Composite polymer electrolyte diaphragm, preparation method and application
By mixing PVDF-HFP with LATP and graphite phase carbon nitride, composite polymer electrolyte separators are prepared, which solves the safety hazards and insufficient performance problems of traditional lithium-ion battery electrolyte separators in high-temperature environments, and achieves efficient charging of lithium-ion batteries Discharge and long-term stability.
Patent Information
- Application Number
- CN202411023920.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The electrolyte separator materials in traditional lithium-ion batteries have safety risks in high temperature environments, and the existing solid electrolyte materials such as aluminum titanium phosphate and polyvinylidene fluoride-hexafluoropropylene have short cycle life and insufficient mechanical strength, which limits their wide range. application.
Using the preparation method of composite polymer electrolyte separator, PVDF-HFP and LATP are mixed and graphite phase carbon nitride (g-C3N4) is added to improve conductivity and mechanical strength to form PVDF-HFP/LATP Or PVDF-HFP/LATP/g-C3N4 composite polymer electrolyte separator.
The high migration number of lithium ions and the high ionic conductivity of the electrolyte membrane are achieved, the charging and discharging speed and energy efficiency of the lithium ion battery are improved, and the good cycle stability and battery safety are shown through constant current charging and discharging tests.
Smart Images

Figure CN119092933A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of new nano materials, and in particular to the field of a novel diaphragm for electrochemical energy conversion and utilization. Background Art
[0002] With the rapid development of science and technology, energy storage devices have become an indispensable part of modern life, especially in portable electronic devices (such as mobile phones, computers) and new energy fields (such as electric vehicles). The performance of lithium-ion batteries, as one of the current mainstream energy storage technologies, is directly related to the operating efficiency and safety of these devices. Among them, the electrolyte membrane, as the core component of lithium-ion batteries, plays a key role in separating the positive and negative electrodes, allowing ion transmission and preventing electrons from passing directly.
[0003] Traditional polyolefin separator materials, such as polypropylene (PP) and polyethylene (PE), have been widely used in the market, but their low heat resistance limits their application in high temperature environments, which can easily lead to safety hazards such as separator shrinkage and battery short circuit. Therefore, developing a separator material with high conductivity, good stability and long cycle life has become an important research direction to solve the safety problem of lithium-ion batteries.
[0004] In recent years, solid electrolyte materials have attracted much attention in the field of diaphragm materials due to their excellent performance. Among them, lithium aluminum titanium phosphate (LATP, general formula is Li 1+x Al x Ti 2-x (PO4)3), as a glass-ceramic material with a three-dimensional network structure, is considered a promising candidate for solid electrolytes due to its high mechanical strength, chemical stability, high conductivity and high temperature resistance. However, LATP has problems of low density and large interface impedance after tableting and sintering, which limits its direct application in batteries.
[0005] On the other hand, polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP), as a porous polymer, also shows potential as a solid electrolyte material due to its high melting temperature, low crystallinity, good lithium metal interface compatibility and excellent liquid absorption rate. However, the short cycle life and insufficient mechanical strength of PVDF-HFP separators are still the main obstacles to their widespread application.
[0006] Although some studies have been conducted to improve the performance of PVDF-HFP by adding nano / micron-scale ceramic materials (such as Al2O3, TiO2, LLZO, etc.), these additives can reduce the crystallinity of PVDF-HFP, promote the movement of molecular chains, and facilitate the transmission of lithium ions. However, how to accurately control the type and proportion of additives and their interaction with the matrix material to achieve the best performance improvement is still an urgent problem to be solved. Summary of the invention
[0007] In order to solve the deficiencies of the prior art, the present application provides a composite polymer electrolyte membrane, a preparation method and an application thereof.
[0008] The first aspect of the present application is to provide a method for preparing a composite polymer electrolyte membrane, the steps comprising:
[0009] Provide a LATP, namely Li 1+x Al x Ti 2-x (PO4)3;
[0010] PVDF-HFP (polyvinylidene fluoride-hexafluoropropylene) is mixed with LATP to obtain PVDF-HFP / LATP, i.e., a composite polymer electrolyte membrane;
[0011] Here, x is a positive number not greater than 2.
[0012] More preferably, x is a positive number not greater than 1.
[0013] More preferably, x is 0.05-1.5, more preferably 0.1-1.0, and may be selected from one or more combinations of 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, and 1.0.
[0014] In a preferred embodiment, the PVDF-HFP and LATP are further mixed with g-C3N4 (graphite-phase carbon nitride) to obtain a composite polymer electrolyte membrane of PVDF-HFP / LATP / g-C3N4.
[0015] In a preferred embodiment, g-C3N4 is also added during the mixing process of the PVDF-HFP and LATP.
[0016] In a preferred embodiment, the method for preparing LATP comprises the following steps:
[0017] Lithium (Li + ) salt, TiO2, Al2O3 and phosphate are mixed and calcined.
