Method for producing particulate alumina

By adjusting the pH and using controlled heating processes, the method enhances the mechanical properties of alumina, addressing the need for high strength and low density in catalyst supports.

CN119095798APending Publication Date: 2024-12-06BASF CORPORATON
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380036033.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-25
Filing Date
2023-04-24
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing methods for preparing particulate alumina do not adequately address the need for materials with high lateral compressive strength and low packing apparent bulk density, which are essential for effective use as catalyst supports.

Method used

A method involving the preparation of alumina by adjusting the pH of the aqueous solution to a range of 12 to 14 during specific heating stages, including the use of non-polar organic solvents and controlled heating processes to form precursor particles, followed by calcination, results in alumina with enhanced mechanical properties.

Benefits of technology

The method produces particulate alumina with high lateral compressive strength and low packing apparent bulk density, suitable for use as catalyst supports, improving their physical integrity and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005099645960000281
    Figure BDA0005099645960000281
  • Figure BDA0005099645960000311
    Figure BDA0005099645960000311
  • Figure BDA0005099645960000321
    Figure BDA0005099645960000321
Patent Text Reader

Abstract

The present invention relates to a process for preparing particulate alumina, the process comprising (i) preparing a mixture comprising water and one or more alumina sources; (ii) spraying the mixture to form droplets; (iii) heating the droplets in the non-polar organic solvent system to a specific temperature to obtain precursor particles; (iv) heating the precursor particles in the aqueous solution to a specific temperature, wherein the pH of the aqueous solution is adjusted to a value in the range from 12 to 14. Furthermore, the present invention relates to a particulate alumina as obtained and / or obtainable by said method. Yet further, the invention relates to a particulate alumina having a lateral compressive strength in the range of from 9 to 25 N / mm and a fill apparent bulk density in the range of from 0.45 to 0.55 g / cm3, and to the use thereof.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for preparing particulate aluminium oxide. Furthermore, the present invention relates to particulate aluminium oxide itself as well as particulate aluminium oxide obtained or obtainable according to the method and to its use. Background Art

[0002] The selective hydrogenation of pyrolysis gas (pyrolysis gas) or unsaturated C3-C4 hydrocarbons is usually achieved using a catalytic material comprising a catalytically active metal supported on a support material. As a catalytically active metal, one or more of Ni, Pd and Pt are usually used. Therefore, usually one or more of the metals are supported on a support material via impregnation. As a support material, typically particulate alumina is used, also commonly referred to as an alumina sphere. There are several types of particulate alumina with different chemical and physical properties, which can be selected according to the intended use.

[0003] Typically, the process for preparing micronized alumina starts with an alumina source (e.g., ρ-alumina) and deionized water, which are mixed into a slurry. Micronized alumina, in particular alumina spheres, are then formed by spraying the slurry through a vibrating nozzle, and they are solidified in a forming tower containing oil. The micronized alumina is then conveyed to an aging vessel together with a stream of water, which is heated to a temperature in the range of from 90° C. to 100° C. The micronized alumina resides therein for a certain time, for example, about 16 hours. Subsequently, the micronized alumina is washed to reduce the sodium concentration. The micronized alumina is then dried and calcined to produce micronized alumina having a certain strength and surface area. Depending on the intended use, the micronized alumina may be loaded with a metal, such as nickel.

[0004] US 7090825B2 relates to alumina agglomerates and a method for their preparation. The method comprises dehydrating aluminum oxyhydroxide or aluminum hydroxide, agglomerating the aluminum oxide thus obtained, hydrothermally treating the agglomerates and calcining them. Specifically, the alumina agglomerates obtained have a volume greater than or equal to 75 ml / 100 g occupied by pores with a diameter greater than or equal to 37 angstroms. The volume occupied by pores with a diameter greater than or equal to 0.1 micrometer (V 0.1微米 ), and a volume greater than or equal to 20 ml / 100 g occupied by pores with a diameter greater than or equal to 0.2 μm (V 0.2微米 ).

