Perovskite light absorption layer, preparation method and perovskite solar cell
By using passivating agents such as stearic acid and its salts, quaternary ammonium compounds and amino acid type zwitterionic surfactants in perovskite solar cells, the problem of insufficient efficiency and stability of perovskite solar cells has been solved, and the problem of insufficient efficiency and stability of perovskite solar cells has been achieved. Higher photoelectric conversion efficiency and better stability.
Patent Information
- Application Number
- CN202310663974.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-06
- Publication Date
- 2024-12-06
AI Technical Summary
The efficiency and stability of existing perovskite solar cells are insufficient, which affects their commercial applications.
Using passivating agents, such as stearic acid and its salts, quaternary ammonium compounds and amino acid-type zwitterionic surfactants, improve the defects and environment of the perovskite layer by combining their hydrophilic and hydrophobic groups with the perovskite layer. Stability, improve the device efficiency and stability of perovskite solar cells.
Through the use of passivating agent, the photoelectric conversion efficiency and stability of perovskite solar cells are significantly improved, the service life of the equipment is extended and the defect density is reduced.
Smart Images

Figure CN119095392A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solar cell devices, and in particular to a perovskite light absorbing layer, a preparation method and a perovskite solar cell. Background Art
[0002] At present, the efficiency of perovskite solar cells has reached 25.6%, which is close to the silicon-based solar cells that have been mature for many years. Improving the efficiency and stability of the device are important aspects of realizing the commercialization of perovskite solar cells. Summary of the invention
[0003] The main technical problem solved by this application is the need to improve the device efficiency and stability of perovskite solar cells.
[0004] In order to solve the above technical problems, a technical solution adopted in the present application is: a perovskite light-absorbing layer, comprising a perovskite layer and a passivator, wherein the passivator comprises one or more of stearic acid and its salts, quaternary ammonium compounds, and amino acid type zwitterionic surfactants.
[0005] In one or more embodiments of the present application, a perovskite light-absorbing layer is provided, defects in the perovskite layer are passivated by the hydrophilic groups of the passivator, and the environmental stability of the perovskite layer is improved by the hydrophobic groups of the passivator, so as to improve the device efficiency and stability of the perovskite solar cell.
[0006] Specifically, the hydrophilic groups of the passivators provided in the embodiments of the present application include but are not limited to atoms with lone pairs of electrons such as O, N, S, and P, so that the hydrophilic groups are easily combined with the defects of the perovskite layer, thereby increasing the passivation ability of the perovskite layer. The passivators provided in the embodiments of the present application include but are not limited to hydrophobic groups such as non-polar alkyl chains, aromatic groups, or fluorine-containing long chains, which can serve as a protective layer to hinder the entry of water molecules and improve the environmental stability of the perovskite layer. Therefore, the embodiments of the present application introduce a passivator into the perovskite layer, which can simultaneously improve the device efficiency and stability of the perovskite solar cell.
[0007] In some embodiments, stearic acid and its salts include one or more of stearic acid, sodium stearate, magnesium stearate, calcium stearate, lead stearate, aluminum stearate, cadmium stearate, iron stearate, potassium stearate, and hydroxystearic acid.
[0008] In one or more embodiments of the present application, the hydrophilicity of the acyl group (-COO-) of stearic acid and its salts improves the degree of binding with the defects of the perovskite layer, thereby improving the passivation ability of the perovskite layer. The hydrophobicity of the non-polar alkyl chain of stearic acid and its salts prevents water molecules from entering the perovskite layer, thereby improving the environmental stability of the perovskite layer.
[0009] In some embodiments, the quaternary ammonium compound includes one or more of tetrabutylammonium bromide, dodecyltrimethylammonium chloride, hexadecyltrimethylammonium bromide, dioctadecyldimethylammonium bromide, dodecyldimethylbenzylammonium chloride, octadecyldimethylhydroxyethylammonium nitrate, and octadecylbishydroxyethylmethylammonium chloride.
[0010] In one or more embodiments of the present application, the hydrophilicity of the ammonium ions of the quaternary ammonium compound increases the degree of binding with the defects of the perovskite layer, thereby improving the passivation ability of the perovskite layer. The hydrophobicity of the non-polar alkyl chain of the quaternary ammonium compound prevents water molecules from entering the perovskite layer, thereby improving the environmental stability of the perovskite layer.
[0011] In some embodiments, the amino acid zwitterionic surfactant includes N ɑ -Acyl lysine, sodium dodecyl aminopropionate, sodium dodecyl dimethylene amino dicarboxylate, N ɑ -Methyl-N ɑ -Lauroyl lysine, N-acyl sarcosine, di(octylaminoethyl)glycine, N-acyl glutamic acid, N β -Acyl-L-lysine, N ɑ -Dimethyl-N ɑ -acyl lysine, N-acyl glutamic acid, one or more of N-acyl glutamic acid diester.
[0012] In one or more embodiments of the present application, the hydrophilicity of the amine salt type cationic part and the carboxylic acid type anionic part of the amino acid type zwitterionic surfactant improves the degree of binding with the defects of the perovskite layer, thereby improving the passivation ability of the perovskite layer. The hydrophobicity of the non-polar alkyl chain of the amino acid type zwitterionic surfactant prevents water molecules from entering the perovskite layer, thereby improving the environmental stability of the perovskite layer.
[0013] In some embodiments, the passivating agent is dispersed in the perovskite layer.
[0014] In one or more embodiments of the present application, the passivator is dispersed in the perovskite layer so that the passivator acts as a bulk passivator. During the formation of the perovskite layer, the passivator can passivate various defects that may appear in the perovskite layer and improve the hydrophobicity of the perovskite layer, thereby improving the device efficiency and stability of the perovskite solar cell.
[0015] In some embodiments, the passivator forms a passivator modification layer on a surface of the perovskite layer.
[0016] In one or more embodiments of the present application, a passivator modification layer is formed on a surface of the perovskite layer by a passivator to passivate surface defects of the perovskite layer and improve the hydrophobicity of the perovskite layer.
[0017] In some embodiments, the passivator includes a first passivator and a second passivator; the first passivator is dispersed in the perovskite layer, and the second passivator forms a passivator modification layer on a surface of the perovskite layer.
[0018] In one or more embodiments of the present application, a first passivator is dispersed in the perovskite layer, and a second passivator is formed on at least one surface of the perovskite layer. The first passivator acts as a bulk passivator to passivate various defects that may appear in the perovskite layer, and the second passivator acts as an interface passivator to passivate interface defects between the perovskite layer and the charge transfer layer, thereby improving the hydrophobicity of the perovskite layer and enhancing the photoelectric conversion efficiency and stability of the perovskite solar cell.
[0019] In some embodiments, the perovskite layer has a thickness of 300 nm to 700 nm.
[0020] In one or more embodiments of the present application, by providing some specific thicknesses of the perovskite layer, the perovskite layer has good photoelectric conversion efficiency within the thickness range.
[0021] In some embodiments, the thickness of the passivating agent modification layer is 10 nm to 50 nm.
[0022] In one or more embodiments of the present application, by providing some specific thicknesses of the passivator modified layers, the passivator modified layers within this thickness range have, on the one hand, good passivation effects and hydrophobic properties for the perovskite layer, and on the other hand, have little effect on the photoelectric conversion efficiency of the perovskite layer.
[0023] In some embodiments, the material of the perovskite layer includes ABX3 or A2CDX6, wherein A is an inorganic or organic or organic-inorganic mixed cation; B is an inorganic or organic or organic-inorganic mixed cation; C is an inorganic or organic or organic-inorganic mixed cation; D is an inorganic or organic or organic-inorganic mixed cation; and X is an inorganic or organic or organic-inorganic mixed anion.
