Carbon-coated solid electrolyte material, preparation method thereof and sodium ion battery
By performing carbon coating on sodium zirconium silicon phosphorus solid electrolyte material, its conductivity is improved, the problem of low conductivity in sodium ion batteries is solved, and the efficient performance and low-cost industrial production of sodium ion batteries are achieved.
Patent Information
- Application Number
- CN202410940503.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-12-06
AI Technical Summary
The conductivity of solid electrolyte materials in sodium ion batteries is low, which is difficult to meet industrial needs, and traditional materials are not easy to match the large radius of sodium ions.
By using the preparation method of carbon-coated solid electrolyte material, the sodium zirconium silicon-phosphorus sintered block is crushed and nano-treated, and mixed with a carbon source to calcinate in a protective gas atmosphere to form a carbon-coated solid electrolyte material with high conductivity.
It significantly improves the conductivity of sodium zirconium silicon phosphorus solid electrolyte materials, is suitable for sodium ion batteries, reduces production costs, and is suitable for large-scale industrial production.
Smart Images

Figure CN119092802A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a carbon-coated solid electrolyte material and a preparation method thereof, and a sodium ion battery. Background Art
[0002] Lithium-ion batteries have developed rapidly in the past decade. However, rising prices have hindered the further application of lithium-ion batteries, so it is imperative to find cheaper batteries to replace lithium-ion batteries. Due to the abundant sodium resources in the earth's crust and low cost, sodium-ion batteries are considered to be the best energy storage device to replace lithium-ion batteries. Unlike organic liquid electrolytes that are easy to leak, flammable, and cannot effectively inhibit dendrites, solid sodium electrolytes are widely used in sodium metal batteries to improve safety.
[0003] However, sodium ions have a large radius and require unique ion channel materials to match sodium ion batteries. The ion channel of NASICON structure materials is large enough to allow sodium ions to pass through, and sodium zirconium silicon phosphate is a NASICON structure material. However, sodium zirconium silicon phosphate itself does not have good conductivity and is not easy to industrialize. Summary of the invention
[0004] Based on this, it is necessary to provide a carbon-coated solid electrolyte material, a preparation method thereof, and a sodium ion battery in order to improve the electrical conductivity of the solid electrolyte material.
[0005] A method for preparing a carbon-coated solid electrolyte material comprises the following steps:
[0006] The sodium source, zirconium source, silicon source and phosphorus source are uniformly mixed, and after sintering, a sodium zirconium silicon phosphorus sintered block is obtained;
[0007] The sodium zirconium silicon phosphorus sintered block is crushed to obtain sodium zirconium silicon phosphorus sintered powder;
[0008] The sodium zirconium silicon phosphorus sintered powder is subjected to nano-processing to obtain nano-grade sodium zirconium silicon phosphorus powder;
[0009] uniformly mixing the nano-scale sodium zirconium silicon phosphorus powder and a carbon source to obtain a mixed material; and
[0010] The mixed material is calcined in a protective gas atmosphere to obtain a carbon-coated solid electrolyte material after sufficient reaction.
[0011] The preparation method of the above-mentioned carbon-coated solid electrolyte material is simple to operate, the equipment used is simple, the overall production cost is low, and it is very suitable for large-scale industrial production; the technical solution of the present invention greatly improves the conductivity of the sodium zirconium silicon phosphorus solid electrolyte material by carbon coating the sodium zirconium silicon phosphorus solid electrolyte, which is conducive to industrialization.
[0012] In a feasible implementation, the sodium source is selected from at least one of sodium hydroxide, sodium carbonate, perchloric acid and sodium bis(trifluoromethylsulfonyl)imide;
[0013] The zirconium source is selected from at least one of zirconium oxide, zirconium nitrate and zirconium acetate;
[0014] The silicon source is silicon dioxide;
[0015] The phosphorus source is selected from at least one of phosphorus pentoxide, diammonium hydrogen phosphate and ammonium hydrogen phosphate;
[0016] The sodium source, zirconium source, silicon source and phosphorus source are mixed evenly. During the sintering operation, the sintering temperature is 1000° C. to 1200° C. and the sintering time is 5 h to 20 h.
