Repairing liquid and in-situ repairing and regenerating method of waste lithium iron phosphate battery
By using repair solution in waste lithium iron phosphate batteries for in-situ repair, regenerating lithium iron phosphate batteries solves the problems of complex processes and high energy consumption in the existing technology, and achieves low-cost and efficient battery regeneration and circulation performance improvements .
Patent Information
- Application Number
- CN202411341092.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-12-06
AI Technical Summary
The existing lithium iron phosphate battery recycling and regeneration methods are complex in technology, consuming a large amount of acid, alkali and high temperature calcination, resulting in high energy consumption and high cost, and lack of efficient reuse methods.
Using a repair solution, including lithium salt, organic solvent, negative electrode film forming additive and redox medium, the lithium iron phosphate battery is regenerated by in-situ repair in waste lithium iron phosphate batteries, the method includes deep discharge of small current and filling Repair liquid and charge in a low humidity environment to avoid disassembly and high temperature calcination.
The in-situ repair and regeneration of lithium iron phosphate batteries is achieved, with simple process, low energy consumption and low cost, which improves the battery circulation performance and significantly reduces the economic cost of battery repair.
Smart Images

Figure CN119092851A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of lithium battery recycling and reuse, and in particular to a repair liquid and an in-situ repair and regeneration method for waste lithium iron phosphate batteries. Background Art
[0002] With the development of lithium iron phosphate (LiFePO 4 With the continuous expansion of the market demand for lithium iron phosphate (LFP) batteries, the treatment of waste batteries will be a severe challenge. At present, the recycling and regeneration methods of lithium iron phosphate batteries are as follows:
[0003] First, the battery needs to be physically disassembled to separate the positive and negative electrode mixed powder, battery casing, copper foil, aluminum foil and diaphragm.
[0004] Secondly, the separated positive and negative electrode mixed powders need to be dissolved in an alkaline solution, and after removing the residual Al element, they are placed in an organic acid solution of a certain concentration to leach out Li, Fe and PO. 4 3- , filter out insoluble graphite and separate the positive electrode material and the negative electrode graphite material.
[0005] The third is to directly add a certain proportion of lithium source to the waste lithium iron phosphate material and regenerate the lithium iron phosphate positive electrode material through high-temperature calcination.
[0006] The above method is complex and consumes a lot of acid and alkali, and high-temperature calcination also causes a lot of energy consumption. It can be seen that for the recycling and upgrading of lithium iron phosphate batteries, it is urgent to find a more suitable method. Summary of the invention
[0007] In view of the above-mentioned defects of the prior art, the technical problem to be solved by the present invention is to provide a repair liquid and an in-situ repair and regeneration method for waste lithium iron phosphate batteries, wherein the in-situ repair and regeneration method has a simple process, low energy consumption and low cost.
[0008] To achieve the above-mentioned purpose, the present invention provides a repair liquid, comprising a lithium salt, an organic solvent, a negative electrode film-forming additive, and a redox medium. The organic solvent is used as a carrier, and the lithium salt, the negative electrode film-forming additive, and the redox medium are added respectively, stirred evenly, and dissolved, so that the lithium salt concentration is 0.1-5 mol / L, the mass fraction of the redox medium is 0.01-3%, and the filling volume of the negative electrode film-forming additive is 0.1-10% of the total liquid volume;
[0009] The lithium salt is lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethylsulfonyl)imide (LiTFSI), lithium difluorooxalatoborate (LiODFB), lithium dioxalatoborate (LiBOB), lithium difluorophosphate (LiPO 2 F 2 ), lithium hexafluorophosphate (LiPF6 ) or lithium tetrafluoroborate (LiBF 4 ) or any combination thereof;
[0010] The organic solvent is one or any combination of ethylene carbonate (EC), dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), and ethyl acetate (EA);
[0011] The negative electrode film-forming additive is one or any combination of vinylene carbonate (VC), fluoroethylene carbonate (FEC), vinyl ethylene carbonate (VEC) or 1,3-propane sultone (PS);
[0012] The redox medium is one or any combination of iodine (I2), lithium iodide (LiI), copper iodide (CuI2), cuprous iodide (CuI), and tin iodide (SnI2);
[0013] The role of iodide here is based on the following principles:
[0014] 3I - +2FePO 4 +2Li + →2LiFePO 4 +I 3 - ,During this process, the iodide ions in the repair solution react with the iron phosphate produced by the positive electrode to generate lithium iron phosphate; ,and triiodide anions are also produced;
[0015] 3I - -2e - →I 3 - ,During this process, the iodide ions in the repair solution generate triiodide anions;
[0016] I 3 - +2Li 0 →2Li + +3I - In this process, the triiodide anion reacts with the deactivated Li 0 reaction, regenerating electrochemically active Li + .
