Composite diaphragm as well as preparation method and application thereof

By using composite separators in lithium manganese iron phosphate batteries, combining the MOFs material layer and acetylene carbon layer, the problems of manganese dissolution and short life are solved, and the cycle performance and service life of the battery are significantly improved.

CN119092943APending Publication Date: 2024-12-06SVOLT ENERGY TECHNOLOGY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411242613.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Lithium manganese iron phosphate positive electrode material has problems such as manganese dissolution and short life, which affects its circulation performance and service life in the battery.

Method used

Using a composite separator, including a base film, a MOFs material layer and an acetylene carbon layer, manganese ions are fixed through the MOFs material layer and their dissolution is inhibited, and the catalytic effect of the MOFs structure on the electrolyte is reduced through the acetylene carbon layer packaging to improve the cycling performance of the battery.

Benefits of technology

It effectively inhibits the dissolution of manganese ions in lithium manganese iron phosphate batteries, extends the cycle life of the battery, improves the rate performance, reduces the occurrence of side reactions, and improves the overall performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005029732510000131
    Figure BDA0005029732510000131
Patent Text Reader

Abstract

The invention belongs to the technical field of secondary batteries, and particularly relates to a composite diaphragm as well as a preparation method and application thereof. The composite diaphragm provided by the invention comprises a base membrane; the MOFs material layer is positioned on the surface of one side of the base film; the acetylene carbon layer is located on the surface of the side, away from the base film, of the MOFs material layer. The MOFs material layer is arranged on the surface of the base membrane, and the acetylene carbon layer is adopted to package the base membrane, so that the composite membrane can fix Mn ions dissolved out due to a J-T effect in a long-cycle process of lithium manganese iron phosphate. Besides, the MOFs material layer is encapsulated by using the acetylene carbon layer, so that the dissolution of the organic MOFs structure in electrolyte can be effectively inhibited, the catalysis of the MOFs frame structure on the electrolyte can be reduced, and the occurrence of side reaction can be inhibited, thereby improving the cycle performance, rate capability and the like of the ferromanganese phosphate battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of secondary batteries, and specifically relates to a composite diaphragm and a preparation method and application thereof. Background Art

[0002] In recent years, with the continuous technological breakthroughs in the new energy market, the battery market operation has gone through a cycle of more than 10 years. Consumers' demand for energy density has gradually been solved. At the same time, the demand for safety has become more and more prominent. Therefore, phosphate positive electrodes are respected for their safety characteristics.

[0003] Lithium iron phosphate is the most widely used positive electrode material at present, but its energy density is slightly low. Therefore, it is of great significance to develop high energy density phosphate positive electrode materials. Lithium manganese iron phosphate has a high voltage platform, which leads to an energy density increase of 20% compared with lithium iron phosphate. However, there are still some problems with lithium manganese iron phosphate, such as manganese dissolution and short life.

[0004] Therefore, improving manganese dissolution and extending life will help the rapid promotion of lithium manganese iron phosphate batteries and increase their mileage and extend their service life. Summary of the invention

[0005] Therefore, the technical problem to be solved by the present application is to overcome the defects of manganese dissolution and short life of lithium manganese iron phosphate positive electrode materials in the prior art, thereby providing a composite diaphragm and its preparation method and application.

[0006] To this end, this application provides the following technical solutions:

[0007] According to one aspect of the present application, a composite diaphragm is provided, comprising:

[0008] Basement membrane;

[0009] A MOFs material layer is located on one side surface of the base film;

[0010] The acetylene carbon layer is located on a surface of the MOFs material layer that is away from the base film.

[0011] In some optional embodiments, the thickness of the MOFs material layer is 1 μm-7 μm; optionally, 2 μm-5 μm.

[0012] In some optional embodiments, the thickness of the acetylene carbon layer is 1.5 μm-6.5 μm; optionally 3 μm-6 μm;

[0013] And / or, the composite membrane has a thickness of 10 μm-21 μm.

[0014] In some optional embodiments, the longitudinal heat shrinkage ratio X of the composite diaphragm is 0.1%-1.3%; optionally 0.1%-0.5%;

[0015] And / or, the porosity P of the composite membrane is 8%-30%.