[0005] US 4065407A relates to a method for preparing shaped particles from rehydratable alumina. In particular, a method for preparing shaped alumina particles for catalysts or catalyst supports by passing droplets of an aqueous slurry of a rehydratable alumina composition through a shaping medium (such as a column of a water-immiscible liquid) is disclosed, wherein the alumina composition undergoes rehydration while being shaped as it passes through the shaping medium, producing a solid, discrete alumina body.

[0006] US 4169874A relates to a method for preparing low-density shaped alumina particles from rehydratable alumina. In particular, the method comprises introducing an aqueous slurry comprising water, alumina containing a substantial portion of rehydratable alumina and a combustible filler into a shaping medium selected from (a) a water-immiscible phase into which droplets of the alumina slurry are introduced to be shaped into spherical bead-like forms by surface tension, and (b) a tube of desired cross-sectional size and shape to shape the alumina into an extrudate form, thereby shaping the alumina into a desired configuration, and heating the shaping medium to rehydrate and harden the alumina while the alumina is subjected to the influence of the shaping medium.

[0007] US 6197073 B 1 relates to a method for producing alumina beads. In particular, it is disclosed that an acidic alumina sol or an acidic alumina suspension is converted into droplets by a vibrating nozzle plate and, after forming the bead shape, is pre-solidified by bubbling gaseous ammonia laterally and then condensed in an ammonia solution.

[0008] US 4318896A relates to alumina particles and a method for making the same. The method comprises, inter alia, preparing a mixture of an acidic alumina hydrosol and an ammonia precursor below the gelling temperature, dispersing the mixture in the form of droplets in a water-immiscible liquid at a temperature and for a period of time to achieve at least partial gelling of the hydrosol to form hydrogel particles, contacting the hydrogel particles with a liquid having a pH of no greater than about 7 and an osmotic pressure sufficient to prevent disintegration of the hydrogel particles, aging the hydrogel particles in an aqueous solution having a pH greater than 7, and then drying and calcining the hydrogel particles.

[0009] US 4542113A relates to a method for preparing spherical aluminum oxide. The method comprises, in particular, preparing an aluminum oxide sol having a solid content of aluminum oxide greater than 20% to 40% by weight from an aluminum oxide hydrate by sufficient stirring in a dilute acid aqueous solution, the aluminum oxide hydrate consisting of boehmite / pseudoboehmite. The aluminum oxide sol is then dripped into a forming column in the presence of 1% to 10% by weight of urea, the top of the forming column being filled with liquid hydrocarbons and the bottom of which being filled with an aqueous ammonia solution, and which is kept at room temperature, and the spherical particles thus formed are dried and activated.

[0010] EP 0153674A2 relates to rehydratable bonded alumina. In particular, the document relates to low-density alumina spheres and a method for producing the same. The method comprises in particular mixing a rehydratable alumina powder with water to form a fluid slurry, and mixing with a hot immiscible fluid, in such a way that the slurry is dispersed into droplets that become spherical due to surface tension, and then solidified by rehydration bonding.

[0011] US 3223483A relates to a method for producing activated alumina. In particular, the method for producing an alumina material comprises calcining hydrated aluminum, agglomerating the calcined alumina by mixing with water, rehydrating the alumina agglomerates and heating the rehydrated agglomerates, only partially rehydrating the alumina agglomerates, and circulating water with a low sodium content through the partially rehydrated alumina agglomerates to remove soluble sodium compounds therefrom and reduce the sodium content thereof, while continuing the rehydration of the partially rehydrated alumina agglomerates.

[0012] US 4279779A relates to an alumina composition, a catalyst support comprising spherical alumina particles which can be prepared from the alumina composition, and a catalyst using these alumina particles as a support. In addition, the patent relates to a method for preparing alumina and spherical alumina particles.

[0013] US 4411771A relates to improvements in alumina particles useful as catalyst supports and improved methods for preparing such particles, and to improved hydroprocessing catalysts containing such particles as catalyst supports. The catalyst support particles are made from partially dehydrated, rehydratable alumina prepared by flash calcining hydrated alumina (such as Bayer process alumina). In the method of forming the shaped alumina particles, the partially dehydrated alumina is rehydrated to solidify and harden the particles, and then calcined to convert the alumina into substantially anhydrous alumina, such as gamma alumina and eta alumina.

