Movtetaox and movtenbox catalysts with high strength and odh properties

By developing a heterogeneous molding catalyst of MoVTeNbOx catalyst and a vapor-phase silica support phase, combining polymer binder and inorganic binder, the problems of high energy consumption and coke accumulation in the existing olefin production methods are solved, and high mechanical strength and Excellent oxidative dehydrogenation activity improves the stability and selectivity of the catalyst.

CN119095668APending Publication Date: 2024-12-06NOVA CHEM (INT) SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380032422.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-01
Filing Date
2023-03-08
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing olefin production methods such as steam cracking and oxidative dehydrogenation have high energy consumption, coke accumulation and thermal explosion risks, limiting their commercial applications, and insufficient selectivity and stability of the catalyst.

Method used

A multiphase forming catalyst was developed, including the MoVTeNbOx catalyst active phase and the vapor phase silica support phase, combined with a polymer binder and an inorganic binder, and prepared with high mechanical strength and excellent oxidation and dehydration by wet preparation and sintering technology. A catalyst for hydrogen activity.

Benefits of technology

High mechanical strength and excellent ethylene selectivity are achieved, production costs are reduced, coke accumulation and thermal explosion risks are avoided, and the stability and selectivity of the catalyst are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119095668A_ABST
    Figure CN119095668A_ABST
Patent Text Reader

Abstract

Shaped catalyst compositions and methods for making and using the shaped catalyst compositions are provided. In an example, the catalyst active phase comprises a MoVTeNbOx catalyst. The composition further comprises a support phase, where the support phase comprises fumed silica, and where the catalytically active phase and the support phase form a heterogeneous mixture.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This document relates to heterogeneous shaped catalysts, methods of synthesizing the catalysts, and methods of using the catalysts. Background Art

[0002] Olefins such as ethylene, propylene and butene are the basic building blocks of a variety of commercially valuable polymers. Since naturally occurring olefin sources are not present in commercial quantities, polymer producers rely on methods for converting more abundant lower alkanes into olefins. The method of choice for commercial-scale producers today is steam cracking, a highly endothermic process in which steam-diluted alkanes are subjected to temperatures of at least 800° C. very briefly. The fuel requirements to produce the required temperatures and the need for equipment that can withstand the temperatures significantly increase the overall cost. In addition, high temperatures promote the formation of coke, which accumulates within the system, resulting in the need for expensive periodic reactor shutdowns for maintenance and coke removal.

[0003] Selective oxidation processes such as oxidative dehydrogenation (ODH) are alternatives to steam cracking that are exothermic and produce little or no coke. In ODH, lower alkanes such as ethane are mixed with oxygen in the presence of a catalyst and optionally an inert diluent such as carbon dioxide, methane, nitrogen or steam at temperatures as low as 300°C to produce the corresponding olefins. Various other oxidation products may be produced in this process, including carbon dioxide and acetic acid, among others. ODH has a lower conversion when compared to steam cracking, a fact that, when combined with lower selectivity and the risk of thermal explosion due to the mixing of hydrocarbons with oxygen, may prevent ODH from achieving widespread commercial application.

[0004] Shaped catalysts can be used for ODH of ethane. When producing heterogeneous catalysts, shaping is important. For fixed bed catalysts, the shape of the catalyst material facilitates many key things, including pressure drop across the reactor, heat and mass transfer, avoidance of fines during loading and handling, catalyst attribution / decomposition during process operation, and catalyst cost. Summary of the invention

[0005] The present disclosure describes a fumed silica formulation that produces a shaped catalyst with very high mechanical strength while maintaining excellent performance as measured by activity for the oxidative dehydrogenation (ODH) of ethane and ethylene selectivity.

[0006] In one embodiment, a composition is provided, the composition comprising a catalyst active phase, wherein the catalyst active phase comprises a MoVTeNbOx catalyst, the composition further comprising a support phase, wherein the support phase comprises fumed silica, and wherein the catalyst active phase and the support phase form a multiphase mixture.

[0007] In one aspect, the composition comprises a binder, wherein the binder comprises a polymeric organic acid, an amine or an alcohol. In one aspect, the binder comprises polyvinyl alcohol or polyethylene glycol or both. In one aspect, the binder comprises 60-80 wt.% polyvinyl alcohol and 20-40 wt.% polyethylene glycol.

[0008] In one aspect, the composition further comprises an inorganic binder, wherein the inorganic binder comprises talc or calcium carbonate.

[0009] In one aspect, the composition is sintered to form a ceramic.

[0010] In one aspect, the composition further comprises a plasticizer, wherein the plasticizer comprises polyethylene glycol.

[0011] In one aspect, the composition further comprises a lubricant. In one aspect, the lubricant comprises 1-2 wt. % of the composition, and the lubricant comprises graphite.

[0012] In one aspect, the fumed silica comprises 5-95 wt. % of the composition.

[0013] In one aspect, the composition is formed into a pressed tablet, wherein the pressed tablet has a density of 1.0-1.5 g / cm 3 .

[0014] In one aspect, the composition is formed into a sintered ceramic catalyst.

[0015] Another embodiment described herein provides a method for preparing a shaped catalyst. The method includes combining a catalyst active phase, a support phase, and a binder in an aqueous solvent to form an aqueous solution, wherein the catalyst active phase comprises MoVTeNbOx and the support phase comprises fumed silica. The method also includes heating the aqueous solution to form a thick paste, drying the thick paste to evaporate the aqueous solvent to form a solid powder, grinding the solid powder to form particles, and pressing the particles to form tablets.

[0016] In one aspect, grinding the solid powder to form particles comprises grinding the solid powder to form particles, wherein the particles have a diameter between 105 μm and 710 μm.

[0017] In one aspect, the method further comprises debinding the flakes, wherein debinding the flakes comprises heating the flakes to remove the binder, and sintering the flakes, wherein sintering the flakes comprises heating the flakes to coalesce the flakes into a dense solid. In one aspect, debinding the flakes comprises heating the flakes to 200° C.-400° C. at a rate of 1-2° C. / min. In one aspect, sintering the flakes comprises heating the flakes to 400° C.-600° C. at a rate of up to 5° C. / min.

[0018] Another embodiment described herein provides a method for preparing a shaped catalyst. The method includes combining a catalyst active phase, a carrier phase and a binder in an aqueous solvent to form an aqueous solution, wherein the catalyst active phase comprises MoVTeNbOx and the carrier phase comprises fumed silica, heating the aqueous solution to form a thick paste, and drying the thick paste to evaporate the aqueous solvent to form a solid powder. The solid powder is ground to form particles, and the particles are pressed to form a flake. The method includes debonding the flake, wherein debonding the flake includes heating the flake to remove the binder, and sintering the flake, wherein sintering the flake includes heating the flake to agglomerate the flake into a dense solid.

[0019] Another embodiment described herein provides a method for oxidative dehydrogenation of ethane. The method includes flowing a feed gas through a microreactor unit, wherein the feed gas comprises ethane, oxygen and nitrogen, pressurizing the feed gas in the microreactor, and contacting the feed gas with a shaped catalyst. The shaped catalyst comprises a catalyst active phase, wherein the catalyst active phase comprises a MoVTeNbOx catalyst; and a carrier phase, wherein the carrier phase comprises fumed silica, wherein the catalyst active phase and the carrier phase form a multiphase mixture. The method also includes heating the feed gas to 450°C-470°C and recovering ethylene gas.

[0020] In one aspect, the feed gas comprises ethane and oxygen in a molar ratio of 1:0.5.

[0021] The details of one or more embodiments of the present disclosure are set forth in the following drawings and description. Other features, objects, and advantages of the present disclosure will become apparent from the description and drawings, and from the claims. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 An exemplary schematic diagram of a shaped catalyst is shown.

[0023] Figure 2 An exemplary method of forming a shaped catalyst is shown.

[0024] Figure 3 A flow chart of an exemplary method of debinding and sintering a catalyst is shown.

[0025] Figure 4 is a flow chart of an exemplary process for the oxidative dehydrogenation of ethane.

[0026] Figure 5 The tabletability characteristic curve of the shaped catalyst 1.5 green tablet (shaped catalyst 1.5GB) is shown.

[0027] Figure 6 The tabletability characteristic curve of the shaped catalyst 1.7 green tablet (shaped catalyst 1.7GB) is shown.

[0028] Figure 7 The tabletability characteristic curves of the shaped catalyst 2.1GB comparative example tablets and the shaped catalyst 2.2GB comparative example tablets are shown.

[0029] Figure 8 MRU data for long term ethane to ethylene conversion of shaped catalyst 1.2SB pellets containing only MoVTeTaOx catalyst are shown.

[0030] Fig. 9 The results of long term ethylene selectivity testing of shaped catalyst 1.2SB pellets are shown.

[0031] Fig.10 The conversion rate MRU data of MoVTeTaOx supported shaped catalyst 1.3SB tablets is shown.

[0032] Fig.11 Shown is a graph of selectivity MRU data for MoVTeTaOx supported shaped catalyst 1.3SB pellets.

[0033] Fig.12 The conversion rate MRU data of MoVTeTaOx supported shaped catalyst 1.5SB tablets is shown.

[0034] Fig.13 Shown is a graph of selectivity MRU data for MoVTeTaOx supported shaped catalyst 1.5SB pellets.

[0035] Fig.14 The results of long-term ethane conversion testing of the shaped catalyst 1.7SB tablets are shown.

[0036] Fig.15 The results of long-term ethylene selectivity testing of shaped catalyst 1.7SB pellets are shown.

[0037] Fig.16 The long term ethane conversion of the shaped catalyst 1.8SB pellets is shown.

[0038] Fig.17 The ethane selectivity of the shaped catalyst 1.8SB tablets is shown.

[0039] Fig.18 Long term ethylene selectivity testing of formed catalyst 1.7SB and formed catalyst 1.8SB are shown, overlaid in a single figure.

[0040] Like reference symbols in the various drawings indicate like elements. DETAILED DESCRIPTION

[0041] Reference will now be made in detail to certain embodiments of the disclosed subject matter, examples of which are partially illustrated in the accompanying drawings.While the disclosed subject matter will be described in conjunction with the enumerated claims, it will be understood that the illustrated subject matter is not intended to limit the claims to the disclosed subject matter.

[0042] The present disclosure provides, in part, a composition and method for converting ethane into ethylene. The composition comprises a shaped catalyst, that is, a mixture of heterogeneous catalyst components that can be compacted into a predetermined shape (e.g., a cylinder). The shaped catalyst comprises a catalyst active phase, a carrier, and a binder. The catalyst active phase is a component responsible for catalyzing the conversion of ethane into ethylene in the presence of oxygen. In some embodiments, the catalyst active phase comprises a MoVTeTaOx catalyst. The MoVTeTaOx catalyst comprises molybdenum (Mo), vanadium (V), tellurium (Te), tantalum (Ta), and oxygen (O). The catalyst is represented by the formula MoVTeTaOx. In some embodiments, the ratio of the elements in the catalyst active phase is Mo1V 0.66 Te 0.17 Ta 0.09 In some embodiments, the ratio of the elements in the catalyst active phase is Mo1V 0.31 Te 0.22 Ta 0.10 In some embodiments, the catalyst active phase comprises a MoVTeNbOx catalyst.

[0043] The carrier in the shaped catalyst is important for the performance of the resulting shaped catalyst. For example, the carrier promotes the shaping and mechanical strength of the supported catalyst, can avoid fine particles during loading, can prevent catalyst loss during process operation, and can also be one of the ways to reduce the total cost of the shaped catalyst. The shape and carrier of the catalyst also improve heat transfer and mass transfer, can provide pores and channels to allow gaseous products to enter and leave the shaped catalyst, and can promote heat transfer away from the catalyst and reactants. In addition, the shape and size of the shaped catalyst can determine the pressure drop design on the reactor. The carrier can also reduce the total cost of manufacturing the shaped catalyst by allowing the catalyst particles to be dispersed through the carrier, allowing the reactants to more easily approach the active site. Therefore, the carrier plays many roles in the shaped catalyst. The example of the carrier / catalyst carrier (carrier) includes precipitated silica, fumed silica and alpha-alumina. The shaped catalyst described herein is synthesized with fumed silica.