[0016] According to another aspect of the present application, a method for preparing the above-mentioned composite diaphragm is provided, comprising the following steps:

[0017] S1, mixing a metal salt, an organic ligand, a binder and an organic solvent to obtain a slurry;

[0018] S2, coating the slurry onto the surface of the base film to perform a self-assembly reaction to form a MOFs material layer on the surface of the base film;

[0019] S3, dissolving an organic compound containing an acetylene group in ethyl acetate to obtain a mixed solution, coating the mixed solution on the surface of the MOFs material layer, allowing it to stand, and heat treating it to obtain the composite diaphragm.

[0020] In some optional embodiments, in step S1, the metal salt includes at least one of ZrCl4, FeCl3, NiCl, CuNO3, ZnNO3, FeNO3, CoCl2, cobalt acetate, iron acetate, and nickel acetate;

[0021] And / or, the organic ligand includes at least one of 2,4-dihydroxybiphenyl dicarboxylic acid, 4,4'-biphenyl dicarboxylic acid, 2,3-diaminoterephthalic acid, 1,3,7-naphthalenetricarboxylic acid, 2(4-chlorophenylthio)phenylacetic acid, 2-nitrotrimesic acid, 3-phosphobenzoic acid, 6-(dimethylamino)-2-naphthoic acid, 4-methylphosphonic acid, 4,6-dinitro-1,3-benzenedicarboxylic acid, anthraquinone-1-carboxylic acid, 3,4-diaminophenylacetic acid, 12-amino-5(dimethylamino)benzoic acid, and 5-(dimethylamino)-2-nitrobenzoic acid;

[0022] and / or, the molar ratio of the metal salt to the organic ligand is 1-3;

[0023] And / or, the binder includes at least one of PVDF (polyvinylidene fluoride), PMMA (polymethyl methacrylate), and PTFE (polytetrafluoroethylene);

[0024] And / or, the organic solvent includes at least one of N,N-dimethylformamide, N-hexylpyrrolidone, and N-methylpyrimidine;

[0025] and / or, the binder accounts for 0.2%-11% of the total mass of the metal salt and the organic ligand, optionally 2%-5%;

[0026] In some optional embodiments, in step S2, the conditions of the self-assembly reaction include: temperature of 120°C-180°C; illumination power of 1000-2000W; illumination wavelength of 100-2000nm, optionally 800-1600nm; illumination time of 12-16h.

[0027] In some optional embodiments, the organic compound containing acetylene groups includes at least one of 4-ethynyl-1,2-phenylenediamine, 3-ethynyl-1,2-phenylenediamine, ethynylcyclohexanol, 4-ethynylbenzoic acid, phenylacetylene, 4-ethynylaniline, 1,3,6,8-tetra(ethynyl)pyrene, 3-ethynylpyridine, ethynylcyclohexanol, 1-ethynylcyclopentanol, and 1-ethynyl-4-methylbenzene;

[0028] and / or, the concentration of the organic compound containing acetylene groups in the mixed solution is 0.5-1 mol / L;

[0029] And / or, the standing time is 10-20 min;

[0030] And / or, the heat treatment temperature is 100°C-350°C, optionally 200°C-280°C, and the time is 1-2h;

[0031] And / or, the heat treatment is performed under a protective atmosphere.

[0032] According to another aspect of the present application, a secondary battery is provided, comprising the composite diaphragm described above or the composite diaphragm prepared by the preparation method described above.

[0033] According to another aspect of the present application, there is provided an electrical device comprising the above-mentioned secondary battery.

[0034] In the present application, the protective gas includes at least one of nitrogen and argon.

[0035] In the present application, the base film is a conventional separator in the field of secondary batteries, including but not limited to a polyimide (PI) separator.

[0036] In the present application, other compositions and preparation methods of the secondary battery provided are conventional in the art and are not specifically limited here.

[0037] In the present application, the secondary battery can be used as a power source for the electrical device, or as an energy storage unit for the electrical device. The electrical device may include, but is not limited to, mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc. The electrical device may select a secondary battery, a battery module, or a battery pack according to its usage requirements.