[0018] Preferably, the lithium salt may be an inorganic acid salt or an organic acid salt, and is preferably one or more combinations selected from LiNO3, Li2CO3, Li2SO4, LiCl, LiBr, CH3COOLi, HCOOLi.
[0019] Preferably, the phosphate is selected from phosphate (PO4 3- ), phosphite (PO2 - ), hypophosphite (PO2 3- )
[0020] Specifically, the phosphate includes one or more combinations of ammonium phosphate, trisodium phosphate, diammonium phosphate, tripotassium phosphate, potassium dihydrogen phosphate, sodium dihydrogen phosphate, dipotassium hydrogen phosphate, disodium hydrogen phosphate, sodium hypophosphite, potassium hypophosphite, sodium phosphite, and potassium phosphite.
[0021] Preferably, the molar ratio of the lithium salt, TiO2, Al2O3 and phosphate is (0.2-1.0)﹕(0.05-0.8)﹕(1.0-2.5)﹕(1.5-4.5), preferably (0.3-0.9)﹕(0.1-0.7)﹕(1.2-2.2)﹕(2.0-4.0), and more preferably (0.4-0.8)﹕(0.15-0.65)﹕(1.3-2.1)﹕(2.5-3.5).
[0022] Specifically, the molar ratio may be one or more combinations of 0.55﹕0.25﹕1.8﹕3.2, 0.45﹕0.35﹕1.4﹕2.8, 0.65﹕0.15﹕1.7﹕3.
[0023] In a preferred embodiment, the method for mixing lithium salt, TiO2, Al2O3 and phosphate comprises the following steps:
[0024] The lithium salt, TiO2, Al2O3 and phosphate are mixed and stirred in a first solvent to obtain a mixture; and the mixture is dried.
[0025] Preferably, one or more of the lithium salt, TiO2, Al2O3, and phosphate are ground before mixing, either separately or together.
[0026] Preferably, the first solvent can be one or more of water, alcohol, ether, ester, ketone, nitrile, halogenated hydrocarbon, aromatic hydrocarbon, and ionic liquid, and is preferably a solvent mixture selected from: water, N,N-dimethylformamide, methanol, ethanol, ether, tetrahydrofuran, acetonitrile, valeronitrile, methoxypropionitrile, butyronitrile, adiponitrile, benzyl cyanide, chloroacetonitrile, dichloromethane, carbon tetrachloride, ethyl acetate, acetone, N-methylpyrrolidone, toluene, and ionic liquids (such as 1-butyl-3-methylimidazole hexafluorophosphate).
[0027] In a preferred embodiment, the drying temperature of the mixture is 50-120°C, preferably 60-100°C, more preferably 70-80°C.
[0028] In a preferred embodiment, the drying time of the mixture is 4-20 hours, preferably 8-16 hours, and more preferably 10-12 hours.
[0029] In a preferred embodiment, the calcination includes primary calcination and secondary calcination.
[0030] Preferably, the primary calcination temperature is 200-450°C, preferably 250-400°C, more preferably 300-350°C.
[0031] Preferably, the primary calcination time is 0.5-3.5 h, preferably 1-3 h, more preferably 1.5-2 h.
[0032] Preferably, the heating rate of the primary calcination is 2-8°C / min, preferably 3-6°C / min, more preferably 4-5°C / min.
[0033] Preferably, the temperature of the secondary calcination is 500-1400° C., preferably 600-1200° C., more preferably 800-1000° C. Specifically, the temperature of the secondary calcination can be one of 800° C., 850° C., 900° C., 950° C., 1000° C. or a combination thereof.
[0034] Preferably, the secondary calcination time is 2-8 h, preferably 3-6 h, more preferably 4-5 h.
[0035] Preferably, the heating rate of the secondary calcination is 2-8°C / min, preferably 3-6°C / min, more preferably 4-5°C / min.
[0036] Preferably, the atmosphere of the primary calcination is air or an inert gas.
[0037] Preferably, the atmosphere of the secondary calcination is air or inert gas.
[0038] Preferably, the atmospheres of the primary calcination and the secondary calcination may be the same or different.
[0039] More preferably, the inert gas includes one or more combinations of nitrogen, argon and helium.
[0040] In a preferred embodiment, the preparation method of g-C3N4 comprises the following steps:
[0041] Calcinate urea to obtain the g-C3N4.
[0042] Preferably, the temperature for calcining urea is 300-700°C, preferably 460-640°C, more preferably 520-580°C.
[0043] Preferably, the urea calcination time is 2-8 h, preferably 3-6 h, more preferably 4-5 h.
[0044] Preferably, the heating rate of urea calcination is 1-6°C / min, preferably 2-5°C / min, more preferably 3-4°C / min.
[0045] In a preferred embodiment, the PVDF-HFP is mixed with LATP and then cast or coated to prepare a composite polymer electrolyte membrane.
[0046] In a preferred embodiment, the PVDF-HFP, LATP and g-C3N4 are mixed and then prepared by casting or coating to obtain a composite polymer electrolyte membrane.
[0047] In a preferred embodiment, the PVDF-HFP and LATP are mixed in a second solvent.