[0014] US 4315839A relates to a method for preparing spherical alumina particles which is suitable for preparing very strong, lightweight spherical alumina particles having dual porosity without the presence of any pore former in the starting mixture and without any "aging" step.

[0015] US10232346B2 relates to the preparation of amorphous mesoporous alumina formed into beads by droplet condensation, starting from an alumina gel with high dispersibility, obtained by precipitation of at least one aluminum salt. In particular, the patent relates to a method for preparing said alumina by forming an alumina gel, prepared according to a specific method of preparation by precipitation, starting from a first precipitation step, the amount of alumina formed at the end of the first precipitation step possibly even reaching 100%, in order to obtain at least 40% by weight of alumina relative to the total amount of alumina formed at the end of the gel preparation process.

[0016] US 4390456A relates to an alumina composition, a catalyst support comprising spherical alumina particles which can be prepared from the alumina composition, and a catalyst using these alumina particles as a support.

[0017] However, there is still a need to provide particulate alumina having excellent physical integrity, in particular relatively high lateral compressive strength and relatively low packing apparent bulk density. The particulate alumina should also be suitable as a support for catalytically active metals. Therefore, there is still a need for novel methods for preparing particulate alumina having the described characteristics. DETAILED DESCRIPTION

[0018] It is therefore an object of the present invention to provide a method for preparing particulate alumina, wherein the particulate alumina is characterized in particular by excellent physical integrity. In particular, it is an object of the present invention to provide a method for preparing particulate alumina having a relatively high lateral compressive strength and a relatively low packing apparent bulk density. Still further, it is an object of the present invention to provide a particulate alumina, wherein the particulate alumina is characterized in particular by a relatively high lateral compressive strength and a relatively low packing apparent bulk density.

[0019] Surprisingly, it has been found that particulate alumina can be prepared according to a novel method, whereby the particulate alumina obtained has specific characteristics, in particular a relatively high lateral compressive strength and a relatively low packing apparent bulk density. In particular, it has been surprisingly found that a novel method for preparing such particulate alumina can be provided, wherein in particular the pH of the aqueous solution in which the particulate alumina is aged is adjusted to a value in the range from 12 to 14. Thereby, particulate alumina having a relatively high lateral compressive strength and a relatively low packing apparent bulk density can be prepared.

[0020] Therefore, the present invention relates to a method for preparing microparticle aluminum oxide, comprising:

[0021] (i) preparing a mixture comprising water and one or more alumina sources;

[0022] (ii) spraying the mixture obtained in (i) to form droplets;

[0023] (iii) heating the droplets obtained in (ii) in a non-polar organic solvent system to a temperature ranging from 85° C. to 100° C. to obtain precursor particles;

[0024] (iv) heating the precursor particles obtained in (iii) in an aqueous solution S2 to a temperature ranging from 85° C. to 110° C. to obtain particulate aluminum oxide, wherein the pH of the aqueous solution S2 is ranging from 12 to 14.

[0025] Preferably, preparing the mixture in (i) comprises cooling the mixture to a temperature in the range from 0°C to 15°C, more preferably in the range from 2°C to 10°C, more preferably in the range from 3°C to 7°C.

[0026] Preferably (i) comprises

[0027] (i.1) cooling the water to a temperature in the range of from 0°C to 15°C, preferably in the range of from 2°C to 10°C, more preferably in the range of from 3°C to 7°C;

[0028] (i.2) mixing one or more alumina sources with the water cooled in (i.1); to obtain a mixture comprising water and the one or more alumina sources.

[0029] Preferably, preparing the mixture in (i) comprises stirring, more preferably stirring with a propeller stirrer, wherein preparing the mixture in (i) more preferably comprises stirring at 200 to 300 rpm, more preferably at 225 to 275 rpm.

