Photoelectric device, preparation method thereof and display device

By connecting organic materials with metal oxide surfaces using physical vapor deposition in optoelectronic devices, the problem of metal oxide surface defects is solved and the stability and photoelectric properties of the device are improved.

CN119095455APending Publication Date: 2024-12-06TCL TECHNOLOGY GROUP CORPORATION +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310665904.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-06-06
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Metal oxides have many surface defects in optoelectronic devices, resulting in poor stability and affecting the performance and life of the device.

Method used

The physical vapor deposition method is used to deposit organic materials on the carrier functional layer, and is connected to the cationic suspended bonds on the surface of the metal oxide to form chemical bonds, passivate surface defects, and improve the photoelectric performance and service life of the device through the evaporation process.

Benefits of technology

It effectively reduces defects on the metal oxide surface, improves the stability and photoelectric performance of optoelectronic devices, and extends the service life of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119095455A_ABST
    Figure CN119095455A_ABST
Patent Text Reader

Abstract

The invention discloses a photoelectric device, a preparation method thereof and a display device, and the method comprises the steps: providing a prefabricated device and an organic material, and enabling the prefabricated device to comprise a first electrode and an initial carrier function layer disposed at one side of the first electrode, the material of the initial carrier functional layer comprises a metal oxide with a cationic dangling bond on the surface, and the organic material contains an active group; depositing the organic material on one side, deviating from the first electrode, of the initial carrier function layer to obtain a carrier function layer; and arranging a second electrode on one side, deviating from the first electrode, of the carrier functional layer to obtain the photoelectric device. The invention aims to solve the problem of more defects on the surface of the metal oxide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of optoelectronic devices, and in particular to an optoelectronic device, a preparation method thereof, and a display device. Background Art

[0002] Photoelectric devices refer to devices made based on the photoelectric effect, including light-emitting devices, photocells, photoelectric tubes, etc. Taking light-emitting devices as an example, light-emitting devices emit light by releasing energy through the recombination of electrons and holes, and are widely used in the field of lighting. Light-emitting devices are usually composed of an anode, a cathode, and a functional layer arranged between the anode and the cathode. The functional layer includes but is not limited to a light-emitting layer, a hole functional layer, an electron functional layer, etc. The hole functional layer and the electron functional layer can also be defined as a carrier functional layer.

[0003] Metal oxide semiconductor materials are often used to prepare carrier functional layers of optoelectronic devices. Currently, metal oxides are usually prepared by solution method or sol-gel method. However, the surfaces of the metal oxides prepared in this way often have a large number of defects, which makes them less stable in electric field environments, thus affecting the stability of the device. Summary of the invention

[0004] In view of this, the present application provides an optoelectronic device, a method for preparing the same, and a display device, aiming to solve the problem of many surface defects of metal oxides.

[0005] The embodiment of the present application is implemented as follows:

[0006] In a first aspect, the present application provides a method for preparing a photoelectric device, comprising the following steps:

[0007] Providing a prefabricated device and an organic material, wherein the prefabricated device comprises a first electrode and an initial carrier functional layer disposed on one side of the first electrode, wherein the material of the initial carrier functional layer comprises a metal oxide having cationic dangling bonds on the surface, and the organic material contains active groups;

[0008] Depositing the organic material on a side of the initial carrier functional layer away from the first electrode to obtain a carrier functional layer;

[0009] Disposing a second electrode on a side of the carrier functional layer away from the first electrode to obtain a photoelectric device;

[0010] Wherein, the active groups include one or more of carboxyl, thiol and amino groups.

[0011] Optionally, in some embodiments of the present application, the step of depositing the organic material on the side of the initial carrier functional layer facing away from the first electrode to obtain the carrier functional layer includes: using physical vapor deposition to deposit the organic material on the side of the initial carrier functional layer facing away from the first electrode to obtain the carrier functional layer.

[0012] Optionally, in some embodiments of the present application, the step of depositing the organic material on a side of the initial carrier functional layer away from the first electrode by physical vapor deposition includes:

[0013] Providing a vacuum evaporation device having an evaporation chamber;

[0014] The prefabricated device is placed in the evaporation chamber, and the organic material is used as a target to perform evaporation to obtain a carrier functional layer, wherein the carrier functional layer comprises the metal oxide and the organic material, and the active group of the organic material is connected to the cationic dangling bond.

[0015] Optionally, in some embodiments of the present application, during the evaporation, the evaporation conditions include:

[0016] Vacuum degree is 10 -3 ~10 -5 pa; and / or,

[0017] The evaporation temperature is 350-450° C.; and / or,

[0018] The evaporation rate is 0.5 to 5 angstroms / min; and / or,

[0019] The evaporation time is 1 to 5 minutes.

[0020] Optionally, in some embodiments of the present application, after obtaining the carrier functional layer and before setting the second electrode on the side of the carrier functional layer away from the first electrode, the preparation method further includes: heating the carrier functional layer to 60 to 150° C. and annealing for 10 to 120 minutes.

[0021] Optionally, in some embodiments of the present application, after obtaining the carrier functional layer and before providing the second electrode on the side of the carrier functional layer facing away from the first electrode, the preparation method further includes: washing the carrier functional layer with a solvent.

[0022] Optionally, in some embodiments of the present application, the solvent includes one or more of an alcohol solvent having 1 to 8 carbon atoms, acetone, and an alkane solvent having 5 to 8 carbon atoms; and / or,

[0023] The solvent includes a first solvent and a second solvent, and the step of washing the carrier functional layer with the solvent includes: immersing the carrier functional layer in the first solvent for 0.5 to 10 minutes, and then coating the second solvent on a side of the carrier functional layer away from the first electrode.

[0024] Optionally, in some embodiments of the present application, the organic material includes one or more of substituted or unsubstituted aromatic carboxylic acids and salts thereof, substituted or unsubstituted aromatic amines and salts thereof, wherein the substituent is selected from at least one of C1-C8 alkyl, C1-C8 alkoxy, nitro, amino, thiol and halogen; and / or,

[0025] The melting point of the organic material is less than or equal to 300° C.; and / or,

[0026] In the carrier functional layer, the molar ratio of the metal oxide to the organic material is 1:(0.001-0.05).

[0027] Optionally, in some embodiments of the present application, the substituted or unsubstituted aromatic carboxylic acid includes one or more of trifluorobenzoic acid, 4-chlorobenzoic acid, and 2-mercaptobenzoic acid, and the trifluorobenzoic acid includes one or more of 2,4,5-trifluorobenzoic acid, 2,4,6-trifluorobenzoic acid, 2,3,6-trifluorobenzoic acid, and 2,3,4-trifluorobenzoic acid; and / or,

[0028] The substituted or unsubstituted aromatic amine includes one or more of 2-nitroaniline and 4,4'-diaminodiphenylamine.

[0029] Optionally, in some embodiments of the present application, the initial carrier functional layer includes one or both of an electron functional layer and a hole functional layer; the electron functional layer includes one or both of an electron transport layer and an electron injection layer; the hole functional layer includes one or both of a hole transport layer and a hole injection layer.

[0030] Optionally, in some embodiments of the present application, the material of the electron transport layer is selected from at least one of ZnO, BaO, TiO2, SnO2; and / or,

[0031] The material of the electron injection layer is selected from at least one of Al2O3 and Ga2O3; and / or,

[0032] The material of the hole transport layer is selected from at least one of NiO, MoO3, WO3, V2O5 and CuO; and / or,

[0033] The material of the hole injection layer is selected from at least one of NiO, MoO3, WO3, V2O5 and CuO.