[0038] The technical solution of this application has the following advantages:

[0039] The composite diaphragm provided by the present application includes: a base film; a MOFs material layer, which is located on one side surface of the base film; and an acetylene carbon layer, which is located on the side surface of the MOFs material layer away from the base film. The present application sets a MOFs material layer on the surface of the base film and uses an acetylene carbon layer to encapsulate it. The composite diaphragm can fix the Mn ions dissolved due to the JT effect during the long cycle of lithium manganese iron phosphate. In addition, encapsulating the MOFs material layer with an acetylene carbon layer can effectively inhibit the dissolution of the organic MOFs structure in the electrolyte, and at the same time can reduce the catalysis of the MOFs framework structure on the electrolyte, inhibit the occurrence of side reactions, thereby improving the cycle performance of the manganese iron phosphate battery. In addition, the organic combination of the acetylene carbon layer and the MOFs material layer can improve the contact with the positive electrode interface and improve the rate performance of the battery. This diaphragm can also be used in lithium iron phosphate batteries to inhibit the dissolution of metallic iron to a certain extent, and it also has the function of reducing the black spots and short circuit problems caused by the entry of impurity metals into the positive electrode.

[0040] The composite diaphragm provided in the present application can regulate the dissolution process of manganese dissolved in lithium manganese iron phosphate by limiting the thickness of the MOFs material layer and / or the acetylene carbon layer, while making the internal resistivity of the battery reach the optimal value.

[0041] The composite diaphragm provided in the present application limits the longitudinal heat shrinkage ratio X, the porosity P and the thickness of the composite diaphragm, so that the composite layer diaphragm coating does not crack, thereby improving the solid-solid bonding degree between the positive electrode and the diaphragm.

[0042] The preparation method of the composite diaphragm provided in the present application anchors metal Mn ions through the large pores and framework structure of the MOFs structure, and reduces the catalytic effect of MOF on the electrolyte by encapsulating acetylene carbon into MOFs, while reducing the dissolution of the MOFs framework structure.

[0043] The preparation method of the composite diaphragm provided in the present application limits the reaction parameters, selects ligands to regulate the framework structure for fixing manganese ions, and regulates the stability of the MOFs framework on the base membrane by light intensity and time, so that the composite layer does not fall off the base membrane. DETAILED DESCRIPTION

[0044] The following examples are provided for a better understanding of the present application, but are not limited to the best implementation mode described, and do not limit the content and protection scope of the present application. Any product identical or similar to the present application obtained by anyone under the inspiration of the present application or by combining the features of the present application with other prior arts shall fall within the protection scope of the present application.

[0045] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0046] Example 1

[0047] This embodiment provides a composite diaphragm, and its composition and specific preparation method are as follows:

[0048] In the first step, 1 mol of ZrCl4, 1 mol of 1,3,7-naphthalenetricarboxylic acid and 20 g of PVDF were put into DMF and stirred for 3 hours to prepare a slurry.

[0049] In the second step, take the PI (polyimide) diaphragm, put it on the glass plate, and then take the slurry prepared in the first step and apply it on the PI diaphragm. Place the coated PI composite diaphragm under a light source of 1000W and 850nm at 120°C for 15 hours.

[0050] The third step is to dissolve 0.5 mol of trimethylsilylethynylbenzene in ethyl acetate and stir evenly, then drop the dissolved solution (concentration is 0.5 mol / L) on the side with the coating material, let it stand for 20 minutes, then put the wetted electrode into an oven and bake it at 250°C in a nitrogen atmosphere for 1 hour, remove the diaphragm and cool it to room temperature to obtain the composite diaphragm.

[0051] Example 2

[0052] This embodiment provides a composite diaphragm. Compared with the embodiment 1, the only difference is that the amount of PVDF used in the first step is 50 g, and the rest is the same as the embodiment 1.

[0053] Example 3

[0054] This embodiment provides a composite membrane. Compared with the embodiment 1, the only difference is that the amount of PVDF used in the first step is 1 g, and the rest is the same as the embodiment 1.

[0055] Example 4

[0056] This embodiment provides a composite diaphragm. Compared with the embodiment 1, the only difference is that the wavelength of the light source in the second step is 100 nm, and the rest is the same as the embodiment 1.