[0030] Preferably, the total amount of one or more alumina sources in the mixture obtained in (i), calculated as Al2O3, is in the range from 40 wt.-% to 65 wt.-%, more preferably in the range from 45 wt.-% to 60 wt.-%, more preferably in the range from 50 wt.-% to 55 wt.-%, more preferably in the range from 52 wt.-% to 53 wt.-%, based on the weight of the mixture obtained in (i).

[0031] Preferably, the one or more alumina sources comprise, preferably consist of, one or more of aluminum hydroxide, Al2O3·0.5H2O, ρ-alumina and sodium aluminate, more preferably one or more of gibbsite (α-aluminum hydroxide), bayerite (β-aluminum hydroxide), nordstrandite (γ-aluminum hydroxide), pseudo-amorphous aluminum hydroxide, Al2O3·0.5H2O, ρ-alumina and sodium aluminate, wherein the one or more alumina sources more preferably comprise, more preferably consist of, one or more of sodium aluminate, Al2O3·0.5H2O and ρ-alumina.

[0032] Rho-alumina is also known as hydratable or rehydratable alumina.

[0033] By varying the amount of NaAlO added, the viscosity of the mixture can be affected. Typically, the viscosity increases slowly due to the rehydration of the alumina used. This increase can decrease or the viscosity can remain constant for an extended period of time to allow a batch of slurry to be processed during 4-8 hours.

[0034] Thus, it is preferred that the one or more alumina sources comprise sodium aluminate and that preparing the mixture according to (i) comprises adding an aqueous solution of sodium aluminate in an amount in the range from 0.05 volume-% to 1.5 volume-%, more preferably in the range from 0.1 volume-% to 1.0 volume-%, based on the volume of the mixture obtained in (i).

[0035] In the case where the one or more alumina sources comprise sodium aluminate and wherein preparing the mixture according to (i) comprises adding an aqueous sodium aluminate solution in an amount in the range from 0.05 volume-% to 1.5 volume-%, preferably in the range from 0.1 volume-% to 1.0 volume-%, based on the volume of the mixture obtained in (i), it is preferred that the aqueous sodium aluminate solution comprises from 32 weight-% to 44 weight-%, more preferably from 36 weight-% to 40 weight-%, more preferably from 37 weight-% to 39 weight-% of sodium aluminate, based on the weight of the aqueous sodium aluminate solution.

[0036] Preferably, the one or more alumina sources contained in the mixture obtained in (i) are ground, more preferably ball-milled, hammer-milled or jet-milled, more preferably ball-milled.

[0037] Preferably, one or more of the one or more alumina sources contained in the mixture obtained in (i) is solid, wherein the one or more alumina solid sources in the mixture obtained in (i) have a volume-based particle size D50 value in the range from 1 to 11 microns, more preferably in the range from 2 to 8 microns, more preferably in the range from 3 to 7 microns, preferably determined according to Reference Example 7.

[0038] Preferably, the mixture obtained in (i) has a viscosity in the range from 700 to 900 mPa·s, more preferably in the range from 750 to 850 mPa·s, more preferably in the range from 790 to 810 mPa·s.

[0039] Preferably, the mixture obtained in (i) comprises sodium hydroxide in an amount in the range from 0 mol-% to 1 mol-%, more preferably in the range from 0 mol-% to 0.1 mol-%, preferably in the range from 0 mol-% to 0.01 mol-%, calculated as Al2O3, based on the total amount of the one or more alumina sources.

[0040] Preferably, the mixture obtained in (i) is sprayed in (ii) through a nozzle, preferably with vibration of the nozzle.

[0041] In the case where the mixture obtained in (i) is sprayed in (ii) through a nozzle, preferably under vibration of the nozzle, it is preferred that the nozzle comprises holes having a diameter in the range from 1.0 to 1.4 mm, more preferably in the range from 1.1 to 1.3 mm.

[0042] Furthermore, in the case where the mixture obtained in (i) is sprayed in (ii) by a nozzle, preferably under vibration of the nozzle, it is preferred that the nozzle is arranged to allow spraying of the mixture obtained in (i) in the falling direction of the formed droplets.