[0017] In a feasible implementation, the particle size of the nano-scale sodium zirconium silicon phosphorus powder is 200nm to 700nm.
[0018] In a feasible implementation, the operation of uniformly mixing the nano-scale sodium zirconium silicon phosphorus powder and the carbon source is: mixing the nano-scale sodium zirconium silicon phosphorus powder and the carbon source, then adding a dispersant, mixing by ball milling, and then drying; wherein the drying temperature does not exceed 100° C.; and / or
[0019] The dispersant is selected from one or more of methanol, ethanol and ethylene glycol; and / or
[0020] The frequency of the ball milling is 100 rpm to 800 rpm, and the time of the ball milling is 1 h to 10 h.
[0021] In a feasible implementation, the mass ratio of the nano-scale sodium zirconium silicon phosphorus powder to the carbon source is 1:(0.01-0.1).
[0022] In a feasible implementation, the carbon source is selected from at least one of citric acid, glucose, starch, carbon black and asphalt.
[0023] In a feasible implementation, the mixed material is calcined in a protective gas atmosphere at a temperature of 800° C. to 900° C. and a calcination time of 5 h to 20 h; the protective gas is selected from at least one of nitrogen and argon.
[0024] In a feasible implementation, the operation of crushing the sodium zirconium silicon phosphorus sintered block is: crushing the sodium zirconium silicon phosphorus sintered block by jaw crushing and ball milling in sequence.
[0025] A carbon-coated solid electrolyte material is prepared by any of the above-mentioned methods for preparing the carbon-coated solid electrolyte material.
[0026] Experimental verification has shown that the carbon-coated solid electrolyte material obtained by the above preparation method has high electrical conductivity and is suitable for sodium ion batteries.
[0027] A sodium ion battery comprises the above-mentioned carbon-coated solid electrolyte material.
[0028] It has been verified through experiments that the sodium ion battery of the technical solution of the present invention has high conductivity and is conducive to industrialization. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is a flow chart of a method for preparing a carbon-coated solid electrolyte material according to one embodiment of the present invention;
[0030] Figure 2 This is an X-ray diffraction diagram of a sodium zirconium silicon phosphorus sintered block during the preparation of the carbon-coated solid electrolyte material of Example 1 of the present invention;
[0031] Figure 3 This is an X-ray diffraction pattern of the sodium zirconium silicon phosphorus sintered block during the preparation process of the carbon-coated solid electrolyte material of Example 2 of the present invention. DETAILED DESCRIPTION
[0032] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.
[0033] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0034] See also Figure 1 A method for preparing a carbon-coated solid electrolyte material according to an embodiment of the present invention comprises the following steps:
[0035] S10, mixing the sodium source, zirconium source, silicon source and phosphorus source evenly, and sintering to obtain a sodium-zirconium-silicon-phosphorus sintered block.
[0036] In a feasible implementation, the sodium source is selected from at least one of sodium hydroxide, sodium carbonate, perchloric acid and sodium bis(trifluoromethylsulfonyl)imide; the zirconium source is selected from at least one of zirconium oxide, zirconium nitrate and zirconium acetate; the silicon source is silicon dioxide; and the phosphorus source is selected from at least one of diammonium phosphate, phosphorus pentoxide, diammonium hydrogen phosphate and ammonium hydrogen phosphate.
[0037] In step S10, according to the general formula: Na3Zr2Si2PO 12 , weigh a suitable ratio of sodium source, zirconium source, silicon source and phosphorus source and mix them evenly. In a feasible implementation, the sodium source is sodium carbonate (Na2CO3), the zirconium source is zirconium oxide (ZrO2), the silicon source is silicon dioxide (SiO2), and the phosphorus source is ammonium dihydrogen phosphate (NH4H2PO4), and the raw materials of sodium carbonate, zirconium oxide, silicon dioxide and ammonium dihydrogen phosphate are mixed in a molar ratio of 1.5:2:2:1.