[0057] Example 5

[0058] This embodiment provides a composite diaphragm. Compared with the embodiment 1, the only difference is that the wavelength of the light source in the second step is 2000 nm, and the rest is the same as the embodiment 1.

[0059] Example 6

[0060] This embodiment provides a composite diaphragm. Compared with the embodiment 1, the only difference is that the temperature of the heat treatment in the third step is 350° C., and the rest is the same as the embodiment 1.

[0061] Example 7

[0062] This embodiment provides a composite diaphragm. Compared with the embodiment 1, the only difference is that the temperature of the heat treatment in the third step is 100° C., and the rest is the same as the embodiment 1.

[0063] Example 8

[0064] This embodiment provides a composite diaphragm, and its composition and specific preparation method are as follows:

[0065] In the first step, 1 mol of CoCl2, 1 mol of 1,3,7-naphthalenetricarboxylic acid and 20 g of PVDF were put into DMF and stirred for 3 hours to prepare a slurry.

[0066] In the second step, take the PI (polyimide) diaphragm, put it on the glass plate, and then take the slurry prepared in the first step and apply it on the PI diaphragm. Place the coated PI composite diaphragm under a light source of 1000W and 850nm at 120°C for 15 hours.

[0067] The third step is to dissolve 0.5 mol of trimethylsilylethynylbenzene in ethyl acetate and stir evenly, then drop the dissolved solution (concentration is 0.5 mol / L) on the side with the coating material, let it stand for 20 minutes, then put the wetted electrode into an oven and bake it at 250°C in a nitrogen atmosphere for 1 hour, remove the diaphragm and cool it to room temperature to obtain the composite diaphragm.

[0068] Example 9

[0069] This embodiment provides a composite diaphragm, and its composition and specific preparation method are as follows:

[0070] In the first step, 1 mol of ZrCl4, 2 mol of 1,3,7-naphthalenetricarboxylic acid and 20 g of PVDF were put into DMF and stirred for 3 h to prepare a slurry.

[0071] In the second step, take the PI (polyimide) diaphragm, put it on the glass plate, and then take the slurry prepared in the first step and apply it on the PI diaphragm. Place the coated PI composite diaphragm under a light source of 1000W and 850nm at 120°C for 15 hours.

[0072] The third step is to dissolve 0.5 mol of trimethylsilylethynylbenzene in ethyl acetate and stir evenly, then drop the dissolved solution (concentration is 0.5 mol / L) on the side with the coating material, let it stand for 20 minutes, then put the wetted electrode into an oven and bake it at 250°C in a nitrogen atmosphere for 1 hour, remove the diaphragm and cool it to room temperature to obtain the composite diaphragm.

[0073] Example 10

[0074] This embodiment provides a composite diaphragm, and its composition and specific preparation method are as follows:

[0075] In the first step, 1 mol of ferric acetate, 2 mol of 1,3,7-naphthalenetricarboxylic acid and 20 g of PVDF were put into DMF and stirred for 3 hours to prepare a slurry.

[0076] In the second step, take the PI (polyimide) diaphragm, put it on the glass plate, and then take the slurry prepared in the first step and apply it on the PI diaphragm. Place the coated PI composite diaphragm under a light source of 1000W and 850nm at 120°C for 15 hours.

[0077] The third step is to dissolve 0.5 mol of trimethylsilylethynylbenzene in ethyl acetate and stir evenly, then drop the dissolved solution (concentration is 0.5 mol / L) on the side with the coating material, let it stand for 20 minutes, then put the wetted electrode into an oven and bake it at 250°C in a nitrogen atmosphere for 1 hour, remove the diaphragm and cool it to room temperature to obtain the composite diaphragm.

[0078] Comparative Example 1

[0079] This comparative example provides a membrane which is the same as the PI membrane in Example 1.

[0080] Comparative Example 2

[0081] This comparative example provides a composite diaphragm, which is different from Example 1 only in that the third step is not included in the preparation process, that is, the composite diaphragm does not include an acetylene carbon layer.

[0082] Comparative Example 3

[0083] This comparative example provides a composite membrane, which is different from Example 1 only in that the second step is not included in the preparation process, that is, the composite membrane does not include a MOFs material layer.