[0017] The present invention also discloses an in-situ repair and regeneration method for a lithium iron phosphate battery, comprising the following steps:
[0018] S100, deep discharge the used lithium iron phosphate battery with a small current, the discharge rate is 0.001C-0.5C, and the discharge cut-off voltage is 2.0-2.6V; the principle is: after long-term cycling of lithium iron phosphate batteries, the negative electrode SEI film thickens, and part of the Li+ It is consumed here and becomes a component that loses electrochemical activity. The purpose of this step is to partially decompose the solid electrolyte membrane (SEI) of the negative electrode to release lithium ions and electrons;
[0019] S200, prepare the repair solution; there is no order requirement for S100 and S200;
[0020] S300, add repair fluid into the battery, and place the battery in a fixed position for a preset time; the ratio of the mass of the repair fluid to the nominal capacity of the battery is: 0.1-5.00g / Ah. This step is preferably performed in a low humidity environment, where the dew point temperature is ≤-40°C; first, make a hole in the battery top cover, and the hole area can be selected to be less than 2mm 2 , then a certain amount of repair liquid is injected into the battery and sealed, and after sealing, the battery is left standing for 12 hours on both sides; of course, it is also possible not to make a hole, as long as the repair liquid can be injected into the battery; in addition, the standing time is not strictly limited, and in theory, as long as the repair effect of the present invention can be achieved, that is, the standing time for 12 hours on both sides is an empirical time, and it can be flexibly selected according to needs in actual implementation. In specific implementation, 9 hours, 10 hours, 11 hours, 13 hours, 14 hours, 15 hours, 20 hours and above can be selected;
[0021] S400, charge the battery to full power with a small current, the charging rate is 0.001C-0.5C, and the charging cut-off voltage is 3.6-4.0V; the purpose of this step is to replenish the lithium loss of the positive electrode, reduce Fe(III) in the positive electrode to Fe(II), and eliminate the anti-site defect;
[0022] S500, repeat S100 and S400, the number of repetitions is 1-10 times. In actual implementation, the number of repetitions can be selected according to needs to achieve the corresponding repair effect. Theoretically, there is no limit to the number of repetitions.
[0023] The beneficial effects of the present invention are:
[0024] The present invention does not need to disassemble the battery, and then carry out the calcination and reassembly process, and can realize the in-situ repair and regeneration of waste lithium iron phosphate batteries, and does not need complicated disassembly, acid washing, alkali washing, high temperature calcination process and battery reassembly process, so the process is simple and the energy consumption is low. At the same time, through actual testing, the repair effect of the present invention is good, the efficiency is high, and the positive electrode crystal structure is repaired, the battery cycle performance is improved, and the cost is obviously lower than the prior art, which is more suitable for the recovery, repair and reuse of existing lithium iron phosphate batteries, and has huge technical value, economic value and market application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1The embodiment 7 and the comparative example 2 were disassembled, the lithium iron phosphate positive electrode sheets were taken out, and the powder was scraped off and then an X-ray diffraction test was performed to obtain the spectrum. DETAILED DESCRIPTION
[0026] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the accompanying drawings in the embodiments of the present invention.