[0024] In one or more embodiments of the present application, a specific perovskite layer material is provided, which together with the passivator provided in the present application forms a perovskite light absorption layer, and the device efficiency and stability of the perovskite solar cell are improved by passivating various defects that may appear in the perovskite layer and / or passivating the interface defects between the perovskite layer and the charge transfer layer.
[0025] In a second aspect, an embodiment of the present application provides a method for preparing a perovskite light absorbing layer, comprising:
[0026] Coating a perovskite precursor solution containing a passivator on the first carrier transport layer; wherein the passivator includes one or more of stearic acid and its salts, quaternary ammonium compounds, and amino acid type zwitterionic surfactants;
[0027] The perovskite precursor solution containing the passivating agent is annealed.
[0028] In one or more embodiments of the present application, by providing a method for preparing a perovskite light absorbing layer, the passivator can uniformly passivate various defects that may appear in the perovskite layer during the formation of the perovskite layer, thereby improving the quality and performance stability of the perovskite layer.
[0029] In some embodiments, the amount of the passivating agent added to the perovskite precursor solution containing the passivating agent is 0.1 mg / mL-1 mg / mL.
[0030] In one or more embodiments of the present application, the amount of any passivator added to the perovskite precursor solution is within the protection scope of the present application. In one or more embodiments of the present application, the amount of the passivator added to the perovskite precursor solution containing the passivator is within the range of 0.1 mg / mL-1 mg / mL, and the defects of the formed perovskite layer are reduced and the quality is improved, which effectively improves the device efficiency and stability of the perovskite solar cell.
[0031] In a third aspect, an embodiment of the present application provides a method for preparing a perovskite light absorbing layer, comprising:
[0032] forming a perovskite layer on the first carrier transport layer;
[0033] A passivating agent solution is coated on the surface of the perovskite layer away from the first carrier transport layer; wherein the passivating agent comprises one or more of stearic acid and its salts, quaternary ammonium compounds, and amino acid type zwitterionic surfactants;
[0034] The passivating agent solution is annealed to form a passivating agent modification layer.
[0035] In one or more embodiments of the present application, a method for preparing a perovskite light absorbing layer is provided, and the formed perovskite light absorbing layer includes a perovskite layer and a passivator modified layer, which passivates the interface defects between the perovskite layer and the carrier transport layer, reduces the defect density of the perovskite layer, and improves the device efficiency and stability of the perovskite solar cell.
[0036] In some embodiments, the concentration of the passivating agent solution is 0.1 mg / ml-10 mg / ml.
[0037] In one or more embodiments of the present application, the concentration of any passivator solution is within the protection scope of the present application. In one or more embodiments of the present application, the concentration of the passivator solution is in the range of 0.1 mg / mL-10 mg / mL, which has a good effect of passivating the interface defects between the perovskite layer and the carrier transport layer, and effectively improves the device efficiency and stability of the perovskite solar cell.
[0038] In some embodiments, forming a perovskite layer on the first carrier transport layer includes:
[0039] coating a perovskite precursor solution containing a passivating agent on the first carrier transport layer;
[0040] The perovskite precursor solution containing the passivating agent is annealed.
[0041] In one or more embodiments of the present application, by providing a method for forming a perovskite layer on a first carrier transport layer, the passivator can uniformly passivate various defects that may appear in the perovskite layer during the formation of the perovskite layer, thereby improving the quality and performance stability of the perovskite layer.
[0042] In some embodiments, the amount of the passivating agent added to the perovskite precursor solution containing the passivating agent is 0.1 mg / mL-1 mg / mL.
[0043] In one or more embodiments of the present application, the concentration of any passivator solution is within the protection scope of the present application. In one or more embodiments of the present application, the concentration of the passivator solution is in the range of 0.1 mg / mL-1 mg / mL, which has a good effect of passivating the interface defects between the perovskite layer and the carrier transport layer, and effectively improves the device efficiency and stability of the perovskite solar cell.
[0044] In a fourth aspect, an embodiment of the present application provides a perovskite solar cell, comprising a substrate, a first electrode layer, a first carrier transport layer, a perovskite light absorption layer, a second carrier transport layer and a second electrode layer stacked in sequence; wherein the perovskite light absorption layer is any of the perovskite light absorption layers provided in the first aspect, or the perovskite light absorption layer is a perovskite light absorption layer prepared by any of the methods provided in the second aspect or the third aspect.
[0045] In one or more embodiments of the present application, some specific structures of perovskite solar cells are provided, wherein the perovskite light absorption layer is any perovskite light absorption layer provided in the first aspect to the third aspect, which is beneficial to improving the device efficiency and stability of the perovskite solar cell.
[0046] In some embodiments, the perovskite light absorption layer is some perovskite light absorption layer provided in the first aspect, or the perovskite light absorption layer is a perovskite light absorption layer prepared by any method provided in the third aspect; the passivator modification layer is arranged on the surface of the perovskite layer away from the first carrier transport layer.
[0047] In one or more embodiments of the present application, some specific structures of perovskite solar cells are provided, wherein the perovskite light absorption layer is some perovskite light absorption layer provided in the first aspect or the perovskite light absorption layer is a perovskite light absorption layer prepared by any method provided in the third aspect, which is beneficial to improving the device efficiency and stability of the perovskite solar cell.
[0048] In some embodiments, the material of the perovskite layer includes ABX3 or A2CDX6, wherein A is an inorganic or organic or organic-inorganic mixed cation; B is an inorganic or organic or organic-inorganic mixed cation; C is an inorganic or organic or organic-inorganic mixed cation; D is an inorganic or organic or organic-inorganic mixed cation; X is an inorganic or organic or organic-inorganic mixed anion.
[0049] In one or more embodiments of the present application, a specific perovskite layer material is provided, which together with the passivator provided in the present application forms a perovskite light absorption layer, and the device efficiency and stability of the perovskite solar cell are improved by passivating various defects that may appear in the perovskite layer and / or passivating the interface defects between the perovskite layer and the charge transfer layer.
[0050] In a fifth aspect, an embodiment of the present application provides a photovoltaic module, comprising any perovskite solar cell provided in the fourth aspect.
[0051] In the embodiment of the present application, the photovoltaic module includes a plurality of battery strings, each of which includes a plurality of perovskite solar cells connected in series through connectors such as welding strips. In addition to the battery strings, the photovoltaic module also includes front glass, front encapsulation film, back encapsulation film, back glass, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0052] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments of the present application will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the drawings without paying creative work.
[0053] Figure 1 is a schematic structural diagram of a perovskite solar cell provided in an embodiment of the present application;
[0054] Figure 2 It is a schematic diagram of the structure of a photovoltaic module provided in an embodiment of the present application.
[0055] In the drawings, the drawings are not drawn to scale.
[0056] Marking Description:
[0057] 1000-photovoltaic module, 100-perovskite solar cell, 200-cell string, 300-front glass, 400-front encapsulation film, 500-back encapsulation film, 600-back glass, 10-substrate, 20-first electrode layer, 30-electron transport layer, 40-perovskite light absorption layer, 50-hole transport layer, 60-second electrode layer. DETAILED DESCRIPTION
[0058] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0059] The terms "first", "second", "third" in this application are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. Thus, the features defined as "first", "second", "third" can expressly or implicitly include at least one of the features. In the description of this application, the meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined. In the embodiments of this application, all directional indications (such as up, down, left, right, front, back...) are only used to explain the relative position relationship, movement, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication also changes accordingly. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device comprising a series of steps or units is not limited to the steps or units listed, but optionally also includes steps or units that are not listed, or optionally also includes other steps or units inherent to these processes, methods, products or devices.