[0048] In a preferred embodiment, the PVDF-HFP, LATP and g-C3N4 can also be mixed in the second solvent.
[0049] Preferably, the second solvent can be one or more of water, alcohol, ether, ester, ketone, nitrile, halogenated hydrocarbon, aromatic hydrocarbon, and ionic liquid, and is preferably a solvent mixture selected from: water, N,N-dimethylformamide, methanol, ethanol, ether, tetrahydrofuran, acetonitrile, valeronitrile, methoxypropionitrile, butyronitrile, adiponitrile, benzyl cyanide, chloroacetonitrile, dichloromethane, carbon tetrachloride, ethyl acetate, acetone, N-methylpyrrolidone, toluene, and ionic liquids (such as 1-butyl-3-methylimidazolium hexafluorophosphate).
[0050] Preferably, the PVDF-HFP and LATP need to be heated when mixed, and the heating temperature is preferably 40-100°C, more preferably 50-80°C, and more preferably 60-70°C.
[0051] Preferably, the PVDF-HFP, LATP and g-C3N4 also need to be heated when mixed, and the heating temperature is preferably 40-100°C, more preferably 50-80°C, and more preferably 60-70°C.
[0052] Preferably, the composite polymer electrolyte membrane is further dried.
[0053] More preferably, the drying temperature is 45-80°C, more preferably 50-70°C, more preferably 55-65°C.
[0054] More preferably, the drying time is 12-64 h, preferably 18-48 h, more preferably 24-36 h.
[0055] The second aspect of the present invention is to provide a composite polymer electrolyte membrane, comprising a PVDF-HFP base membrane, and LATP dispersed in the PVDF-HFP base membrane; more preferably, it also comprises g-C3N4 dispersed in the PVDF-HFP base membrane.
[0056] Preferably, the composite polymer electrolyte membrane is obtained based on the aforementioned preparation method.
[0057] More preferably, in one of the composite polymer electrolyte membranes, the mass ratio of the PVDF-HFP to the LATP is (2-10):1, preferably (3-8):1, and more preferably (5-6):1.
[0058] More preferably, in a composite polymer electrolyte membrane, the mass ratio of LATP to g-C3N4 is (5-30):1, preferably (10-25):1, and more preferably (15-20):1.
[0059] More preferably, the lithium ion transference number of the composite polymer electrolyte separator is ≧0.4, preferably ≧0.5, and more preferably ≧0.6.
[0060] More preferably, the porosity of the composite polymer electrolyte membrane is 2-50%, preferably 5-45%, more preferably 10-40%.
[0061] More preferably, the pore size of the composite polymer electrolyte membrane is 5-180 nm, preferably 10-160 nm, and more preferably 20-150 nm.
[0062] More preferably, the thermal shrinkage of the composite polymer electrolyte membrane is 0.5-15%, preferably 1-13%, and more preferably 2-12%.
[0063] More preferably, the ionic conductivity of the composite polymer electrolyte membrane is 1.2×10 -5S / cm-2.1×10 - 4 S / cm, preferably 1.5×10 -5 S / cm-1.9×10 -4 S / cm, more preferably 1.8×10 -5 S / cm-1.7×10 -4 S / cm.
[0064] The third aspect of the present invention provides an application of the aforementioned composite polymer electrolyte membrane, wherein the composite polymer electrolyte membrane can be applied to batteries, especially lithium-ion batteries.
[0065] Compared with the prior art, the present invention has the following beneficial technical effects:
[0066] The present invention provides a method for preparing a composite polymer electrolyte membrane. The composite polymer electrolyte membrane obtained by the preparation method overcomes the shortcomings of the electrolyte membrane in the field of traditional lithium ion batteries. Its unique structure and properties effectively promote the migration of lithium ions, and the lithium ion migration number is as high as 0.647. The ion conductivity of the electrolyte membrane is also improved, providing a faster charging and discharging speed and higher energy efficiency for lithium ion batteries. Moreover, the Li-Li battery using the composite polymer electrolyte membrane of the present invention has a relatively stable voltage distribution after constant current charging and discharging for 200 hours, and has good cycle stability, ensuring the safety and reliability of the battery during long-term use.
[0067] Secondly, the preparation method of the present invention is simple and efficient, and PVDF-HFP, LATP or PVDF-HFP, LATP and g-C3N4 are successfully combined by the tape casting method to form a composite electrolyte membrane with uniform structure and excellent performance. This structural design not only overcomes the shortcomings of traditional electrolyte membranes, but also further improves the comprehensive performance of the material.