[0044] The shaped catalysts herein comprise a fumed silica formulation that supports the catalyst and produces a shaped catalyst having very high mechanical strength while maintaining excellent performance as demonstrated by activity and ethylene selectivity for the oxidative dehydrogenation of ethane.

[0045] Compared with the flakes containing only catalyst, adding carrier to the catalyst flakes improves the overall catalyst performance. This is a surprising result. Without wishing to be bound by theory, despite the dense compaction of the shaped catalyst, the improved performance of the shaped catalyst may also be attributed to the improved ability of the feed gas to approach all catalyst particles in the shaped catalyst flakes. In theory, due to the lack of porosity, an increasingly dense catalyst flake associated with high mechanical strength is produced. However, by including a silica carrier in the catalyst, the catalyst retains some porosity without compromising mechanical strength. In addition to high mechanical strength, the shaped catalyst comprising fumed silica shows new material properties due to the inclusion of a fumed silica carrier. Typically, silica is usually a challenging material that is expanded (agglomerated) into a mechanically strong macroscopic shape. For example, it is difficult to agglomerate silica into a shape greater than 200 μm, which is typical for the spray-dried silica used in other multiphase technologies such as gas phase polyethylene production. However, as described herein, the catalyst comprising fumed silica with an oxidative dehydrogenation catalyst active phase produces a catalyst material with unique characteristics different from single fumed silica. Shaped catalysts with fumed silica support materials have processability characteristics that outperform other tableted ceramic materials such as alumina. This characteristic is illustrated by a tabletability profile, a comparison of the radial tensile strength of the tablets as a function of compaction pressure. The tabletability profile is discussed herein in Examples 2 and 3. In addition, as shown in Examples 5 and 6, the catalyst tablets described herein have very high density and mechanical strength.

[0046] The shaped catalyst described herein also includes a binder. The binder in the shaped catalyst described herein is an additive that helps to agglomerate and makes the entire mixture easier to form. In some embodiments, an organic additive can be used as a binder. Suitable organic binders include polymer organic acids, amines or alcohols or particles that can allow cross-linking, such as polyvinyl alcohol. In some embodiments, an inorganic binder can be used. Suitable inorganic binders include soft (low Mohs hardness value) salt minerals, such as talc or calcium carbonate. In some embodiments, the binder can be a mixture of two or more binders. For example, the binder can include a mixture of polyvinyl alcohol (PVA) and polyethylene glycol (PEG). In some embodiments, the binder includes 80wt.% PVA and 20wt.% PEG. In some embodiments, the binder includes 60wt.% PVA and 40wt.% PEG.

[0047] In some embodiments, the shaped catalyst can also include plasticizer, lubricant or both plasticizer and lubricant.Plasticizer is an additive that acts on an organic binder.The combination of organic binder and plasticizer is more plastic than these two independent compositions.The amount and type of plasticizer can be selected based on the ability of the plasticizer to reduce the glass transition temperature of the polymer binder.In some embodiments, plasticizer can include polyethylene glycol.

[0048] In some embodiments, the shaped catalyst further comprises an inter-particle or intra-particle lubricant. A lubricant is an additive added to the granulated powder to help the compressed shape release more easily from the mold cavity and to prevent equipment clogging and excessive wear.

[0049] Figure 1 An exemplary schematic diagram of a shaped catalyst 100 is shown. The shaped catalyst 100 can include active phase catalyst particles 102, carrier particles 104, a binder 106, an inter-particle lubricant 108, and an intra-particle lubricant 110. The shaped catalyst 100 can include any combination of features 102-110, but not necessarily all features 102-110. For example, the shaped catalyst 100 can include active phase catalyst particles 102, carrier particles 104, and a binder 106.

[0050] The shaped catalysts described herein can be used to catalyze the oxidative dehydrogenation of ethane. The oxidative dehydrogenation of ethane is shown in Eq.

[0051]

[0052] In some embodiments, the shaped catalyst described herein comprises a MoVTeTaOx active catalyst phase. In some embodiments, the shaped catalyst described herein comprises a MoVTeNbOx active catalyst phase. Comparative examples of shaped catalysts without active catalyst phases or with alternative carrier phases are also produced. The formulas of the shaped catalysts analyzed in Examples 1-11 are shown in Table 1. The silica carrier in Table 1 is fumed silica. However, in some embodiments, silica can be other forms of silica. For example, precipitated silica (hydrated), fumed silica (small size dehydrated) or colloidal silica (small size hydrated) or any mixture thereof can be used as a silica carrier. The silica carrier can account for 5-95wt.% of the composition. In some embodiments, silica accounts for 40-80wt.% of the composition. In some embodiments, the flakes contain intragranular lubricants. The lubricant is applied by dry mixing by manually tumbling in a drum for 5 minutes. The shaped catalysts described herein and in Table 1 are synthesized using wet preparation, briquetting, granulation and tableting, as described in more detail herein. Figure 2 An exemplary method 200 for forming a shaped catalyst is shown. At 202, a catalyst active phase, a support phase, and a binder are combined in an aqueous solvent to form an aqueous solution. At 204, the aqueous solution is heated to form a thick paste. At 206, the thick paste is dried to evaporate the aqueous solvent and form a solid powder. At 208, the solid powder is ground to form particles. At 210, the particles are pressed to form tablets. In some embodiments, the method also includes debonding and sintering the tablets. The method of forming a shaped catalyst is described in more detail herein.

[0053] Wet preparation

[0054] The synthetic shaped catalyst includes wet preparation. The ingredients added to the formulation to produce the composition that can be formed depend on the specific molding method used (for example, tableting or extrusion) and what characteristics are built into the final shape. In the catalyst formulation selection stage, the shape, processing equipment and composition must be fully considered. The judicious selection of ingredients (for example, adhesives or lubricants) will affect how wet powder or dry powder agglomerates, is processed by equipment, is pressed under force, sintered and resists wear / crushing force. In addition, the composition and shape have a decisive influence on the final performance of the catalyst. In addition to meeting the requirements of the expected processing unit, the shape and composition must also give enough mechanical properties to withstand transportation, reactor loading, operation and reactor unloading.

[0055] In order to convert the material into a formable composition, the ingredients are blended into a homogeneous mixture of uniform distribution to produce catalyst components. The ingredients of the shaped catalyst described herein are wet formulated into a uniform paste, which is then dried and processed into particles. The wet formulation method mixes the ingredients and starts the agglomeration process. The shaped catalyst described herein is wet formulated with a benchtop mixing device, such as a beaker, an oil bath, and a low shear overhead stirrer. Wet formulation is performed under heating and mixing to evaporate excess water and convert the suspension of ingredients into a uniform paste. The paste is then dried overnight in an oven at 105-110°C.

[0056] Briquetting / agglomeration

[0057] After drying overnight, the resulting dry "cake" is then ground with a mortar and pestle, and fed into a die set with a diameter of 40mm to form a compact in a press. 7g of formula powder is loaded into a 40mm die set, pressed under a force of 12 metric tons, and kept for 60 seconds under this force. The force applied to the formula powder varies with cross-sectional area, and therefore, depending on the size of the compact, enough force should be used to cause the reunion of powder. Compact can be formed in a press. Alternatively, compact and granulation can be completed with a high shear mixer. Take out the disc-shaped compact produced. By grinding the compact into particles and sieving particles to collect required particle size distribution, particles are produced by compact.

[0058] Granulation

[0059] An important step in tableting is the conversion of the fine powders of the individual components of the shaped catalyst into agglomerated, size-enhanced particles. This step is known as granulation. Granulation is important for a number of reasons.

[0060] Granulation can improve the flow characteristics of materials so that they can flow from the hopper into the mold cavity. The flowability of ceramic powders can be defined and measured using the definitions and methods available in ASTM D6103 / D6103M. Powders with too small particle sizes will result in "caking", in which particles cannot flow smoothly over each other. Agglomeration of small particles can be caused by static electricity, or by increasing van der Waals interactions due to increased surface area relative to volume. These forces can overcome the gravity acting on the particles. In addition, granular particles are better compacted than unmodified fine powders, resulting in flakes with higher and more consistent density. Without wishing to be bound by theory, particles show better compaction than fine powders because they can plastically deform and / or break during the rearrangement of granular particles when the particles are uniaxially compressed. Plastic deformation and / or breaking allow particles to fill void spaces and have more inter-particle contact with other particles.

[0061] Granule size distribution was found to affect mechanical strength, particularly for tablets manufactured using the automatic loading mode of an automated tablet press. Therefore, a study was conducted to determine how different granule size distributions would affect the crush strength of automatically loaded tablets.

[0062] suppress

[0063] As described herein, the shaped catalyst is formed using tableting (also known as uniaxial molding or dry pressing).

[0064] Tablets formulated as described in Table 1 were made using a CPR-6 automatic press from DOTT.BONAPACE&C.SRL, Milan, Italy or a CPR-6 automatic press from Carver, Inc., Wabash, Indiana, USA. Manual press produces. CPR-6 automatic press has adjustable force and replaceable diameter die set of up to 2.5 metric tons. The die set used herein is a cylindrical cavity of 0.125 inches (3.175mm) OD with a flat punch. The sheet is formed by the combined pressing action of two punches in the die. In the first step of the press operation, the bottom punch descends in the die to produce a cavity, and the catalyst material powder is fed into the cavity via a hopper shoe. The precise depth of the lower punch is accurately set to measure the volume of the powder filling the cavity. The excess part is scraped off from the top of the die by the hopper shoe. Next, the upper punch is contacted with the powder downward, and the compression force is delivered by a high-pressure compression roller, which compresses the catalyst material together to form a hard granular material in the shape of a die. After the compression step, the lower punch rises to discharge the granules from the die cavity. Finally, during the subsequent die cavity filling, the sheet is pushed away from the tableting table by the hopper shoe. The granules are knocked off from the table into a collecting tray.

[0065] The compression force can be adjusted by moving the upper die up or down. The upper die set has a configuration of settings 1 to 8, where 8 is the highest compression force. The compression force ranges from 520MPa to 1040MPa. In addition, the lower die adjustment can also change the resulting linear displacement and affect the final compression force. The lower die can be twisted up or down to make the final sheet height lower (more compression) or higher (less compression). The lower die can be labeled with three settings "1", "2" and "3". Lower die setting 3 is the highest compression force, while 1 is the lowest compression force. Since the compression varies with the recipe of the sheet itself, the upper and lower dies can be adjusted based on recipe to recipe.

[0066] The speed of the automatic press can also be adjusted. Lower speeds allow the compressed material to be shaped and conform to the die set, thereby producing a stronger and less prone to "capping" flakes when the upper and lower portions of the flakes separate horizontally from the body. However, the speed of the automatic press should be high enough to provide adequate throughput. It was found that for a range of different formulation materials, speed setting "2" produced flakes with high crush strength. The speed can be adjusted depending on the equipment used to produce the flakes.

[0067] In some embodiments, the tablets can be formed using a CARVER press, which is a manual press with a force reading gauge that can form tablets at different compression forces. The CARVER press can be used to form tablets with a diameter of 6 mm.

[0068] Compressing the formulated particles produces green tablets, i.e., tablets that have not been debonded or sintered. The green tablets are analyzed to produce a tabletability profile. The tabletability profile can be used to compare the response of the particle formulation to compaction, wherein an ideal material will have a tensile strength that increases with increasing compaction pressure. The tensile strength of an ideal formulation increases with compaction pressure until a maximum tensile strength is reached, after which additional compaction pressure will not improve mechanical strength.