[0034] Optionally, in some embodiments of the present application, the first electrode and the second electrode are each independently selected from a doped metal oxide particle electrode, a composite electrode of metal and metal oxide, a graphene electrode, a carbon nanotube electrode, a metal electrode or an alloy electrode, the material of the doped metal oxide particle electrode is selected from one or more of indium-doped tin oxide, fluorine-doped tin oxide, antimony-doped tin oxide, aluminum-doped zinc oxide, gallium-doped zinc oxide, indium-doped zinc oxide, magnesium-doped zinc oxide and aluminum-doped magnesium oxide, the composite electrode of metal and metal oxide is selected from AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, TiO2 / Ag / TiO2, TiO2 / Al / TiO2, ZnS / Ag / ZnS, ZnS / Al / ZnS, the material of the metal electrode is selected from one or more of Ag, Al, Cu, Mo, Au, Pt, Si, Ca, Mg and Ba; and / or,

[0035] The prefabricated device further comprises a light-emitting layer, which is arranged between the initial carrier functional layer and the first electrode. The material of the light-emitting layer comprises one or more selected from organic light-emitting materials and quantum dot light-emitting materials. The organic light-emitting material is selected from 4,4'-bis(N-carbazole)-1,1'-biphenyl:tri[2-(p-tolyl)pyridine iridium(III), 4,4',4"-tri(carbazole-9-yl)triphenylamine:tri[2-(p-tolyl)pyridine iridium, diaromatic anthracene derivatives, distilbene aromatic derivatives, pyrene derivatives, fluorene derivatives, TBPe fluorescent materials, TT One or more of PX fluorescent materials, TBRb fluorescent materials, DBP fluorescent materials, delayed fluorescent materials, TTA materials, thermally activated delayed materials, polymers containing BN covalent bonds, hybrid localized charge transfer excited state materials, and exciplex luminescent materials, the quantum dot luminescent material is selected from at least one of single structure quantum dots, core-shell structure quantum dots, and perovskite semiconductor materials; the material of the single structure quantum dots, the core material of the core-shell structure quantum dots, and the shell material of the core-shell structure quantum dots are selected from II-VI group compounds, IV-VI group compounds, III-V group compounds, and At least one of the I-III-VI group compounds; the II-VI group compound is selected from CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, HgTe, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, At least one of CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe and HgZnSTe; the IV-VI group compound is at least one of SnS, SnSe, SnTe, PbS, PbSe, PbTe, SnSeS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, SnPbSSe, SnPbSeTe and SnPbSTe;The III-V compound is selected from the group consisting of GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaPSb, and AlN P, AlNAs, AlNSb, AlPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInN P, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs and InAlPSb; the I-III-VI group compound is selected from at least one of CuInS2, CuInSe2 and AgInS2; the perovskite semiconductor material is selected from doped or undoped inorganic perovskite semiconductors, or organic-inorganic hybrid perovskite semiconductors; the inorganic perovskite semiconductor has a general structural formula of AMX3, wherein A is Cs; + ion, M is a divalent metal cation selected from Pb 2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ , Mn 2+ 、Co 2+ , Fe 2+ ,Ge 2+ , Yb 2+ 、Eu 2+ At least one of, X is a halogen anion selected from Cl - Br - ,I - At least one of the following; the general structural formula of the organic-inorganic hybrid perovskite semiconductor is BMX3, wherein B is an organic amine cation selected from CH3(CH2) n-2 NH3 + or [NH3(CH2) n NH3] 2+ , where n≥2, M is a divalent metal cation selected from Pb 2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ , Mn 2+ 、Co 2+ , Fe 2+ ,Ge 2+ , Yb 2+ 、Eu2+ At least one of, X is a halogen anion selected from Cl - Br - ,I - At least one of .

[0036] In a second aspect, the present application further proposes a photoelectric device, comprising a stacked first electrode, a carrier functional layer, and a second electrode, wherein the carrier functional layer comprises a metal oxide and an organic material, wherein the organic material contains an active group, and the metal oxide surface has a cationic dangling bond, wherein the active group is connected to the cationic dangling bond;

[0037] Wherein, the active groups include one or more of carboxyl, thiol and amino groups.

[0038] Optionally, in some embodiments of the present application, the organic material includes one or more of substituted or unsubstituted aromatic carboxylic acids and salts thereof, substituted or unsubstituted aromatic amines and salts thereof, wherein the substituent is selected from at least one of C1-C8 alkyl, C1-C8 alkoxy, nitro, amino, thiol and halogen; and / or,

[0039] The melting point of the organic material is less than or equal to 300° C.; and / or,

[0040] In the carrier functional layer, the molar ratio of the metal oxide to the organic material is 1:(0.001-0.05).

[0041] Optionally, in some embodiments of the present application, the substituted or unsubstituted aromatic carboxylic acid includes one or more of trifluorobenzoic acid, 4-chlorobenzoic acid, and 2-mercaptobenzoic acid, and the trifluorobenzoic acid includes one or more of 2,4,5-trifluorobenzoic acid, 2,4,6-trifluorobenzoic acid, 2,3,6-trifluorobenzoic acid, and 2,3,4-trifluorobenzoic acid; and / or,

[0042] The substituted or unsubstituted aromatic amine includes one or more of 2-nitroaniline and 4,4'-diaminodiphenylamine.

[0043] In a third aspect, the present application further proposes a display device, comprising an optoelectronic device manufactured by the preparation method as described above, or an optoelectronic device as described above.

[0044] The present application provides a method for preparing a photoelectric device. The method mainly uses a deposition process to chemically bond an organic material with a metal oxide film, thereby obtaining a light-emitting device comprising an organic material and a metal oxide film. The defective metal oxide in the light-emitting device is reduced, and the stability of the device is improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without creative work.

[0046] Figure 1 It is a schematic diagram of a process for preparing a photoelectric device proposed in an embodiment of the present application;

[0047] Figure 2 is a schematic structural diagram of an optoelectronic device proposed in one embodiment of the present application;

[0048] Reference numerals:

[0049] 100 - photoelectric device; 10 - anode; 20 - electron transport layer; 30 - light-emitting layer; 40 - cathode; 50 - hole injection layer; 60 - hole transport layer. DETAILED DESCRIPTION

[0050] The technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without making creative work belong to the scope of protection of the present application. In addition, it should be understood that the specific implementation methods described herein are only used to illustrate and explain the present application, and are not used to limit the present application.

[0051] In this application, unless otherwise specified, the directional words used, such as "upper" and "lower", refer specifically to the directions of the drawings in the accompanying drawings. In addition, in the description of the specification of this application, the term "including" means "including but not limited to".

[0052] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0053] In this application, "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural.

[0054] In the present application, "at least one" means one or more, and "plurality" means two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.

[0055] In the first aspect, the present application provides a method for preparing a photoelectric device 100, wherein the photoelectric device 100 includes but is not limited to a light emitting device, a photovoltaic cell, and a photodetector, and the photoelectric device 100 includes a stacked first electrode, a carrier functional layer, and a second electrode, wherein the first electrode is one of the cathode 40 and the anode 10, and the second electrode is the other of the cathode 40 and the anode 10. Figure 1 In some embodiments, the method for preparing the optoelectronic device 100 comprises the following steps:

[0056] S10, providing a prefabricated device and an organic material, wherein the prefabricated device includes a first electrode and an initial carrier functional layer disposed on one side of the first electrode, wherein the material of the initial carrier functional layer includes a metal oxide having cationic dangling bonds on the surface, and the organic material contains active groups;

[0057] S20, depositing the organic material on a side of the initial carrier functional layer away from the first electrode to obtain a carrier functional layer;

[0058] S30 , disposing a second electrode on a side of the carrier functional layer away from the first electrode to obtain a photoelectric device 100 .