[0043] Preferably, the mixture obtained in (i) is sprayed through a nozzle according to (ii) with a frequency in the range of 1 to 5 drops / second, more preferably in the range of from 1 to 3 drops / second.

[0044] Preferably, the mixture obtained in (i) is sprayed through a nozzle according to (ii) to obtain droplets having an average diameter in the range from 1 to 5 mm, more preferably in the range from 2 to 4 mm, more preferably in the range from 2.5 to 3.5 mm.

[0045] Preferably, spraying the mixture obtained in (i) according to (ii) comprises applying at a depth of from 50 to 80 cm 3 / min, more preferably in the range of from 55 to 75cm / min 3 / min, more preferably in the range of from 60 to 70 cm / min 3 The flow rate is in the range of 1000 / min.

[0046] Preferably, spraying the mixture obtained in (i) according to (ii) comprises applying an overpressure in the range from 0.1 to 0.8 bar, more preferably in the range from 0.2 to 0.7 bar, more preferably in the range from 0.3 to 0.6 bar.

[0047] Preferably, the method further comprises after (ii) and before (iii)

[0048] causing the droplets obtained in (ii) to fall through the atmosphere,

[0049] wherein the atmosphere has a temperature in the range from 10° C. to 60° C., preferably in the range from 15° C. to 50° C.,

[0050] The atmosphere more preferably comprises one or more of nitrogen and oxygen, and the atmosphere is more preferably air.

[0051] Preferably, the droplets obtained in (ii) are heated in (iii) for a duration in the range of from 10 to 50 s, more preferably in the range of from 14 to 40 s, more preferably in the range of from 15 to 30 s, more preferably in the range of from 20 to 25 s, more preferably in the range of from 21 to 22 s.

[0052] Preferably, the droplets obtained in (ii) are heated in (iii) to a temperature in the range from 90 to 98°C, more preferably in the range from 94 to 96°C.

[0053] Preferably, the droplets obtained in (ii) are heated in a column in (iii).

[0054] In the case where the droplets obtained in (ii) are heated in a column in (iii), it is preferred that the column has a length in the range from 0.5 to 5 m, more preferably in the range from 1 to 4 m, more preferably in the range from 2 to 3 m.

[0055] Furthermore, in the case where the droplets obtained in (ii) are heated in a column in (iii), it is preferred that the column has a diameter in the range from 30 to 70 mm, preferably in the range from 45 to 55 mm.

[0056] Preferably, heating the droplets obtained in (ii) according to (iii) comprises maintaining the droplets suspended in the non-polar organic solvent, preferably by causing the droplets to fall through the non-polar organic solvent system.

[0057] Preferably, the non-polar organic solvent system comprises S in an amount in the range from 0 wt.-% to 0.2 wt.-%, more preferably in the range from 0 wt.-% to 0.1 wt.-%, based on the weight of the non-polar organic solvent system, wherein the amount of S is preferably determined according to DIN EN ISO 14596.

[0058] Preferably, the non-polar organic solvent system has a density in the range of from 850 to 880 g / ml, more preferably in the range of from 860 to 870 g / ml, wherein the density is preferably measured at a temperature of 20° C., wherein the density is more preferably measured according to DIN 51757 test procedure 3 (German DIN 51757 Verf. 3).

[0059] Preferably, the non-polar organic solvent system has a molecular weight of from 4.8 to 5.6 mm 2 / s, more preferably in the range of from 5.0 to 5.4 mm 2 The kinematic viscosity is preferably in the range of 100° C. to 200° C., wherein the kinematic viscosity is preferably determined at a temperature of 100° C., wherein the kinematic viscosity is more preferably determined according to DIN EN ISO 3104.

[0060] Preferably, the non-polar organic solvent system has a refractive index in the range from 1.4763 to 1.4769, more preferably in the range from 1.4765 to 1.4767, wherein the refractive index is preferably measured at a temperature of 100° C., wherein the refractive index is more preferably measured according to DIN 51423-02.