[0038] In a feasible implementation, the sintering temperature is 1000° C. to 1200° C., and the sintering time is 5 h to 20 h. Further, the sintering temperature may be, but is not limited to, 1000° C., 1100° C. or 1200° C., and the sintering time may be, but is not limited to, 5 h, 6 h, 7 h, 8 h, 9 h, 10 h, 11 h, 12 h, 13 h, 14 h, 15 h, 16 h, 17 h, 18 h, 19 h or 20 h.
[0039] After step S10, the overall size of the obtained sodium zirconium silicon phosphorus sintered block is larger.
[0040] S20, crushing the sodium zirconium silicon phosphorus sintered block obtained in step S10 to obtain sodium zirconium silicon phosphorus sintered powder.
[0041] In a feasible implementation, the operation of crushing the sodium zirconium silicon phosphorus sintered block is: crushing the sodium zirconium silicon phosphorus sintered block by jaw crushing and ball milling in sequence.
[0042] Compared with the sodium zirconium silicon phosphorus sintered block obtained in step S10, after step S20, the size of the sodium zirconium silicon phosphorus sintered powder is smaller, but still needs to be further reduced to facilitate its application in sodium ion batteries.
[0043] S30, subjecting the sodium zirconium silicon phosphorus sintered powder obtained in step S20 to nano-treatment to obtain nano-grade sodium zirconium silicon phosphorus powder.
[0044] In a feasible implementation, the particle size of the nano-scale sodium zirconium silicon phosphorus powder is 200nm to 700nm. Further, the particle size of the nano-scale sodium zirconium silicon phosphorus powder can be, but is not limited to, 200nm, 300nm, 400nm, 500nm, 600nm or 700nm.
[0045] S40, uniformly mixing the nanometer-scale sodium zirconium silicon phosphorus powder obtained in step S30 with a carbon source to obtain a mixed material.
[0046] In a feasible implementation, the operation of uniformly mixing the nano-scale sodium zirconium silicon phosphorus powder and the carbon source is as follows: the nano-scale sodium zirconium silicon phosphorus powder and the carbon source are mixed, and then a dispersant is added, mixed by ball milling, and then dried; wherein the drying temperature does not exceed 100°C.
[0047] In a feasible implementation, the dispersant is selected from one or more of methanol, ethanol and ethylene glycol.
[0048] In a feasible implementation, the frequency of ball milling is 100 rpm to 800 rpm, and the time of ball milling is 1 h to 10 h. Further, the frequency of ball milling can be but not limited to 100 rpm, 200 rpm, 300 rpm, 400 rpm, 500 rpm, 600 rpm, 700 rpm or 800 rpm, and the time of ball milling can be but not limited to 1 h, 2 h, 3 h, 4 h, 5 h, 6 h, 7 h, 8 h, 9 h or 10 h.
[0049] In a feasible implementation, the mass ratio of the nano-scale sodium zirconium silicon phosphorus powder to the carbon source is 1:(0.01-0.1). Further, the mass ratio of the nano-scale sodium zirconium silicon phosphorus powder to the carbon source can be, but is not limited to, 1:0.01, 1:0.02, 1:0.03, 1:0.04, 1:0.05, 1:0.06, 1:0.07, 1:0.08, 1:0.09 or 1:0.1.
[0050] In a feasible implementation, the carbon source is selected from at least one of citric acid, glucose, starch, carbon black and asphalt.
[0051] S50, calcining the mixed material obtained in step S40 in a protective gas atmosphere to obtain a carbon-coated solid electrolyte material after sufficient reaction.
[0052] Among them, roasting the mixed material in a protective gas atmosphere can prevent the mixed material from being oxidized and affecting the generated product.
[0053] In a feasible implementation, the mixed material is roasted in a protective gas atmosphere at a temperature of 800°C to 900°C and a time of 5 to 20 hours; the protective gas is selected from at least one of nitrogen and argon. Further, the roasting temperature may be, but is not limited to, 800°C, 810°C, 820°C, 830°C, 840°C, 850°C, 860°C, 870°C, 880°C, 890°C or 900°C, and the roasting time may be, but is not limited to, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 11 hours, 12 hours, 13 hours, 14 hours, 15 hours, 16 hours, 17 hours, 18 hours, 19 hours or 20 hours.