[0059] Dangling bonds are chemical bonds. Generally, the crystal lattice terminates suddenly at the surface. Each atom in the outermost layer of the surface will have an unpaired electron, that is, an unsaturated bond, which is called a dangling bond. Cationic dangling bonds refer to some unpaired cations on the surface of metal oxides. For example, there are some uncoordinated Zn on the surface of ZnO nanoparticles. 2 + , Zn 2+In the technical solution provided by the present application, the organic material is brought into contact with the metal oxide film through a deposition process, and the active groups of the organic material are connected with the cationic dangling bonds on the surface of the metal oxide, so that the organic material and the surface of the metal oxide film are chemically bonded, thereby effectively passivating the film defects and helping to improve the optoelectronic performance and service life of the device.

[0060] In step S10:

[0061] See also Figure 2 In some embodiments, the initial carrier functional layer includes one or both of an electron functional layer and a hole functional layer; the electron functional layer includes one or both of an electron transport layer 20 and an electron injection layer; the hole functional layer includes one or both of a hole transport layer 60 and a hole injection layer 50. It can be understood that in some embodiments, the optoelectronic device 100 includes but is not limited to one or more of an electron functional layer and a hole functional layer, wherein both the electron functional layer and the hole functional layer can use a suitable metal oxide as a film material. Under this premise, one or both of the electron functional layers can be subjected to the deposition process in the subsequent steps S20 and S30, and one or both of the hole functional layers can be subjected to the deposition process, or the electron functional layer and the hole functional layer can be subjected to the deposition process at the same time.

[0062] In some embodiments, when the initial carrier functional layer to be deposited includes an electron transport layer 20, the material of the electron transport layer 20 includes an N-type metal oxide, and the N-type metal oxide is selected from at least one of ZnO, BaO, TiO2, and SnO2; when the initial carrier functional layer includes an electron injection layer, the material of the electron injection layer includes an N-type metal oxide, and the N-type metal oxide is selected from at least one of Al2O3 and Ga2O3; when the initial carrier functional layer includes a hole transport layer 60, the material of the hole transport layer 60 includes a P-type metal oxide, and the P-type metal oxide is selected from at least one of NiO, MoO3, WO3, V2O5 and CuO; when the initial carrier functional layer includes a hole injection layer 50, the material of the hole injection layer 50 includes a P-type metal oxide, and the P-type metal oxide is selected from at least one of NiO, MoO3, WO3, V2O5 and CuO.

[0063] It is understandable that when at least one of the electron functional layer and the hole functional layer is not deposited, the material of the at least one film layer can have more choices. For ease of description, the film layer of the electron functional layer and the hole functional layer that is not deposited is defined as the third carrier functional layer.

[0064] When the third carrier functional layer includes an electron transport layer 20, the material of the third carrier functional layer can be a material commonly used in the art for preparing the electron transport layer 20, for example, it can include but is not limited to one or more of metal oxides, doped metal oxides, IIB-VIA group materials, IIIB-VA group materials and IB-IIIB-VIA group materials; the metal oxide includes one or more of ZnO, TiO2, SnO2; the metal oxide in the doped metal oxide includes one or more of ZnO, TiO2, SnO2, and the doping element includes one or more of Al, Mg, Li, In, Ga; the IIB-VIA group semiconductor material includes one or more of ZnS, ZnSe, CdS, CdSe; the IIIB-VA group semiconductor material includes one or more of InP and GaP; the IB-IIIB-VIA group semiconductor material includes one or more of CuInS and CuGaS.

[0065] When the third carrier functional layer includes an electron injection layer, the material of the third carrier functional layer can be a material commonly used in the art to prepare an electron injection layer, for example, it can include but is not limited to at least one of Al2O3, Ga2O3, cesium carbonate, cesium fluoride, cesium azide and lithium fluoride.

[0066] When the third carrier functional layer includes a hole transport layer 60, the material of the third carrier functional layer can be a material commonly used in the art for preparing the hole transport layer 60, for example, it can include but is not limited to 4,4'-N,N'-dicarbazolyl-biphenyl, N,N'-diphenyl-N,N'-bis(1-naphthyl)-1,1'-biphenyl-4,4"-diamine, N,N'-diphenyl-N,N'-bis(3-methylphenyl)-(1,1'-biphenyl)-4,4'-diamine, N,N'-bis(3-methylphenyl)-(1,1'-biphenyl)-4,4'-diamine, )-N,N'-bis(phenyl)-spiro, N,N'-bis(4-(N,N'-diphenyl-amino)phenyl)-N,N'-diphenylbenzidine, 4,4',4'-tri(N-carbazolyl)-triphenylamine, 4,4',4'-tri(N-3-methylphenyl-N-phenylamino)triphenylamine, poly[(9,9'-dioctylfluorene-2,7-diyl)-co-(4,4'-(N-(4-sec-butylphenyl)diphenylamine))], poly(4-butylphenyl-diphenylamine), polyaniline, polypyrrole, poly( p-)phenylene vinylene, poly(phenylene vinylene), poly[2-methoxy-5-(2-ethylhexyloxy)-1,4-phenylene vinylene] and poly[2-methoxy-5-(3',7'-dimethyloctyloxy)-1,4-phenylene vinylene], copper phthalocyanine, aromatic tertiary amines, polynuclear aromatic tertiary amines, 4,4'-bis(p-carbazolyl)-1,1'-biphenyl compounds, N,N,N',N'-tetraarylbenzidine, PEDOT:PSS and its derivatives, poly(N-vinylcarbazole) and its derivatives At least one of biomaterials, polymethacrylate and its derivatives, poly(9,9-octylfluorene) and its derivatives, poly(spirofluorene) and its derivatives, N,N'-di(naphthalene-1-yl)-N,N'-diphenylbenzidine, spiro NPB, doped graphene, undoped graphene, C60, doped or undoped NiO, doped or undoped MoO3, doped or undoped WO3, doped or undoped V2O5, doped or undoped P-type gallium nitride, doped or undoped CrO3, and doped or undoped CuO.

[0067] When the third carrier functional layer includes a hole injection layer 50, the material of the third carrier functional layer can be a material commonly used in the art for preparing the hole injection layer 50, for example, it can include but is not limited to at least one of 2,3,6,7,10,11-hexacyano-1,4,5,8,9,12-hexaazatriphenylene, PEDOT, PEDOT:PSS, PEDOT:PSS doped with s-MoO3 derivatives, 4,4',4'-tris(N-3-methylphenyl-N-phenylamino)triphenylamine, tetracyanoquinodimethane, copper phthalocyanine, nickel oxide, molybdenum oxide, tungsten oxide, vanadium oxide, molybdenum sulfide, tungsten sulfide and copper oxide.

[0068] In some embodiments, the prefabricated device further includes a light-emitting layer 30, and the light-emitting layer 30 is disposed between the initial carrier functional layer and the first electrode. The light-emitting layer 30 may be an organic light-emitting layer or a quantum dot light-emitting layer. When the light-emitting layer 30 is an organic light-emitting layer, the optoelectronic device 100 may be an organic light-emitting device; when the light-emitting layer 30 is a quantum dot light-emitting layer, the optoelectronic device 100 may be a quantum dot light-emitting device.