[0061] Preferably, the non-polar organic solvent system comprises aromatic hydrocarbons in an amount in the range from 2 wt.-% to 4 wt.-%, more preferably in the range from 2.5 wt.-% to 3.5 wt.-%, based on the weight of the non-polar organic solvent system, wherein the amount of aromatic hydrocarbons is preferably determined according to calculation method U of DIN 51378.

[0062] Preferably, the non-polar organic solvent system comprises cycloalkanes in an amount in the range from 28 wt.-% to 34 wt.-%, more preferably in the range from 30 wt.-% to 32 wt.-%, based on the weight of the non-polar organic solvent system, wherein the amount of cycloalkanes is preferably determined according to calculation method U of DIN 51378.

[0063] Preferably, the non-polar organic solvent system comprises paraffins in an amount in the range from 61 wt.-% to 69 wt.-%, more preferably in the range from 63 wt.-% to 67 wt.-%, based on the weight of the non-polar organic solvent system, wherein the amount of paraffins is preferably determined according to calculation method U of DIN 51378.

[0064] Preferably, the non-polar organic solvent system has a viscosity index in the range from 97 to 103, more preferably in the range from 99 to 101, wherein the viscosity index is preferably determined according to DIN ISO 2909.

[0065] Preferably, heating the droplets obtained in (ii) according to (iii) comprises applying a flow of the non-polar organic solvent system in the opposite direction to the falling direction of the droplets.

[0066] Preferably, the method further comprises collecting the precursor particles in an aqueous solution S1 after (iii) and before (iv).

[0067] In the case where the method further comprises collecting the precursor particles in an aqueous solution S1 after (iii) and before (iv), preferably, the pH of the aqueous solution S1 is in the range from 11.0 to 14.0, more preferably in the range from 12.0 to 13.7, more preferably in the range from 13.0 to 13.5.

[0068] In addition, in the case where the method further comprises collecting the precursor particles in the aqueous solution S1 after (iii) and before (iv), it is preferred that the precursor particles are collected in the aqueous solution S1 in a column, wherein it is more preferred that the precursor particles are collected in the same column in which the droplets obtained in (ii) are heated according to (iii).

[0069] Furthermore, in the case where the method further comprises collecting the precursor particles in the aqueous solution S1 after (iii) and before (iv), it is preferred that the heating of the droplets obtained in (ii) in the non-polar organic solvent system and the collecting of the droplets in the aqueous solution S1 according to (iii) are carried out in a column, wherein the column comprises the non-polar organic solvent system and the aqueous solution S1,

[0070] wherein the droplets obtained in (ii) are heated according to (iii) before being collected in the aqueous solution S1,

[0071] Therein the method preferably comprises passing the droplets obtained in (ii) through a non-polar organic solvent system before being collected in the aqueous solution S1.

[0072] Preferably, the precursor particles obtained in (iii) in the aqueous solution S2 are heated in a container according to (iv).

[0073] Preferably, in (iv), the weight ratio of the precursor particles calculated as the sum of the weights of the precursor particles to the aqueous solution S2 calculated as the weight of the aqueous solution S2 is in the range of from 1:2 to 1:20, more preferably in the range of from 1:4 to 1:15, and more preferably in the range of from 1:6 to 1:10.

[0074] Preferably, the aqueous solution S2 contains one or more of sodium aluminate (NaAlO2), ammonia and sodium hydroxide (NaOH), more preferably sodium aluminate (NaAlO2) and sodium hydroxide.

[0075] In the case where the aqueous solution S2 contains one or more of sodium aluminate (NaAlO2), ammonia and sodium hydroxide (NaOH), more preferably sodium aluminate (NaAlO2) and sodium hydroxide, it is preferred that the aqueous solution S2 contains, in addition to the aluminum contained in the precursor particles, an amount of aluminum calculated as Al2O3 in the range from 3.00 to 6.50 g / l, more preferably in the range from 4.50 to 5.00 g / l, more preferably in the range from 4.65 to 4.80 g / l.