[0027] Embodiment 1:
[0028] The recycled 15Ah (Gotion-15Ah) square aluminum shell lithium iron phosphate battery produced by Hefei Guoxuan High-tech Battery Technology Co., Ltd. was used, and its initial discharge capacity was tested to be 10.1Ah;
[0029] S100, discharging the lithium iron phosphate battery at a rate of 0.001C to a depth of 2.6V;
[0030] S200, prepare repair solution:
[0031] S210, preparing an organic solvent, taking the following components and mixing them evenly according to a volume ratio to obtain an organic solvent: EC:DMC:DEC:EMC:EA=1:1:1:1:0.5:0.5;
[0032] S220, add LiPF to the organic solvent 6 ,(FEC,PS),I 2 Stir evenly and dissolve, finally making LiPF 6 The concentration is 1 mol / L, I 2 The mass fraction is 0.01%, and the filling volumes of FEC and PS are 1% and 2% of the total liquid volume respectively to complete the configuration of the repair liquid; the above steps are only for obtaining the corresponding proportion of the repair liquid, and there is no process design. Theoretically, as long as the repair liquid with the corresponding components and proportions can be obtained, there is no need to limit the corresponding steps.
[0033] S300, in an environment with a dew point temperature of -40°C, make a hole in the battery cover with an area of 1mm 2 , then inject 15g of repair liquid into the battery and seal it; leave the battery in both directions for 12 hours;
[0034] S400, charge the battery at a charge rate of 0.01C and a charge voltage of 3.65V;
[0035] S500, repeat S100 and S400 5 times.
[0036] Embodiment 2:
[0037] The recycled 15Ah (Gotion-15Ah) square aluminum shell lithium iron phosphate battery produced by Hefei Guoxuan High-tech Battery Technology Co., Ltd. was used, and its initial discharge capacity was tested to be 10.3Ah;
[0038] S100, discharging the lithium iron phosphate battery to a depth of 2.5V at a rate of 0.01C;
[0039] S200, prepare repair solution:
[0040] S210, preparing an organic solvent, taking the following components and mixing them evenly according to a volume ratio to obtain an organic solvent: EC:DMC:DEC:EMC=1:1:1:1;
[0041] S220, add LiPF to the organic solvent 6 、(VC、FEC、PS)、CuI 2 Stir evenly and dissolve, finally making LiPF 6 The concentration is 1 mol / L, CuI 2 The mass fraction of is 1.5%, and the filling volumes of VC, FEC, and PS are 3%, 3%, and 4% of the total liquid volume, respectively, to complete the configuration of the repair liquid;
[0042] S300, in an environment with a dew point temperature of -40°C, make a hole in the battery cover with an area of 1mm 2 , then inject 45g of repair liquid into the battery and seal it; leave the battery in both directions for 12 hours;
[0043] S400, charge the battery at a charge rate of 0.1C and a charge voltage of 3.65V;
[0044] S500, repeat S100 and S400 6 times.
[0045] Embodiment 3:
[0046] The recycled 15Ah (Gotion-15Ah) square aluminum shell lithium iron phosphate battery produced by Hefei Guoxuan High-tech Battery Technology Co., Ltd. was used, and its initial discharge capacity was tested to be 11.6Ah;
[0047] S100, discharging the lithium iron phosphate battery at a rate of 0.01C to a depth of 2.1V;
[0048] S200, prepare repair solution:
[0049] S210, preparing an organic solvent, taking the following components and mixing them evenly according to a volume ratio to obtain an organic solvent: EC:DMC:DEC:EMC=1:1:1:1;
[0050] S220, add (LiPF 6 ,LiFSI),VC,CuI 2 Stir evenly and dissolve, finally making LiPF 6 The concentrations of LiFSI were 1 mol / L and 0.2 mol / L, respectively, and CuI 2 The mass fraction of is 2%, and the filling volume of VC is 3% of the total liquid volume, thus completing the configuration of the repair fluid;
[0051] S300, in an environment with a dew point temperature of -40°C, make a hole in the battery cover with an area of 1mm 2 , then inject 5g of repair liquid into the battery and seal it; leave the battery in both directions for 12 hours;
[0052] S400, charge the battery at a charge rate of 0.001C and a charge voltage of 3.65V;
[0053] S500, repeat S100 and S400 5 times.