[0069] The material of the organic light-emitting layer is a material known in the art for the organic light-emitting layer of the optoelectronic device 100, for example, it can be selected from but not limited to 4,4'-bis(N-carbazole)-1,1'-biphenyl:tri[2-(p-tolyl)pyridine iridium(III), 4,4',4"-tri(carbazole-9-yl)triphenylamine:tri[2-(p-tolyl)pyridine iridium, diaromatic anthracene derivatives, distilbene aromatic derivatives, pyrene derivatives, fluorene derivatives, TBPe fluorescent materials, TTPX fluorescent materials, TBRb fluorescent materials, DBP fluorescent materials, delayed fluorescent materials, TTA materials, thermally activated delayed materials, polymers containing BN covalent bonds, hybrid localized charge transfer excited state materials, and exciplex light-emitting materials. One or more of the following.

[0070] The material of the quantum dot light-emitting layer is a quantum dot material known in the art for the quantum dot light-emitting layer of the optoelectronic device 100, for example, it can be selected from but not limited to at least one of a single structure quantum dot, a core-shell structure quantum dot and a perovskite semiconductor material; the material of the single structure quantum dot, the core material of the core-shell structure quantum dot and the shell material of the core-shell structure quantum dot are respectively selected from at least one of II-VI group compounds, IV-VI group compounds, III-V group compounds and I-III-VI group compounds; the II-VI group compound is selected from CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, Hg At least one of S, HgSe, HgTe, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe and HgZnSTe; the IV-VI group compounds The compound is selected from at least one of SnS, SnSe, SnTe, PbS, PbSe, PbTe, SnSeS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, SnPbSSe, SnPbSeTe, and SnPbSTe; the III-V compound is selected from at least one of GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaPSb, and AlNP , AlNAs, AlNSb, AlPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs and InAlPSb; the I-III-VI group compound is selected from at least one of CuInS2, CuInSe2 and AgInS2.

[0071] As an example, the core-shell structured quantum dots may be selected from but not limited to at least one of CdZnSe / CdZnSe / ZnSe / CdZnS / ZnS, CdZnSe / CdZnSe / CdZnS / ZnS CdSe / CdSeS / CdS, InP / ZnSeS / ZnS, CdZnSe / ZnSe / ZnS, CdSeS / ZnSeS / ZnS, CdSe / ZnS, CdSe / ZnSe / ZnS, ZnSe / ZnS, ZnSeTe / ZnS, CdSe / CdZnSeS / ZnS and InP / ZnSe / ZnS.

[0072] It should be noted that, for the material of the aforementioned single structure quantum dot, or the material of the core of the core-shell structure quantum dot, or the material of the shell of the core-shell structure quantum dot, the chemical formula provided only indicates the elemental composition, but does not indicate the content of each element. For example, CdZnSe only indicates that it is composed of three elements, Cd, Zn and Se. If the content of each element is indicated, it corresponds to Cd x Zn 1-x Se,0 <x<1。

[0073] The perovskite semiconductor material is selected from doped or undoped inorganic perovskite semiconductors, or organic-inorganic hybrid perovskite semiconductors; the inorganic perovskite semiconductor has a general structural formula of AMX3, wherein A is Cs + ion, M is a divalent metal cation selected from Pb 2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ , Mn 2+ 、Co 2+ , Fe 2+ ,Ge 2+ , Yb 2+ 、Eu 2+ At least one of, X is a halogen anion selected from Cl - Br - ,I - At least one of the following; the general structural formula of the organic-inorganic hybrid perovskite semiconductor is BMX3, wherein B is an organic amine cation selected from CH3(CH2) n-2 NH3 + or [NH3(CH2) n NH3] 2+ , where n≥2, M is a divalent metal cation selected from Pb 2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd2+ Cr 2+ , Mn 2+ 、Co 2+ , Fe 2+ ,Ge 2+ , Yb 2+ 、Eu 2+ At least one of, X is a halogen anion selected from Cl - Br - ,I - At least one of .

[0074] It should be noted that when a plurality of film layers are provided between the first electrode and the second electrode of the photoelectric device 100, and the plurality of film layers are selected from the light-emitting layer 30, the electron transport layer 20, the electron injection layer, the hole transport layer 60, and the hole injection layer 50, the film layer stacking order of the photoelectric device 100 is the anode 10, the hole injection layer 50, the hole transport layer 60, the light-emitting layer 30, the electron transport layer 20, the electron injection layer and the cathode 40; it can be understood that the photoelectric device 100 can be an upright device or an inverted device. In some embodiments, the photoelectric device 100 is a positive device, and accordingly, the photoelectric device 100 includes an anode 10, a hole injection layer 50, a hole transport layer 60, a light-emitting layer 30, an electron transport layer 20, an electron injection layer and a cathode 40 stacked in sequence from bottom to top; in other embodiments, the photoelectric device 100 is an inverted device, and accordingly, the photoelectric device 100 includes a cathode 40, an electron injection layer, an electron transport layer 20, a light-emitting layer 30, a hole transport layer 60, a hole injection layer 50 and an anode 10 stacked in sequence from bottom to top. In actual preparation, each film layer is prepared in sequence according to the film layer stacking sequence from the first electrode to the second electrode. When the initial carrier functional layer is prepared, after the solid film is obtained, it is deposited to form a carrier functional layer, and then the subsequent film layers are prepared until the second electrode is obtained, and the photoelectric device 100 is obtained.

[0075] Specifically, the preparation methods of the anode 10, the light-emitting layer 30, the electron transport layer 20, the electron injection layer, the hole transport layer 60, the hole injection layer 50 and the cathode 40 can be implemented by conventional techniques in the art, such as chemical methods or physical methods. Among them, the chemical method includes chemical vapor deposition, continuous ion layer adsorption and reaction, anodization, electrolytic deposition, and coprecipitation. The physical method includes physical plating and solution method, among which the physical plating method includes: thermal evaporation coating, electron beam evaporation coating, magnetron sputtering, multi-arc ion plating, physical vapor deposition, atomic layer deposition, pulsed laser deposition, etc.; the solution method can be spin coating, printing, inkjet printing, doctor blade coating, printing, dip pulling, immersion, spraying, roller coating, casting, slit coating, strip coating, etc.

[0076] In addition, the anode 10 can be an anode 10 for a photoelectric device 100 known in the art, for example, it can be selected from but not limited to a doped metal oxide particle electrode, a composite electrode of a metal and a metal oxide, a graphene electrode, a carbon nanotube electrode, a metal electrode or an alloy electrode, the material of the doped metal oxide particle electrode is selected from one or more of indium-doped tin oxide, fluorine-doped tin oxide, antimony-doped tin oxide, aluminum-doped zinc oxide, gallium-doped zinc oxide, indium-doped zinc oxide, magnesium-doped zinc oxide and aluminum-doped magnesium oxide, the composite electrode of a metal and a metal oxide is selected from AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, TiO2 / Ag / TiO2, TiO2 / Al / TiO2, ZnS / Ag / ZnS, ZnS / Al / ZnS, and the material of the metal electrode is selected from one or more of Ag, Al, Cu, Mo, Au, Pt, Si, Ca, Mg and Ba.