[0084] Test Case

[0085] 1. Thickness test: The prepared composite membrane is polished (known method), and the functional layers are distinguished and the thickness of the functional layers is measured by marking elements through SEM and EDS.

[0086] 2. Longitudinal heat shrinkage ratio: the test method is: take the prepared composite diaphragm with an initial test thickness of h1, place it in a 90°C environment and heat it for 1 hour, then let it stand at room temperature and the test thickness is h2. The longitudinal heat shrinkage ratio is X=100%×(h1-h2) / h1.

[0087] 3. Composite membrane porosity: Generally, physical methods are used, which is based on the volume of liquid absorbed by the membrane. The specific steps include: first, weigh the membrane sample before the test, and record the mass of the dry membrane as m1. Then soak the membrane in n-butanol and take it out after 2 hours. Before weighing, gently wipe the liquid on its surface with filter paper, and record the weighed mass as m2. The composite membrane porosity P = 100% × (m2-m1) / ρV, ρ is the density of n-butanol, which is 0.8098 g / cm 3 , V is the volume of the composite diaphragm.

[0088] 4. Electrical performance test:

[0089] (1) Preparation of power button

[0090] Material preparation: Commercially available lithium manganese iron phosphate material and conductive carbon black (SP): 120℃, vacuum drying time ≥10h; polyvinylidene fluoride (PVDF): 60℃, vacuum drying time ≥4h; prepare the battery shell in advance, put it in alcohol, ultrasonically clean it for 30min, blow dry it at 60℃ overnight, and transfer it to the glove box for use; sandwich the diaphragm between weighing paper and use Punch the diaphragm with a punching machine, transfer the punched diaphragm to a vacuum drying oven, bake at 60°C for more than 4h, and then transfer to a glove box for use; Preparation of 6.25wt% PVDF glue: weigh 4.0000±0.0020g of PVDF powder and 60.0000±0.0020g of NMP in proportion, add them to a beaker, and stir with a mechanical stirrer at 500rpm for 3h; pour the prepared PVDF glue into a fluorinated bottle, seal it with a sealing film, and store it in a desiccator; Preparation of 1% CMC glue: weigh 297.000±0.002g of deionized water in a 500mL beaker, add 3.000±0.002g of CMC, and stir with a mechanical stirrer, first at a slow speed and then at a medium speed, and finally adjust to 800rpm. During the stirring process, seal the mouth of the beaker with sealing film, stir for 3 hours until the glue solution is transparent and has no obvious particles, and pour it into a reagent bottle for storage (CMC glue solution needs to be placed for more than 12 hours to ensure that the bubbles in the glue solution are eliminated before use).

[0091] Positive electrode homogenate: add 0.0450g of D300 dispersant, 1.7877±0.0020g of PVDF glue, 2.0000±0.0020g of NMP, 0.1117±0.0005g of SP, 2.0000±0.0005g of lithium iron manganese phosphate powder, 1 large zirconium bead (φ10mm) and 4 small zirconium beads (φ5mm) into a stirring tank; stir for 7min at 1000rpm orbital revolution and 2000rpm rotation conditions, repeat 4-5 times with an interval of 2min.

[0092] Positive electrode coating and baking: Spread a 20μm thick aluminum foil with a width of 11cm flat on the coating platform, and wipe it repeatedly with alcohol to ensure that the surface of the aluminum foil is clean and flat; use a 300μm flat-head scraper to pour the slurry on a 150-mesh screen and let it flow naturally onto the aluminum foil to be coated; then take a medicine spoon and spread it evenly on the middle part of the scraper, press the "Start" button to start coating; remove the scraper and wipe it clean, transfer the coated electrode to a blast drying oven, and dry it at 100±5℃ for 100min and 100±5℃ for 720min; take out the dried electrode and use Punch the positive electrode sheet with a punching machine and weigh its surface density to see if it is within 8.0±0.2mg / cm 2 If it is not qualified, it needs to be re-applied.