[0069] The tabletability characteristic curve can also be used to interpolate the compaction pressure required to obtain a green sheet with sufficient strength (i.e., at least 1-2 MPa tensile strength). As described herein, the green sheet strength must be high enough to allow the sheet to be discharged intact from the tablet press and to maintain subsequent processing before the debonding and sintering steps. The axial and radial crushing strengths of the shaped catalysts and comparative examples are described in Examples 2-5. The tensile strength used in the tabletability characteristic curve is typically calculated based on the radial crushing strength.

[0070] When comparing tablets of different sizes, it is common to convert crush strength (breaking force, in Newtons) to tensile strength (compression, MPa) because the tensile strength calculation takes into account the tablet size. Radial (or diametral) tensile strength is calculated based on the following formula:

[0071]

[0072] where σ t is the tensile strength in MPa, P is the breaking load in Newtons (N) (radial crushing strength), D is the tablet diameter in millimeters, and t is the tablet height in millimeters. The radial tensile strength is typically used to generate tabletability profiles as well as tablet compaction and compression profiles.

[0073] Debonding

[0074] As described herein, the green pellets have been pressed but not debinded or sintered. Before the shaped catalyst can be used in a catalytic reaction, such as oxidative dehydrogenation, the shaped catalyst is debinded and sintered.

[0075] The debinded body table has undergone a debinding step to remove the organic binder. This step is performed before moving to the final sintering step. In some embodiments, the debinding step includes a heat treatment step. The heat treatment is performed slowly during thermal debinding. The green sheet is heated under air to burn off the organic additives. During the debinding step, the combustion produces water and carbon dioxide gas. Therefore, the debinding step is carefully controlled to prevent high pressure gas from accumulating in the table.

[0076] Debonding removes organic binders and plasticizers from the green sheet. Therefore, the maximum temperature of the debonding step is based on the organic binder and / or plasticizer in the green sheet. For example, pure polyvinyl alcohol (PVA) has a decomposition range of about 200°C to about 300°C, depending on the molecular weight distribution of PVA. In another example, pure polyethylene glycol has a decomposition range of about 150°C to about 250°C, depending on the molecular weight distribution of PEG. Therefore, if PEG is used as a binder in the shaped catalyst formulation, the minimum debonding temperature should be about 250°C.

[0077] In some embodiments, the heat treatment is carried out under an air atmosphere to promote the combustion of the binder (e.g., polyvinyl alcohol). In some embodiments, the ramp rate of the heat treatment step is 1-2°C / min or less to avoid cracking or splitting of the flakes due to carbon dioxide, steam, and other gases released during the heat treatment step. The highest debonding temperature applied in the debonding method described herein is 550-600°C. However, the debonding temperature herein is lower than 400°C to avoid oxidizing the catalyst. For the MoVTeTaOx molded catalysts described in Table 1 (molded catalysts 1.2-1.7), the debonding temperature is 400°C and the ramp rate is 1°C / min. The debonding temperature does not exceed 400°C because such high temperatures in the presence of an air atmosphere can cause the catalyst to deactivate. Debonding is carried out in a catalyst calcining furnace.

[0078] sintering

[0079] After debonding, the flakes are subjected to a sintering step to increase their mechanical strength and produce a ceramic final product. Ceramics are any of a variety of hard, brittle, heat-resistant and corrosion-resistant materials made by shaping inorganic non-metallic materials such as clay and then firing them at high temperatures. The sintering step also produces bridges / bonds between particles and agglomerates the particles into a dense solid with increased mechanical strength. Sintering is a kinetic phenomenon between particles and can occur naturally if enough time is allowed. However, high temperatures can greatly accelerate sintering, reducing the sintering time to a few hours. For the flakes described herein, heat treatment is performed under an inert atmosphere during hot sintering to avoid catalyst oxidation. Sintering is typically performed at a higher temperature than debonding, and since there is no additional gas product or almost no gas product released from the compacted tablet at this stage, the ramp rate can be higher, for example, up to 5°C / min. In some embodiments, the maximum temperature applied during the sintering step is 600°C. The sintering step produces a final ceramic shaped catalyst without a binder. Sintering can control both densification and grain growth. Densification reduces the porosity in the sample, making it denser and stronger. Grain growth is the process of grain boundary movement to increase the average grain size. Mechanical strength properties benefit from both high relative density and small grain size. Therefore, when sintering tablets, it is desirable to use a higher ramp rate to prevent large grain size. Although the loss of gaseous products is low during the sintering step, some water in the form of steam can still escape from the formed catalyst. The amount of water loss can be determined via the loss on ignition test (LOI), which is the ASTM test described in UOP954-11.

[0080] For the MoVTeTaOx catalysts described in Table 1, the sintering temperature applied was 600°C and the ramp rate was 1.6°C / min. Although the MoVTeTaOx shaped catalysts described in Table 1 were sintered at a ramp rate of 1.6°C / min, faster ramp rates may also be suitable. However, faster ramp rates may produce weaker final materials, which is caused by thermal stresses or sudden release of water inside each particle, which may crack the particles or reduce their mechanical integrity. The MoVTeTaOx and MoVTeNbOx catalysts in Table 1 were sintered in a catalyst calciner. Sintering was carried out under nitrogen flow because, as described herein, temperatures above 400°C in air can cause catalyst deactivation.

[0081] Figure 3A flow chart of an exemplary method 300 for debonding and sintering a catalyst is shown. At step 304, a green sheet 302 containing an organic binder 301 is debonded in air at 400°C. Carbon dioxide (CO2) gas 305 is released from the green body to produce a debonded body 306. Next, at step 308, the debonded body is sintered at 600°C under an inert gas. In some embodiments, the inert gas is nitrogen. Sintering produces a shaped catalyst 310 with increased mechanical strength. Surprisingly, the shaped catalysts described herein exhibit high mechanical strength despite the lack of a binder.

[0082] The formed catalysts described herein were tested for their ability to catalyze the oxidative dehydrogenation of ethane using a microreactor unit (MRU). The MRU has a The reactor tube was made of tubing with an outer diameter of 0.5 inches (1.27 cm), an inner diameter of about 0.4 inches (1.02 cm) and a length of about 13.4-15 inches (34.0-38.1 cm). The experimental temperature of the MRU was measured using a 6-point WIKA Instruments Ltd. K-type thermocouple, which had an outer diameter of 0.125 inches (0.318 cm) and was inserted through the reactor. The 6-point thermocouple was used to measure and control the temperature in the catalyst bed. A room temperature stainless steel condenser was located after the reactor to collect water / acetic acid condensate. The gas product stream was allowed to discharge or during the time required for product gas analysis, the gas product was directed to an Agilent 8890 "hot gas" gas chromatograph (HGGC). Due to size restrictions during the MRU test, the catalyst pellets were gently crushed into particles using a mortar and pestle. The resulting particles were sieved, and particles with a particle size distribution between 425 μm and 1000 μm were collected and loaded onto the MRU for testing. In some embodiments, the shaped flakes can be used as catalysts without pelletizing. Depending on whether the shaped catalyst contains a carrier, two loading methods are used to maintain 5.46h -1 of constant weight hourly space velocity (WHSV).

[0083] For the shaped catalyst without a support (i.e., shaped catalyst 1.2), 2.00 g of sieved catalyst with a particle size range of 425 μm to 1000 μm from the crushed pressed catalyst was physically mixed with quartz sand (50-70 mesh) such that the mixture produced a total catalyst bed volume of 6 mL. Once the catalyst bed was loaded into the reactor and connected to the MRU equipment, the test was performed as described herein.

[0084] For the shaped catalysts with supports, 4.00-5.00 g of compressed catalyst material with a particle size range of 425 μm to 1000 μm was physically mixed with quartz sand such that the mixture produced a total catalyst bed volume of 6 mL. Since all catalyst materials were prepared with about 40 wt.% catalyst active phase, the weight loading of catalyst in the MRU test device was in the range of 1.60-2.00 g.

[0085] For both supported and unsupported catalysts, the catalyst bed was loaded in the middle region of the reactor - between points 2 and 5 of the thermocouple - and the remaining volume of the reactor was filled with quartz sand. The reactor loading was then secured with glass wool at both the top and bottom of the reactor. The addition of quartz sand was performed to produce a catalyst bed volume of 6 mL to ensure that the catalyst volume was sufficient to cover the thermocouple area between points 2 and 5. When the catalyst was supported, the support increased the bed volume, so that less quartz sand was needed to produce 6 mL of bed volume.

[0086] For the MRU test, a premixed feed gas composition is obtained via an upstream gas blending device including a calibrated mass flow controller. The premixed feed gas composition is fed through the reactor. The premixed feed gas entering the reactor is 20 mol.% ethane, 10 mol.% oxygen and 70 mol.% nitrogen (the molar ratio of ethane to oxygen is 1 / 0.5), and the reactor outlet is pressurized to 20 psig (0.14 MPa) using a back pressure regulator. In addition, the premixed feed gas flow rate is adjusted by a calibrated mass flow controller to obtain a constant weight hourly space velocity (WHSV) based on the weight of the catalyst active phase in the entire catalyst bed.

[0087] The flow rate of the premixed feed gas was controlled between 152 and 157 standard cubic centimeters (sccm) depending on the weight loading to achieve a 5.46 h -1The constant WHSV of the catalyst. The gas hourly space velocity (GHSV) is calculated based on the measured volume of the pressed particles (before mixing with quartz sand) and varies according to the bulk density of each catalyst or catalyst material. In the case where WHSV is defined as the mass flow rate of the feed gas to the reactor divided by the weight of the catalyst in the catalyst bed, GHSV is defined as the volume flow rate of the reactor feed gas divided by the volume of the catalyst bed. For the GHSV value of the supported catalyst, the catalyst bed contains a diluent (including the carrier volume). Only the GHSV value of the catalyst can be calculated, where the total volume of the measured catalyst material is calculated as the volume of the catalyst when multiplied by the wt.% of the catalyst. In this article, the GHSV value is provided as the total volume of both the catalyst and the catalyst material. This is a different reporting method from the method applied for WHSV, which is only for the catalyst weight without considering the carrier weight. Therefore, supported catalysts and non-supported catalysts will have similar WHSVs, but different GHSVs. For supported catalysts, the reported GHSV is only for the catalyst, where the total volume of the measured catalyst material is calculated as the volume of the catalyst when multiplied by the wt.% of the catalyst.

[0088] For the MRU experiment, at 5.46h -1 WHSV and between 3000 and 7000h -1 The mol.% ethane conversion is determined at a gas hourly space velocity (GHSV) in the range of 100 ℃ to 200 ℃. During the run, the gaseous products leaving the catalyst bed are directed to exhaust. When the gaseous products are to be analyzed, they are immediately redirected to a gas chromatography unit to determine the percentages of ethane, ethylene, O2, CO2, CO and acetic acid. The gases leaving the reactor are analyzed by hot gas, gas chromatography (HGGC). The conversion (C) of the ethane feed gas is calculated as the change in the volume flow rate of ethane in the product compared to the mass flow rate of the feed ethane using the following formula:

[0089]

[0090] In Equation 3, X is the molar concentration of the corresponding compound in the gaseous effluent leaving the reactor at the corresponding temperature.

[0091] In addition, the gases leaving the reactor are analyzed by GC to determine the selectivity of the catalyst or catalyst material to ethylene (i.e., the mole percentage of ethane that forms ethylene). 乙烯 ) is determined using the following equation:

[0092]

[0093] In the above equation, S 乙烯 is the selectivity to ethylene and X is the molar concentration of the corresponding compound in the gaseous effluent leaving the reactor at the corresponding temperature.

[0094] Figure 4 4 is a flow chart of an exemplary method 400 for oxidative dehydrogenation of ethane. At 402, a feed gas comprising ethane, oxygen, and nitrogen is flowed through a microreactor unit. At 404, the feed gas is pressurized to 20 psig (0.14 MPa). In some embodiments, the feed gas can be pressurized to 2-80 psig. At 406, the feed gas is contacted with a shaped catalyst as described herein. At 408, the feed gas is heated to 450°C-470°C. At 410, ethylene gas is recovered.