[0054] The carbon-coated solid electrolyte material obtained in step S50 is carbon-coated sodium zirconium silicon phosphorus (Na3Zr2Si2PO 12 ) solid electrolyte material. Compared with the traditional non-coated sodium zirconium silicon phosphorus solid electrolyte material, the carbon-coated sodium zirconium silicon phosphorus solid electrolyte material of this embodiment has a higher conductivity.
[0055] The preparation method of the above-mentioned carbon-coated solid electrolyte material is simple to operate, the equipment used is simple, the overall production cost is low, and it is very suitable for large-scale industrial production; the technical solution of the present invention greatly improves the conductivity of the sodium zirconium silicon phosphorus solid electrolyte material by carbon coating the sodium zirconium silicon phosphorus solid electrolyte, which is conducive to industrialization.
[0056] A carbon-coated solid electrolyte material according to one embodiment is prepared by any of the above-mentioned methods for preparing a carbon-coated solid electrolyte material.
[0057] Experimental verification has shown that the carbon-coated solid electrolyte material obtained by the above preparation method has high electrical conductivity and is suitable for sodium ion batteries.
[0058] A sodium ion battery according to one embodiment comprises the above-mentioned carbon-coated solid electrolyte material. The carbon-coated solid electrolyte material of the technical solution of the present invention can be used in electrode coating slurry, battery pole pieces and electrolytes of sodium ion batteries.
[0059] It has been verified through experiments that the sodium ion battery of the technical solution of the present invention has a high conductivity and is conducive to industrialization because it includes the above-mentioned carbon-coated solid electrolyte material.
[0060] With reference to the above implementation contents, in order to make the technical solution of the present application more specific, clear and easy to understand, the technical solution of the present application is now exemplified. However, it should be noted that the contents to be protected by the present application are not limited to the following Examples 1 to 2.
[0061] Example 1
[0062] 214g of sodium carbonate, 765g of zirconium dioxide, 56g of silicon dioxide and 980g of ammonium dihydrogen phosphate were mixed, and then ball-milled at a fixed ball-milling frequency of 180rpm for 1h, and then placed in a high-temperature box furnace and sintered at 1100℃ for 5h to obtain a sintered product. The sintered product was subjected to X-ray diffraction, and the obtained product was Figure 2 .Depend on Figure 2 It can be seen that the diffraction peaks of the sintered material correspond to those of the standard card PDF#97-006-7012, and no impurity peaks appear, indicating that the sintered material is a sodium zirconium silicon phosphorus sintered block.
[0063] The sodium zirconium silicon phosphorus sintered block is successively subjected to jaw crushing and ball milling to obtain sodium zirconium silicon phosphorus powder; wherein the ball milling frequency is 180 rpm and the ball milling time is 1 hour.
[0064] The sodium zirconium silicon phosphorus powder is subjected to air flow milling to obtain nano-scale sodium zirconium silicon phosphorus powder; wherein the particle size distribution of the nano-scale sodium zirconium silicon phosphorus powder is between 200nm and 700nm, as shown in Table 1.
[0065] Table 1 Particle size distribution of nano sodium zirconium silicon phosphorus powder
[0066] Particle size distribution D10(micrometer) D50(micrometer) D90(micrometer) D100(micrometer) Nano sodium zirconium silicon phosphorus powder 0.235 0.377 0.589 0.698
[0067] 1000g of nanometer sodium zirconium silicon phosphorus powder was mixed with 40g of citric acid, and 900ml of ethanol dispersant was added, and the mixture was mixed by ball milling at a frequency of 180rpm for 1h. The mixture was then dried at 80°C to obtain a mixed material, which was a carbon-sodium zirconium silicon phosphorus mechanical mixed material.
[0068] The mixed material was placed in an atmosphere furnace, nitrogen was introduced, and calcined at 850°C for 10 hours to obtain a carbon-coated solid electrolyte material. The conductivity of the material before and after coating was tested at room temperature, as shown in Table 2. As can be seen from Table 2, the conductivity of the material was significantly improved after carbon coating.