[0093] Positive electrode roll punching: cutting 3 pieces The disc coated with the pole piece aluminum foil is weighed and the average value is taken as the mass of the empty aluminum foil. The thickness of the surrounding blank foil is measured three times as the thickness of the empty foil. The roller press is adjusted to the 0.5 scale and rolled to the target compaction density of 2.20±0.05mg / cm 3 , and then cut into For a mm round piece, use a 1 / 100,000 balance to weigh the mass of the pole piece, use a micrometer to measure the thickness data, and record the mass and thickness data.

[0094] Negative electrode slurry: weigh 10.0000±0.0020g graphite powder and 0.1580±0.0020g SP and add them to the stirring tank, stir at 800rpm for 3min, and use a spatula to crush the undispersed SP particles; add 8.0000±0.5000g CMC glue to the stirring tank, stir at 800rpm for 3min, then stir at 2000rpm for 2min, repeat 5 times until the slurry becomes a paste; add the remaining 7.7900±0.5000g CMC glue to the stirring tank, stir at 2000rpm for 2min, repeat 5 times; add 0.4390±0.0050g SBR emulsion and stir at 2000rpm for 3min.

[0095] Negative electrode coating and baking: Spread the matte surface of 8μm copper foil evenly on the coating platform, and wipe it repeatedly with alcohol to ensure that the surface of the copper foil is clean and flat; use a 120μm fixed scraper and 2 layers of 6μm copper foil on both sides (coating area height 132μm), pour the slurry on the middle part of the scraper and press the "Start" button to start coating; remove the scraper and wipe it clean, transfer the coated electrode to a blast drying oven, and dry it at 70±5℃ for 15min; take out the dried electrode and use Punch out three pole pieces and determine whether their surface density is within 4.5±0.5mg / cm 2 If the surface of the electrode is smooth, even, flat and has no burrs on the edge, select the electrode; if it is unqualified, adjust the scraper scale and re-apply.

[0096] Negative electrode rolling and baking: cutting 3 pieces The disc coated with the electrode copper foil is weighed and the average value is taken as the mass of the bare copper foil; the thickness of the surrounding blank foil is measured three times as the thickness of the bare foil;

[0097] Select the appropriate quality of the electrode, use a 16mm punching machine to punch the electrode, weigh and select the qualified electrode, and classify the selected electrode by quality. Cover the punched electrode with copper foil on the top and bottom, and roll it to the target compaction density of 1.60±0.05g / cm 3 , weigh the pole piece again and record the mass and thickness data;

[0098] Transfer the weighed electrode into a vacuum drying oven and dry it under vacuum at 110°C for 12 h.

[0099] Assembly

[0100] The stacking order of assembled batteries is: negative electrode shell → nickel foam → stainless steel gasket → electrolyte → negative electrode plate → diaphragm (composite diaphragm or diaphragm provided in each embodiment and comparative example) → electrolyte → positive electrode plate → positive electrode shell → packaging;

[0101] Battery assembly steps and requirements:

[0102] Transfer the electrode to the glove box and place the positive and negative electrode shells of the button battery on dust-free paper for later use;

[0103] Arrange the negative electrode shells in a row, add nickel foam and stainless steel gaskets (convex side facing up) in turn, add 3 drops of electrolyte with a 5mL dropper, the current collector direction of the negative electrode sheet is close to the gasket, and the diaphragm is placed in the middle (note to separate the weighing paper from the diaphragm); use a 5mL dropper to add 15 drops of electrolyte, put in the positive electrode sheet to ensure that the active material side is facing down and the electrode sheet is completely soaked; buckle the positive electrode shell with insulated tweezers, transfer the battery to the sealing machine, and apply 850kg pressure to seal; remove the packaged battery from the sealing machine, wipe the residual electrolyte on the battery and the sealing machine with dust-free paper; number the batteries, transfer them out of the glove box, wipe them with alcohol and put them into a ziplock bag, test the open circuit voltage of the battery with a voltage internal resistance meter, and select batteries with an open circuit voltage of about 0.2V for testing.