[0054] Embodiment 4:
[0055] The recycled 15Ah (Gotion-15Ah) square aluminum shell lithium iron phosphate battery produced by Hefei Guoxuan High-tech Battery Technology Co., Ltd. was used, and its initial discharge capacity was tested to be 10.6Ah;
[0056] S100, discharging the lithium iron phosphate battery at a rate of 0.01C to a depth of 2.2V;
[0057] S200, prepare repair solution:
[0058] S210, preparing an organic solvent, taking the following components and mixing them evenly according to a volume ratio to obtain an organic solvent: EC:DMC:DEC=1:1:1;
[0059] S220, add LiPF to the organic solvent 6 , FEC, and LiI are stirred evenly and dissolved, and finally LiPF 6 The concentration is 0.5 mol / L, the mass fraction of LiI is 0.01%, and the filling volume of FEC is 5% of the total liquid volume, thus completing the preparation of the repair solution;
[0060] S300, in an environment with a dew point temperature of -40°C, make a hole in the battery cover with an area of 1mm 2 , then inject 75g of repair liquid into the battery and seal it; leave the battery in both directions for 12 hours;
[0061] S400, charge the battery at a charge rate of 0.1C and a charge voltage of 3.7V;
[0062] S500, repeat S100 and S400 5 times.
[0063] Embodiment 5:
[0064] The recycled 15Ah (Gotion-15Ah) square aluminum shell lithium iron phosphate battery produced by Hefei Guoxuan High-tech Battery Technology Co., Ltd. was used, and its initial discharge capacity was tested to be 9.7Ah;
[0065] S100, discharging the lithium iron phosphate battery to a depth of 2.0V at a rate of 0.5C;
[0066] S200, prepare repair solution:
[0067] S210, preparing an organic solvent, taking the following components and mixing them evenly according to a volume ratio to obtain an organic solvent: EC:DMC:DEC=1:1:1;
[0068] S220, add LiPF to the organic solvent 6 、FEC、(SnI 2 , LiI) are stirred evenly and dissolved, and finally LiPF 6 The concentration of SnI is 0.1 mol / L. 2 The mass fraction of LiI is 1%, and the filling volume of FEC is 2% of the total liquid volume, thus completing the preparation of the repair liquid;
[0069] S300, in an environment with a dew point temperature of -40°C, make a hole in the battery cover with an area of 1mm 2 , then inject 2g of repair solution into the battery and seal it; leave the battery in both directions for 12 hours;
[0070] S400, charge the battery at a charge rate of 1.0C and a charge voltage of 3.7V;
[0071] S500, repeat S100 and S400 5 times.
[0072] Embodiment 6:
[0073] The recycled 15Ah (Gotion-15Ah) square aluminum shell lithium iron phosphate battery produced by Hefei Guoxuan High-tech Battery Technology Co., Ltd. was used, and its initial discharge capacity was tested to be 9.8Ah;
[0074] S100, discharging the lithium iron phosphate battery at a rate of 0.01C to a depth of 2.1V;
[0075] S200, prepare repair solution:
[0076] S210, preparing an organic solvent, taking the following components and mixing them evenly according to a volume ratio to obtain an organic solvent: EC:DMC=1:1;
[0077] S220, add LiPF to the organic solvent 6 、FEC、SnI 2 Stir evenly and dissolve, finally making LiPF 6 The concentration of SnI is 3 mol / L. 2 The mass fraction is 3%, and the filling volume of FEC is 5% of the total liquid volume, completing the preparation of the repair liquid;
[0078] S300, in an environment with a dew point temperature of -40°C, make a hole in the battery cover with an area of 1mm 2 , then inject 1.5g of repair solution into the battery and seal it; leave the battery in both directions for 12 hours;
[0079] S400, charge the battery at a charge rate of 0.5C and a charge voltage of 4V;
[0080] S500, repeat S100 and S400 9 times.