[0077] The cathode 40 can be a cathode 40 for the optoelectronic device 100 known in the art, for example, can be selected from but not limited to a doped metal oxide particle electrode, a composite electrode of metal and metal oxide, a graphene electrode, a carbon nanotube electrode, a metal electrode or an alloy electrode, the material of the doped metal oxide particle electrode is selected from one or more of indium-doped tin oxide, fluorine-doped tin oxide, antimony-doped tin oxide, aluminum-doped zinc oxide, gallium-doped zinc oxide, indium-doped zinc oxide, magnesium-doped zinc oxide and aluminum-doped magnesium oxide, the composite electrode of metal and metal oxide is selected from AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, TiO2 / Ag / TiO2, TiO2 / Al / TiO2, ZnS / Ag / ZnS, ZnS / Al / ZnS, and the material of the metal electrode is selected from one or more of Ag, Al, Cu, Mo, Au, Pt, Si, Ca, Mg and Ba.

[0078] In step S20:

[0079] In some embodiments, the organic material may be any one or more solid-phase organic compounds having active groups, for example, one or more of substituted or unsubstituted aromatic carboxylic acids and salts thereof, substituted or unsubstituted aromatic amines and salts thereof; wherein, "substituted or unsubstituted" means that the defined group may be substituted or unsubstituted. When the defined group is substituted, it should be understood that the defined group may be substituted by one or more substituents; the substituents are selected from at least one of C1-C8 alkyl, C1-C8 alkoxy, nitro, amino, thiol and halogen. The nitro refers to -NO2, the amino refers to -NH2, the thiol refers to -SH, and the halogen refers to -F, -Cl, -Br or -I. The active group may be connected to the cationic dangling bond, thereby playing the role of passivating defects.

[0080] In some embodiments, the deposition process is a physical vapor deposition process, that is, step S20 includes: S21, using physical vapor deposition to deposit the organic material on the side of the initial carrier functional layer away from the first electrode to obtain a carrier functional layer.

[0081] Through the physical vapor deposition process, the solid organic material is brought into contact with the metal oxide film, and the active groups of the organic material are connected to the cationic dangling bonds on the surface of the metal oxide, so that the organic material and the surface of the metal oxide film are chemically bonded, thereby effectively passivating the film defects and helping to improve the photoelectric performance and service life of the device; on the other hand, since the physical vapor deposition process is used, this avoids the problem of liquid solvent penetrating into the lower film layer of the metal oxide, which in turn causes damage to the lower film layer, thereby further improving the photoelectric performance and service life of the device.

[0082] Furthermore, in some embodiments, the melting point of the organic material is less than or equal to 300°C. For example, the melting point may be 300°C, 290°C, 280°C, 250°C, 230°C, 200°C, 180°C, 150°C, 130°C, 110°C, 100°C, 80°C, any value below 80°C, and the like. This helps to reduce the difficulty of physical vapor deposition and improve its deposition effect.

[0083] In some specific embodiments, the substituted or unsubstituted aromatic carboxylic acid includes one or more of trifluorobenzoic acid, 4-chlorobenzoic acid (CAS No.: 74-11-3; melting point 238-241°C; CBA), 2-mercaptobenzoic acid (CAS: 147-93-3; melting point: 165.5°C; MBA); the trifluorobenzoic acid includes 2,4,5-trifluorobenzoic acid (CAS No.: 446-17-3; melting point 100°C), 2,4,6-trifluorobenzoic acid (CAS No.: 28314-80-9; Melting point 142~145℃), 2,3,6-trifluorobenzoic acid (CAS No.: 2358-29-4; melting point 130~131℃), 2,3,4-trifluorobenzoic acid (CAS No.: 61079-72-9; melting point 142~145℃); the substituted or unsubstituted aromatic amine includes one or more of 2-nitroaniline (CAS No.: 88-74-4; melting point: 75℃), 4,4'-diaminodiphenylamine (CAS No.: 637-31-0; melting point: 121℃). The above compounds can not only effectively passivate defects, but also play a role in regulating the work function of the electronic functional layer material and enhancing electron injection when used to passivate the electron transport layer 20 or the electron injection layer.

[0084] The physical vapor deposition method includes but is not limited to vacuum evaporation method, vacuum sputtering method, etc. In specific implementation, step S,21 may include:

[0085] S211, providing a vacuum evaporation device having an evaporation chamber;

[0086] S212, placing the prefabricated device in the evaporation chamber, using the organic material as a target material, performing evaporation to obtain a carrier functional layer, wherein the carrier functional layer comprises the metal oxide and the organic material, and the active group of the organic material is connected to the cationic dangling bond.

[0087] Wherein, the evaporation conditions include: vacuum degree of 10 -3 ~10 -5 pa, for example, the vacuum degree can be 1×10 -5 pa, 1.5×10 -5 pa, 5×10 -5 pa, 1×10 -4 pa, 1.5×10 -4 pa, 5×10 -4 pa, 1×10 -3pa and a value between any two of the values ​​listed above; the evaporation temperature is 350-450°C, for example, it can be 350°C, 360°C, 380°C, 390°C, 400°C, 410°C, 420°C, 450°C and a value between any two of the values ​​listed above; the evaporation rate is 0.5-5 angstroms / min, for example, it can be 0.5 angstroms / min, 0.8 angstroms / min, 1 angstrom / min, 1.5 angstroms / min, 2 angstroms / min, 2.5 angstroms / min, 3 angstroms / min, 3.5 angstroms / min, 4 angstroms / min, 4.5 angstroms / min, 5 angstroms / min and a value between any two of the values ​​listed above, within this range, the evaporation efficiency and effect can be improved as a whole, thereby improving the passivation effect; the evaporation time is 1-5 min, for example, it can be 1 min, 2 min, 3 min, 4 min, 5 min and a value between any two of the values ​​listed above.

[0088] In some embodiments, in the carrier functional layer, the molar ratio of the metal oxide to the organic material is 1:(0.001-0.05), for example, 1:0.001, 1:0.005, 1:0.008, 1:0.01, 1:0.02, 1:0.03, 1:0.04, 1:0.05 and values ​​between any two of the values ​​listed above.

[0089] In some embodiments, after step S30 and before step S40, the preparation method further comprises: heating the carrier functional layer to 60-150°C and annealing for 10-120 minutes. The annealing temperature may be 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 140°C, 150°C, or any value between two of the above values; the annealing time may be 10 minutes, 20 minutes, 50 minutes, 70 minutes, 90 minutes, 100 minutes, 110 minutes, 120 minutes, or any value between two of the above values.

[0090] In some embodiments, after step S30 and before step S40, the preparation method further comprises the step of cleaning away the organic material remaining on the film layer and not connected to the metal oxide: washing the carrier functional layer with a solvent.

[0091] The solvent includes one or more of an alcohol solvent with a carbon number of 1 to 8, acetone, and an alkane solvent with a carbon number of 5 to 8; the alcohol solvent with a carbon number of 1 to 8 may be methanol, ethanol, isopropanol, n-butanol, pentanol, hexanol, heptanol, octanol, etc.; the alkane solvent with a carbon number of 5 to 8 may be cyclopentane, cyclohexane, cycloheptane, cyclooctane, etc.

[0092] In some embodiments, the solvent includes a first solvent and a second solvent, and the step of washing the carrier functional layer with the solvent includes: immersing the carrier functional layer in the first solvent for 0.5 to 10 minutes, and then coating the second solvent on the side of the carrier functional layer away from the first electrode. Wherein, the first solvent and the second solvent are independently selected from one or more of an alcohol solvent with a carbon number of 1 to 8, acetone, and an alkane solvent with a carbon number of 5 to 8, and the two can be the same or different; in addition, the coating method includes but is not limited to spin coating, scraping, etc. Taking spin coating as an example, the spin coating speed is 1.5 to 5 k / min, for example, 1.5 k / min, 2 k / min, 3 k / min, 4 k / min, 5 k / min, and the values ​​between any two values ​​listed above; the spin coating time is 30s-2min, for example, 30s, 45s, 1min, 1.5min, 2min, and the values ​​between any two values ​​listed above.