[0104] (2) 50-cycle capacity retention and rate performance: The button cells corresponding to the above-prepared embodiments and comparative examples were tested (nominal capacity 150 mAh / g); charged to 4.3 V at 0.1 C, then discharged to 3.0 V at 0.1 C, charged to 4.3 V at 0.5 C, then discharged to 3.0 V at 1 C, and the ratio of the discharge gram capacity under 1 C to 0.1 C conditions was recorded; then a charge-discharge cycle of 0.5 C charge / 1 C discharge was performed for 50 cycles, and the cycle capacity retention was recorded; the battery was disassembled after 50 cycles to obtain the negative electrode sheet, and its Mn element content was tested. The results of the above electrical performance tests are recorded in Table 1 below.

[0105] (4) Manganese dissolution test method: The negative electrode sheet after 50 cycles is disassembled to test the Mn element content, specifically: 1. The cycled battery is disassembled on a disassembly machine; 2. In a fume hood, use a clean measuring cylinder to take 30 ml of concentrated hydrochloric acid and introduce it into a 250 ml glass beaker. Use a clean measuring cylinder to measure 10 ml of concentrated nitric acid and stir it continuously with a glass rod while pouring. It can be seen that the solution quickly turns yellow and the reaction is violent. When the solution temperature drops to room temperature, move it into a brown reagent bottle and cover it with a lid; 3. Use tweezers to take the negative electrode from the glass bottle and weigh it, record the mass, place the electrode in a conical flask, add deionized water, stir and heat it with a magnetic stirrer to dissolve the electrode, and evaporate the water by vacuum drying. Take the newly prepared aqua regia and add it to the conical flask for digestion, stir and heat it with a magnetic stirrer, and filter it with filter paper after the solution is cooled; 4. ICP test: draw a working curve with a standard solution, test the spectral line intensity of the sample solution, and obtain the concentration of the Mn element in the solution on the standard curve. Enter the sample batch number and volume 50mL, enter the correction factor 1000, and the other parameters are 1. The computer automatically gives the result.

[0106] The specific test results are shown in the table below:

[0107] Table 1

[0108]

[0109] From the data in the above table, it can be seen that the comparison between the embodiment and the comparative example shows that the composite diaphragm prepared in the embodiment of the present application has greatly improved cycle performance, Mn dissolution amount and rate performance compared with ordinary diaphragms.

[0110] Compared with Example 1 and Example 2, it can be seen that when too much PVDF is added in the first step, the porosity of the diaphragm will be reduced, resulting in a decrease in the rate performance. Compared with Example 3, it can be seen that a decrease in the amount of PVDF added will lead to a decrease in the bonding force between the self-grown MOFs structure and the diaphragm, thereby reducing its stability and causing poor performance.

[0111] By comparing Example 1 with Example 4, it can be seen that the wavelength used in the second step is too low to produce a high-energy reaction, resulting in a relatively unstable MOFs framework structure, which in turn leads to poor performance. By comparing with Example 5, it can be seen that the wavelength is too high, resulting in excessive light, which causes partial collapse of the MOFs framework structure, resulting in poor performance.

[0112] By comparing Example 1 with Example 6, it can be seen that the baking temperature used in the third step is too high, resulting in shrinkage of the base film, which will affect the bonding between the MOFs material layer, the acetylene carbon layer and the base film, thereby resulting in poor performance. By comparing with Example 7, it can be seen that the heat treatment (baking) temperature is too low, resulting in the inability to completely generate acetylene carbon and incomplete encapsulation of the MOFs material layer, thereby resulting in poor cycle performance.

[0113] By comparing Example 1 with Example 8, it can be seen that the adsorption performance of Zr-MOFs and Co-MOFs for metal Mn ions is equivalent. By comparing with Example 9, it can be seen that when the ligand framework increases, but within a reasonable range, the framework structure channel increases, and the metal ion adsorption and rate performance are improved. By comparing with Example 10, it can be seen that the adsorption capacity of Zr-MOFs for Mn ions is slightly worse than that of Fe-MOFs, but the rate performance is equivalent.

[0114] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.

Claims

1. A composite diaphragm, characterized in that: include: Basement membrane; A MOFs material layer is located on one side surface of the base film; The acetylene carbon layer is located on a surface of the MOFs material layer that is away from the base film.

2. The composite diaphragm according to claim 1, characterized in that: The thickness of the MOFs material layer is 1 μm-7 μm; optionally, 2 μm-5 μm.