[0068] In summary, the present invention aims at the deficiencies of existing solid electrolyte materials, studies a new type of diaphragm material, optimizes the material structure, and improves the material performance, providing a key path for promoting the advancement of lithium-ion battery technology and ensuring battery safety. BRIEF DESCRIPTION OF THE DRAWINGS
[0069] Figure 1In the figure, (a) is the XRD graph of LATP and composite polymer electrolyte membrane PVDF-HFP / LATP obtained in Example 1 of the present invention, the composite polymer electrolyte membrane PVDF-HFP / LATP / g-C3N4 obtained in Example 2, and the composite polymer electrolyte membrane PVDF-HFP obtained in Comparative Example 1; (b) is the DSC graph of the composite polymer electrolyte membrane PVDF-HFP / LATP obtained in Example 1 of the present invention, the composite polymer electrolyte membrane PVDF-HFP / LATP / g-C3N4 obtained in Example 2, and the composite polymer electrolyte membrane PVDF-HFP obtained in Comparative Example 1, the abscissa is temperature, and the ordinate is heat flow.
[0070] Figure 2 In the figure, (a, b) are SEM images of the PVDF-HFP membrane obtained in Comparative Example 1 of the present invention; (c, d) are SEM images of the composite polymer electrolyte membrane PVDF-HFP / LATP obtained in Example 1 of the present invention; (e, f) are SEM images of the composite polymer electrolyte membrane PVDF-HFP / LATP / g-C3N4 obtained in Example 2 of the present invention.
[0071] Figure 3 In the figure, (a) is the linear sweep voltammetric curve of LATP, composite polymer electrolyte membrane PVDF-HFP / LATP obtained in Example 1 of the present invention, and composite polymer electrolyte membrane PVDF-HFP / LATP / g-C3N4 obtained in Example 2 at room temperature, the horizontal axis is voltage (voltage), and the vertical axis is current (current); (b) is the impedance spectrum and DC voltage bias curve of the composite polymer electrolyte membrane PVDF-HFP obtained in Comparative Example 1, (c) is the impedance spectrum and DC voltage bias curve of LATP and composite polymer electrolyte membrane PVDF-HFP / LATP obtained in Example 1, (d) is the impedance spectrum and DC voltage bias curve of the composite polymer electrolyte membrane PVDF-HFP / LATP / g-C3N4 obtained in Example 2, the horizontal axis is time (time), and the vertical axis is current (current).
[0072] Figure 4 (a) is a cyclic charge-discharge diagram of the composite polymer electrolyte membrane PVDF-HFP / LATP obtained in Example 1 of the present invention in a lithium symmetric battery, Figure 2 This is a cyclic charge and discharge diagram of the composite polymer electrolyte membrane PVDF-HFP / LATP / g-C3N4 obtained in Example 2 in a lithium symmetric battery, where the horizontal axis is time and the vertical axis is voltage. DETAILED DESCRIPTION
[0073] The embodiments of the present invention provide a composite polymer electrolyte membrane, a preparation method and an application. In order to make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail with reference to the accompanying drawings and examples. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0074] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged under appropriate circumstances. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0075] Example 1
[0076] This embodiment provides a method for preparing a PVDF-HFP / LATP membrane, the steps comprising:
[0077] (1) Preparation of LATP samples: Li 1.3 Al 0.3 Ti 1.7 The (PO4)3 sample was prepared by a high-temperature solid-phase reaction method. Li2CO3, TiO2, Al2O3 and (NH4)H2PO4 were placed in a blast drying oven for drying to completely remove moisture. Then Li2CO3, Al2O3, TiO2 and (NH4)H2PO4 were weighed according to a molar ratio of 0.65:0.15:1.7:3, and mixed in a mortar one by one and ground thoroughly. The mixture was then transferred to a certain volume of anhydrous ethanol, magnetically stirred for 4 hours, and then placed in a vacuum drying oven and dried at 80°C for 12 hours. The treated mixed powder was transferred to a corundum crucible, placed in a muffle furnace, calcined at 350°C in air (heating rate 5°C / min), and kept warm for 2 hours. After natural cooling, the product was taken out and placed in a muffle furnace again, and calcined in air at different temperatures (900°C) for 4 hours. After natural cooling to room temperature, the product was fully ground. Finally, powdered LATP was obtained.
[0078] (2) Preparation of PVDF-HFP / LATP membrane: The PVDF-HFP / LATP membrane was prepared by a simple casting method. 0.1 g PVDF-HFP was added to a small amount of N-methylpyrrolidone and magnetically stirred at 60°C until it was completely dissolved. Then 0.02 g LATP was added and stirred for 12 h to form a suspension. The suspension was then ultrasonically treated for 1 h. The suspension was then evenly coated on a quartz glass sheet and placed in a vacuum drying oven at 55°C for vacuum drying for 24 h. Finally, a PVDF-HFP / LATP membrane was obtained.