[0095] The catalyst was analyzed with MRU short-term operation and MRU long-term operation. The MRU short-term operation was carried out one day before the long-term operation to determine the conditions for about 50 mol.% ethane conversion. For the MRU short-term operation, the catalyst was tested on the MRU under several temperature conditions of 340-480°C while keeping the feed composition and weight hourly space velocity (WHSV) constant. Under each temperature condition, the gas sample was subjected to gas chromatography (GC) to obtain the composition of the gas product. The conversion is calculated by the percentage of atomic carbon in the ethane product relative to the atomic carbon in all carbon products containing ethane, ethylene, carbon dioxide and carbon monoxide, as shown in Equation 3. Ethylene selectivity is calculated by the percentage of ethane to ethylene at each temperature. When calculating the conversion and selectivity, the amount of acetic acid formed is small enough to exclude the amount of acetic acid from Equations 3 and 4.

[0096] Once the 50 mol.% ethane conversion temperature is determined in the short run, a long-term MRU experiment is performed at this temperature. The MRU is raised to the determined temperature and the process is allowed to stabilize (usually about 30 minutes). After the process stabilizes, a GC injection is performed to confirm that the ethane conversion is close to 50 mol.% (± 2%). If the conditions are suitable to achieve 50 mol.% ethane conversion, the MRU long-term run is started, otherwise the conditions (temperature) are adjusted to make the conversion closer to the target conversion. Once the stable conversion and selectivity target conditions are met, the experimental timer for the long-term run is started.

[0097] Long-term MRU operation produces information about the stability of catalyst performance as the duration increases, or in heterogeneous catalysis, often referred to as "time on stream" (TOS). Ideally, as the duration of TOS increases, the catalyst conversion and selectivity percentages should be stable and remain relatively unchanged throughout the duration of the experiment. It is common for heterogeneous catalysts to be more active (higher conversion percentages) within the first 24-72 hours, after which the conversion stabilizes. However, the key trend observed in long-term operation is that at a certain point in the experiment, the conversion trend of the catalyst tends to be unchanged (a flat or nearly flat line trend on the x relative to y curve) as the experimental time increases. Similarly, if not more important, ethylene selectivity also shows a stable trend that does not decrease with increasing TOS. MRU long-term effectiveness testing was conducted over a run time of 42 days or 1008 hours.

[0098] In MRU experiments or other catalytic processes, the catalyst may also exhibit deactivation over time. Advantageously, the formed catalysts described herein have very subtle deactivation trends that only become apparent in long-term experiments (e.g., 300+ hours). The deactivation rate can be expressed as mol.% ethane conversion absolute / hour. Therefore, the catalysts described herein are stable in long-term experiments and can be reused multiple times.

[0099] Table 1: Catalyst formulations and compositions of Examples 1-11

[0100]

[0101]

[0102]

[0103] Reagents used for the experiments described herein were purchased from the manufacturers and used as received without further purification. The following chemicals were purchased from Sigma Aldrich: fumed amorphous silica (Product No. S5130), natural graphite (Product No. 1002969522),

[0104] 4-88 31,000 MW polyvinyl alcohol (Product No. 81381), 1000 MW polyethylene glycol (Product No. 81189), and magnesium stearate (Product No. 415057). The following chemicals were obtained from Saint-Gobain: α-alumina Silica XS 69025 catalyst support flakes (sample number 2001910060), aluminum silicate SA 3X32 catalyst support flakes (sample number 2002920068) and gamma-alumina SA 6X73 catalyst support flakes (sample number 2007910008). PM100 was prepared by dry ball milling of α-alumina (DENSTONE 99) for use. Dry ball milling was performed using 3 mm zirconia balls and a 500 mL zirconia grinding jar. Precipitated synthetic amorphous silica was obtained from PQ Corporation, product identification number C935.

[0105] In some embodiments, the active phase of the MoVTeTaOx catalyst is obtained by mixing (NH4)6Mo7O 24 4H2O(s) salt (2372.0 g; 1.9 mol) was dissolved in 27 L of distilled water in a 50 L heated glass vessel at 60°C, with another 3 L of distilled water used for rinsing (part: 1 L for rinsing powder + 2 L after transferring the solution to the SS reactor).

[0106] (NH4)6Mo7O 24 The (aq) solution was clear and colorless, and the pH was 5.04 at 55.0°C. Te(OH)6(s) salt (514 g; 2.25 mol) was dissolved in 2 L of distilled water in a 20 L heated PFA container at 55°C, with an additional 3 L of distilled water rinse (1 L + 2 L portions). The Te(OH)6(aq) solution was clear and colorless. The Te(OH)6(aq) solution was transferred all at once to the (NH4)6Mo7O 24 There was no visible change in the solution after the addition, however, the pH dropped to 3.20 at 53.0 °C. 24After the solution reached 55°C, the pH of the solution was adjusted to pH 5.2 via dropwise addition using 104.7 g of 28 wt.% NH4OH(aq). The final pH was measured at 56.9°C to be 5.23. The temperature of the solution was raised to 78°C and the solution was allowed to reach 78°C over 1 hour and 25 minutes. The solution was allowed to stir at 78°C for 1 hour. The pH was measured again at 78°C to be 4.91 and the solution was then cooled back to 60°C. The 60°C solution was pumped into a 100 L glass-lined SS reactor vessel that was preheated to a shell temperature of 60°C. VOSO4·3.36H2O salt (1989 g; 8.902 mol) was dissolved in 8 L of distilled H2O in a heated perfluoroalkoxy (PFA) 20 L vessel at a temperature of 55°C and rinsed with an additional 4 L of water (2L+2L). The VOSO4(aq) solution was clear and bright blue. Once homogenous, the 55°C VOSO4(aq) solution was transferred to a 100 L SS reactor vessel at a controlled pump rate of 367 mL / min to react with (NH4)6Mo6TeO while stirring at 22 rpm. 24 (aq) solution mixing.

[0107] At room temperature, 1.3L of tantalum reagent (192g Ta2O5 and 122g oxalate per 1L aqueous solution) was diluted with 2L of distilled water in a 20L PFA container. Another 3L of distilled water was used for rinsing (1L+2L). The tantalum oxalate solution was pumped into the MoTeV solution in the SS reactor at a rate of 183mL / min while mixing the reactor contents at 22rpm. Once the addition was complete, the reaction mixture was allowed to stir in air at 60°C for 1 hour. The total volume of water used for the reaction (including rinsing) was 53L. The reactor was sealed and the headspace was purged 4x with 10psig nitrogen and vacuumed alternately. The reactor was kept sealed with 20psig nitrogen headspace. The back pressure regulator was set to a set point of about 140psig, and the thermal controller was set to 165°C. The limit setting of the reactor shell temperature was 195°C. After about 20 hours, the slurry in the reactor reached 160°C. The time of the reaction started from this point. The reaction time was 48 hours. The registered reactor internal pressure reached a maximum of 103 psig. After 48 hours of reaction, the reactor heater was turned off and the slurry was allowed to cool to 68° C. while continuing to stir. The dark purple slurry was transferred to a filtration unit where the solids were filtered. The catalyst cake formed on the filter was rinsed with a total of 200 L of distilled water in 40 L and 20 L portions.

[0108] This device is attached to the reactor head, but is a double tube heat exchanger (condenser) with cooling water circulating on the external line at about 25°C (controlled via a closed system, cooling bath), and the internal line is connected to the reactor (process) to allow excess gas pressure to be vented via a back pressure regulator.

[0109] The resulting solid cake was removed from the filter unit and transferred to an oven where it was dried in air at 90° C. for 4 days. The weight of the dry cake was 1937 g, with a yield of 57%. The filter cake was ground into a powder using a RETSCH jaw crusher BB50 grinder.

[0110] The uncalcined filter cake was loaded into two quartz boats and the catalyst was air conditioned in an oven at 250°C for 6 hours. After air conditioning, the boats were transferred to the quartz tube of the catalyst calcining furnace and purged overnight with a large amount of nitrogen at a flow rate of 1000 sccm. Two hours before starting the furnace, a large inlet nitrogen purge (<10 ppm oxygen) was redirected through an oxygen trap (LabClear Oxiclear TM A gas purge was used to purge the tube with purified nitrogen (<1 ppm oxygen). The catalyst was calcined at 600°C for 4 hours under purified nitrogen. The calcination was ramped at a rate of 1.6°C / min. After cooling to room temperature, the calcination yield was determined to be 93.5 wt.% recovery.

[0111] The final calcined MoVTeTaOx is referred to herein as Catalyst 1. It will be appreciated that other procedures may be used to form Catalyst 1. Furthermore, any number of metal ratios may be used.

[0112] In some embodiments, the MoVTeNbOx catalyst active phase is prepared by weighing 11.37 g Nb2O5·H2O and about 127 mL deionized water into a 250 mL RBF. 19.09 g oxalic acid (H2C2O4) is added and stirred at 65°C for 24 hours to produce a white turbid niobium oxalate solution.

[0113] Weigh 84.28g (NH4)6Mo7O 24 4H2O and about 200mL of deionized water into a 500mL round bottom flask (RBF), and stir to dissolve the powder. Weigh 18.27g of telluric acid and about 50mL of deionized water into a 100mL beaker, and stir the mixture at about 50°C to dissolve the powder. At room temperature, add the telluric acid solution dropwise to the (NH4)6Mo7O 24·4H2O solution. Heat the Mo / Te solution to about 80°C using an oil bath. At 80°C, add 28.0 mL of NH4OH solution dropwise to the Mo / Te solution to adjust the pH to 7.5; keep the contents of the flask stirred at 80°C for 2 hours. Add 28.0 mL of 5M H2SO4 solution dropwise to the flask to adjust the pH to 4.99. Stir the contents of the flask at 80°C for about 2 hours.

[0114] Weigh 70.04 g of VOSO4·3.41H2O and about 150 mL of deionized water into a 250 mL beaker; stir the mixture to dissolve the powder. In a 2 L RBF, at 70°C, add the VOSO4 solution dropwise to the Mo / Te solution using a dropping funnel and stir for about 30 minutes to form an opaque purple solution.

[0115] At 70°C, the previously prepared niobium oxalate solution was slowly added to the purple solution using a dropping funnel and stirred for approximately 30 minutes to form a light green slurry with a purple film on the RBF walls. The green slurry was transferred to a 2 L glass liner with a large magnetic stir bar.

[0116] The glass liner is placed inside the steel body of the autoclave, and the lid is sealed to the steel body. The autoclave is slowly filled with nitrogen, and then evacuated 10 times to remove the air in the head space. The autoclave is allowed to stand overnight (about 10 to about 16 hours) under about 15psig nitrogen, and stirred at about 200rpm. The nitrogen head space pressure is released by a bubbler to purge the air in the pipeline.

[0117] After stirring overnight, the back pressure regulator on the autoclave was set to 160 psig, the temperature controller was raised to 170° C., and the condenser water bath on the profile was set to 25° C. The temperature profile was monitored. The reaction was maintained at 165° C. with stirring at 200 rpm for an additional 17 hours, for a total of approximately 24 hours.

[0118] The heating was turned off, the top valve was closed, the insulation was removed, and the reactor was allowed to cool overnight while stirring at 200 rpm. The pressure in the reactor was released by opening the top valve.

[0119] Disassemble the reactor and remove the glass liner. Use an aspirator to remove the glass liner through a The contents were filtered through a Buchner funnel with #4 filter paper (obtained from Sigma Aldrich). The resulting filter cake was washed with deionized water until the filtrate was clear. The filter cake was placed in an oven at 90°C to dry over a weekend (about 48 to about 60 hours) and allowed to cool to room temperature.

[0120] A portion of the dried filter cake was manually ground using a mortar and pestle.The ground catalyst was loaded into a boat and calcined at 600°C under nitrogen flow.

[0121] The final calcined MoVTeNbOx is referred to herein as Catalyst 2. It will be appreciated that other procedures may be used to form Catalyst 2. Furthermore, any number of metal ratios may be used.