[0076] Furthermore, in the case where the aqueous solution S2 contains one or more of sodium aluminate (NaAlO2), ammonia and sodium hydroxide (NaOH), more preferably sodium aluminate (NaAlO2) and sodium hydroxide, it is preferred that the aqueous solution S2 contains, in addition to the sodium optionally contained in the precursor particles, sodium in an amount calculated as Na in the range from 2.00 to 5.00 g / l, more preferably in the range from 3.40 to 3.80 g / l, more preferably in the range from 3.55 to 3.65 g / l.

[0077] Preferably, the pH of the aqueous solution S2 according to (iv) is in the range of from 12.2 to 13.9, more preferably in the range of from 12.4 to 13.8, more preferably in the range of from 12.6 to 13.7, more preferably in the range of from 12.8 to 13.6, more preferably in the range of from 13.0 to 13.5, wherein the pH is preferably determined according to Reference Example 1.

[0078] Preferably, the precursor particles obtained in (iii) are heated to a temperature in the range of from 87 to 105°C, more preferably in the range of from 89 to 102°C, more preferably in the range of from 90 to 100°C according to (iv).

[0079] Preferably, the precursor particles obtained in (iii) are heated according to (iv) for a duration in the range from 3 to 25 h, more preferably in the range from 4 to 20 h, more preferably in the range from 5 to 17 h.

[0080] Preferably, the method further comprises

[0081] (v) separating the particulate alumina obtained in (iv) from the aqueous solution S2, wherein the separation preferably comprises filtering or centrifuging the aqueous solution S2.

[0082] Preferably, the method further comprises

[0083] (vi) washing the particulate alumina obtained in (iv) or (v) with a liquid solvent system, wherein the liquid solvent system preferably comprises one or more of water, alcohol, and a mixture of two or more thereof, wherein the particulate alumina is more preferably washed with water, wherein the particulate alumina is more preferably washed with deionized water, wherein the particulate alumina is more preferably washed with deionized water until the conductivity of the washing water is less than 400 μS.

[0084] Preferably, the method further comprises

[0085] (vii) drying the fine-particle alumina obtained in (iv), (v) or (vi) in an atmosphere.

[0086] In the case where the method further comprises drying the particulate alumina obtained in (iv), (v) or (vi) in an atmosphere according to (vii), it is preferred that the atmosphere in (vii) has a temperature in the range from 90°C to 130°C, more preferably in the range from 100°C to 120°C, more preferably in the range from 105°C to 115°C.

[0087] Furthermore, in the case where the method further comprises drying the particulate alumina obtained in (iv), (v) or (vi) in an atmosphere according to (vii), it is preferred that the atmosphere in (vii) contains one or more of oxygen and nitrogen, wherein the atmosphere in (vii) is more preferably oxygen or air.

[0088] Furthermore, in the case where the method further comprises drying the particulate alumina obtained in (iv), (v) or (vi) in an atmosphere according to (vii), it is preferred that in (vii) the particulate alumina obtained in (iv), (v) or (vi) is dried in an oven or in a belt dryer, more preferably in a belt dryer.

[0089] Furthermore, in the case where the method further comprises drying the particulate alumina obtained in (iv), (v) or (vi) in an atmosphere according to (vii), it is preferred that the particulate alumina obtained in (iv), (v) or (vi) is dried for 1 to 5 h, more preferably 2 to 3 h in (vii).

[0090] Preferably, the method further comprises

[0091] (viii) precalcining the particulate alumina obtained in (iv), (v), (vi) or (vii) in an atmosphere.

[0092] In the case where the method further comprises pre-calcining the particulate alumina obtained in (iv), (v), (vi) or (vii) in an atmosphere according to (viii), it is preferred that the atmosphere in (viii) has a temperature in the range from 400°C to 460°C, more preferably in the range from 420°C to 440°C, more preferably in the range from 425°C to 435°C.