[0079] Example 2
[0080] This embodiment provides a method for preparing a PVDF-HFP / LATP / g-C3N4 membrane, the steps comprising:
[0081] (1) Preparation of LATP samples: Li 1.3 Al 0.3 Ti 1.7 The (PO4)3 sample was prepared by a high-temperature solid-phase reaction method. Li2CO3, TiO2, Al2O3 and (NH4)H2PO4 were placed in a blast drying oven for drying to completely remove moisture. Then Li2CO3, Al2O3, TiO2 and (NH4)H2PO4 were weighed according to a molar ratio of 0.65:0.15:1.7:3, and mixed in a mortar one by one and ground thoroughly. The mixture was then transferred to a certain volume of anhydrous ethanol, magnetically stirred for 4 hours, and then placed in a vacuum drying oven and dried at 80°C for 12 hours. The treated mixed powder was transferred to a corundum crucible, placed in a muffle furnace, calcined at 350°C in air (heating rate 5°C / min), and kept warm for 2 hours. After natural cooling, the product was taken out and placed in a muffle furnace again, and calcined in air at different temperatures (900°C) for 4 hours. After natural cooling to room temperature, the product was fully ground. Finally, powdered LATP was obtained.
[0082] (2) Preparation of g-C3N4 sample: A certain amount of urea was placed in a quartz crucible with a lid, and then transferred to a muffle furnace, heated to 580°C, and kept at this temperature for 4 hours at a heating rate of 3°C / min. After cooling naturally to room temperature, a pale yellow powder sample of graphite phase carbon nitride (g-C3N4) was obtained.
[0083] (3) Preparation of PVDF-HFP / LATP / g-C3N4 membrane: The preparation method is similar to that of PVDF-HFP / LATP membrane. 0.1 g PVDF-HFP was added to a small amount of N-methylpyrrolidone and magnetically stirred at 60°C until it was completely dissolved. Then 0.02 g LATP and 0.001 g g-C3N4 were added, stirred for 12 h, and then ultrasonically treated for 1 h. The resulting suspension was applied on a glass slide and vacuum dried at 55°C for 24 h. PVDF-HFP / LATP / g-C3N4 membrane was obtained.
[0084] Comparative Example 1
[0085] This comparative example provides a method for preparing a PVDF-HFP membrane, the steps comprising:
[0086] (1) Preparation of PVDF-HFP membrane: The preparation method is similar to that of PVDF-HFP / LATP and PVDF-HFP / LATP / g-C3N4 membranes. 0.1 g of PVDF-HFP was added to a small amount of N-methylpyrrolidone and magnetically stirred at 60°C until it was completely dissolved. The resulting suspension was then coated on a glass slide and vacuum dried at 55°C for 24 h. A PVDF-HFP membrane was obtained.
[0087] Figure 1The XRD patterns of (a) composite polymer electrolyte membranes PVDF-HFP / LATP, PVDF-HFP / LATP / g-C3N4 and PVDF-HFP, LATP obtained in Examples 1 and 2 of the present invention and Comparative Example 1 respectively; (b) DSC patterns. Figure a is the XRD pattern of composite polymer electrolyte membranes PVDF-HFP, PVDF-HFP / LATP, PVDF-HFP / LATP / g-C3N4 and LATP (900°C). It can be seen from the figure that the diffraction curve of the diaphragm PVDF-HFP / LATP / g-C3N4 has weak diffraction peaks at 2θ=13.1° and 27.5°, corresponding to the (100) crystal plane and (002) crystal plane of g-C3N4, respectively. The characteristic diffraction peaks of PVDF-HFP are located at 2θ=18.5°, 20°, 26.5° and 39.5°, and the obvious peak intensity indicates that pure PVDF-HFP has good crystallinity. Among them, weak diffraction peaks at 2θ=26.5° and 39.5° can be observed in the XRD diffraction curves of the two composite polymer electrolyte membranes, but the diffraction peak intensity is very weak, indicating that the crystallinity of the polymer PVDF-HFP decreases. Among them, the diffraction peak intensity of PVDF-HFP / LATP / g-C3N4 is the lowest. This may be because after the addition of g-C3N4, the crystallization of the polymer chain is inhibited to a certain extent, and the increase in the amorphous area is beneficial to improving the ionic conductivity of the membrane. Figure b is the DSC curves of three composite polymer electrolyte membranes PVDF-HFP, PVDF-HFP / LATP, and PVDF-HFP / LATP / g-C3N4. The test temperature range is 50-300℃, and the heating rate is 10℃ / min. It can be observed from the figure that the three membranes all have an endothermic peak between 140-160℃, which is the melting temperature (T m ). The melting peak of PVDF-HFP / LATP / g-C3N4 film is 142.6℃, which is lower than 147.8℃ of PVDF-HFP / LATP and 157.5℃ of PVDF-HFP. The decrease of melting temperature indicates that the amorphous area in the composite increases and the crystallinity decreases, which is consistent with the XRD results of Figure a.