[0122] Using Corning Mega Pure TM The 12A System ACS is used as a distillation unit to prepare distilled water in-house.

[0123] Example 1: Particle size distribution

[0124] The effect of particle size distribution on green tablet strength was studied. As described herein, a shaped catalyst formulation comprising an active catalyst phase, a carrier, a binder and an optional lubricant was prepared in a tablet press. Table 2 shows the particle size distribution for studying the effect of particle size on the crushing strength of the automatic pressed tablets of the shaped catalyst 1.4 (green). The tablets in Table 2 were produced using a CPR-6 automatic press. First, 0.3616g of polyethylene glycol (PEG) and 1.4437g of polyvinyl chloride (PVA) were combined in a 1000mL beaker. Next, 80mL of distilled water was added to the beaker. The beaker was placed in a 65°C water bath on a stirring hot plate to dissolve the chemicals while stirring. After the chemicals were dissolved, 24.0622g of catalyst 1 and 36.16g of fumed silica were combined in a separate container and then added to a 1000mL beaker with dissolved PVA / PEG. Another 160mL of distilled water was added to form a flowing slurry. The water bath setting was increased to 95°C. An overhead stirrer stirred the slurry until most of the water evaporated and the mixture formed a thick paste. The beaker containing the paste was placed in an oven at 105°C overnight to completely dry.

[0125] The prepared catalyst is then granulated by producing a briquette, crushing the briquette, sieving the formed particles and collecting the particles within the size range of (>105 μm and <710 μm). Before briquetting, the prepared solid catalyst is first pulverized in a mortar and pestle. About 7 g of powder is loaded into a die set of 4 cm diameter and pressed to 12 metric tons on a CARVER manual press for 60 seconds to produce a briquette. The briquette is then crushed using a mortar and pestle to produce particles. The particles are sieved using sieves of 105 μm, 250 μm, 500 μm and 710 μm in size. The particles collected on the 105 μm to 500 μm sieves are used for further experiments (size range>105 μm and <710 μm). The granulation process is repeated several times until a satisfactory amount of particles is obtained. Table 2 shows the particle size distribution used in this experiment. The particles are then tableted into 3 mm flakes. The pelletized catalyst samples were mixed with 2 wt.% of graphite as a lubricant and then tableted using a CPR-6 automatic single punch tablet press.

[0126] The tablet press settings for all the above samples were: top die pressure 8, bottom die setting 2, and tableting speed 4. The axial crush strength was determined by slowly applying a load to the axial (i.e., flat) side of a cylindrical tablet, to the tablet sandwiched between two flat plates. The highest force recorded when the tablet broke was recorded as the crush strength. The apparatus used to determine the crush strength included TCM 201 drive and the AFG 2500N dynamometer.

[0127] Comparing the crush strength values ​​of the shaped catalysts 1.4, 1.4-E1, 1.4-E2 and 1.4-E3, it was found that E2 with a particle size distribution (x) of 250 μm < x < 500 μm obtained the highest crush strength.

[0128] Table 2: Particle size distribution used for crushing strength test

[0129]

[0130] Example 2: Tablet Processability Data of Formed Catalyst 1.5 Tablets

[0131] In addition to the axial strength measurement of 3mm shaped catalyst 1.4 tablets, the radial crushing strength of 6mm shaped catalyst 1.5 (green, GB) tablets was also studied. The tablets were prepared on an automatic press. The shaped catalyst 1.5 (GB) tablets were prepared by merging 0.4009g polyethylene glycol (PEG) and 1.6159g polyvinyl chloride (PVA) in a 500mL beaker. Then, 60mL of distilled water was added to the beaker. The beaker was placed in a 65°C water bath on a stirring hot plate to dissolve the chemicals while stirring. After the chemicals were dissolved, 16.0457g of catalyst active phase catalyst 1 and 24.0425g of fumed silica were weighed and combined in a separate container. Then, the catalyst / silicon dioxide mixture was added to a 500mL beaker with dissolved PVA / PEG. Another 150mL of distilled water was added to form a flowing slurry. The water bath was increased to 95°C. The slurry was stirred using an overhead stirrer until most of the water evaporated and the mixture formed a thick paste. The beaker with the paste was placed in an oven at 105°C overnight to completely dry.

[0132] Next, the prepared solid catalyst is pulverized in a mortar and pestle. About 7 g of powder is loaded into a die set of 4 cm diameter and pressed to 12 metric tons on a CARVER manual press for 60 seconds to produce a compact. The compact is then crushed into particles using a mortar and pestle. The particles are sieved using a sieve of 250 μm and 500 μm in size. The particles collected on the 250 μm sieve are used for further experiments (size range>250 μm and <500 μm). The granulation process is repeated several times until a satisfactory particle weight is obtained. The particles are used for tableting.

[0133] The granular catalyst was tableted using a CPR-6 automatic single punch tablet press. The instrument settings were: top die setting 8, bottom die setting 2, tableting speed varied between 1 and 3. Tabletting produced shaped catalyst 1.5 (green body, GB).

[0134] Figure 5 The tablet compressibility characteristic curve of shaped catalyst 1.5 green sheet (shaped catalyst 1.5GB) is shown. The sheet diameter of the test is 6mm. By slowly applying a load to the sheet sandwiched between two planar plates, radial crushing strength (in MPa) is tested along the cylindrical sheet diameter under various compaction pressures. The highest force recorded when the sheet breaks is recorded as radial crushing strength. The device for determining crushing strength includes a CHATILLON TCM 201 driver and a MECMESIN AFG 2500N dynamometer installed on the driver. As described herein, radial crushing strength is converted into tensile strength value.

[0135] like Figure 5As shown, the shaped catalyst 1.5GB tablets show an increased radial tensile strength at increasing compaction pressure. The increasing radial tensile strength of the catalyst tablets 1.5GB with increasing compaction pressure indicates that these tablets are very suitable for tableting. In addition, the radial tensile strength of these tablets is greater than 2MPa, further indicating that they are suitable as catalysts.

[0136] Example 3: Tablet Processability Data of Formed Catalyst 1.7 Tablets

[0137] Formed catalyst 1.7 flakes are prepared by combining 0.8079g polyethylene glycol (PEG) and 1.1960g polyvinyl chloride (PVA) in a 1000mL beaker. Next, 100mL distilled water is added to the beaker. The beaker is placed in a 65°C water bath on a stirring hot plate to dissolve the chemicals while stirring. After the chemicals are dissolved, 16.0320g catalyst 1 and 24.05g fumed silica are combined in a separate container and then added to a 1000mL beaker with dissolved PVA / PEG. Another 150mL DI water is added to form a flowing slurry. The water bath is increased to 95°C. An overhead stirrer stirs the slurry until most of the water evaporates, and the mixture forms a thick paste. The beaker with the paste is placed in an oven at 105°C overnight to dry completely.

[0138] Then, the prepared solid catalyst is pulverized in a mortar and pestle. About 7g of powder is loaded into a die set of 4cm diameter, and pressed to 12 metric tons on a CARVER manual press for 60 seconds to produce a compact. The compact is then crushed using a mortar and pestle to produce particles. The particles are sieved using a sieve of 250μm and 500μm in size. The particles collected on the 250μm sieve are used for further experiments (size range>250μm and <500μm). The granulation process is repeated several times until a sufficient amount of particles for tableting is obtained.

[0139] The granular catalyst was tableted using a CPR-6 automatic single punch tablet press. The instrument settings were: top die setting 8, bottom die setting 2, tableting speed varied between 1 and 3. Tableting produced shaped catalyst 1.7 (green body, GB).

[0140] The radial crushing strength of the shaped catalyst 1.7GB tablets was tested along the cylindrical tablet diameter at various compaction pressures by slowly applying a load to the tablets sandwiched between two flat plates. The highest force recorded when the tablets broke was recorded as the radial crushing strength. The device for determining the crushing strength included a CHATILLON TCM 201 driver and a MECMESIN AFG 2500N dynamometer mounted on the driver. As described herein, the radial crushing strength was converted into a tensile strength value.

[0141] Figure 6 The tabletability characteristic curve of the shaped catalyst 1.7GB tablet is shown, that is, the functional relationship between the radial tensile strength in MPa and the compaction pressure in MPa. Figure 6 As shown, the shaped catalyst 1.7GB tablets show an increased radial tensile strength at increasing compaction pressure. The increasing radial tensile strength of the catalyst tablets 1.7GB with increasing compaction pressure indicates that these tablets are very suitable for tableting. In addition, the radial tensile strength of these tablets is greater than 2MPa, further indicating that they are suitable as catalysts.

[0142] As shown in Experiments 2 and 3, the crush strength of the shaped catalyst tablets (1.5GB) with 5 wt.% binder was about 63% higher than those prepared with about 3 wt.% binder (1.4-E2-GB). Thus, the crush strength of the shaped catalyst green tablets prepared with higher binder content was more than twice that of those prepared with lower binder content. This was a surprising result.

[0143] Example 4: Comparative Tabletability of Examples 2.1 and 2.2 Levy curve

[0144] To evaluate the compressibility of the catalyst special Levy curve , comparative examples were analyzed. These examples contained support and binder components but no catalyst. Two comparative formulations contained α-alumina (formed catalyst 2.1) and fumed silica (formed catalyst 2.2) support materials. Comparative example formed catalysts 2.1 and 2.2 were formulated as shown in Table 1.

[0145] For the shaped catalyst 2.1 comparative example flakes, 0.8143g polyethylene glycol (PEG) and 1.2111g polyvinyl chloride (PVA) were combined in a 1000mL beaker. Next, 50mL distilled water was added to the beaker. The beaker was placed in a 65°C water bath on a stirring hot plate to dissolve the chemicals while stirring. After the chemicals were dissolved, 39.9g of fumed silica was added to the 1000mL beaker with dissolved PVA / PEG. Another 120mL of distilled water was added to form a flowing slurry. The water bath was increased to 95°C. An overhead stirrer stirred the slurry until most of the water evaporated and the mixture formed a thick paste. The beaker with the paste was placed in an oven at 105°C overnight to dry completely.

[0146] The resulting dry "cake" was crushed into granules in a mortar and pestle, but was not pressed into briquettes like the other samples. The granules were sieved using sieves of size 250 μm and 500 μm. The granules on the sieve of size 250 μm were collected for further experiments (size range >250 μm and <500 μm). The granulation process was repeated several times until a satisfactory granule weight was obtained. The granules were used for tableting. The granulated catalyst was tableted using a CPR-6 automatic single punch tablet press. The samples were manually loaded into the compression mold.

[0147] For the shaped catalyst 2.2 comparative example flakes, 0.7976g polyethylene glycol (PEG) and 1.2018g polyvinyl chloride (PVA) were combined in a 350mL beaker. Then, 50mL distilled water was added to the beaker. The beaker was placed in a 65°C water bath on a stirring hot plate to dissolve the chemicals while stirring. After the chemicals were dissolved, 40.1682g of dry ball-milled DENSTONE 99 α-alumina was added to the 350mL beaker with dissolved PVA / PEG. A flowing slurry was formed. The temperature of the water bath was increased to 95°C. An overhead stirrer stirred the slurry until most of the water evaporated and the mixture formed a thick paste. The beaker with the paste was placed in an oven at 105°C overnight to dry completely.

[0148] After drying overnight, the paste becomes a dry "cake", i.e., an agglomerated solid powder that can be ground or shaped. The resulting solid powder is crushed into granules in a mortar and pestle, but is not pressed into compacts like the other samples. The granules are sieved using sieves of size 250 μm and 500 μm. The granules on the sieve of size 250 μm are collected for further experiments (size range > 250 μm and < 500 μm). The granulation process is repeated several times until a sufficient amount for tableting is obtained.

[0149] The granular catalyst was pressed into pellets using a CPR-6 automated press. The samples were manually loaded into the compression mold.