[0069] Table 2 Electrical conductivity of materials before and after carbon coating at room temperature
[0070] Test items Before coating (S / cm) After coating (S / cm) Material conductivity <![CDATA[6.32×10 -4 ]]> <![CDATA[9.83×10 -3 ]]>
[0071] Example 2
[0072] 214g of sodium carbonate, 765g of zirconium dioxide, 56g of silicon dioxide and 980g of ammonium dihydrogen phosphate were mixed, and then ball-milled at a fixed ball-milling frequency of 180rpm for 1h, and then placed in a high-temperature box furnace and sintered at 1100℃ for 5h to obtain a sintered product. After high-temperature sintering, a sodium zirconium silicon phosphorus sintered block was obtained. The sintered product was subjected to X-ray diffraction, and the obtained Figure 3 .Depend on Figure 3It can be seen that the diffraction peaks of the sintered material correspond to those of the standard card PDF#97-006-7012, and no impurity peaks appear, indicating that the sintered material is a sodium zirconium silicon phosphorus sintered block.
[0073] The sodium zirconium silicon phosphorus sintered block is successively subjected to jaw crushing and ball milling to obtain sodium zirconium silicon phosphorus powder; wherein the ball milling frequency is 180 rpm and the ball milling time is 1 hour.
[0074] The sodium zirconium silicon phosphorus powder is subjected to air flow milling to obtain nano-scale sodium zirconium silicon phosphorus powder; wherein the particle size distribution of the nano-scale sodium zirconium silicon phosphorus powder is between 200nm and 700nm, as shown in Table 3.
[0075] Table 1 Particle size distribution of nano sodium zirconium silicon phosphorus powder
[0076] Particle size distribution D10(micrometer) D50(micrometer) D90(micrometer) D100(micrometer) Sodium Zirconium Silicon Phosphate 0.243 0.379 0.593 0.688
[0077] 1000g of nanometer sodium zirconium silicon phosphorus powder is mixed with 40g of carbon black, and 900ml of ethanol dispersant is added, and the mixture is mixed by ball milling at a frequency of 180rpm for 1h; then, the mixture is dried at 80°C to obtain a mixture, which is a carbon-sodium zirconium silicon phosphorus mechanical mixed material.
[0078] The mixed material was placed in an atmosphere furnace, nitrogen was introduced, and calcined at 850°C for 10 hours to obtain a carbon-coated solid electrolyte material. The conductivity of the material before and after coating was tested at room temperature, as shown in Table 4. As can be seen from Table 4, the conductivity of the material was significantly improved after carbon coating.
[0079] Table 4 Electrical conductivity of materials before and after carbon coating at room temperature
[0080] Test items Before coating (S / cm) After coating (S / cm) Material conductivity <![CDATA[6.41×10 -4 ]]> <![CDATA[1.04×10 -2 ]]>
[0081] Example 2 is compared with Example 1, the difference is that different carbon sources are used, the carbon source in Example 1 is citric acid, and the carbon source in Example 2 is carbon black. Combining Table 2 and Table 4, the conductivity improvement effect of the carbon-coated solid electrolyte material obtained in Example 2 is better than that of the carbon-coated solid electrolyte material obtained in Example 1, indicating that the use of carbon black as a carbon source to carbon-coat the sodium zirconium silicon phosphorus solid electrolyte is more conducive to improving the conductivity of the sodium zirconium silicon phosphorus solid electrolyte material.
[0082] Comparative Example 1
[0083] 214 g of sodium carbonate, 765 g of zirconium dioxide, 56 g of silicon dioxide and 980 g of diammonium phosphate were mixed, and then ball-milled at a fixed ball-milling frequency of 180 rpm for 1 hour, and then placed in a high-temperature box furnace and sintered at 1100° C. for 5 hours to obtain a sintered product.
[0084] The sodium zirconium silicon phosphorus sintered block is successively subjected to jaw crushing and ball milling to obtain sodium zirconium silicon phosphorus powder; wherein the ball milling frequency is 180 rpm and the ball milling time is 1 hour.