[0088] Figure 2The SEM images are of the PVDF-HFP membrane (a, b) obtained in Comparative Example 1 of the present invention, the composite polymer electrolyte membrane PVDF-HFP / LATP (c, d) obtained in Example 1, and the PVDF-HFP / LATP / g-C3N4 (e, f) obtained in Example 2. Figures a and b show the surface morphology of the PVDF-HFP membrane. It can be observed that the small-sized pores of the PVDF-HFP membrane are relatively uniform, but the number of pores is small, and the surface of the membrane is relatively flat, which is not conducive to the infiltration of the electrolyte and the transmission of lithium ions. Figures c and d are SEM images of the surface morphology of the PVDF-HFP / LATP membrane. It can be seen that there are regularly arranged large-sized pores, and some LATP particles are attached to the surface. It may be because the presence of these LATP particles causes more pores to appear during the film formation process. However, the excessive pore size (about 50 μm) is not conducive to effectively retaining the electrolyte. Figures e and f are SEM images of the surface morphology of the PVDF-HFP / LATP / g-C3N4 membrane. It can be observed that the pore size (about 5 μm) is smaller than that of the PVDF-HFP / LATP membrane, but the number of pores is large. The appropriate pore size helps to accommodate more electrolyte and improve the ionic conductivity of the polymer electrolyte membrane.
[0089] Figure 3The linear sweep voltammetry curves of (a) PVDF-HFP, PVDF-HFP / LATP and PVDF-HFP / LATP / g-C3N4 membranes obtained in Examples 1 and 2 of the present invention and Comparative Example 1 at room temperature; (b, c, d) impedance spectra and DC voltage bias curves. The electrochemical stability window is an important criterion for measuring the electrochemical stability of the electrolyte membrane, which is determined by linear sweep voltammetry (LSV). The charge and discharge voltage range of a general lithium-ion battery is between 2.0V and 4.2V. Therefore, judging the decomposition potential of the diaphragm through the LSV test is crucial for the selection of the positive electrode material. The composite polymer electrolyte membrane is assembled into a button cell with a lithium metal / diaphragm / stainless steel sheet structure, with the stainless steel sheet as the working electrode and the lithium metal as the counter electrode and reference electrode. Figure a is a linear sweep voltammetry curve of the two diaphragms. It can be seen that the PVDF-HFP / LATP membrane has no obvious current between 3.0-4.2V, and the decomposition voltage is around 4.3V. After adding g-C3N4, the electrochemical stability window of the PVDF-HFP / LATP / g-C3N4 membrane becomes wider, there is no obvious current between 3.0-5.0V, and the decomposition voltage is around 5.0V. The reason why the current increases significantly when the working voltage exceeds the decomposition voltage is that an oxidation reaction occurs in the electrolyte in the battery. Therefore, the PVDF-HFP / LATP / g-C3N4 membrane has a wider electrochemical stability window than the PVDF-HFP / LATP membrane and has wide application potential in lithium-ion batteries. Figures b, c and d are the current-time curves of PVDF-HFP, PVDF-HFP / LATP and PVDF-HFP / LATP / g-C3N4 membranes under a DC bias voltage of 10mV and the electrochemical AC impedance spectra before and after the bias. The test was completed by assembling a Li symmetric battery. The lithium ion migration number (t Li + ) is obtained through the Bruce-Vincent formula
[0090] Calculated.
[0091] Where ΔV=10mV, I o and I s are the initial current and the stable current, R o and R s The PVDF-HFP / LATP / g-C3N4 membrane has a higher lithium ion migration number (0.647), which is higher than the t Li + =0.261 and PVDF-HFP / LATP t Li +=0.627. This indicates that the addition of g-C3N4 improves the mobility of lithium ions, which helps to improve the electrochemical performance of chlorinated polyethylene (CPE) membrane.
[0092] Figure 4 The figure shows the cyclic charge and discharge test diagram of the composite polymer electrolyte membranes PVDF-HFP / LATP and PVDF-HFP / LATP / g-C3N4 obtained in Examples 1 and 2 of the present invention in a lithium symmetric battery. The figure shows the cyclic charge and discharge test diagram of the two composite polymer electrolyte membranes PVDF-HFP / LATP and PVDF-HFP / LATP / g-C3N4 in a Li symmetric battery at room temperature, wherein each charge or discharge time is 30 minutes, and the charge and discharge current density is 0.1 mA / cm 2 . The voltage distribution of the Li-Li battery using PVDF-HFP / LATP membrane gradually increased during the 200h charge and discharge process, and the voltage increased significantly at 140h and 167h of charge and discharge, which may be due to the fact that the growth of lithium dendrites was not effectively suppressed. However, the voltage distribution of the Li-Li battery using PVDF-HFP / LATP / g-C3N4 membrane was relatively stable after constant current charge and discharge for 200h, and it had good cycle stability. This is because the two-dimensional structure of g-C3N4 facilitates good contact between the electrolyte membrane and the lithium metal electrode and inhibits the crystallization of the polymer, so that lithium can be evenly deposited on the electrode surface, avoiding the growth of lithium dendrites.
[0093] In summary, the PVDF-HFP / LATP / g-C3N4 membrane was prepared by a simple method. The membrane has a good electrochemical stability window and good cycle stability, and is a composite polymer electrolyte membrane with good application prospects in the field of lithium-ion batteries.