[0093] In some embodiments, after step S40, the step of packaging the optoelectronic device 100 is also included. The packaging process can be performed by a common machine packaging or by manual packaging. Preferably, in the packaging process environment, the oxygen content and the water content are both lower than 0.1 ppm to ensure the stability of the optoelectronic device 100.

[0094] In the second aspect, the present application also proposes a photoelectric device 100, which is prepared by the above-mentioned preparation method, and the photoelectric device 100 includes a first electrode, a carrier functional layer and a second electrode, the material of the carrier functional layer includes a metal oxide and the organic material, the surface of the metal oxide has a cationic dangling bond, the organic material contains an active group, the active group is connected to the cationic dangling bond, and the active group includes one or more of a carboxyl group, a thiol group, and an amino group.

[0095] In some embodiments, in the carrier functional layer, the molar ratio of the metal oxide to the organic material is 1:(0.001-0.05).

[0096] In some embodiments, the organic material includes one or more of substituted or unsubstituted aromatic carboxylic acids and salts thereof, substituted or unsubstituted aromatic amines and salts thereof; the substituted or unsubstituted aromatic carboxylic acids include one or more of trifluorobenzoic acid, 4-chlorobenzoic acid, and 2-mercaptobenzoic acid; the trifluorobenzoic acid includes one or more of 2,4,5-trifluorobenzoic acid, 2,4,6-trifluorobenzoic acid, 2,3,6-trifluorobenzoic acid, and 2,3,4-trifluorobenzoic acid; the substituted or unsubstituted aromatic amines include one or more of 2-nitroaniline and 4,4'-diaminodiphenylamine.

[0097] In a third aspect, the present application further proposes a display device, which may be a smart phone, a portable phone, a tablet computer, a personal digital assistant (PDA), a portable multimedia player (Portable Multimedia Player), a television, a game console, a watch-type electronic device, a head-mounted display, a display of a personal computer, a notebook computer, a car navigation system, a car dashboard, a digital camera, a portable camera, an external advertising board, an electro-optical board, a medical device, a detection device, a refrigerator, a washing machine, etc. The display device includes the optoelectronic device 100 as described above.

[0098] The technical scheme and technical effects of the present application are described in detail below through specific embodiments and comparative examples. The following embodiments are only some embodiments of the present application and do not specifically limit the present application.

[0099] Example 1

[0100] (1) Provide an ITO anode with a thickness of 100 nm, wipe the ITO surface with a cotton swab dipped in a small amount of soapy water to remove impurities visible to the naked eye, then ultrasonically clean it with deionized water, acetone, anhydrous ethanol, and deionized water for 20 minutes, and then blow dry it with nitrogen for later use.

[0101] (2) Spin coating the PEDOT:PSS material on the anode at a rotation speed of 3000 rpm for 30 seconds and annealing at 100° C. for 10 minutes to obtain a hole injection layer with a thickness of 50 nm.

[0102] (3) The surface of the hole injection layer was spin-coated with TFB chlorobenzene solution at a speed of 3000 r / min for 30 s and annealed at 150° C. for 30 min to obtain a hole transport layer with a thickness of 40 nm.

[0103] (4) A hexane solution of CdZnSe blue quantum dots was spin-coated on the hole transport layer at a rotation speed of 3000 rpm for 30 s and annealed at 80° C. for 30 min to obtain a light-emitting layer with a thickness of 30 nm.

[0104] (5) Spin-coat a ZnO ethanol solution on the light-emitting layer at a rotation speed of 3000 rpm for 30 seconds and anneal at 80° C. for 30 minutes to obtain an electron transport layer with a thickness of 30 nm.

[0105] (6) Place the sheet prepared in step (5) into a vacuum coating machine and set the evaporation conditions to: vacuum degree 10 -4Pa, the evaporation temperature is 400°C, the evaporation rate is 1 angstrom / min, the evaporation time is 5min, and the passivation material - 2-nitroaniline is used as the target material. The evaporation is carried out on the electron transport layer, and the thickness of the obtained film is still 30nm, and in the film layer, the molar ratio of ZnO and 2-nitroaniline is 1:0.01.

[0106] (7) Place the sheet prepared in step (6) into a vacuum coating machine and set the evaporation conditions to: vacuum degree of 4×10 - 6 mbar, the evaporation temperature was 350°C, the evaporation rate was 3 angstroms / min, and the electrode was evaporated with an Ag target to obtain a cathode with a thickness of 60 nm. The device was then packaged in an environment where the oxygen content and water content were both lower than 0.1 ppm to obtain a QLED device.

[0107] Example 2

[0108] The scheme of this embodiment is basically the same as that of Embodiment 1, with the only difference being that in this embodiment, in step (6), the evaporation rate is changed to 0.5 angstroms / min.

[0109] Example 3

[0110] The scheme of this embodiment is basically the same as that of Embodiment 1, with the only difference being that in this embodiment, in step (6), the evaporation rate is changed to 5 angstroms / min.

[0111] Example 4

[0112] The scheme of this embodiment is basically the same as that of Embodiment 1, except that, in this embodiment, in step (6), the evaporation rate is changed to 5.5 angstroms / min.

[0113] Example 5

[0114] The scheme of this embodiment is basically the same as that of embodiment 1, except that in this embodiment, in step (6), the molar ratio of ZnO to 2-nitroaniline is 1:0.001.

[0115] Example 6

[0116] The scheme of this embodiment is basically the same as that of embodiment 1, except that in this embodiment, in step (6), the molar ratio of ZnO to 2-nitroaniline is 1:0.05.

[0117] Example 7

[0118] The scheme of this embodiment is basically the same as that of embodiment 1, except that in this embodiment, in step (6), the molar ratio of ZnO to 2-nitroaniline is 1:0.055.

[0119] Example 8

[0120] The scheme of this embodiment is basically the same as that of Embodiment 1, except that, in this embodiment, in step (6), the passivating agent used is 4-chlorobenzoic acid.

[0121] Example 9

[0122] The scheme of this embodiment is basically the same as that of embodiment 1, except that in this embodiment, in step (6), the passivating agent used is a combination of 2-nitroaniline and 4-chlorobenzoic acid, and the molar ratio of the two is 1: 1. During actual evaporation, 2-nitroaniline is first used as a target material for evaporation, and then 4-chlorobenzoic acid is used as a target material for evaporation.

[0123] Example 10

[0124] The scheme of this embodiment is basically the same as that of Embodiment 1, except that, in this embodiment, 2-nitroaniline is evaporated on the hole transport layer, and the electron transport layer is not evaporated. Correspondingly:

[0125] 1. Step (3) was changed to: Spin-coat the surface of the hole injection layer with a chlorobenzene solution of molybdenum oxide at a speed of 3000 r / min for 30 seconds, and anneal at 150°C for 30 minutes to obtain a hole transport layer with a thickness of 40 nm. Put the wafer with the hole transport layer into a vacuum coating machine, and set the evaporation conditions as follows: vacuum degree of 10 -4 Pa, the evaporation temperature is 250°C, the evaporation rate is 1 angstrom / min, the evaporation time is 5 min, and the passivation material - 2-nitroaniline is used as the target material to evaporate on the hole transport layer.