[0085] The sodium zirconium silicon phosphorus powder is subjected to air flow milling to obtain nano-scale sodium zirconium silicon phosphorus powder; wherein the particle size distribution of the nano-scale sodium zirconium silicon phosphorus powder is between 200nm and 700nm, as shown in Table 5.
[0086] Table 5 Particle size distribution of nano sodium zirconium silicon phosphorus powder
[0087] Particle size distribution D10(micrometer) D50(micrometer) D90(micrometer) D100(micrometer) Sodium Zirconium Silicon Phosphate 0.233 0.397 0.587 0.691
[0088] 1000g of nanometer sodium zirconium silicon phosphorus powder is mixed with 40g of carbon black, and 900ml of ethanol dispersant is added, and the mixture is mixed by ball milling at a frequency of 180rpm for 1h; then, the mixture is dried at 80°C to obtain a mixture, which is a carbon-sodium zirconium silicon phosphorus mechanical mixed material.
[0089] The mixed material was placed in an atmosphere furnace, nitrogen was introduced, and it was baked at 700°C for 10 hours to obtain a carbon-coated solid electrolyte material. The conductivity of the material before and after coating was tested at room temperature, as shown in Table 6. As can be seen from Table 6, the calcination temperature is low and the improvement of the conductivity of the material is not obvious. It is speculated that the low calcination temperature leads to an incomplete reaction, and the coated carbon is relatively small, so the improvement of the conductivity of the material is not obvious.
[0090] Table 6 Electrical conductivity of materials before and after carbon coating at room temperature
[0091] Test items Before coating (S / cm) After coating (S / cm) Material conductivity <![CDATA[6.35×10 -4 ]]> <![CDATA[6.41×10 -4 ]]>
[0092] Comparative Example 2
[0093] A sodium zirconium silicon phosphorus carbon coated solid electrolyte material and a preparation method thereof, the specific preparation method is as follows:
[0094] 214 g of sodium carbonate, 765 g of zirconium dioxide, 56 g of silicon dioxide and 980 g of diammonium phosphate were mixed, and then ball-milled at a fixed ball-milling frequency of 180 rpm for 1 hour, and then placed in a high-temperature box furnace and sintered at 1100° C. for 5 hours to obtain a sintered product.
[0095] The sodium zirconium silicon phosphorus sintered block is successively subjected to jaw crushing and ball milling to obtain sodium zirconium silicon phosphorus powder; wherein the ball milling frequency is 180 rpm and the ball milling time is 1 hour.
[0096] The sodium zirconium silicon phosphorus powder is subjected to air flow milling to obtain nano-scale sodium zirconium silicon phosphorus powder; wherein the particle size distribution of the nano-scale sodium zirconium silicon phosphorus powder is between 200nm and 700nm, as shown in Table 7.
[0097] Table 7 Particle size distribution of nano sodium zirconium silicon phosphorus powder
[0098] Particle size distribution D10(micrometer) D50(micrometer) D90(micrometer) D100(micrometer) Sodium Zirconium Silicon Phosphate 0.224 0.403 0.594 0.699
[0099] 1000g of nanometer sodium zirconium silicon phosphorus powder is mixed with 40g of carbon black, and 900ml of ethanol dispersant is added, and the mixture is mixed by ball milling at a frequency of 180rpm for 1h; then, the mixture is dried at 80°C to obtain a mixture, which is a carbon-sodium zirconium silicon phosphorus mechanical mixed material.
[0100] The mixed material was placed in an atmosphere furnace, nitrogen was introduced, and it was calcined at 1000°C for 10 hours to obtain a carbon-coated solid electrolyte material. The conductivity of the material before and after coating was tested at room temperature, as shown in Table 8. As can be seen from Table 8, the calcination temperature is high, and the improvement of the conductivity of the material is not obvious. It is speculated that the calcination temperature is too high, causing the phase change of sodium zirconium silicon phosphorus, the appearance of impurity peaks, and the impure components, so the improvement of the conductivity of the material is not obvious.