[0060] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0061] In some existing schemes, a stabilizer is doped during the formation of the perovskite layer, and the sulfonic, mercapto, carboxyl or ammonium functional groups of the stabilizer are combined with the defects of the perovskite to reduce the defects of the perovskite film layer and improve the stability of the perovskite film layer. In the above method, the presence of the stabilizer in the process of perovskite film flushing will affect the crystallization of the perovskite film, easily produce uncontrollable crystal morphology, and thus affect the device performance.
[0062] The embodiments of the present application provide a perovskite light-absorbing layer, a preparation method, and a perovskite solar cell, which passivate defects in the perovskite layer through the hydrophilic groups of the passivator, and improve the environmental stability of the perovskite layer through the hydrophobic groups of the passivator, so as to improve the device efficiency and stability of the perovskite solar cell.
[0063] The technical solution described in the embodiments of the present application is applicable to the perovskite light absorbing layer, the preparation method and the perovskite solar cell. The perovskite solar cell disclosed in the present application that can be used to prepare the stacked layer can also be used to prepare the stacked silicon-perovskite cell.
[0064] The present application is described in detail below with reference to the accompanying drawings and embodiments.
[0065] In a first aspect, an embodiment of the present application provides a perovskite light-absorbing layer, comprising a perovskite layer and a passivator, wherein the passivator comprises one or more of stearic acid and its salts, quaternary ammonium compounds, and amino acid-type zwitterionic surfactants.
[0066] In the embodiments of the present application, the perovskite light-absorbing layer represents the core component of the perovskite solar cell, which is used to absorb the photon energy of sunlight, generate electron-hole pairs, and separate the electron-hole pairs into free electrons and holes under the action of the built-in electric field. The holes are collected by the first electrode layer through the hole transport layer, and the electrons are collected by the second electrode layer through the electron transport layer. The first electrode layer and the second electrode layer are connected to form a circuit to generate photocurrent. The perovskite layer represents a layered structure formed by the perovskite material. The perovskite material refers to a material having the same crystal structure as CaTiO3, which presents a cubic crystal phase in a stable state and is used as the main forming material of the perovskite light-absorbing layer. The passivator refers to a substance that is added in a small amount to passivate the perovskite bulk phase or interface. Stearic acid and its salts represent stearic acid and stearates. The molecular formula of stearic acid is C 18 H 36O2, stearate refers to a compound in which the hydrogen of the carboxyl functional group of stearic acid is replaced by a metal element. Stearic acid and its salts have an acyl group (-COO-) as a hydrophilic group and a non-polar alkyl chain as a hydrophobic group. Quaternary ammonium compounds are compounds in which all four hydrogen atoms in the ammonium ion are replaced by hydrocarbon groups, and the general molecular formula is R4NX, where R is a hydrocarbon group and X is a halogen ion acid radical or a hydroxide radical. The ammonium ion of the quaternary ammonium compound serves as a hydrophilic group and the non-polar hydrocarbon group serves as a hydrophobic group. The general molecular formula of amino acid type zwitterionic surfactants is R-NH + -(CH2)n-COO-, wherein R is a hydrocarbon group. The amino acid type zwitterionic surfactant has an amine salt type cation part and a carboxylic acid type anion part as a hydrophilic group, and has a non-polar alkyl chain as a hydrophobic group.
[0067] In one or more embodiments of the present application, a perovskite light-absorbing layer is provided, defects in the perovskite layer are passivated by the hydrophilic groups of the passivator, and the environmental stability of the perovskite layer is improved by the hydrophobic groups of the passivator, so as to improve the device efficiency and stability of the perovskite solar cell.
[0068] Specifically, the hydrophilic groups of the passivators provided in the embodiments of the present application include but are not limited to atoms with lone pairs of electrons such as O, N, S, and P, so that the hydrophilic groups are easily combined with the defects of the perovskite layer, thereby increasing the passivation ability of the perovskite layer. The passivators provided in the embodiments of the present application include but are not limited to hydrophobic groups such as non-polar alkyl chains, aromatic groups, or fluorine-containing long chains, which can serve as a protective layer to hinder the entry of water molecules and improve the environmental stability of the perovskite layer. Therefore, the embodiments of the present application introduce a passivator into the perovskite layer, which can simultaneously improve the device efficiency and stability of the perovskite solar cell.
[0069] In some embodiments, stearic acid and its salts include one or more of stearic acid, sodium stearate, magnesium stearate, calcium stearate, lead stearate, aluminum stearate, cadmium stearate, iron stearate, potassium stearate, and hydroxystearic acid.
[0070] In the embodiments of the present application, the molecular formula of stearic acid is C 18 H 36 O2, stearate refers to a compound in which the hydrogen of the carboxyl functional group of stearic acid is replaced by a metal element. The molecular formula of sodium stearate is C 17 H 35 COONa. The molecular formula of magnesium stearate is C 36 H 70 MgO4. The molecular formula of calcium stearate is C 36 H 70 CaO4. The molecular formula of lead stearate is C 36 H 70 O4Pb. The molecular formula of aluminum stearate is C54 H 105 AlO6. The molecular formula of cadmium stearate is C 36 H 70 CdO4. The molecular formula of iron stearate is C 54 H 105 FeO6. The molecular formula of potassium stearate is C 18 H 35 KO2. The molecular formula of hydroxystearic acid is C 18 H 36 O3.
[0071] In one or more embodiments of the present application, the hydrophilicity of the acyl group (-COO-) of stearic acid and its salts improves the degree of binding with the defects of the perovskite layer, thereby improving the passivation ability of the perovskite layer. The hydrophobicity of the non-polar alkyl chain of stearic acid and its salts prevents water molecules from entering the perovskite layer, thereby improving the environmental stability of the perovskite layer.
[0072] In some embodiments, the quaternary ammonium compound includes one or more of tetrabutylammonium bromide, dodecyltrimethylammonium chloride, hexadecyltrimethylammonium bromide, dioctadecyldimethylammonium bromide, dodecyldimethylbenzylammonium chloride, octadecyldimethylhydroxyethylammonium nitrate, and octadecylbishydroxyethylmethylammonium chloride.
[0073] In the embodiments of the present application, the molecular formula of tetrabutylammonium bromide is CH BrN. The molecular formula of dodecyltrimethylammonium chloride is C 15 H 34 ClN. The molecular formula of hexadecyltrimethylammonium bromide is C 19 H 42 BrN. The molecular formula of dioctadecyldimethylammonium bromide is [CH3(CH2) 11 ]2N(CH3)2(Br). The molecular formula of dodecyl dimethyl benzyl ammonium chloride is C6H5CH2N(CH3)2C n H 2n+1 Cl (n = 8, 10, 12, 14, 16 or 18). The molecular formula of octadecyl dimethyl hydroxyethyl ammonium nitrate is C 22 H 48 N2O5. The molecular formula of octadecyl dihydroxyethyl methyl ammonium chloride is C 21 H 46 ClNO2.
[0074] In one or more embodiments of the present application, the hydrophilicity of the ammonium ions of the quaternary ammonium compound increases the degree of binding with the defects of the perovskite layer, thereby improving the passivation ability of the perovskite layer. The hydrophobicity of the non-polar alkyl chain of the quaternary ammonium compound prevents water molecules from entering the perovskite layer, thereby improving the environmental stability of the perovskite layer.