[0150] By slowly applying a load to the tablet sandwiched between two flat plates, the radial crushing strength of the comparative example shaped catalyst 2.1GB and 2.2GB tablets was tested along the cylindrical tablet diameter under various compaction pressures. The highest force recorded when the tablet broke was recorded as the radial crushing strength. The device for determining the crushing strength included a CHATILLON TCM 201 driver and a MECMESIN AFG 2500N dynamometer mounted on the driver. As described herein, the radial crushing strength value was converted into a tensile strength value.

[0151] Figure 7The tablet compressibility characteristic curves of the shaped catalyst 2.1GB comparative example tablet and the shaped catalyst 2.2GB comparative example tablet (circular) are shown. The tablet diameter tested is 6 mm. Figure 7 As shown, the shaped catalyst 2.2GB comparative example tablets did not show an increase in radial tensile strength with increasing compaction pressure, indicating that fumed silica itself is not an ideal tabletting material. Instead, the fumed silica support and the catalyst active phase work synergistically to improve the strength and tabletability of the shaped catalyst tablets. This is another surprising result.

[0152] The Shaped Catalyst 2.1GB Comparative Example tablets did exhibit increased radial tensile strength at increased compaction pressures, however, the Shaped Catalyst 2.1GB Comparative Example tablets contained an alpha-alumina support phase.

[0153] Without wishing to be bound by theory, it appears that when the MoVTeTaOx catalyst active phase is combined with fumed silica, the new material mixture behaves like an ideal compressible material, whereas fumed silica formulations without the catalyst do not display these characteristics. Additionally, the combination of fumed silica and the MoVTeTaOx catalyst active phase produces a material that compresses better than established supports such as alpha-alumina.

[0154] Example 5: Mechanical Strength Data

[0155] The mechanical strength of the shaped catalysts 1.2-1.8 pellets as green bodies and as sintered bodies was analyzed. Table 3 lists the particle sizes used to produce the shaped catalysts 1.2-1.8 used in this experiment.

[0156] Table 3: Particle size distribution of shaped catalysts 1.1-2.2

[0157] Molded catalyst number Particle size distribution (μm) 1.2 105-710 1.3 105-710 1.4 105-710 1.5 250-500 1.6 250-500 1.7 250-500 1.8 250-500

[0158] Synthesis of shaped catalyst 1.2

[0159] Formed catalyst 1.2 flakes are synthesized by combining 0.0824g polyethylene glycol (PEG) and 0.3473g polyvinyl chloride (PVA) in a 100mL beaker. Then, 10mL distilled water is added to the beaker. The beaker is placed in a 65°C water bath on a stirring hot plate to dissolve the chemicals while stirring. In a separate 500mL beaker, 5.7040g catalyst active phase catalyst 1 and 8.3985g fumed silica are combined. After the PGA / PVA mixture is dissolved, it is combined with the catalyst / silicon dioxide mixture. The 500mL beaker with all four chemicals mixed together is placed in a water bath set to 95°C. An overhead stirrer stirs the slurry until most of the water evaporates, and the mixture forms a thick paste. The beaker containing the paste is placed in an oven at 105°C overnight to dry completely.

[0160] Then, the solid catalyst prepared is pulverized in a mortar and pestle. About 7g of powder is loaded into a die set of 4cm diameter, and pressed to 12 metric tons on a CARVER manual press for 60 seconds to produce a compact. The compact is then crushed using a mortar and pestle. The resulting particles are sieved using a sieve of size 105μm, 250μm, 500μm and 710μm. The particles collected on the 105μm to 500μm sieves are used for further experiments (size range>105μm and <710μm). The granulation process is repeated several times until sufficient amount for tableting is obtained.

[0161] For tableting, 2 wt.% natural graphite was added to the granules as a lubricant and mixed very thoroughly. The granulated catalyst was tableted using a CPR-6 automatic single punch tablet press. The instrument settings were: top die pressure 8, bottom die setting 1, tableting speed 4. Tabletting produced green tablets.

[0162] For the sintered body experiments, the green sheets were further debonded and sintered. Debonding was performed on a catalyst calcining furnace (CCF). The sheets were loaded into a quartz boat and the boat was inserted into the quartz tube of the CCF. The tube was sealed except for the inlet and outlet lines, which were used to flow purified air through the quartz tube at 300 sccm during the process. Purified air does not contain impurities, such as bottled air or zero air. Zero air is air in which hydrocarbons have been removed via an oxidation catalytic process so that it contains only less than 0.1 parts per million of total hydrocarbons. The furnace was heated to 400°C at a rate of 1°C / min, kept at 400°C for 1 hour, then the heating was turned off and the furnace was cooled.

[0163] After the furnace cooled to room temperature, the sintering process was started in the same furnace. The air flow was switched to a N2 flow of 300 sccm. The formed catalyst was purged with N2 at room temperature for at least 6 hours. After the purge, the furnace was heated to 600°C at a rate of 1.6°C / min in a continuous N2 flow, kept at 600°C for 2 hours, and then allowed to cool naturally to room temperature. The resulting formed catalyst flakes were then taken out for analysis.

[0164] Synthesis of shaped catalyst 1.3

[0165] The formed catalyst 1.3 flakes are synthesized by combining 0.1236g of polyethylene glycol and 0.4870g of polyvinyl chloride in a 400mL beaker. Next, 50mL of distilled water is added to the beaker. The beaker is placed in a 65°C water bath on a stirring hot plate to dissolve the chemicals while stirring. After the chemicals are dissolved, 8.0356g of catalyst active phase catalyst 1 and 12.0590g of fumed silica are mixed together and then added to the same beaker to merge with the other two chemicals. Another 40mL of distilled water is added to form a flowing slurry. The water bath setting is increased to 95°C. The overhead stirrer stirs the slurry until most of the water evaporates and the mixture becomes a thick paste. The beaker with the paste is placed in an oven at 105°C overnight to dry completely.

[0166] The formulated solid catalyst was then pelletized using the same procedure as used for the shaped catalyst 1.2. The resulting pellets were tableted. The granulated catalyst was tableted using a CPR-6 automatic press. The instrument was set up with a top die pressure of 8 and a bottom die setting of 1. The tableting speed was 5 for both. The goal was to get two types of tablets: one with a lower crushing strength and one with a higher crushing strength for future experiments to see if those catalyst tablets have different activities. Tabletting produced green tablets.

[0167] For the sintered body experiments, the green sheets were further debinded and sintered. Debinding and sintering of the shaped catalyst 1.3 was performed using the same procedure as for the shaped catalyst 1.2.

[0168] Synthesis of Formed Catalyst 1.4-E2

[0169] The synthesis of shaped catalyst 1.4-E2 tablets was carried out using the same procedure as described in Example 1. For sintered body experiments, the green tablets were further debinded and sintered using the same procedure as shaped catalyst 1.2.

[0170] Synthesis of Formed Catalyst 1.5

[0171] The synthesis of the shaped catalyst 1.5 was carried out using the same procedure as described in Example 2. For the sintered body experiments, the green sheets were further debinded and sintered. The debinding and sintering of the shaped catalyst 1.5 was carried out using the same procedure as for the shaped catalyst 1.2.

[0172] Synthesis of Formed Catalyst 1.6

[0173] Formed catalyst 1.6 is synthesized by combining 0.8061g polyethylene glycol (PEG) and 1.2062g polyvinyl chloride (PVA) in a 1000mL beaker. Then, 100mL distilled water is added to the beaker. The beaker is placed in a 65°C water bath on a stirring hot plate to dissolve the chemicals while stirring. After the chemicals are dissolved, 16.0443g catalyst active phase catalyst 1 and 24.0130g fumed silica are combined in a separate container, and then the catalyst / silicon dioxide is added to the 1000mL beaker with dissolved PVA / PEG. Another 120mL distilled water is added to form a flowing slurry. The water bath setting is increased to 95°C. The overhead stirrer stirs the slurry until most of the water evaporates, and the mixture forms a thick paste. The beaker with the paste is placed in an oven at 105°C overnight to dry completely.

[0174] Then, the obtained dry "cake" was pulverized in a mortar and pestle. About 7 g of powder was loaded into a die set of 4 cm diameter and pressed to 12 metric tons on a CARVER manual press for 60 seconds to produce a compact. The compact was then crushed using a mortar and pestle to form particles. The particles were sieved using sieves of 250 μm and 500 μm in size. The particles collected on the 250 μm sieve were used for further experiments (size range>250 μm and <500 μm). The granulation process was repeated several times until sufficient amount for tableting was obtained.

[0175] The granular catalyst was tableted using a CPR-6 automatic single punch tablet press. The instrument settings were: top die setting 8, bottom die setting 2, and tableting speed varied between 1 and 3.

[0176] For the sintered body experiments, the green sheets were further debinded and sintered using the same procedure as for the shaped catalyst 1.2.

[0177] Synthesis of shaped catalyst 1.7

[0178] The synthesis of the shaped catalyst 1.7 was carried out using the same procedure as described in Example 3. For the sintered body experiments, the green sheets were further debinded and sintered using the same procedure as for the shaped catalyst 1.2.

[0179] Synthesis of Formed Catalyst 1.8

[0180] Formed catalyst 1.8 flakes are synthesized by combining 0.8099g polyethylene glycol (PEG) and 1.1990g polyvinyl chloride (PVA) in a 1000mL beaker. Then, 50mL distilled water is added to the beaker. The beaker is placed in a 65°C water bath on a stirring hot plate to dissolve the chemicals while stirring. After the chemicals are dissolved, 16.0320g catalyst active phase catalyst 2 and 24.00g fumed silica are combined in a separate container and then added to the 1000mL beaker with dissolved PVA / PEG. Another 200mL distilled water is added to form a flowing slurry. The water bath setting is increased to 95°C. The overhead stirrer stirs the slurry until most of the water evaporates, and the mixture forms a thick paste. The beaker with the paste is placed in an oven at 105°C overnight to dry completely.

[0181] Then, the obtained solid powder is pulverized in a mortar and pestle. About 7g of powder is loaded into a die set of 4cm diameter and pressed to 12 metric tons on a CARVER manual press for 60 seconds to produce a compact. The compact is then crushed into particles using a mortar and pestle. The particles are sieved using a sieve of 250μm and 500μm in size. The particles collected on the 250μm sieve are used for further experiments (size range>250μm and <500μm). The granulation process is repeated several times until a sufficient amount for tableting is obtained.

[0182] The granular catalyst was tableted using a CPR-6 automatic single punch tablet press. The instrument settings were: top die setting 8, bottom die setting 2, and tableting speed varied between 1 and 3.

[0183] For the sintered body experiments, the green pellets were further debinded and sintered using the same procedure as described for the shaped catalyst 1.2.

[0184] Mechanical strength test

[0185] Two mechanical strength measurements were collected: axial crushing strength and radial crushing strength, and both are reported in Newtons (N). The axial crushing strength and radial crushing strength were obtained using the same procedure as described in Experiments 1-3. The axial crushing strength (Newton, N) of the green body and sintered body are shown in Table 4. The radial crushing strength of the sintered body is shown in Table 5.

[0186] As shown in Table 4, the shaped catalysts described herein have high mechanical strength as green bodies and as sintered bodies. Tablets containing about 3% binder (shaped catalysts 1.3, 1.4, and 1.6) show increased mechanical strength after sintering, regardless of whether the binder comprises 80 / 20 PVA / PEG or 60 / 40 PVA / PEG. For tablets containing about 5% binder (shaped catalysts 1.5, 1.7, and 1.8), tablets containing PVA / PEG in a ratio of 60 / 40 show increased mechanical strength after sintering.

[0187] Furthermore, the shaped catalysts comprising the MoVTeNbOx active phase exhibited high mechanical strength both as green bodies and as sintered bodies as shown in Tables 4 and 5. This is a surprising result and demonstrates that there is a synergistic effect between the MoVTeNbOx active phase and the fumed silica support.

[0188] The tabletability profiles showed that these formulations were suitable for processing by tableting equipment.

