounts for 10% of the area S0 of the substrate layer.

[0114] Example 3

[0115] The preparation method of Example 3 is substantially the same as that of Example 1, except that:

[0116] The coverage area S1 of the formed adhesive layer accounts for 40% of the area S0 of the substrate layer.

[0117] Example 4

[0118] The preparation method of Example 4 is substantially the same as that of Example 1, except that:

[0119] The relationship between the thickness d1 of the substrate layer containing the adhesive layer and the total thickness d0 of the substrate layer satisfies: d1=1%d0.

[0120] Example 5

[0121] The preparation method of Example 5 is substantially the same as that of Example 1, except that:

[0122] The relationship between the thickness d1 of the substrate layer containing the adhesive layer and the total thickness d0 of the substrate layer satisfies: d1=20%d0.

[0123] Example 6

[0124] The preparation method of Example 6 is substantially the same as that of Example 1, except that:

[0125] In step (1), the thickness of the substrate layer is 10 μm.

[0126] Example 7

[0127] The preparation method of Example 7 is substantially the same as that of Example 1, except that:

[0128] In step (1), the thickness of the substrate layer is 120 μm.

[0129] Example 8

[0130] The preparation method of Example 8 is substantially the same as that of Example 1, except that:

[0131] In step (1), the porosity of the substrate layer is 65%.

[0132] Example 9

[0133] The preparation method of Example 9 is substantially the same as that of Example 1, except that:

[0134] In step (1), the porosity of the substrate layer is 95%.

[0135] Example 10

[0136] The preparation method of Example 10 is substantially the same as that of Example 1, except that:

[0137] In step (2), the particle size D50 of the solid electrolyte is 1 μm.

[0138] Embodiment 11

[0139] The preparation method of Example 11 is substantially the same as that of Example 1, except that:

[0140] In step (2), the particle size D50 of the solid electrolyte is 10 μm.

[0141] Example 12

[0142] The preparation method of Example 12 is substantially the same as that of Example 1, except that:

[0143] The coverage area S1 of the formed adhesive layer accounts for 50% of the area S0 of the substrate layer;

[0144] The relationship between the thickness d1 of the substrate layer containing the adhesive layer and the total thickness d0 of the substrate layer satisfies: d1=30%d0.

[0145] The porosity of the substrate layer was 60% and the thickness of the substrate layer was 45 μm.

[0146] The particle size D50 of the solid electrolyte is 15 μm.

[0147] In step (2), no oscillation is performed.

[0148] Comparative Example 1

[0149] The preparation method of Comparative Example 1 is substantially the same as that of Example 1, except that:

[0150] The process does not include step (1), that is, the adhesive is not sprayed on the substrate layer.

[0151] The process parameters of Examples 1 to 12 and Comparative Example 1 are listed in Table 1. Among them: the porosity is tested by using an SSA-4200 pore size and specific surface area analyzer, and the solid electrolyte particle size is tested by using a Malvern dry particle size analyzer.

[0152] Table 1

[0153]

[0154] The test results are shown in Table 2 below, where the test conditions or test standards for each performance test item are:

[0155] (1) Ionic conductivity test

[0156] At 25°C, a test structure of stainless steel sheet / solid electrolyte membrane / stainless steel sheet was used, the frequency range was 0.1Hz~7MHz, and the AC signal amplitude Z was 10 -2 The AC impedance test was carried out under the condition of V, and the ionic conductivity was calculated according to the formula σ=L / (S*R), where L is the thickness of the solid electrolyte membrane, S is the cross-sectional area of ​​the solid electrolyte membrane, and R represents the charge transfer resistance.

[0157] (2) Cyclic performance test

[0158] At a temperature of 25℃±2℃, in the first step, charge at 0.1C or specified current to the termination voltage, with a cutoff current of 0.01C, and let stand for 30 minutes; in the second step, discharge at 0.1C to the discharge final voltage (2.75V), record the discharge capacity, and let stand for 30 minutes; cycle the first and second steps to test the cycle performance of the lithium-ion battery for 300 cycles.

[0159] Table 2

[0160]

[0161] It can be seen from Table 2 above that, by comparing Examples 1 to 12 and Comparative Example 1, the solid electrolyte membrane provided by the present application has good ionic conductivity and cycle capacity retention rate. By forming a binder on one side of the substrate layer, the binder is partially contained in the inlet hole, which forms a barrier to the solid electrolyte, thereby preventing the solid electrolyte from escaping from the substrate layer, improving the cycle performance of the solid electrolyte membrane in battery operation, and extending the battery life.

[0162] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0163] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims.

Claims

1. A method for preparing a solid electrolyte membrane, It is characterized in that The steps include: Spraying glue liquid on one side of the substrate layer to form a glue layer; wherein the substrate layer is a porous structure; Spraying a solid electrolyte on the surface of the substrate layer facing away from the adhesive layer to form an electrolyte membrane precursor; Press to form a solid electrolyte membrane.

2. The preparation method according to claim 1, It is characterized in that In the step of spraying the glue solution on one surface of the substrate layer, the porosity of the substrate layer is 65% to 95%.

3. The preparation method according to claim 1, It is characterized in that The step of spraying glue on one side of the substrate layer includes applying glue in a mesh or dot pattern on one side of the substrate layer so that the glue layer covers an area of ​​10% to 40% of the surface area of ​​the substrate layer.

4. The preparation method according to claim 1, It is characterized in that In the step of spraying glue on one side of the substrate layer, the glue is sprayed on one side of the substrate layer so that the glue layer has a thickness d 1 The total thickness of the substrate layer is d 0 The relationship satisfies: d 1 = (1%~20%)d 0 .

5. The preparation method according to claim 1, It is characterized in that The step of spraying the glue solution on one side surface of the substrate layer includes spraying the glue solution on one side surface of the substrate layer and then drying it.

6. The preparation method according to claim 1, It is characterized in that The step of spraying the glue solution on one side of the substrate layer further includes: dissolving a binder and a lithium salt in a solvent to prepare the glue solution; The binder includes at least one of polyvinylidene fluoride, polyacrylic acid, carboxymethyl cellulose, styrene-butadiene rubber and polyethylene oxide.

7. The preparation method according to claim 1, It is characterized in that After spraying the solid electrolyte on the surface of the substrate layer facing away from the adhesive layer to form an electrolyte membrane precursor, the step further includes: oscillating the electrolyte membrane precursor; Preferably, the number of oscillating the electrolyte membrane precursor is 1 time or more; Preferably, the step of oscillating the electrolyte membrane precursor specifically comprises: oscillating the electrolyte membrane precursor using a vibrating screen; Preferably, the oscillation frequency of the vibrating screen is 20kHz~1000kHz.

8. The preparation method according to claim 1, It is characterized in that In the pressing step, the pressing temperature is 60°C to 100°C; and / or, The pressing pressure is 2t~3t; and / or, The pressing time is 0.5 min ~5 min; Preferably, the surface of the substrate layer sprayed with the solid electrolyte is pressed.

9. A solid electrolyte membrane, It is characterized in that The method is prepared according to any one of claims 1 to 8.

10. A solid-state battery, It is characterized in that The solid-state battery comprises a positive electrode sheet, a negative electrode sheet and the solid electrolyte membrane according to claim 9.