[0126] 2. Omit step (6).

[0127] Comparative Example 1

[0128] The scheme of this comparative example is basically the same as that of Example 1, except that in this comparative example, no passivation layer is provided, and accordingly, step (6) is omitted in the preparation method.

[0129] Comparative Example 2

[0130] The scheme of this comparative example is basically the same as that of Example 1, except that in this comparative example, in step (6), the passivating agent used is aluminum oxide, and a passivation layer is formed on the electron transport layer.

[0131] Comparative Example 3

[0132] The scheme of this comparative example is basically the same as that of Example 7, except that in this comparative example, the passivation layer is prepared by a solution method, and accordingly, step (6) is changed to:

[0133] Dispersing trifluorobenzoic acid in ethanol to obtain a passivation material solution with a concentration of 3 mg / ml;

[0134] The passivation material solution was spin-coated on the electron transport layer at a spin-coating speed of 3000 rpm for 30 s, and then annealed at 100° C. for 30 min to obtain a passivation layer.

[0135] Comparative Example 4

[0136] The scheme of this comparative example is basically the same as that of Example 1, except that in this comparative example, no passivation layer is provided, and the hole transport layer material is changed to molybdenum oxide. Accordingly, in the preparation method:

[0137] 1. Omit step (6);

[0138] 2. In step (3), TFB is replaced by molybdenum oxide.

[0139] The devices prepared in the above embodiments and comparative examples were tested for external quantum efficiency (EQE), turn-on voltage and lifespan T95@1000nit. The results are recorded in Table 1. Then, the devices were stored at room temperature and natural light for 10 days, and the external quantum efficiency (EQE), turn-on voltage and lifespan T95@1000nit were tested again, and the results are recorded in Table 1. The test method is as follows:

[0140] (1) External quantum efficiency EQE test

[0141] External quantum efficiency EQE represents the ratio of the number of electron-hole pairs injected into quantum dots to the number of emitted photons. The unit is %, which is an important parameter to measure the quality of electroluminescent devices. It can be obtained by measuring with EQE optical testing instruments. The specific calculation formula is as follows:

[0142]

[0143] Among them, η e is the light output coupling efficiency, η γ is the ratio of the number of recombined carriers to the number of injected carriers, x is the ratio of the number of excitons that generate photons to the total number of excitons, K R is the radiation process rate, K NR is the rate of the non-radiative process.

[0144] Test conditions: carried out at room temperature, air humidity is 30-60%.

[0145] (2) Lifespan T95@1000nit test

[0146] The lifespan T95@1000nit indicates the time required for the brightness of the device to decrease to a certain percentage of the maximum brightness when driven by a constant current or voltage. The time when the brightness drops to 95% of the maximum brightness is defined as T95, and this lifespan is the measured lifespan. In order to shorten the test cycle, the device lifespan test is usually carried out at high brightness by accelerating device aging, and the lifespan at high brightness is obtained by fitting the extended exponential decay brightness attenuation fitting formula. For example, the lifespan at 1000nit is calculated as T95@1000nit. The specific calculation formula is as follows:

[0147]

[0148] Among them, T95 L For lifespan at low brightness, T95 H is the measured lifetime under high brightness, L H To accelerate the device to the highest brightness, L L is 1000nit, A is the acceleration factor, and this experiment measured the lifespan of several groups of green QLED devices at rated brightness and found that the A value was 1.7.

[0149] Table 1

[0150]

[0151]

[0152] Refer to Table 1, we can see that:

[0153] Compared with Comparative Example 1, Examples 1 to 9 all have higher EQE and T95@1000nit, lower EQE change rate and turn-on voltage. At the same time, compared with Comparative Example 4, Example 10 has higher EQE and T95@1000nit, lower EQE change rate and turn-on voltage, indicating that the present application helps to improve the EQE of the device, enhance its stability and extend its life by evaporating on the carrier functional layer by physical vapor deposition. This may be because the evaporated organic material can passivate the defects on the surface of the carrier functional layer material, thereby improving its luminous efficiency and life;

[0154] Compared with Comparative Examples 2 and 3, Example 1 has higher EQE and T95@1000nit, lower EQE change rate and turn-on voltage. This may be because the evaporation process allows the organic material to enter the electron transport layer to a certain thickness and combine with the metal oxide, resulting in a better passivation effect. At the same time, the organic material itself also has the function of adjusting the work function, which helps to enhance electron injection.

[0155] In addition, compared with Examples 1 to 4, Examples 1 to 3 have significantly higher EQE and T95@1000nit, lower EQE change rate and turn-on voltage. This may be because when performing evaporation, controlling the evaporation rate within the range of 0.5 to 5 angstroms / min helps to improve the passivation effect, which is reflected in the improvement of luminous efficiency, lifespan and stability on a macro scale.

[0156] The optoelectronic devices, preparation methods and display devices provided in the embodiments of the present application are introduced in detail above. Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the methods and core ideas of the present application. At the same time, for technicians in this field, according to the ideas of the present application, there will be changes in the specific implementation methods and application scopes. In summary, the content of this specification should not be understood as a limitation on the present application.

Claims

1. A method for preparing a photoelectric device, characterized in that: The following steps are involved: Providing a prefabricated device and an organic material, wherein the prefabricated device comprises a first electrode and an initial carrier functional layer disposed on one side of the first electrode, wherein the material of the initial carrier functional layer comprises a metal oxide having cationic dangling bonds on the surface, and the organic material contains active groups; Depositing the organic material on a side of the initial carrier functional layer away from the first electrode to obtain a carrier functional layer; Disposing a second electrode on a side of the carrier functional layer away from the first electrode to obtain a photoelectric device; Wherein, the active groups include one or more of carboxyl, thiol and amino groups.

2. The preparation method according to claim 1, characterized in that: The step of depositing the organic material on the side of the initial carrier functional layer away from the first electrode to obtain the carrier functional layer includes: using physical vapor deposition to deposit the organic material on the side of the initial carrier functional layer away from the first electrode to obtain the carrier functional layer.

3. The preparation method according to claim 2, characterized in that: The step of depositing the organic material on the side of the initial carrier functional layer away from the first electrode by physical vapor deposition to obtain the carrier functional layer comprises: Providing a vacuum evaporation device having an evaporation chamber; The prefabricated device is placed in the evaporation chamber, and the organic material is used as a target to perform evaporation to obtain a carrier functional layer, wherein the carrier functional layer comprises the metal oxide and the organic material, and the active group of the organic material is connected to the cationic dangling bond.

4. The preparation method according to claim 3, characterized in that: During the evaporation, the evaporation conditions include: Vacuum degree is 10 -3 ~10 -5 pa; and / or, The evaporation temperature is 350-450° C.; and / or, The evaporation rate is 0.5 to 5 angstroms / min; and / or, The evaporation time is 1 to 5 minutes.

5. The preparation method according to claim 1, characterized in that: After obtaining the carrier functional layer and before arranging the second electrode on the side of the carrier functional layer away from the first electrode, the preparation method further includes: heating the carrier functional layer to 60-150° C. and annealing for 10-120 min.

6. The preparation method according to claim 1, characterized in that: After obtaining the carrier functional layer and before arranging the second electrode on the side of the carrier functional layer away from the first electrode, the preparation method further comprises: washing the carrier functional layer with a solvent.