[0101] Table 8 Electrical conductivity of materials before and after carbon coating at room temperature
[0102] Test items Before coating (S / cm) After coating (S / cm) Material conductivity <![CDATA[6.38×10 -4 ]]> <![CDATA[6.27×10 -4 ]]>
[0103] Comparative Example 3
[0104] 214 g of sodium carbonate, 765 g of zirconium dioxide, 56 g of silicon dioxide and 980 g of diammonium phosphate were mixed, and then ball-milled at a fixed ball-milling frequency of 180 rpm for 1 hour, and then placed in a high-temperature box furnace and sintered at 1100° C. for 5 hours to obtain a sintered product.
[0105] The sodium zirconium silicon phosphorus sintered block is successively subjected to jaw crushing and ball milling to obtain sodium zirconium silicon phosphorus powder; wherein the ball milling frequency is 180 rpm and the ball milling time is 1 hour.
[0106] The sodium zirconium silicon phosphorus powder is subjected to air flow milling to obtain nano-scale sodium zirconium silicon phosphorus powder; wherein the particle size distribution of the nano-scale sodium zirconium silicon phosphorus powder is between 200nm and 700nm, as shown in Table 5.
[0107] Table 9 Particle size distribution of nano sodium zirconium silicon phosphorus powder
[0108] Particle size distribution D10(micrometer) D50(micrometer) D90(micrometer) D100(micrometer) Sodium Zirconium Silicon Phosphate 0.228 0.364 0.580 0.689
[0109] 1000g of nanometer sodium zirconium silicon phosphorus powder was mixed with 40g of citric acid, and 900ml of ethanol dispersant was added, and the mixture was mixed by ball milling at a frequency of 180rpm for 1h. The mixture was then dried at 80°C to obtain a mixed material, which was a carbon-sodium zirconium silicon phosphorus mechanical mixed material.
[0110] The mixed material was placed in an atmosphere furnace, nitrogen was introduced, and calcined at 700°C for 10 hours to obtain a carbon-coated solid electrolyte material. The conductivity of the material before and after coating was tested at room temperature, as shown in Table 6. As can be seen from Table 6, the calcination temperature is low and the conductivity of the material is not significantly improved.
[0111] Table 10 Electrical conductivity of materials before and after carbon coating at room temperature
[0112] Test items Before coating (S / cm) After coating (S / cm) Material conductivity <![CDATA[6.29×10 -4 ]]> <![CDATA[6.37×10 -4 ]]>
[0113] Comparative Example 4
[0114] A sodium zirconium silicon phosphorus carbon coated solid electrolyte material and a preparation method thereof, the specific preparation method is as follows:
[0115] 214 g of sodium carbonate, 765 g of zirconium dioxide, 56 g of silicon dioxide and 980 g of diammonium phosphate were mixed, and then ball-milled at a fixed ball-milling frequency of 180 rpm for 1 hour, and then placed in a high-temperature box furnace and sintered at 1100° C. for 5 hours to obtain a sintered product.
[0116] The sodium zirconium silicon phosphorus sintered block is successively subjected to jaw crushing and ball milling to obtain sodium zirconium silicon phosphorus powder; wherein the ball milling frequency is 180 rpm and the ball milling time is 1 hour.
[0117] The sodium zirconium silicon phosphorus powder is subjected to air flow milling to obtain nano-scale sodium zirconium silicon phosphorus powder; wherein the particle size distribution of the nano-scale sodium zirconium silicon phosphorus powder is between 200nm and 700nm, as shown in Table 7.
[0118] Table 11 Particle size distribution of nano sodium zirconium silicon phosphorus powder
[0119] Particle size distribution D10(micrometer) D50(micrometer) D90(micrometer) D100(micrometer) Sodium Zirconium Silicon Phosphate 0.224 0.403 0.594 0.699
[0120] 1000g of nanometer sodium zirconium silicon phosphorus powder was mixed with 40g of citric acid, and 900ml of ethanol dispersant was added, and the mixture was mixed by ball milling at a frequency of 180rpm for 1h. The mixture was then dried at 80°C to obtain a mixed material, which was a carbon-sodium zirconium silicon phosphorus mechanical mixed material.