3. The composite diaphragm according to claim 1, characterized in that: The thickness of the acetylene carbon layer is 1.5 μm-6.5 μm; optionally, 3 μm-6 μm; And / or, the composite membrane has a thickness of 10 μm-21 μm.

4. The composite diaphragm according to any one of claims 1 to 3, characterized in that: The longitudinal heat shrinkage ratio X of the composite diaphragm is 0.1%-1.3%; optionally 0.1%-0.5%; And / or, the porosity P of the composite membrane is 8%-30%.

5. A method for preparing the composite diaphragm according to any one of claims 1 to 4, characterized in that: The steps include: S1, mixing a metal salt, an organic ligand, a binder and an organic solvent to obtain a slurry; S2, coating the slurry onto the surface of the base film to perform a self-assembly reaction to form a MOFs material layer on the surface of the base film; S3, dissolving an organic compound containing an acetylene group in ethyl acetate to obtain a mixed solution, coating the mixed solution on the surface of the MOFs material layer, allowing it to stand, and heat treating it to obtain the composite diaphragm.

6. The method for preparing the composite diaphragm according to claim 5, characterized in that: In step S1, the metal salt includes at least one of ZrCl4, FeCl3, NiCl, CuNO3, ZnNO3, FeNO3, CoCl2, cobalt acetate, iron acetate, and nickel acetate; And / or, the organic ligand includes at least one of 2,4-dihydroxybiphenyl dicarboxylic acid, 4,4'-biphenyl dicarboxylic acid, 2,3-diaminoterephthalic acid, 1,3,7-naphthalenetricarboxylic acid, 2(4-chlorophenylthio)phenylacetic acid, 2-nitrotrimesic acid, 3-phosphobenzoic acid, 6-(dimethylamino)-2-naphthoic acid, 4-methylphosphonic acid, 4,6-dinitro-1,3-benzenedicarboxylic acid, anthraquinone-1-carboxylic acid, 3,4-diaminophenylacetic acid, 12-amino-5(dimethylamino)benzoic acid, and 5-(dimethylamino)-2-nitrobenzoic acid; and / or, the molar ratio of the metal salt to the organic ligand is 1-3; And / or, the binder includes at least one of PVDF, PMMA, and PTFE; And / or, the organic solvent includes at least one of N,N-dimethylformamide, N-hexylpyrrolidone, and N-methylpyrimidine; And / or, the binder accounts for 0.2%-11% of the total mass of the metal salt and the organic ligand, and optionally 2%-5%.

7. The method for preparing a composite diaphragm according to claim 5, characterized in that: In step S2, the conditions of the self-assembly reaction include: temperature of 120°C-180°C; illumination power of 1000-2000W; illumination wavelength of 100-2000nm, optionally 800-1600nm; illumination time of 12-16h.

8. The method for preparing a composite diaphragm according to any one of claims 5 to 7, characterized in that: The organic compound containing acetyl groups includes at least one of 4-ethynyl-1,2-phenylenediamine, 3-ethynyl-1,2-phenylenediamine, ethynylcyclohexanol, 4-ethynylbenzoic acid, phenylacetylene, 4-ethynylaniline, 1,3,6,8-tetra(ethynyl)pyrene, 3-ethynylpyridine, ethynylcyclohexanol, 1-ethynylcyclopentanol, and 1-ethynyl-4-methylbenzene; and / or, the concentration of the organic compound containing acetylene groups in the mixed solution is 0.5-1 mol / L; And / or, the standing time is 10-20 min; And / or, the heat treatment temperature is 100°C-350°C, optionally 200°C-280°C, and the time is 1-2h; And / or, the heat treatment is performed under a protective atmosphere.

9. A secondary battery, characterized in that: The invention comprises the composite diaphragm described in claims 1 to 4 or the composite diaphragm prepared by the preparation method described in any one of claims 5 to 8.

10. An electrical device, characterized in that: A secondary battery comprising the secondary battery according to claim 9.

Citation Information

Patent Citations

  • MOF composite material and preparation method and application thereof

    CN113871598A

  • Coating diaphragm based on MOF material and preparation method thereof

    CN115954616A