[0081] Embodiment 7:
[0082] The recycled 15Ah (Gotion-15Ah) square aluminum shell lithium iron phosphate battery produced by Hefei Guoxuan High-tech Battery Technology Co., Ltd. was used, and its initial discharge capacity was tested to be 10.1Ah;
[0083] S100, discharging the lithium iron phosphate battery at a rate of 0.01C to a depth of 2.2V;
[0084] S200, prepare repair solution:
[0085] S210, preparing an organic solvent, taking the following components and mixing them evenly according to a volume ratio to obtain an organic solvent: EC:DMC:DEC=1:1:1;
[0086] S220, add LiPF to the organic solvent 6 , (VC, FEC, PS), LiI are stirred evenly and dissolved, and finally LiPF 6 The concentration is 1 mol / L, the mass fraction of LiI is 0.5%, and the filling volumes of VC, FEC, and PS are all 1% of the total liquid volume, completing the preparation of the repair liquid;
[0087] S300, in an environment with a dew point temperature of -40°C, make a hole in the battery cover with an area of 1mm2 , then inject 5g of repair liquid into the battery and seal it; leave the battery in both directions for 12 hours;
[0088] S400, charge the battery at a charge rate of 0.01C and a charge voltage of 3.8V;
[0089] S500, repeat S100 and S400 10 times.
[0090] Embodiment 8:
[0091] The recycled 15Ah (Gotion-15Ah) square aluminum shell lithium iron phosphate battery produced by Hefei Guoxuan High-tech Battery Technology Co., Ltd. was used, and its initial discharge capacity was tested to be 10.9Ah;
[0092] S100, discharging the lithium iron phosphate battery at a rate of 0.01C to a depth of 2.2V;
[0093] S200, prepare repair solution:
[0094] S210, preparing an organic solvent, taking the following components and mixing them evenly according to a volume ratio to obtain an organic solvent: EC:DMC:DEC=1:1:1;
[0095] S220, add LiPF to the organic solvent 6 , (VC, FEC, PS), LiI are stirred evenly and dissolved, and finally LiPF 6 The concentration is 1 mol / L, the mass fraction of LiI is 0.5%, and the filling volumes of VC, FEC, and PS are all 1% of the total liquid volume, completing the preparation of the repair liquid;
[0096] S300, in an environment with a dew point temperature of -40°C, make a hole in the battery cover with an area of 1mm 2 , then inject 5g of repair liquid into the battery and seal it; leave the battery in both directions for 12 hours;
[0097] S400, charge the battery at a charge rate of 0.01C and a charge voltage of 3.8V;
[0098] S500, repeat S100 and S400 10 times.
[0099] Embodiment 9:
[0100] The recycled 30Ah (EVE-30Ah cell) square aluminum shell lithium iron phosphate battery from Huizhou EVE Energy Co., Ltd. was used, and its initial discharge capacity was tested to be 25Ah;
[0101] S100, discharging the lithium iron phosphate battery at a rate of 0.1C to a depth of 2.3V;
[0102] S200, prepare repair solution:
[0103] S210, preparing an organic solvent, taking the following components and mixing them evenly according to a volume ratio to obtain an organic solvent: EC:DMC:DEC:EMC=1:1:1:1;
[0104] S220, add LiTFSI, VC, CuI to the organic solvent respectively 2 Stir evenly and dissolve, finally making LiPF 6 The concentration is 1 mol / L, CuI 2 The mass fraction of is 1.5%, and the filling volume of VC is 3% of the total liquid volume, thus completing the configuration of the repair liquid;
[0105] S300, in an environment with a dew point temperature of -40°C, open a hole on the battery cover with an area of 2mm 2 , then inject 3g of repair liquid into the battery and seal it; leave the battery in both directions for 12 hours;
[0106] S400, charge the battery at a charge rate of 0.01C and a charge voltage of 3.65V;
[0107] S500, repeat S100 and S400 6 times.