[0075] In some embodiments, amino acid zwitterionic surfactants include Nα-acyl lysine, sodium dodecylaminopropionate, sodium dodecyl dimethyleneaminodicarboxylate, Nα-methyl-N ɑ -Lauroyl lysine, N-acyl sarcosine, di(octylaminoethyl)glycine, N-acyl glutamic acid, N β -Acyl-L-lysine, N ɑ -Dimethyl-N ɑ -acyl lysine, N-acyl glutamic acid, one or more of N-acyl glutamic acid diester.
[0076] In the embodiments of the present application, N ɑ The molecular formula of -acyl lysine is C8H 16 N2O3. The molecular formula of sodium dodecylaminopropionate is C 15 H 30 NNaO2. The molecular formula of sodium dodecyl dimethylene amino dicarboxylate is C 16 H 29 NNa2O4. ɑ -Methyl-N ɑ -The molecular formula of lauroyl lysine is RCONH(CH2)4CH[ + NH(CH3)]COO - , R is a hydrocarbon group. The molecular formula of N-acylsarcosine is RCONH(CH2CH2COO - )CHCOO - , R is a hydrocarbon group. The molecular formula of di(octylaminoethyl)glycine is C 22 H 47 N3O2. The molecular formula of N-acylglutamic acid is RC6H8NO5, where R is a hydrocarbon group. β The molecular formula of -acyl-L-lysine is RCONH(CH2)4CH( + NH4)COO - . N ɑ -Dimethyl-N ɑ The molecular formula of -acyl lysine is RCONH(CH2)4CH[ + NH(CH3)2]COO - The molecular formula of N-acylglutamic acid is RCONH(CH2CH2COO - )CHCOO - The molecular formula of N-acyl glutamic acid diester is RCONH(CH2CH2COOR)CHCOOR, where R is a hydrocarbon group.
[0077] In one or more embodiments of the present application, the hydrophilicity of the amine salt type cationic part and the carboxylic acid type anionic part of the amino acid type zwitterionic surfactant improves the degree of binding with the defects of the perovskite layer, thereby improving the passivation ability of the perovskite layer. The hydrophobicity of the non-polar alkyl chain of the amino acid type zwitterionic surfactant prevents water molecules from entering the perovskite layer, thereby improving the environmental stability of the perovskite layer.
[0078] In some embodiments, the passivating agent is dispersed in the perovskite layer.
[0079] In one or more embodiments of the present application, the passivator is dispersed in the perovskite layer so that the passivator acts as a bulk passivator. During the formation of the perovskite layer, the passivator can passivate various defects that may appear in the perovskite layer and improve the hydrophobicity of the perovskite layer, thereby improving the device efficiency and stability of the perovskite solar cell.
[0080] In some embodiments, the passivator forms a passivator modification layer on a surface of the perovskite layer.
[0081] In an embodiment of the present application, the passivator is used to modify at least one surface of the perovskite layer to passivate surface defects of the perovskite layer and improve the hydrophobicity of the perovskite layer.
[0082] In one or more embodiments of the present application, a passivator modification layer is formed on a surface of the perovskite layer by a passivator to passivate surface defects of the perovskite layer and improve the hydrophobicity of the perovskite layer.
[0083] In some embodiments, the passivator includes a first passivator and a second passivator. The first passivator is dispersed in the perovskite layer, and the second passivator forms a passivator modification layer on a surface of the perovskite layer.
[0084] In one or more embodiments of the present application, a first passivator is dispersed in the perovskite layer, and a second passivator is formed on at least one surface of the perovskite layer. The first passivator acts as a bulk passivator to passivate various defects that may appear in the perovskite layer, and the second passivator acts as an interface passivator to passivate interface defects between the perovskite layer and the charge transfer layer, thereby improving the hydrophobicity of the perovskite layer and enhancing the photoelectric conversion efficiency and stability of the perovskite solar cell.
[0085] In some embodiments, the perovskite layer has a thickness of 300 nm to 700 nm.
[0086] In the embodiments of the present application, the thickness of any perovskite layer is within the protection scope of the present application. In one or more embodiments of the present application, the thickness of the perovskite layer is 300nm-700nm. For example, the thickness of the perovskite layer can be 300nm, 400nm, 500nm, 600nm or 700nm, and can also be 350nm, 450nm, 550nm or 650nm, which can be specifically set as needed.
[0087] In one or more embodiments of the present application, by providing some specific thicknesses of the perovskite layer, the perovskite layer has good photoelectric conversion efficiency within the thickness range.
[0088] In some embodiments, the thickness of the passivating agent modification layer is 10 nm to 50 nm.
[0089] In the embodiments of the present application, the thickness of any passivator modified layer is within the scope of protection of the present application. In one or more embodiments of the present application, the thickness of the passivator modified layer is 10nm-50nm. For example, the thickness of the perovskite layer can be 10nm, 20nm, 30nm, 40nm or 50nm, and can also be 15nm, 25nm, 35nm or 45nm, which can be specifically set as needed.
[0090] In one or more embodiments of the present application, by providing some specific thicknesses of the passivator modified layers, the passivator modified layers within this thickness range have, on the one hand, good passivation effects and hydrophobic properties for the perovskite layer, and on the other hand, have little effect on the photoelectric conversion efficiency of the perovskite layer.
[0091] In some embodiments, the material of the perovskite layer includes ABX3 or A2CDX6, wherein A is an inorganic or organic or organic-inorganic mixed cation; B is an inorganic or organic or organic-inorganic mixed cation; C is an inorganic or organic or organic-inorganic mixed cation; D is an inorganic or organic or organic-inorganic mixed cation; and X is an inorganic or organic or organic-inorganic mixed anion.
[0092] In the embodiment of the present application, A includes one or more of methylamine MA, formamidine FA, cesium Cs, and rubidium Rb; B includes one or two of lead Pb and tin Sn; C includes silver Ag+; D includes bismuth Bi 3+ 、Antimony Sb 3+ 、Indium 3+ One or more of; X includes one or two of bromine Br or iodine I.
[0093] In one or more embodiments of the present application, a specific perovskite layer material is provided, which together with the passivator provided in the present application forms a perovskite light absorption layer, and the device efficiency and stability of the perovskite solar cell are improved by passivating various defects that may appear in the perovskite layer and / or passivating the interface defects between the perovskite layer and the charge transfer layer.
[0094] In a second aspect, an embodiment of the present application provides a method for preparing a perovskite light absorbing layer, comprising:
[0095] Coating a perovskite precursor solution containing a passivator on the first carrier transport layer; wherein the passivator includes one or more of stearic acid and its salts, quaternary ammonium compounds, and amino acid type zwitterionic surfactants;
[0096] The perovskite precursor solution containing the passivating agent is annealed.
[0097] In the embodiments of the present application, the first carrier transport layer represents one of the hole transport layer and the electron transport layer. The hole transport layer is used to collect and transport holes to achieve effective separation of electrons and holes. The electron transport layer is a functional layer for collecting electrons generated by the perovskite light absorption layer absorbing photons under illumination conditions. "Coating" can be in the form of spin coating, spray coating, blade coating, slit coating or roll-to-roll printing. The perovskite precursor solution represents a liquid with a precursor for forming perovskite as a solute. In one or more embodiments of the present application, the process parameters of annealing are: heat preservation treatment at a temperature of 60°C to 200°C for 10min to 30min. For example, the annealing temperature can be 60°C, 130°C, 165°C, 200°C, and can also be 95°C, 150°C, 180°C, which can be reasonably set as needed. For example, the annealing time can be 10min, 20min, 30min, and can also be 15min, 25min, which can be reasonably set as needed.