[0121] The mixed material was placed in an atmosphere furnace, nitrogen was introduced, and the mixture was calcined at 1000°C for 10 hours to obtain a carbon-coated solid electrolyte material. The conductivity of the material before and after coating was tested at room temperature, as shown in Table 8. As can be seen from Table 8, the calcination temperature is high and the conductivity of the material is not significantly improved.
[0122] Table 12 Electrical conductivity of materials before and after carbon coating at room temperature
[0123] Test items Before coating (S / cm) After coating (S / cm) Material conductivity <![CDATA[6.25×10 -4 ]]> <![CDATA[6.18×10 -4 ]]>
[0124] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0125] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing a carbon-coated solid electrolyte material, characterized in that: The steps include: The sodium source, zirconium source, silicon source and phosphorus source are uniformly mixed, and after sintering, a sodium zirconium silicon phosphorus sintered block is obtained; The sodium zirconium silicon phosphorus sintered block is crushed to obtain sodium zirconium silicon phosphorus sintered powder; The sodium zirconium silicon phosphorus sintered powder is subjected to nano-processing to obtain nano-grade sodium zirconium silicon phosphorus powder; uniformly mixing the nano-scale sodium zirconium silicon phosphorus powder and a carbon source to obtain a mixed material; and The mixed material is calcined in a protective gas atmosphere to obtain a carbon-coated solid electrolyte material after sufficient reaction.
2. The method for preparing a carbon-coated solid electrolyte material according to claim 1, characterized in that: The sodium source is selected from at least one of sodium hydroxide, sodium carbonate, perchloric acid and sodium bis(trifluoromethylsulfonyl)imide; The zirconium source is selected from at least one of zirconium oxide, zirconium nitrate and zirconium acetate; The silicon source is silicon dioxide; The phosphorus source is selected from at least one of diammonium phosphate, phosphorus pentoxide, diammonium hydrogen phosphate and ammonium hydrogen phosphate; The sodium source, zirconium source, silicon source and phosphorus source are mixed evenly. During the sintering operation, the sintering temperature is 1000° C. to 1200° C. and the sintering time is 5 h to 20 h.
3. The method for preparing a carbon-coated solid electrolyte material according to claim 1, characterized in that: The particle size of the nano-scale sodium zirconium silicon phosphorus powder is 200nm-700nm.
4. The method for preparing a carbon-coated solid electrolyte material according to claim 1, characterized in that: The operation of uniformly mixing the nano-scale sodium zirconium silicon phosphorus powder and the carbon source is: mixing the nano-scale sodium zirconium silicon phosphorus powder and the carbon source, then adding a dispersant, mixing by ball milling, and then drying; wherein the drying temperature does not exceed 100° C.; and / or The dispersant is selected from one or more of methanol, ethanol and ethylene glycol; and / or The frequency of the ball milling is 100 rpm to 800 rpm, and the time of the ball milling is 1 h to 10 h.
5. The method for preparing a carbon-coated solid electrolyte material according to claim 1, characterized in that: The mass ratio of the nanometer-scale sodium zirconium silicon phosphorus powder to the carbon source is 1: (0.01-0.1).
6. The method for preparing a carbon-coated solid electrolyte material according to claim 1, characterized in that: The carbon source is selected from at least one of citric acid, glucose, starch, carbon black and asphalt.
7. The method for preparing a carbon-coated solid electrolyte material according to claim 1, characterized in that: In the operation of calcining the mixed material in a protective gas atmosphere: the calcination temperature is 800° C. to 900° C., and the calcination time is 5 h to 20 h; the protective gas is selected from at least one of nitrogen and argon.
8. The method for preparing a carbon-coated solid electrolyte material according to claim 1, characterized in that: The operation of crushing the sodium zirconium silicon phosphorus sintered block is: crushing the sodium zirconium silicon phosphorus sintered block by jaw crushing and ball milling in sequence.
9. A carbon-coated solid electrolyte material, characterized in that: The carbon-coated solid electrolyte material is prepared by the method for preparing the carbon-coated solid electrolyte material according to any one of claims 1 to 8.
10. A sodium ion battery, characterized in that: Comprising the carbon-coated solid electrolyte material as described in claim 9.