[0094] Example 3
[0095] This embodiment provides a method for preparing a PVDF-HFP / LATP / g-C3N4 membrane, the steps comprising:
[0096] (1) Preparation of LATP samples: Li 1.3 Al 0.3 Ti 1.7The (PO4)3 sample was prepared by a high-temperature solid-phase reaction method. Li2CO3, TiO2, Al2O3 and (NH4)H2PO4 were placed in a blast drying oven for drying to completely remove moisture. Then Li2CO3, Al2O3, TiO2 and (NH4)H2PO4 were weighed according to a molar ratio of 0.75:0.25:1.6:2.8, and mixed in a mortar one by one and ground thoroughly. The mixture was then transferred to a certain volume of anhydrous ethanol, magnetically stirred for 4 hours, and then placed in a vacuum drying oven and dried at 80°C for 12 hours. The treated mixed powder was transferred to a corundum crucible, placed in a muffle furnace, calcined at 350°C in air (heating rate 5°C / min), and kept warm for 2 hours. After natural cooling, the product was taken out, placed in a muffle furnace again, and calcined in air at 800°C for 4 hours. After natural cooling to room temperature, the product was fully ground. Finally, powdered LATP was obtained.
[0097] (2) Preparation of g-C3N4 sample: A certain amount of urea was placed in a quartz crucible with a lid, and then transferred to a muffle furnace, heated to 650°C, and kept at this temperature for 4 hours at a heating rate of 5°C / min. After cooling naturally to room temperature, a pale yellow powder sample of graphite phase carbon nitride (g-C3N4) was obtained.
[0098] (3) Preparation of PVDF-HFP / LATP / g-C3N4 membrane: The preparation method is similar to that of PVDF-HFP / LATP membrane. 0.1 g PVDF-HFP was added to a small amount of N-methylpyrrolidone and magnetically stirred at 60°C until it was completely dissolved. Then 0.02 g LATP and 0.001 g g-C3N4 were added, stirred for 12 h, and then ultrasonically treated for 1 h. The resulting suspension was applied on a glass slide and vacuum dried at 65°C for 36 h. PVDF-HFP / LATP / g-C3N4 membrane was obtained.
[0099] Example 4
[0100] This embodiment provides a method for preparing a PVDF-HFP / LATP / g-C3N4 membrane, the steps comprising:
[0101] (1) Preparation of LATP samples: Li 1.3 Al 0.3 Ti 1.7The (PO4)3 sample was prepared by a high-temperature solid-phase reaction method. Li2CO3, TiO2, Al2O3 and (NH4)H2PO4 were placed in a blast drying oven for drying to completely remove moisture. Then Li2CO3, Al2O3, TiO2 and (NH4)H2PO4 were weighed according to a molar ratio of 0.75:0.25:1.6:2.8, and mixed in a mortar one by one and ground thoroughly. The mixture was then transferred to a certain volume of anhydrous ethanol, magnetically stirred for 4 hours, and then placed in a vacuum drying oven for drying at 100°C for 12 hours. The treated mixed powder was transferred to a corundum crucible, placed in a muffle furnace, calcined at 350°C in air (heating rate 5°C / min), and kept warm for 2 hours. After natural cooling, the product was taken out, placed in a muffle furnace again, and calcined in air at 1000°C for 6 hours. After natural cooling to room temperature, the product was fully ground. Finally, powdered LATP was obtained.
[0102] (2) Preparation of g-C3N4 sample: A certain amount of urea was placed in a quartz crucible with a lid, and then transferred to a muffle furnace, heated to 550°C, and kept at this temperature for 8 hours at a heating rate of 10°C / min. After cooling naturally to room temperature, a pale yellow powder sample of graphite phase carbon nitride (g-C3N4) was obtained.
[0103] (3) Preparation of PVDF-HFP / LATP / g-C3N4 membrane: The preparation method is similar to that of PVDF-HFP / LATP membrane. 0.1 g PVDF-HFP was added to a small amount of N-methylpyrrolidone and magnetically stirred at 60°C until it was completely dissolved. Then 0.02 g LATP and 0.001 g g-C3N4 were added, stirred for 12 h, and then ultrasonically treated for 1 h. The resulting suspension was applied on a glass slide and vacuum dried at 80°C for 36 h. PVDF-HFP / LATP / g-C3N4 membrane was obtained.
[0104] Example 5
[0105] This embodiment provides a method for preparing a PVDF-HFP / LATP / g-C3N4 membrane, the steps comprising:
[0106] (1) Preparation of LATP samples: Li 1.3 Al 0.3 Ti 1.7The (PO4)3 sample was prepared by a high-temperature solid-phase reaction method. Li2CO3, TiO2, Al2O3 and (NH4)H2PO4 were placed in a blast drying oven for drying to completely remove moisture. Then Li2CO3, Al2O3, TiO2 and (NH4)H2PO4 were weighed according to a molar ratio of 0.35:0.55:1.8:2.5, and then placed in a mortar one by one for mixing and grinding. The mixture was then transferred to a certain volume of anhydrous ethanol, magnetically stirred for 4 hours, and then placed in a vacuum drying oven for drying at 100°C for 12 hours. The treated mixed powder was transferred to a corundum crucible, placed in a muffle furnace, calcined at 350°C in air (heating rate 5°C / min), and kept warm for 2 hours. After natural cooling, the product was taken out, placed in a muffle furnace again, and calcined in air at 1000°C for 10 hours. After natural cooling to room temperature, the product was fully ground. Finally, powdered LATP was obtained.