[0098] In one or more embodiments of the present application, by providing a method for preparing a perovskite light absorbing layer, the passivator can uniformly passivate various defects that may appear in the perovskite layer during the formation of the perovskite layer, thereby improving the quality and performance stability of the perovskite layer.
[0099] In some embodiments, the amount of the passivator added to the perovskite precursor solution containing the passivator is 0.1 mg / mL-1 mg / mL.
[0100] In one or more embodiments of the present application, the amount of any passivator added to the perovskite precursor solution is within the scope of protection of the present application. In one or more embodiments of the present application, the amount of the passivator added to the perovskite precursor solution containing the passivator is within the range of 0.1 mg / mL-1 mg / mL, the defects of the formed perovskite layer are reduced, the quality is improved, and the device efficiency and stability of the perovskite solar cell are effectively improved. Exemplarily, the amount of the passivator added to the perovskite precursor solution containing the passivator is 0.1 mg / mL, 0.3 mg / mL, 0.5 mg / mL, 0.7 mg / mL, 0.9 mg / mL, 1 mg / mL, and can also be 0.2 mg / mL, 0.4 mg / mL, 0.6 mg / mL, 0.8 mg / mL, which can be reasonably set as needed.
[0101] In a third aspect, an embodiment of the present application provides a method for preparing a perovskite light absorbing layer, comprising:
[0102] forming a perovskite layer on the first carrier transport layer;
[0103] A passivating agent solution is coated on the surface of the perovskite layer away from the first carrier transport layer; wherein the passivating agent comprises one or more of stearic acid and its salts, quaternary ammonium compounds, and amino acid type zwitterionic surfactants;
[0104] The passivating agent solution is annealed to form a passivating agent modification layer.
[0105] In the embodiments of the present application, the first carrier transport layer represents one of the hole transport layer and the electron transport layer. The hole transport layer is used to collect and transport holes to achieve effective separation of electrons and holes. The electron transport layer is a functional layer for collecting electrons generated by the perovskite light absorption layer absorbing photons under illumination conditions. "Coating" can be in the form of spin coating, spray coating, scraping, slit coating or roll-to-roll printing. In one or more embodiments of the present application, the process parameters of annealing are: heat preservation treatment at a temperature of 60°C to 200°C for 10min to 30min. For example, the annealing temperature can be 60°C, 130°C, 165°C, 200°C, and can also be 95°C, 150°C, 180°C, which can be reasonably set as needed. For example, the annealing time can be 10min, 20min, 30min, and can also be 15min, 25min, which can be reasonably set as needed.
[0106] In one or more embodiments of the present application, a method for preparing a perovskite light absorbing layer is provided, and the formed perovskite light absorbing layer includes a perovskite layer and a passivator modified layer, which passivates the interface defects between the perovskite layer and the carrier transport layer, reduces the defect density of the perovskite layer, and improves the device efficiency and stability of the perovskite solar cell.
[0107] In some embodiments, the concentration of the passivating agent solution is 0.1 mg / ml-10 mg / ml.
[0108] In one or more embodiments of the present application, the concentration of any passivator solution is within the protection scope of the present application. In one or more embodiments of the present application, the concentration of the passivator solution is in the range of 0.1 mg / mL-10 mg / mL, which has a good effect of passivating the interface defects between the perovskite layer and the carrier transport layer, and effectively improves the device efficiency and stability of the perovskite solar cell. Exemplarily, the concentration of the passivator solution is 0.1 mg / mL, 2 mg / mL, 4 mg / mL, 6 mg / mL, 8 mg / mL, 10 mg / mL, and can also be 1 mg / mL, 3 mg / mL, 5 mg / mL, 7 mg / mL, 9 mg / mL, which can be reasonably set as needed.
[0109] In some embodiments, forming a perovskite layer on the first carrier transport layer includes:
[0110] coating a perovskite precursor solution containing a passivating agent on the first carrier transport layer;
[0111] The perovskite precursor solution containing the passivating agent is annealed.
[0112] In the embodiments of the present application, the first carrier transport layer represents one of the hole transport layer and the electron transport layer. The hole transport layer is used to collect and transport holes to achieve effective separation of electrons and holes. The electron transport layer is a functional layer for collecting electrons generated by the perovskite light absorption layer absorbing photons under illumination conditions. "Coating" can be in the form of spin coating, spray coating, blade coating, slit coating or roll-to-roll printing. The perovskite precursor solution represents a liquid with a precursor for forming perovskite as a solute. In one or more embodiments of the present application, the process parameters of annealing are: heat preservation treatment at a temperature of 60°C to 200°C for 10min to 30min. For example, the annealing temperature can be 60°C, 130°C, 165°C, 200°C, and can also be 95°C, 150°C, 180°C, which can be reasonably set as needed. For example, the annealing time can be 10min, 20min, 30min, and can also be 15min, 25min, which can be reasonably set as needed.
[0113] In one or more embodiments of the present application, by providing a method for forming a perovskite layer on a first carrier transport layer, the passivator can uniformly passivate various defects that may appear in the perovskite layer during the formation of the perovskite layer, thereby improving the quality and performance stability of the perovskite layer.
[0114] In some embodiments, the amount of the passivator added to the perovskite precursor solution containing the passivator is 0.1 mg / mL-1 mg / mL.
[0115] In one or more embodiments of the present application, the concentration of any passivator solution is within the protection scope of the present application. In one or more embodiments of the present application, the concentration of the passivator solution is in the range of 0.1 mg / mL-1 mg / mL, which has a good effect of passivating the interface defects between the perovskite layer and the carrier transport layer, and effectively improves the device efficiency and stability of the perovskite solar cell. Exemplarily, the concentration of the passivator solution is 0.1 mg / mL, 0.3 mg / mL, 0.5 mg / mL, 0.7 mg / mL, 0.9 mg / mL, 1 mg / mL, and can also be 0.2 mg / mL, 0.4 mg / mL, 0.6 mg / mL, 0.8 mg / mL, which can be reasonably set as needed.
[0116] See also Figure 1 , Figure 1 It is a schematic diagram of the structure of a perovskite solar cell provided in an embodiment of the present application.
[0117] Fourthly, see Figure 1 The embodiment of the present application provides a perovskite solar cell 100, comprising a substrate 10, a first electrode layer 20, a first carrier transport layer 30, a perovskite light absorption layer 40, a second carrier transport layer 50 and a second electrode layer 60 stacked in sequence. The perovskite light absorption layer 40 is any perovskite light absorption layer 40 provided in the first aspect, or the perovskite light absorption layer 40 is a perovskite light absorption layer 40 prepared by any method provided in the second aspect or the third aspect.
[0118] In the embodiment of the present application, the perovskite solar cell 100 is a solar cell using a perovskite semiconductor as a light absorbing material, and belongs to the third generation of solar cells. The substrate 10 is used to carry the first electrode layer 20, the first carrier transport layer 30, the perovskite light absorbing layer 40, the second carrier transport layer 50 and the second electrode layer 60, and to transmit incident light. In some embodiments, the substrate 10 is a light-transmitting material. In some embodiments, the light-transmitting material is transparent conductive glass. The first electrode layer 20 represents an output end of the perovskite solar cell 100. The first carrier transport layer 30 represents a functional layer for collecting electrons or holes generated by the perovskite light absorbing layer 40 absorbing photons under illumination conditions. The perovskite light absorbing layer 40 is used to absorb the photon energy of sunlight, generate electron-hole pairs, and separate the electron-hole pairs into free electrons and holes under the action of the built-in electric field, and the holes are collected by one electrode layer through the hole transport layer, and the electrons are collected by another electrode layer through the electron transport layer. The two electrode layers are connected into a circuit to generate a photocurrent. The second carrier transport layer 50 represents another functional layer for collecting electrons or holes generated by the perovskite light absorption layer 40 absorbing photons under illumination conditions. The second electrode layer 60 represents another output end of the perovskite solar cell 100 and is required to have high conductivity and stability. In some embodiments, one of the first electrode layer 20 and the second electrode layer 60 is a light-transmitting material.