7. The preparation method according to claim 6, characterized in that: The solvent includes one or more of an alcohol solvent having 1 to 8 carbon atoms, acetone, and an alkane solvent having 5 to 8 carbon atoms; and / or, The solvent includes a first solvent and a second solvent, and the step of washing the carrier functional layer with the solvent includes: immersing the carrier functional layer in the first solvent for 0.5 to 10 minutes, and then coating the second solvent on a side of the carrier functional layer away from the first electrode.

8. The preparation method according to claim 1, characterized in that: The organic material comprises one or more of substituted or unsubstituted aromatic carboxylic acids and salts thereof, substituted or unsubstituted aromatic amines and salts thereof, wherein the substituent is selected from at least one of C1-C8 alkyl, C1-C8 alkoxy, nitro, amino, mercapto and halogen; and / or, The melting point of the organic material is less than or equal to 300° C.; and / or, In the carrier functional layer, the molar ratio of the metal oxide to the organic material is 1:(0.001-0.05).

9. The preparation method according to claim 8, characterized in that: The substituted or unsubstituted aromatic carboxylic acid includes one or more of trifluorobenzoic acid, 4-chlorobenzoic acid, and 2-mercaptobenzoic acid; the trifluorobenzoic acid includes one or more of 2,4,5-trifluorobenzoic acid, 2,4,6-trifluorobenzoic acid, 2,3,6-trifluorobenzoic acid, and 2,3,4-trifluorobenzoic acid; and / or, The substituted or unsubstituted aromatic amine includes one or more of 2-nitroaniline and 4,4'-diaminodiphenylamine.

10. The preparation method according to claim 1, characterized in that: The initial carrier functional layer includes one or both of an electron functional layer and a hole functional layer; the electron functional layer includes an electron transport layer and / or an electron injection layer; the hole functional layer includes a hole transport layer and / or a hole injection layer.

11. The preparation method according to claim 10, characterized in that: The material of the electron transport layer is selected from at least one of ZnO, BaO, TiO2, SnO2; and / or, The material of the electron injection layer is selected from at least one of Al2O3 and Ga2O3; and / or, The material of the hole transport layer is selected from at least one of NiO, MoO3, WO3, V2O5 and CuO; and / or, The material of the hole injection layer is selected from at least one of NiO, MoO3, WO3, V2O5 and CuO.

12. The preparation method according to claim 10, characterized in that: The first electrode and the second electrode are each independently selected from a doped metal oxide particle electrode, a composite electrode of metal and metal oxide, a graphene electrode, a carbon nanotube electrode, a metal electrode or an alloy electrode; the material of the doped metal oxide particle electrode is selected from one or more of indium-doped tin oxide, fluorine-doped tin oxide, antimony-doped tin oxide, aluminum-doped zinc oxide, gallium-doped zinc oxide, indium-doped zinc oxide, magnesium-doped zinc oxide and aluminum-doped magnesium oxide; the composite electrode of metal and metal oxide is selected from AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, TiO2 / Ag / TiO2, TiO2 / Al / TiO2, ZnS / Ag / ZnS, ZnS / Al / ZnS; the material of the metal electrode is selected from one or more of Ag, Al, Cu, Mo, Au, Pt, Si, Ca, Mg and Ba; and / or, The prefabricated device further comprises a light-emitting layer, which is arranged between the initial carrier functional layer and the first electrode. The material of the light-emitting layer comprises one or more selected from organic light-emitting materials and quantum dot light-emitting materials. The organic light-emitting material is selected from 4,4'-bis(N-carbazole)-1,1'-biphenyl:tri[2-(p-tolyl)pyridine iridium(III), 4,4',4"-tri(carbazole-9-yl)triphenylamine:tri[2-(p-tolyl)pyridine iridium, diaromatic anthracene derivatives, distilbene aromatic derivatives, pyrene derivatives, fluorene derivatives, TBPe fluorescent materials, TT One or more of PX fluorescent materials, TBRb fluorescent materials, DBP fluorescent materials, delayed fluorescent materials, TTA materials, thermally activated delayed materials, polymers containing BN covalent bonds, hybrid localized charge transfer excited state materials, and exciplex luminescent materials, the quantum dot luminescent material is selected from at least one of single structure quantum dots, core-shell structure quantum dots, and perovskite semiconductor materials; the material of the single structure quantum dots, the core material of the core-shell structure quantum dots, and the shell material of the core-shell structure quantum dots are selected from II-VI group compounds, IV-VI group compounds, III-V group compounds, and At least one of the I-III-VI group compounds; the II-VI group compound is selected from CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, HgTe, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, At least one of CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe and HgZnSTe; the IV-VI group compound is at least one of SnS, SnSe, SnTe, PbS, PbSe, PbTe, SnSeS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, SnPbSSe, SnPbSeTe and SnPbSTe;The III-V compound is selected from the group consisting of GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaPSb, and AlN P, AlNAs, AlNSb, AlPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInN P, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs and InAlPSb; the I-III-VI group compound is selected from at least one of CuInS2, CuInSe2 and AgInS2; the perovskite semiconductor material is selected from doped or undoped inorganic perovskite semiconductors, or organic-inorganic hybrid perovskite semiconductors; the inorganic perovskite semiconductor has a general structural formula of AMX3, wherein A is Cs; + ion, M is a divalent metal cation selected from Pb 2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ , Mn 2+ 、Co 2+ , Fe 2+ ,Ge 2+ , Yb 2+ 、Eu 2+ At least one of, X is a halogen anion selected from Cl - Br - ,I - At least one of the following; the general structural formula of the organic-inorganic hybrid perovskite semiconductor is BMX3, wherein B is an organic amine cation selected from CH3(CH2) n-2 NH3 + or [NH3(CH2) n NH3] 2+ , where n≥2, M is a divalent metal cation selected from Pb 2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ , Mn 2+ 、Co 2+ , Fe 2+ ,Ge 2+ , Yb 2+ 、Eu 2+ At least one of, X is a halogen anion selected from Cl - Br - ,I - At least one of .

13. A photoelectric device, characterized in that: It comprises a stacked first electrode, a carrier functional layer, and a second electrode, wherein the carrier functional layer comprises a metal oxide and an organic material, wherein the organic material contains an active group, and the surface of the metal oxide has a cationic dangling bond, and the active group is connected to the cationic dangling bond; Wherein, the active groups include one or more of carboxyl, thiol and amino groups.

14. The optoelectronic device according to claim 13, characterized in that: The organic material comprises one or more of substituted or unsubstituted aromatic carboxylic acids and salts thereof, substituted or unsubstituted aromatic amines and salts thereof, wherein the substituent is selected from at least one of C1-C8 alkyl, C1-C8 alkoxy, nitro, amino, mercapto and halogen; and / or, The melting point of the organic material is less than or equal to 300° C.; and / or, In the carrier functional layer, the molar ratio of the metal oxide to the organic material is 1:(0.001-0.05).

15. The optoelectronic device according to claim 14, characterized in that: The substituted or unsubstituted aromatic carboxylic acid includes one or more of trifluorobenzoic acid, 4-chlorobenzoic acid, and 2-mercaptobenzoic acid; the trifluorobenzoic acid includes one or more of 2,4,5-trifluorobenzoic acid, 2,4,6-trifluorobenzoic acid, 2,3,6-trifluorobenzoic acid, and 2,3,4-trifluorobenzoic acid; and / or, The substituted or unsubstituted aromatic amine includes one or more of 2-nitroaniline and 4,4'-diaminodiphenylamine.

16. A display device, characterized in that: The invention comprises a photoelectric device prepared by the preparation method according to any one of claims 1 to 12, or a photoelectric device according to any one of claims 13 to 15.