[0108] Embodiment 10:
[0109] The recycled 30Ah (EVE-30Ah cell) square aluminum shell lithium iron phosphate battery from Huizhou EVE Energy Co., Ltd. was used, and its initial discharge capacity was tested to be 18Ah;
[0110] S100, discharging the lithium iron phosphate battery at a rate of 0.5C to a depth of 2.2V;
[0111] S200, prepare repair solution:
[0112] S210, preparing an organic solvent, taking the following components and mixing them evenly according to a volume ratio to obtain an organic solvent: EC:DMC:DEC:EMC=1:1:1:1;
[0113] S220, add (LiBF 4 、LiODFB)、VEC、SnI 2 Stir evenly and dissolve, finally making LiBF 4 The concentrations of LiODFB and SnI were both 0.5 mol / L. 2The mass fraction of is 2%, the filling volume of VEC is 2% of the total liquid volume, and the configuration of the repair fluid is completed;
[0114] S300, in an environment with a dew point temperature of -40°C, open a hole on the battery cover with an area of 2mm 2 , then inject 15g of repair liquid into the battery and seal it; leave the battery in both directions for 12 hours;
[0115] S400, charge the battery at a charge rate of 0.5C and a charge voltage of 3.8V;
[0116] S500, repeat S100 and S400 10 times.
[0117] Comparative Example 1
[0118] The same 15Ah square aluminum shell lithium iron phosphate battery recycled from Hefei Guoxuan High-tech Battery Technology Co., Ltd. as in Example 1 was used, and its discharge capacity was tested to be 10.2Ah; no other treatment was performed.
[0119] Comparative Example 2
[0120] The same 15Ah square aluminum shell lithium iron phosphate battery recycled from Hefei Guoxuan High-tech Battery Technology Co., Ltd. as in Example 2 was used, and its discharge capacity was tested to be 10.6Ah; no other treatment was performed.
[0121] Comparative Example 3:
[0122] The same 15Ah square aluminum shell lithium iron phosphate battery recycled from Hefei Guoxuan High-tech Battery Technology Co., Ltd. as in Example 9 was tested to have a discharge capacity of 10.8Ah, and the following comparative steps were performed:
[0123] S100, discharging the lithium iron phosphate battery at a rate of 0.01C to a depth of 2.2V; S400, charging the battery at a charge rate of 0.01C and a charge voltage of 3.8V;
[0124] S500, cycle S100, and S400 10 times in total.
[0125] Comparative Example 4:
[0126] The same 15Ah square aluminum shell lithium iron phosphate battery recycled from Hefei Guoxuan High-tech Battery Technology Co., Ltd. as in Example 8 was tested to have a discharge capacity of 10.8Ah; and the following comparative steps were performed:
[0127] S100, discharge the lithium iron phosphate battery at a rate of 0.01C to a depth of 2.8V;
[0128] S200, prepare repair solution:
[0129] S210, preparing an organic solvent, taking the following components and mixing them evenly according to a volume ratio to obtain an organic solvent: EC:DMC:DEC=1:1:1;
[0130] S220, S220, add LiPF to the organic solvent respectively 6 , (VC, FEC, PS), LiI are stirred evenly and dissolved, and finally LiPF 6 The concentration is 1 mol / L, the mass fraction of LiI is 0.5%, and the filling volumes of VC, FEC, and PS are all 1% of the total liquid volume, completing the preparation of the repair liquid;
[0131] S300, in an environment with a dew point temperature of -40°C, open a hole on the battery cover with an area of 2mm 2 , then inject 5g of repair liquid into the battery and seal it; leave the battery in both directions for 12 hours;
[0132] S400, charge the battery at a charge rate of 0.01C and a charge voltage of 3.8V;
[0133] S500, cycle S100, and S400 once in total.
[0134] Comparative Example 5:
[0135] A 30Ah (EVE-30Ah battery cell) square aluminum shell lithium iron phosphate battery produced by Huizhou Yiwei Lithium Energy Co., Ltd. was used as in Example 10, and its initial discharge capacity was tested to be 19.7Ah; no other treatment was performed.
[0136] The parameter statistics of the implementation process of Examples 1-10 and Comparative Examples 1-5 are shown in Table 1:
[0137] Table 1 Process parameters of the embodiments and comparative examples
[0138]
[0139]
[0140] The cycle performance test results of Examples 1-10 and Comparative Examples 1-5 at 25°C, 0.5C charge / 0.5C discharge are shown in Table 2:
[0141] Table 2 Performance comparison between the examples and the comparative examples
[0142]
[0143] From the comparison of the cycle performances of Examples 1-10 and Comparative Examples 1, 2 and 5, it can be seen that the discharge capacity of the lithium iron phosphate positive battery repaired by the method is restored, and the number of cycles is increased when the capacity decays to 50%.