[0189] Table 4: Axial crushing strength of 3 mm green body (GB) and sintered body (SB) MoVTeTaOx shaped catalyst tablets 1.2-1.8 Degree Data

[0190]

[0191]

[0192] Table 5: Radial crushing strength of 3 mm sintered body (SB) supported catalyst tablet samples 1.5SB, 1.7SB and 1.8SB

[0193]

[0194] Example 6: Apparent density data

[0195] The apparent density of the catalyst tablets described herein illustrates the effect of the binder weight percentage on catalyst densification, and shows how the increased density is related to the increased crush strength. Table 6 shows the tablet size, weight and apparent density data for 3 mm sintered body shaped catalyst tablets 1.4-E1-SB, 1.4-E2-SB, 1.4-E3-SB and 1.5SB-1.8SB. Sintered body tablets were prepared as described in Experiments 1-5. For each analysis, five tablets were analyzed.

[0196] As shown herein, shaped catalyst tablet 1.5SB has a higher density than catalyst tablet 1.6SB, and indicates that the 60 / 40 PVA / PEG binder combination is no more effective than the 80 / 20 PVA / PEG mixture when loaded at 3 wt.%. The more important factor is the increase in binder content from 3 wt.% to 5 wt.%. Both shaped catalyst tablet 1.5 and shaped catalyst tablet 1.7 have 5 wt.% binder, have different PVA / PEG ratios, but produce similar densities.

[0197] The shaped catalyst tablet 1.8 has a change in the catalyst phase (MoVTeNbOx versus MoVTeTaOx), but the fumed silica / binder formulation is the same as the shaped catalyst tablet 1.7. This suggests that the catalyst active phase plays a role in the synergistic effect of the overall mixture compressibility / mechanical strength / density. In addition, density and crush strength (i.e., mechanical strength) are directly related to the data presented. As shown herein, higher density is equivalent to higher crush strength.

[0198] Table 6: Dimensions, weight and density of 3 mm sintered catalyst tablet samples

[0199]

[0200]

[0201] Example 7: MRU data, comparative example containing only MoVTeTaOx-catalyst shape

[0202] The MRU data provide a basis for interpreting whether a shaped catalyst produces heterogeneous catalysis with robust, long-term performance with no or minimal loss of activity and / or selectivity. Losses can be regenerated by appropriate means, but the time between regenerations should be as long as possible.

[0203] To evaluate the performance of the supported shaped catalysts, a baseline was established using an unsupported shaped catalyst. Figure 8 MRU data for long term ethane to ethylene conversion of shaped catalyst 1.2SB pellets containing only MoVTeTaOx catalyst are shown. Shaped catalyst 1.2SB pellets were prepared as described in Experiment 5 and the MRU experiment was conducted as described in the Detailed Description with the following parameters.

[0204] Figure 8 The experimental results shown in the figure are obtained at 470°C, 6922 GHSV hr -1 and 5.462WHSV hr -1 The MRU procedure was performed as described herein. For the shaped catalyst 1.2SB flakes, the initial ethane conversion at time = 0 was 47.4 mol.% and increased to 49.6 mol.% at time = about 71 hours. From the time stamp of about 71 hours to the end of the run at about 240 hours, a loss of Δ-0.09 mol.% ethane conversion was observed over this 169 hour time span, which corresponds to a loss of 0.0005 mol.% ethane conversion absolute value / hour.

[0205] Fig. 9 The results of long term ethylene selectivity testing of shaped catalyst 1.2SB pellets are shown. Fig. 9 The experimental results shown in were collected at 470°C. Fig. 9 As shown in , the selectivity of the formed catalyst 1.2 remained relatively constant at about 89 mol.% ethylene selectivity over the duration of the test. Thus, these tablets exhibit high selectivity with minimal loss over time, indicating that they are suitable for the oxidative dehydrogenation of ethane.

[0206] Example 8: MRU data, formed catalyst 1.3SB

[0207] Fig.10 and Fig.11 The MRU data graph of MoVTeTaOx supported shaped catalyst 1.3SB pellets is shown. The shaped catalyst 1.3SB pellets were prepared as described in Example 5.

[0208] The conversion and selectivity results of the long-term test of the supported MoVTeTaOx shaped catalyst 1.3 tablets are presented in Fig.10 and Fig.11 The MRU experiments were performed as described in the detailed description with the following deviations. The long-term experiment with the shaped catalyst 1.3 was run at process temperatures of 450°C (first 263 hours) and 460°C (remaining 1913 hours) for a total duration of approximately 2176 hours. Fig.10 The results of long-term ethane conversion testing of MoVTeTaOx shaped catalyst 1.3SB flakes are shown. The test was run at process temperatures of 450°C (initial 263 hours) and 460°C (remaining 1913 hours) for a total duration of approximately 2176 hours. As described herein, the experiment was conducted in three stages - equilibrium period at 450°C (triangles), higher conversion at 460°C before shutdown (diamonds), and higher conversion at 460°C after shutdown (circles). All data are at 2934 GHSVhr -1 (including catalyst and support volume) and 5.462WHSV hr -1 (catalyst weight only, without support) was collected. The shutdown occurred as part of the routine safety system testing. However, these three data cycles can be used to demonstrate the characteristics of the shaped catalyst 1.3 pellets.

[0209] from Fig.10As can be seen in the MRU experiment, the MoVTeTaOx supported shaped catalyst 1.3SB demonstrated a slight deactivation trend. However, the uniqueness of this MRU experiment is that it pushes the process conditions so that the catalyst will convert almost all of the feed oxygen content. Higher temperatures that lead to higher conversions also lead to more oxygen consumption to produce ethylene. Conditions without oxygen retention may deprive the catalyst of the oxygen required to complete the catalytic cycle and damage the catalyst. This is done to deliberately amplify the deactivation of the catalyst and determine whether it can be regenerated after deactivation. As shown in this article, the shaped catalyst 1.3SB tolerates high conversion / low oxygen conditions without damage. Therefore, industrial processes can be operated at higher conversions with less oxygen in the outlet gas product, which in turn means that less downstream equipment and / or processing is required to remove residual unreacted oxygen. In addition, this experiment demonstrates whether higher oxygen consumption conditions stimulate faster or slower deactivation compared to other experiments provided herein. Without wishing to be bound by theory, it is assumed that drastic oxygen consumption will deactivate the catalyst faster, similar to what is observed in catalysts containing MoVTeNbOx.

[0210] At a process temperature of 450°C, the MoVTeTaOx supported shaped catalyst 1.3SB tablets showed an ethane conversion of 48.4 mol.% at time = 0 hours and 51.9 mol.% at time about 24 hours. Fig.10 From time about 24 hours (51.9 mol. % ethane conversion) to time about 260 hours (50.8 mol. % ethane conversion), the ethane conversion changes by Δ-1.1 mol. % absolute over this 236 hour time span, which corresponds to a loss of 0.0085 mol. % absolute ethane conversion / hour.

[0211] At time stamp approximately 283 hours, the MRU experimental process temperature was increased from 450°C to 460°C, which pushed the ethane conversion to 54.6 mol.%. At 54.6 mol.% conversion, the amount of oxygen in the product measured via GC was 0.53 mol.%. It was previously determined with the MoVTeNbOx catalyst that running <1 mol.% oxygen in the product gas stream could result in catalyst deactivation. Fig.10 In the , this data is marked as "Before safety system shutdown".

[0212] The experiment was run uninterrupted for 76 hours from time about 283 hours to time about 359 hours until a planned shutdown occurred where the MRU unit was cooled from 460° C. to room temperature under a nitrogen purge. During the 76 hours of uninterrupted operation, the ethane conversion changed by Δ-0.4 mol.% ethane, which corresponds to a loss of 0.0053 mol.% ethane conversion absolute / hour. Thus, it was shown that the catalyst flakes were stable with very small losses of ethane conversion absolute / hour.

[0213] The MRU experiment was restarted approximately 7 days later. The experiment was restarted at a temperature of 460°C. From this point on, the timestamp was reset to t=0 hours for data comparison. Fig.10 In the , this data is marked as "after safety system shutdown".

[0214] After shutdown, the ethane conversion changed by Δ-3.8 mol.% absolute from time about 0 hours (52.7 mol.% ethane conversion) to time about 674 hours (48.9 mol.% ethane conversion), which corresponds to a loss of 0.0056 mol.% absolute ethane conversion / hour.

[0215] Even though the oxygen consumption is different, the deactivation rate trends before and after the safety system shutdown are essentially the same (approximately 0.005 mol.% ethane conversion absolute / hour). Before the system shutdown, the ethane conversion was high enough so that the oxygen consumption (conversion) resulted in the product gas having <1 mol.% O2 absolute, taken as a random sample injected from the on-site process. After the shutdown, the oxygen in the product was generally below 1 mol.% O2, but close to this target value, in the range of 0.73-1.00 mol.% O2. This was the case between timestamps 0-hour and approximately 218 hours. After 218 hours, the amount of oxygen in the product gas was greater than 1 mol.% O2. The similar results of the deactivation trends before and after operating the reactor under high oxygen consumption indicate that the deactivation trend is independent of the amount of oxygen consumed in the reactor.

[0216] This result yields insight into the deactivation mechanism. Without wishing to be bound by theory, it has been reported that redox deactivation of molybdenum-based catalysts is associated with overreduction of molybdenum oxide active centers. Overreduced molybdenum sites can be converted to other states, irreversibly changing the active phase into an inactive crystalline phase. If redox deactivation is the primary mechanism for activity loss, it is reasonable to expect that this will lead to overreduction of the catalyst when process conditions are pushed to higher oxygen consumption. Overreduction will lead to a decrease in the overall activity of the catalyst bed, which can be observed as an overall deactivation trend in the MRU data. However, if this redox deactivation mechanism is dominant, higher oxygen consumption will accelerate the deactivation trend, which was not observed in this experiment. Therefore, there may be another deactivation mechanism, such as sintering deactivation. Sintering deactivation is one of the most common deactivation mechanisms for heterogeneous catalysis. As shown herein, the catalyst is stable with minimal deactivation.

[0217] Fig.11 Results of long-term ethylene selectivity testing of shaped catalyst 1.3SB flakes are shown. As described herein, the experiment was conducted in three stages – equilibrium period at 450°C (triangles), higher conversion at 460°C before shutdown (diamonds), and higher conversion at 460°C after shutdown (circles). All data are at 2934 GHSV hr -1 (including catalyst and support volume) and 5.462WHSV hr -1 (catalyst weight only, not including support) was collected. Fig.11 As can be seen in Figure 1, the selectivity remained relatively constant at about 88 mol.% ethylene selectivity over the duration of the test. Thus, these flakes exhibit high selectivity with minimal loss over time, indicating that they are suitable for the oxidative dehydrogenation of ethane.

[0218] Example 9: MRU data of formed catalyst 1.5SB

[0219] Fig.12 and Fig.13 MRU data for MoVTeTaOx supported shaped catalyst 1.5SB flakes are shown. Shaped catalyst 1.5SB was synthesized as described in Example 5. The MRU experiment was performed as described in the detailed description with the following parameters. The experiment was performed for a duration of 120 hours TOS.

[0220] Fig.12 The short-term ethane conversion test results of MoVTeTaOx supported shaped catalyst 1.5SB tablets are shown. Fig.12 The experimental results in the table were collected at 460°C. All data were collected at 3393 GHSV hr -1 (including catalyst and support volume) and 5.462WHSV hr -1 (catalyst weight only, not including support) was collected.

[0221] At time t=0, ethane conversion was 42.1 mol.% and increased to 48.6 mol.% after about 48 hours TOS. From time about 48 hours to the end of the run at about 120 hours, a loss of Δ-1.2 mol.% ethane conversion occurred over this 72 hour time span, which corresponds to an approximate rate of 0.0167 mol.% absolute ethane conversion lost per hour.

[0222] Fig.13 The results of long term ethylene selectivity testing of MoVTeTaOx shaped catalyst pellets 1.5SB are shown. Fig.13 The experimental results shown in were collected at 460°C. All data were collected at 3393 GHSV hr -1 (including catalyst and support volume) and 5.462WHSV hr -1 (catalyst weight only, not including support) was collected. Fig.13 As shown in , the selectivity remained relatively constant at about 88 mol.% ethylene selectivity over the duration of the test. Thus, these flakes exhibit high selectivity with minimal loss over time, indicating that they are suitable for the oxidative dehydrogenation of ethane.