[0119] In one or more embodiments of the present application, some specific structures of perovskite solar cells 100 are provided, wherein the perovskite light absorption layer 40 is any perovskite light absorption layer 40 provided in the first aspect to the third aspect, which is beneficial to improving the device efficiency and stability of the perovskite solar cell 100.
[0120] In some embodiments, the perovskite light absorption layer 40 is some perovskite light absorption layer 40 provided in the first aspect, or the perovskite light absorption layer 40 is a perovskite light absorption layer 40 prepared by any method provided in the third aspect; the passivator modification layer is arranged on the surface of the perovskite layer away from the first carrier transport layer 30.
[0121] In one or more embodiments of the present application, some specific structures of perovskite solar cells 100 are provided, wherein the perovskite light absorption layer 40 is some perovskite light absorption layer 40 provided in the first aspect or the perovskite light absorption layer 40 is a perovskite light absorption layer 40 prepared by any method provided in the third aspect, which is beneficial to improving the device efficiency and stability of the perovskite solar cell 100.
[0122] In some embodiments, the material of the perovskite layer includes ABX3 or A2CDX6, wherein A is an inorganic or organic or organic-inorganic mixed cation; B is an inorganic or organic or organic-inorganic mixed cation; C is an inorganic or organic or organic-inorganic mixed cation; D is an inorganic or organic or organic-inorganic mixed cation; X is an inorganic or organic or organic-inorganic mixed anion.
[0123] In the embodiment of the present application, A includes one or more of methylamine MA, formamidine FA, cesium Cs, and rubidium Rb; B includes one or two of lead Pb and tin Sn; C includes silver Ag+; D includes bismuth Bi 3+ 、Antimony Sb 3+ 、Indium 3+ One or more of; X includes one or two of bromine Br or iodine I.
[0124] In one or more embodiments of the present application, a specific perovskite layer material is provided, which together with the passivator provided in the present application forms a perovskite light absorption layer 40, and the device efficiency and stability of the perovskite solar cell 100 are improved by passivating various defects that may appear in the perovskite layer and / or passivating the interface defects between the perovskite layer and the charge transfer layer.
[0125] See also Figure 2 , Figure 2 It is a schematic diagram of the structure of a photovoltaic module provided in an embodiment of the present application.
[0126] Fifth, see Figure 2 An embodiment of the present application provides a photovoltaic module 1000, comprising any perovskite solar cell 100 provided in the fourth aspect.
[0127] In the embodiment of the present application, the photovoltaic module 1000 represents an integral module including a plurality of perovskite solar cells 100. The photovoltaic module 1000 includes a plurality of cell strings 200, each of which includes a plurality of perovskite solar cells 100 connected in series via connectors such as welding ribbons.
[0128] In the photovoltaic module 1000, in addition to the cell string 200, it also includes a front glass 300, a front encapsulation film 400, a back encapsulation film 500, a back glass 600, etc. As an example, the photovoltaic module 1000 includes the front glass 300, the front encapsulation film 400, the cell string 200, the back encapsulation film 500, and the back glass 600 which are sequentially stacked and distributed along the thickness direction.
[0129] The features and performance of the present application are further described in detail below in conjunction with the embodiments.
[0130] Example 1
[0131] A perovskite solar cell 100 is prepared, comprising the following steps:
[0132] Step (1), ultrasonically clean the substrate 10 with anhydrous ethanol, acetone, and isopropanol in sequence, and blow dry.
[0133] Step (2), treating the cleaned substrate 10 with ultraviolet ozone for 10 min-20 min to prepare the first electrode layer 20.
[0134] Step (3), preparing the first carrier transport layer 30: spin coating SnO2 colloidal solution on the prepared first electrode layer 20 at a rate of 4000 rpm, and annealing on a hot plate at 150°C for 10 minutes.
[0135] Step (4), preparing the perovskite light absorbing layer 40: spin coating the perovskite precursor solution containing the passivator on the surface of the first carrier transport layer 30 away from the first electrode layer 20 at a rate of 4000 rpm for 15 seconds, adding 600 μL of chlorobenzene as an anti-solvent at the 10th second after the spin coating, annealing on a 100°C hot stage for 60 minutes, and obtaining a perovskite light absorbing layer 40 with a thickness of 500 nm. The perovskite precursor solution containing the passivator is prepared by adding 705.34 mg of PbI2, 240.8 mg of FAI, 33.78 mg of MACl and 0.1 mg of stearic acid to 100 μL of DMSO (dimethyl sulfoxide) and 900 μL of DMF (N,N-dimethylformamide), and stirring for 8h-12h.
[0136] Step (5), preparing the second carrier transport layer 50: spin coating the spiro-OMeTAD and Li-TFSI solution on the surface of the perovskite light absorbing layer 40 away from the first carrier transport layer 30 at a rate of 4000 rpm, annealing on a 150°C hot stage for 10 min, and obtaining a second carrier transport layer 50 with a thickness of about 100 nm.
[0137] Step (6), preparing the second electrode layer 60: placing the thin film prepared with the second carrier transport layer 50 in a vacuum environment, and evaporating Au atoms on the surface of the second carrier transport layer 50 at a rate of 0.1 A / s to form a second electrode layer 60 with an average thickness of 80 nm.
[0138] Example 2
[0139] This embodiment provides a method for preparing a perovskite solar cell 100, which is different from the embodiment 1 in that:
[0140] In the perovskite precursor solution containing the passivator in step (4), the amount of stearic acid added is 0.3 mg.
[0141] The rest are the same as in Example 1.
[0142] Example 3
[0143] This embodiment provides a method for preparing a perovskite solar cell 100, which is different from the embodiment 1 in that:
[0144] In the perovskite precursor solution containing the passivator in step (4), the amount of stearic acid added is 0.5 mg.
[0145] The rest are the same as in Example 1.
[0146] Example 4
[0147] This embodiment provides a method for preparing a perovskite solar cell 100, which is different from the embodiment 1 in that:
[0148] In the perovskite precursor solution containing the passivator in step (4), the amount of stearic acid added is 0.7 mg.
[0149] The rest are the same as in Example 1.
[0150] Example 5
[0151] This embodiment provides a method for preparing a perovskite solar cell 100, which is different from the embodiment 1 in that:
[0152] Step (4) spin-coat the surface of the first carrier transport layer 30 away from the first electrode layer 20 with a perovskite precursor solution at a rate of 4000 rpm for 15 seconds, add 600 μL of chlorobenzene as an anti-solvent at the 10th second from the start of spin coating, anneal on a 100°C hot stage for 60 minutes to obtain a perovskite layer with a thickness of 500 nm; spin-coat 5 mg / ml of stearic acid at a rate of 4000 rpm for 15 seconds on the surface of the perovskite layer away from the first carrier transport layer 30, anneal on a 100°C hot stage for 60 minutes to obtain a passivator modified layer with a thickness of 10 nm.
[0153] The rest are the same as in Example 1.