[0107] (2) Preparation of g-C3N4 sample: A certain amount of urea was placed in a quartz crucible with a lid, and then transferred to a muffle furnace, heated to 450°C, and kept at this temperature for 5 hours at a heating rate of 1°C / min. After cooling naturally to room temperature, a pale yellow powder sample of graphite phase carbon nitride (g-C3N4) was obtained.
[0108] (3) Preparation of PVDF-HFP / LATP / g-C3N4 membrane: The preparation method is similar to that of PVDF-HFP / LATP membrane. 0.1 g PVDF-HFP was added to a small amount of N-methylpyrrolidone and magnetically stirred at 80°C until it was completely dissolved. Then 0.02 g LATP and 0.001 g g-C3N4 were added, stirred for 12 h, and then ultrasonically treated for 1 h. The resulting suspension was applied on a glass slide and vacuum dried at 80°C for 24 h. PVDF-HFP / LATP / g-C3N4 membrane was obtained.
[0109] The specific embodiments of the present invention are described in detail above, but they are only examples, and the present invention is not limited to the specific embodiments described above. For those skilled in the art, any equivalent modifications and substitutions made to the present invention are also within the scope of the present invention. Therefore, the equalization changes and modifications made without departing from the spirit and scope of the present invention should be included in the scope of the present invention.
Claims
1. A method for preparing a composite polymer electrolyte membrane, characterized in that the steps include: Provide a LATP, namely Li 1+x Al x Ti 2-x (PO4)3; Mixing PVDF-HFP and LATP to obtain PVDF-HFP / LATP, i.e., a composite polymer electrolyte membrane; Here, x is a positive number not greater than 2.
2. The preparation method according to claim 1, characterized in that: PVDF-HFP and LATP are also mixed with g-C3N4 to obtain a composite polymer electrolyte membrane of PVDF-HFP / LATP / g-C3N4.
3. The preparation method according to claim 1, characterized in that: The preparation method of LATP comprises the following steps: Lithium salt, TiO2, Al2O3 and phosphate are mixed and calcined.
4. The preparation method according to claim 3, characterized in that: The molar ratio of the lithium salt, TiO2, Al2O3 and phosphate is (0.2-1.0)﹕(0.05-0.8)﹕(1.0-2.5)﹕(1.5-4.5), preferably (0.3-0.9)﹕(0.1-0.7)﹕(1.2-2.2)﹕(2.0-4.0), and more preferably (0.4-0.8)﹕(0.15-0.65)﹕(1.3-2.1)﹕(2.5-3.5).
5. The preparation method according to claim 3, characterized in that: The mixing method of lithium salt, TiO2, Al2O3 and phosphate comprises the following steps: Mixing and stirring the lithium salt, TiO2, Al2O3, and phosphate in a first solvent to obtain a mixture; The mixture is dried.
6. The preparation method according to claim 3, characterized in that: The calcination of LATP includes primary calcination and secondary calcination.
7. The preparation method according to claim 6, characterized in that: The primary calcination temperature is 200-450°C, preferably 250-400°C, more preferably 300-350°C; and / or The time of the first calcination is 0.5-3.5h, preferably 1-3h, more preferably 1.5-2h; and / or The heating rate of the primary calcination is 2-8°C / min, preferably 3-6°C / min, more preferably 4-5°C / min; and / or The temperature of the secondary calcination is 500-1400°C, preferably 600-1200°C, more preferably 800-1000°C; and / or The secondary calcination time is 2-8h, preferably 3-6h, more preferably 4-5h; and / or The heating rate of the secondary calcination is 2-8°C / min, preferably 3-6°C / min, more preferably 4-5°C / min; and / or The primary calcination atmosphere is air or an inert gas; and / or The atmosphere of the secondary calcination is air or inert gas.
8. The preparation method according to claim 2, characterized in that: The preparation method of g-C3N4 comprises the following steps: Calcining urea to obtain the g-C3N4; Wherein, the temperature of calcining urea is 300-700°C, preferably 460-640°C, more preferably 520-580°C; and / or The urea calcination time is 2-8h, preferably 3-6h, more preferably 4-5h; and / or The heating rate of urea calcination is 1-6°C / min, preferably 2-5°C / min, and more preferably 3-4°C / min.
9. A composite polymer electrolyte membrane, characterized in that: Obtained based on the preparation method according to any one of claims 1 to 8.
10. Use of the composite polymer electrolyte membrane according to claim 9, characterized in that: The composite polymer electrolyte separator is applied to batteries, especially lithium ion batteries.
Citation Information
Patent Citations
Preparation method of LATP ceramic particle reinforced quasi-solid polymer electrolyte
CN117913357A