[0223] Example 10: MRU data of formed catalyst 1.7SB

[0224] The formed catalyst 1.7SB was prepared as described in Experiment 5. The MRU process was run as described in the specific embodiment, with the following parameters. The long-term experiment with the formed catalyst 1.7SB was run at a process temperature of 470°C for a total duration of approximately 1197 hours. This experiment included intermittent air regeneration to determine if the catalyst could be actively regenerated at set intervals. In this experiment, the "air" regeneration contained a gaseous mixture of nitrogen and oxygen. The catalyst was shown to show improved stability with active air regeneration at scheduled time intervals, at t=285, 643 and 980 hours. All air regenerations were performed at 380°C with a flow rate of 760 seem with 10 volumes of O2 / balance of N2. All data are at 3323 GHSV hr -1 (including catalyst and support volume) and 5.462WHSV hr -1 (catalyst weight only, not including support) was collected.

[0225] Fig.14 Long term ethane conversion test results are shown. The results indicate that the catalyst can be operated without significant deactivation and that regeneration is possible. Another potential means of mitigating the observed deactivation is to change the diluent (e.g., nitrogen) to steam and / or carbon dioxide.

[0226] Fig.15The long-term ethylene selectivity test results of the shaped catalyst 1.7SB tablets are shown. Fig.15 As shown in , the selectivity remained relatively constant at about 87 mol. % ethylene selectivity over the duration of the test.

[0227] The results of the first air regeneration were positive, with no initial selectivity loss, remaining at a steady level of about 87 mol.% ethylene. Secondly, activity recovered and remained elevated for a considerable TOS duration. At t≈315 hours of the experiment, the ethane conversion was measured to be 47.9 mol.%, just after air regeneration, but at t≈332 hours, it increased to 49.0 mol.%. Comparing the 49.0 mol.% ethane conversion with the 48.0 mol.% before air regeneration, it corresponds to a Δ+1.0 mol.% absolute positive improvement. Advantageously, the conversion activity remained in the 48 mol.% range until the TOS timestamp of 621 hours. The next regeneration was performed at 643 hours TOS. Between 332 hours and 643 hours, the ethane conversion data were as follows: range = 47.0-50.0 mol.%, average = 48.4 mol.%, and standard deviation of the data = 0.78 mol.% (47.6-49.2 mol.%). Selecting 48 mol.% ethane conversion as the endpoint of 643 hours TOS and comparing it to the initial activity of 49.5 mol.% at t=0 hours yields a delta-1.5 mol.% absolute change in ethane conversion over this 614 hour time span (minus about 29 hours of air regeneration time), which corresponds to a 0.0024 mol.% absolute / hour loss in ethane conversion. Thus, air regeneration can successfully regenerate the catalyst and can be used to maintain constant conversion for these processes under normal operating conditions.

[0228] Example 11: MRU data of formed catalyst 1.8SB

[0229] The shaped catalyst 1.8SB was prepared as described in Experiment 5. The MRU process was run as described in the detailed description with the following parameters. The long term experiment with shaped catalyst 1.8 was run at a process temperature of 420°C for a total duration of approximately 1032 hours. Fig.16 The long-term ethane conversion of the formed catalyst 1.8SB is shown. Fig.16 As shown in , the MoVTeNbOx supported shaped catalyst 1.8 pellets demonstrated excellent stability.

[0230] At a process temperature of 420°C, the ethane conversion of the MoVTeNbOx shaped catalyst 1.8 tablets started at 44.4 mol.% and time = 0 hours, and increased to 54.7 mol.% at time ≈ 47 hours. From time ≈ 47 hours (54.7 mol.% ethane conversion) to time ≈ 357 hours (56.3 mol.% ethane conversion), the ethane conversion changed by Δ + 1.6 mol.% absolute over this 310 hour time span, which corresponds to 0.0052 mol.% ethane conversion absolute / hour gain. In summary, the ethane conversion changed by Δ + 11.9 mol.% absolute from time = 0 hours to time ≈ 357 hours, which is a desirable result. All long-term testing of the supported MoVTeNbOx shaped catalyst 1.8 tablets was performed without air regeneration. A shutdown was performed at time ≈ 212 hours, during which the feed gas was shut off and a nitrogen purge was started while the process was cooled down from 420°C. However, this nitrogen purge period was brief (<1 hour) and the resulting activity loss was short-lived, and the catalyst behavior was fully recovered by time ≈233 hours, and even improved until time ≈357 hours. A slight deactivation trend began at the timestamp of TOS 357 hours. At timestamp TOS 1032 hours, the ethane conversion was measured to be 54.4 mol.% ethane conversion (average of the last 4 data points measured). Based on the 4-point average result of 54.4 mol.% obtained at the end of the experiment (t≈1032 hours), the deactivation trend of about 1000 hours was Δ-0.3 mol.% absolute relative to the ethane conversion collected at time ≈47 hours (54.7 mol.% ethane conversion). The ethane conversion loss of Δ-0.3 mol.% absolute corresponds to a loss of 0.0003 mol.% absolute ethane conversion / hour over the 985 hour experimental period.

[0231] The increase in ethane conversion is an unexpected result and demonstrates the synergistic effect of the fumed silica support and the shaped catalyst comprising both MoVTeNbOx and MoVTeTaOx catalyst active phases.

[0232] Fig.17 The ethane selectivity of the shaped catalyst 1.8SB tablets is shown. Fig.17 As shown in Figure 1, the selectivity actually increased from about 90 mol.% to 92 mol.% ethylene selectivity over the duration of the test. Again, this was an unexpected but desirable result. Thus, these flakes show high selectivity with minimal loss over time, indicating that they are suitable for the oxidative dehydrogenation of ethane.

[0233] Fig.18Long term ethylene selectivity testing for shaped catalyst 1.7SB and shaped catalyst 1.8SB are shown, overlaid in a single figure. Table 7 summarizes the catalyst performance data for these shaped catalysts. Both shaped catalysts showed little to no deactivation tendency. The slight increase in the deactivation tendency of shaped catalyst 1.7SB compared to shaped catalyst 1.8SB may be attributed to the higher temperature used to analyze shaped catalyst 1.7SB.

[0234] Table 7: Summary of catalyst performance data for shaped catalysts 1.7SB and 1.8SB

[0235]

[0236]

[0237] The following units of measurement have been referred to in this disclosure:

[0238] Units of measurement Full name g gram ℃ Celsius mL mL mm Millimeters <![CDATA[mm 3 ]]> Cubic millimeters <![CDATA[g / cm 3 ]]> g / cm3 μm Micrometer sccm Standard cubic centimeters per minute PsiG Pounds per square inch MPa MPa wt.% Weight Percent mol.% Mole Percent N Newton hr Hour <![CDATA[hr -1 ]]> per hour

[0239] As used in this disclosure, the term "about" can allow for a certain degree of variation in value or range (eg, within 10%, within 5%, or within 1%) of a stated value or a stated range limit.

[0240] As used in this disclosure, the term "substantially" means mostly or predominantly, such as at least about 50%, 60%, 70%, 80%, 90%, 95%, 96%, 97%, 98%, 99%, 99.5%, 99.9%, 99.99%, or at least about 99.999% or more.

[0241] The term "solvent" as used in the present disclosure refers to a liquid that can dissolve a solid, another liquid, or a gas to form a solution. Non-limiting examples of solvents are silicones, organic compounds, water, alcohols, ionic liquids, and supercritical fluids.

[0242] The term "room temperature" as used in this disclosure refers to a temperature of about 15 degrees Celsius (°C) to about 28°C.

[0243] As used in this disclosure, "weight percent" (wt.%) can be considered as the mass fraction or mass ratio of a substance relative to the total mixture or composition. Unless otherwise specified, weight percent can be a weight to weight ratio or a mass to mass ratio.

[0244] Several embodiments of the present disclosure have been described. However, it will be appreciated that various modifications can be made without departing from the spirit and scope of the present disclosure.

Claims

1. A composition comprising: a catalytically active phase, wherein the catalytically active phase comprises a MoVTeNbOx catalyst; and A support phase, wherein the support phase comprises fumed silica, wherein the catalyst active phase and the support phase form a multiphase mixture.

2. The composition of claim 1, further comprising a binder, wherein the binder comprises a polymer organic acid, an amine or an alcohol.

3. The composition of claim 2, wherein the binder comprises polyvinyl alcohol or polyethylene glycol or both.

4. The composition according to claim 3, wherein the binder comprises 60-80 wt.% of polyvinyl alcohol and 20-40 wt.% of polyethylene glycol.

5. The composition according to claim 1, further comprising an inorganic binder, wherein the inorganic binder comprises talc or calcium carbonate.

6. The composition of claim 1 further comprising sintering the composition to form a ceramic.

7. The composition of claim 1, wherein the composition further comprises a plasticizer, wherein the plasticizer comprises polyethylene glycol.

8. The composition of claim 1, wherein the composition further comprises a lubricant.

9. The composition of claim 8, wherein the lubricant comprises 1-2 wt. % of the composition, and wherein the lubricant comprises graphite.

10. The composition of claim 1, wherein the fumed silica comprises 5-95 wt. % of the composition.

11. A pressed tablet comprising the composition according to claim 1, wherein the density of the pressed tablet is 1.0-1.5 g / cm 3 .

12. A sintered ceramic catalyst comprising the composition according to claim 1.

13. A method for preparing a shaped catalyst, the method comprising: combining a catalyst active phase, a support phase, and a binder in an aqueous solvent to form an aqueous solution, wherein the catalyst active phase comprises MoVTeNbOx and the support phase comprises fumed silica; heating the aqueous solution to form a thick paste; drying the thick paste to evaporate the aqueous solvent to form a solid powder; grinding the solid powder to form granules; and The granules are pressed to form tablets. 14 . The method of claim 13 , wherein grinding the solid powder to form particles comprises grinding the solid powder to form particles, wherein the particles have a diameter between 105 μm and 710 μm.

15. The method according to claim 13, further comprising: debonding the sheet, wherein debonding the sheet comprises heating the sheet to remove the adhesive; and The flakes are sintered, wherein sintering the flakes includes heating the flakes to coalesce the flakes into a dense solid.

16. The method of claim 15, wherein debonding the flakes comprises heating the flakes to 200°C-400°C at a rate of 1-2°C / min.

17. The method of claim 15, wherein sintering the tablet comprises heating the tablet to 400°C-600°C at a rate of at most 5°C / min.

18. A method for preparing a shaped catalyst, the method comprising: combining a catalyst active phase, a support phase, and a binder in an aqueous solvent to form an aqueous solution, wherein the catalyst active phase comprises MoVTeNbOx and the support phase comprises fumed silica; heating the aqueous solution to form a thick paste; drying the thick paste to evaporate the aqueous solvent to form a solid powder; grinding the solid powder to form granules; pressing the granules to form tablets; debonding the sheet, wherein debonding the sheet comprises heating the sheet to remove the adhesive; and The flakes are sintered, wherein sintering the flakes includes heating the flakes to coalesce the flakes into a dense solid.

19. A method for oxidative dehydrogenation of ethane, the method comprising: flowing a feed gas through the microreactor unit, wherein the feed gas comprises ethane, oxygen, and nitrogen; pressurizing the feed gas in the microreactor; contacting the feed gas with a shaped catalyst comprising: a catalytically active phase, wherein the catalytically active phase comprises a MoVTeNbOx catalyst; and a support phase, wherein the support phase comprises fumed silica, wherein the catalyst active phase and the support phase form a multiphase mixture; heating the feed gas to 450°C-470°C; and Recover ethylene gas.

20. The process of claim 19, wherein the feed gas comprises ethane and oxygen in a molar ratio of 1:0.5.