[0154] Example 6
[0155] This embodiment provides a method for preparing a perovskite solar cell 100, which is different from Embodiment 3 in that:
[0156] In step (4), a perovskite precursor solution containing a passivator is spin-coated at a rate of 4000 rpm for 15 seconds on the surface of the first carrier transport layer 30 away from the first electrode layer 20, 600 μL of chlorobenzene is added as an anti-solvent at the 10th second from the start of spin coating, and annealing is performed on a hot stage at 100°C for 60 minutes to obtain a preliminary product with a thickness of 500 nm; 5 mg / mL of stearic acid is spin-coated at a rate of 4000 rpm for 15 seconds on the surface of the obtained preliminary product away from the first carrier transport layer 30, and annealing is performed on a hot stage at 100°C for 60 minutes to obtain a passivator modified layer with a thickness of 10 nm.
[0157] Among them, the perovskite precursor solution containing the passivator is formed by adding 705.34 mg of PbI2, 240.8 mg of FAI, 33.78 mg of MACl and 0.5 mg of stearic acid to 100 μL of DMSO (dimethyl sulfoxide) and 900 μL of DMF (N,N-dimethylformamide) and stirring for 8h-12h.
[0158] The rest is the same as Example 3.
[0159] Example 7
[0160] This embodiment provides a method for preparing a perovskite solar cell 100, which is different from Embodiment 3 in that:
[0161] In the perovskite precursor solution containing a passivator in step (4), the passivator used is sodium stearate.
[0162] The rest is the same as Example 3.
[0163] Example 8
[0164] This embodiment provides a method for preparing a perovskite solar cell 100, which is different from Embodiment 3 in that:
[0165] Step (3), preparing a second carrier transport layer 50.
[0166] Step (5), preparing a first carrier transport layer 30.
[0167] The rest are the same as in Example 1.
[0168] Example 9
[0169] This embodiment provides a method for preparing a perovskite solar cell 100, which is different from Embodiment 3 in that:
[0170] In the perovskite precursor solution containing a passivator in step (4), the passivator used is tetrabutylammonium bromide.
[0171] The rest is the same as Example 3.
[0172] Example 10
[0173] This embodiment provides a method for preparing a perovskite solar cell 100, which is different from Embodiment 3 in that:
[0174] In the perovskite precursor solution containing a passivator in step (4), the passivator used is hexadecyltrimethylammonium bromide.
[0175] The rest is the same as Example 3.
[0176] Embodiment 11
[0177] This embodiment provides a method for preparing a perovskite solar cell 100, which is different from Embodiment 3 in that:
[0178] In the perovskite precursor solution containing a passivator in step (4), the passivator used is dodecyldimethylbenzylammonium chloride.
[0179] The rest is the same as Example 3.
[0180] Example 12
[0181] This embodiment provides a method for preparing a perovskite solar cell 100, which is different from Embodiment 3 in that:
[0182] In the perovskite precursor solution containing a passivator in step (4), the passivator used is octadecyl dimethyl hydroxyethyl ammonium nitrate.
[0183] The rest is the same as Example 3.
[0184] Embodiment 13
[0185] This embodiment provides a method for preparing a perovskite solar cell 100, which is different from Embodiment 3 in that:
[0186] In the perovskite precursor solution containing a passivating agent in step (4), the passivating agent used is N ɑ -Acyl lysine.
[0187] The rest is the same as Example 3.
[0188] Embodiment 14
[0189] This embodiment provides a method for preparing a perovskite solar cell 100, which is different from Embodiment 3 in that:
[0190] In the perovskite precursor solution containing a passivator in step (4), the passivator used is sodium dodecylaminopropionate.
[0191] The rest is the same as Example 3.
[0192] Embodiment 15
[0193] This embodiment provides a method for preparing a perovskite solar cell 100, which is different from Embodiment 3 in that:
[0194] In the perovskite precursor solution containing a passivating agent in step (4), the passivating agent used is N ɑ -Methyl-N ɑ -Lauroyl lysine.
[0195] The rest is the same as Example 3.
[0196] Example 16
[0197] This embodiment provides a method for preparing a perovskite solar cell 100, which is different from Embodiment 3 in that:
[0198] In the perovskite precursor solution containing a passivator in step (4), the passivator used is N-acylsarcosine.
[0199] The rest is the same as Example 3.
[0200] Comparative Example 1
[0201] This embodiment provides a method for preparing a perovskite solar cell 100, which is different from the embodiment 1 in that:
[0202] In step (4), no passivating agent is added.
[0203] The rest are the same as in Example 1.
[0204] Comparative Example 2
[0205] This embodiment provides a method for preparing a perovskite solar cell 100, which is different from the embodiment 1 in that:
[0206] Step (3), preparing a second carrier transport layer 50.
[0207] In step (4), no passivating agent is added.
[0208] Step (5), preparing a first carrier transport layer 30.
[0209] The rest are the same as in Example 1.
[0210] Experimental example
[0211] The photoelectric conversion efficiency and stability of the perovskite solar cells 100 prepared in Examples 1 to 16 and the perovskite solar cells 100 prepared in Comparative Examples 1-2 were tested, and the test results are shown in Table 1.
[0212] In this experimental example, the photoelectric conversion efficiency of the perovskite solar cell 100 is measured using Keithley 2400SMUAM 1.5G solar irradiation at 100 mW / cm 2 The photoelectric conversion efficiency of the battery is tested under the light source. The calculation method of the photoelectric conversion efficiency PCE is as follows:
[0213] PCE=Pout / Popt
[0214] =Voc×Jsc×(Vmpp×Jmpp) / (Voc×Jsc)
[0215] =Voc×Jsc×FF
[0216] Where Pout, Popt, Vmpp, Jmpp, Voc and Jsc are the battery output power, incident light power, battery maximum power point voltage, battery maximum power point current, open circuit voltage and short circuit current respectively. FF represents the fill factor.
[0217] In this experimental example, the stability test of the perovskite solar cell 100 is as follows: the perovskite solar cell 100 is placed in an environment with a temperature of 25°C and a relative humidity of 45±5%, and its photoelectric conversion efficiency PCE changes with aging time. The time required for the photoelectric conversion efficiency to decay to 80% of the initial efficiency is recorded as T 80 The size of this parameter indicates the stability of the perovskite solar cell 100.
[0218] Table 1 Performance test data of the perovskite solar cell 100 prepared in the embodiment of the present application
[0219]
[0220]
[0221]
[0222] According to the test results obtained in Table 1, we can see that:
[0223] (1) According to the test results of Examples 1-4 and Comparative Example 1, when the amount of passivator added is in the range of 0.1 mg / mL-1 mg / mL, the photoelectric conversion efficiency and stability of the perovskite solar cell 100 are greatly improved compared with the perovskite solar cell 100 without the addition of the passivator.
[0224] (2) According to the analysis of the test results of Example 5 and Examples 1-4, it can be seen that the passivator formed on the surface of the perovskite layer has better photoelectric conversion efficiency and stability than that formed in the perovskite layer.
[0225] (3) According to the analysis of the test results of Example 6 and Examples 1-5, it can be seen that when the passivator acts as both an interface passivator and a bulk passivator, the stability of the corresponding perovskite solar cell 100 is significantly improved, and the photoelectric conversion efficiency does not change significantly, compared with the passivator acting only as an interface passivator or a bulk passivator.
[0226] (4) According to the analysis of the test results of Example 7 and Example 3, the photoelectric conversion efficiency and stability of the perovskite solar cell 100 formed by sodium stearate as a passivating agent are not significantly changed compared with the perovskite solar cell 100 formed by stearic acid as a passivating agent.
[0227] (5) According to the analysis of the test results of Example 8 and Example 3, it can be seen that the photoelectric conversion efficiency of the inverted perovskite solar cell 100 formed by stearic acid as a passivating agent is significantly reduced compared with the positive perovskite solar cell 100, but the stability is significantly improved.