[0144] By comparing Example 8 with Comparative Example 3, it can be seen that the repair effect of the battery without adding the repair liquid is significantly lower than that of the battery with adding the repair liquid.
[0145] By comparing Example 8 with Comparative Example 4, it can be seen that the repair effect of the battery that has not been deeply discharged is significantly lower than that of the battery that has been deeply discharged.
[0146] Example 7 and Comparative Example 2 were disassembled, the lithium iron phosphate positive electrode sheets were taken out, and the powder was scraped off and then X-ray diffraction test was performed. The test results are shown in Figure 1 .
[0147] Figure 1 XRD of the positive electrode powder after repair in Example 7 (curve A); XRD of the positive electrode powder in Comparative Example 2 (curve B); Curve C is the standard XRD card of lithium iron phosphate positive electrode material. The dotted line frame in the figure is the impurity peak generated during the use of the waste positive electrode.
[0148] From the positive electrode XRD results of Example 7 and Comparative Example 2, it can be seen that the structure of the lithium iron phosphate positive electrode repaired by the present method is restored, and the iron phosphate phase generated during use is eliminated.
[0149] It should be noted that, unless otherwise specified, the technical terms or scientific terms used in this application should have the common meanings understood by technicians in the field to which this application belongs.
[0150] The above is only a preferred specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A repair fluid, characterized in that: It includes lithium salt, organic solvent, negative electrode film-forming additive, and redox medium; with organic solvent as carrier, lithium salt, negative electrode film-forming additive, and redox medium are added respectively, stirred evenly and dissolved, and finally the lithium salt concentration is 0.1-5 mol / L, the mass fraction of the redox medium is 0.01-3%, and the filling volume of the negative electrode film-forming additive is 0.1-10% of the total liquid volume.
2. The repair liquid according to claim 1, characterized in that The lithium salt is one or any combination of lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethylsulfonyl)imide (LiTFSI), lithium difluorooxalatoborate (LiODFB), lithium dioxalatoborate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium hexafluorophosphate (LiPF6) or lithium tetrafluoroborate (LiBF4).
3. The repair solution according to claim 1, characterized in that The organic solvent is one or any combination of ethylene carbonate (EC), dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), and ethyl acetate (EA).
4. The repair liquid according to claim 1, characterized in that The negative electrode film-forming additive is one or any combination of vinylene carbonate (VC), fluoroethylene carbonate (FEC), vinyl ethylene carbonate (VEC) or 1,3-propane sultone (PS).
5. The repair liquid according to any one of claims 1 to 4, characterized in that: The redox medium is one or any combination of iodine (I2), lithium iodide (LiI), copper iodide (CuI2), cuprous iodide (CuI), and tin iodide (SnI2).
6. An in-situ repair and regeneration method for waste lithium iron phosphate batteries, characterized in that: The following steps are involved: S100, deep discharge the used lithium iron phosphate battery with a small current, the discharge rate is 0.001C-0.5C, and the discharge cut-off voltage is 2.0-2.6V; S200, preparing the repair liquid according to any one of claims 1 to 5; there is no order requirement for S100 and S200; S300, add repair fluid into the battery; S400, charge the battery to full power with a low current, the charging rate is 0.001C-0.5C, and the charging cut-off voltage is 3.6-4.0V; S500, repeat S100 and S400.
7. The in situ repair and regeneration method according to claim 6, characterized in that: S300 is performed in a low humidity environment, wherein the dew point temperature of the low humidity environment is ≤-40°C.
8. The in situ repair and regeneration method according to claim 6, characterized in that: After filling the repair fluid in the S300, leave the battery in both directions for a preset time.
9. The in situ repair and regeneration method according to any one of claims 6 to 8, characterized in that: In S300, the ratio of the mass of the repair fluid added to the nominal capacity of the battery is: 0.1-5.00g / Ah.
10. The in situ repair and regeneration method according to claim 6, characterized in that: The number of repetitions in S500 ranges from 1 to 10.