[0228] (6) According to the test results of Example 8 and Comparative Example 2, the inverted perovskite solar cell 100 formed by stearic acid as a passivating agent has significantly improved photoelectric conversion efficiency and stability compared with the inverted perovskite solar cell 100 without adding a passivating agent.
[0229] (7) According to the analysis of the test results of Examples 9-16 and Examples 3 and 7, it can be seen that the stability of the positive perovskite solar cell 100 formed by quaternary ammonium compounds and amino acid type zwitterionic surfactants as passivators is significantly improved compared with the positive perovskite solar cell 100 formed by stearic acid and its salts as passivators, and the photoelectric conversion efficiency does not change significantly.
[0230] In summary, the device efficiency and stability of the perovskite solar cell 100 formed by using one or more of stearic acid and its salts, quaternary ammonium compounds, and amino acid type zwitterionic surfactants provided in the embodiments of the present application as passivators are greatly improved.
[0231] In the several embodiments provided in the present application, it should be understood that the disclosed systems, devices and methods can be implemented in other ways. For example, the device embodiments described above are only schematic. For example, the division of units is only a logical function division. There may be other division methods in actual implementation. For example, multiple units or components can be combined or integrated into another system, or some features can be ignored or not executed. Another point is that the mutual coupling or direct coupling or communication connection shown or discussed can be an indirect coupling or communication connection through some interfaces, devices or units, which can be electrical, mechanical or other forms.
[0232] In addition, each functional unit in each embodiment of the present application may be integrated into one processing unit, or each unit may exist physically separately, or two or more units may be integrated into one unit. The above-mentioned integrated unit may be implemented in the form of hardware or in the form of software functional units.
[0233] The above description is only an implementation method of the present application, and does not limit the patent scope of the present application. Any equivalent structure or equivalent process transformation made using the contents of the present application specification and drawings, or directly or indirectly used in other related technical fields, are also included in the patent protection scope of the present application.
Claims
1. A perovskite light absorbing layer, characterized in that: It comprises a perovskite layer and a passivator, wherein the passivator comprises one or more of stearic acid and its salts, quaternary ammonium compounds, and amino acid type zwitterionic surfactants.
2. The perovskite light absorbing layer according to claim 1, characterized in that: The stearic acid and its salts include one or more of stearic acid, sodium stearate, magnesium stearate, calcium stearate, lead stearate, aluminum stearate, cadmium stearate, iron stearate, potassium stearate, and hydroxystearic acid.
3. The perovskite light absorbing layer according to claim 1, characterized in that: The quaternary ammonium compound includes one or more of tetrabutylammonium bromide, dodecyltrimethylammonium chloride, hexadecyltrimethylammonium bromide, dioctadecyldimethylammonium bromide, dodecyldimethylbenzylammonium chloride, octadecyldimethylhydroxyethylammonium nitrate, and octadecylbishydroxyethylmethylammonium chloride.
4. The perovskite light absorbing layer according to claim 1, characterized in that: The amino acid type zwitterionic surfactant includes N ɑ -Acyl lysine, sodium dodecyl aminopropionate, sodium dodecyl dimethylene amino dicarboxylate, N ɑ -Methyl-N ɑ -Lauroyl lysine, N-acyl sarcosine, di(octylaminoethyl)glycine, N-acyl glutamic acid, N β -Acyl-L-lysine, N ɑ -Dimethyl-N ɑ -acyl lysine, N-acyl glutamic acid, one or more of N-acyl glutamic acid diester.
5. The perovskite light absorbing layer according to claim 1, characterized in that: The passivating agent is dispersed in the perovskite layer.
6. The perovskite light absorbing layer according to claim 1, characterized in that: The passivator forms a passivator modification layer on a surface of the perovskite layer.
7. The perovskite light absorbing layer according to claim 1, characterized in that: The passivator includes a first passivator and a second passivator; the first passivator is dispersed in the perovskite layer, and the second passivator forms a passivator modification layer on a surface of the perovskite layer.
8. The perovskite light absorbing layer according to any one of claims 1 to 7, characterized in that: The thickness of the perovskite layer is 300nm-700nm.
9. The perovskite light absorbing layer according to claim 6 or 7, characterized in that: The thickness of the passivation agent modified layer is 10nm-50nm.
10. The perovskite light absorbing layer according to any one of claims 1 to 7, characterized in that: The material of the perovskite layer includes ABX3 or A2CDX6, wherein A is an inorganic or organic or organic-inorganic mixed cation; B is an inorganic or organic or organic-inorganic mixed cation; C is an inorganic or organic or organic-inorganic mixed cation; D is an inorganic or organic or organic-inorganic mixed cation; and X is an inorganic or organic or organic-inorganic mixed anion.
11. A method for preparing a perovskite light-absorbing layer, characterized in that: include: Coating a perovskite precursor solution containing a passivator on the first carrier transport layer; wherein the passivator includes one or more of stearic acid and its salts, quaternary ammonium compounds, and amino acid type zwitterionic surfactants; The perovskite precursor solution containing the passivating agent is annealed.
12. The method for preparing a perovskite light absorbing layer according to claim 11, characterized in that: The amount of the passivator added to the perovskite precursor solution containing the passivator is 0.1 mg / mL-1 mg / mL.
13. A method for preparing a perovskite light-absorbing layer, characterized in that: include: forming a perovskite layer on the first carrier transport layer; A passivating agent solution is coated on the surface of the perovskite layer away from the first carrier transport layer; wherein the passivating agent comprises one or more of stearic acid and its salts, quaternary ammonium compounds, and amino acid type zwitterionic surfactants; The passivator solution is annealed to form a passivator modification layer.
14. The method for preparing a perovskite light absorbing layer according to claim 13, characterized in that: The concentration of the passivating agent solution is 0.1 mg / ml-10 mg / ml.
15. The method for preparing a perovskite light absorbing layer according to claim 13, characterized in that: The forming of a perovskite layer on the first carrier transport layer comprises: coating a perovskite precursor solution containing a passivating agent on the first carrier transport layer; The perovskite precursor solution containing the passivating agent is annealed.
16. The method for preparing a perovskite light absorbing layer according to claim 15, characterized in that: The amount of the passivator added to the perovskite precursor solution containing the passivator is 0.1 mg / mL-1 mg / mL.
17. A perovskite solar cell, characterized in that: It includes a substrate, a first electrode layer, a first carrier transport layer, a perovskite light absorption layer, a second carrier transport layer and a second electrode layer which are stacked in sequence; wherein the perovskite light absorption layer is the perovskite light absorption layer according to any one of claims 1 to 10, or the perovskite light absorption layer is the perovskite light absorption layer prepared by the method according to any one of claims 11 to 16.
18. The perovskite solar cell according to claim 17, characterized in that: The perovskite light absorbing layer is the perovskite light absorbing layer according to claim 3 or 4, or the perovskite light absorbing layer is the perovskite light absorbing layer prepared by the method according to any one of claims 13-16; the passivator modified layer is arranged on the surface of the perovskite layer away from the first carrier transport layer.
19. The perovskite solar cell according to claim 17 or 18, characterized in that: The material of the perovskite layer includes ABX3 or A2CDX6, wherein A is an inorganic or organic or organic-inorganic mixed cation; B is an inorganic or organic or organic-inorganic mixed cation; C is an inorganic or organic or organic-inorganic mixed cation; D is an inorganic or organic or organic-inorganic mixed cation; and X is an inorganic or organic or organic-inorganic mixed anion.