[0093] Furthermore, in the case where the method further comprises pre-calcining the particulate alumina obtained in (iv), (v), (vi) or (vii) in an atmosphere according to (viii), it is preferred that the pre-calcining according to (viii) comprises heating the atmosphere with a heating ramp of 3 to 7 K / min, more preferably 4 to 6 K / min.

[0094] Furthermore, in the case where the method further comprises pre-calcining the particulate alumina obtained in (iv), (v), (vi) or (vii) in an atmosphere according to (viii), it is preferred that the atmosphere in (viii) contains one or more of oxygen and nitrogen, wherein the atmosphere in (viii) is more preferably oxygen or air.

[0095] Furthermore, in the case where the method further comprises pre-calcining the particulate alumina obtained in (iv), (v), (vi) or (vii) in an atmosphere according to (viii), it is preferred that the particulate alumina obtained in (iv), (v), (vi) or (vii) is pre-calcined in a rotary calciner in (viii).

[0096] Furthermore, in the case where the method further comprises pre-calcining the particulate alumina obtained in (iv), (v), (vi) or (vii) in an atmosphere according to (viii), it is preferred that the particulate alumina obtained in (iv), (v), (vi) or (vii) is pre-calcined for 0.25 to 2 h, more preferably 0.5 to 1 h in (viii).

[0097] Preferably, the method further comprises

[0098] (ix) calcining the particulate alumina obtained in (iv), (v), (vi), (vii) or (viii) in an atmosphere.

[0099] In the case where the method further comprises calcining the particulate alumina obtained in (iv), (v), (vi), (vii) or (viii) in an atmosphere according to (ix), it is preferred that the atmosphere in (ix) has a temperature in the range from 900°C to 1050°C, more preferably in the range from 940°C to 980°C, more preferably in the range from 945°C to 975°C.

[0100] Furthermore, in the case where the method further comprises calcining the particulate alumina obtained in (iv), (v), (vi), (vii) or (viii) in an atmosphere according to (ix), it is preferred that the calcination according to (ix) comprises heating the atmosphere with a heating ramp of 3 to 7 K / min, more preferably 4 to 6 K / min.

[0101] Furthermore, in the case where the method further comprises calcining the particulate alumina obtained in (iv), (v), (vi), (vii) or (viii) in an atmosphere according to (ix), it is preferred that the atmosphere in (ix) contains one or more of oxygen and nitrogen, wherein the atmosphere in (ix) is more preferably oxygen or air.

[0102] Furthermore, in the case where the method further comprises calcining the particulate alumina obtained in (iv), (v), (vi), (vii) or (viii) in an atmosphere according to (ix), it is preferred that the particulate alumina obtained in (iv), (v), (vi), (vii) or (viii) is calcined in a rotary calciner in (ix).

[0103] Furthermore, in the case where the method further comprises calcining the particulate alumina obtained in (iv), (v), (vi), (vii) or (viii) in an atmosphere according to (ix), it is preferred that the particulate alumina obtained in (iv), (v), (vi), (vii) or (viii) is calcined in (ix) for 0.25 to 2 h, more preferably 0.5 to 1 h.

[0104] Furthermore, the present invention relates to a particulate alumina as obtained and / or obtainable by a method according to any one of the embodiments disclosed herein.

[0105] Preferably, the particulate alumina has a lateral compressive strength in the range from 9 to 25 N / mm, more preferably in the range from 10 to 19 N / mm, more preferably in the range from 11 to 18 N / mm, more preferably in the range from 12 to 17 N / mm, preferably measured according to Reference Example 2.

[0106] Preferably, the particulate alumina has a particle size in the range from 2.0 to 3.0 mm, more preferably in the range from 2.5 to 3.0 mm, preferably according to Reference Example 6.

[0107] Preferably, the micronized aluminum oxide has a particle size of from 0.45 to 0.55 g / cm 3 In the range of from 0.48 to 0.52 g / cm 3 In the range of from 0.49 to 0.51 g / cm3 The filling apparent bulk density is within the range of, preferably measured according to Reference Example 3.

[0108] Preferably, the particulate alumina comprises Na in an amount in the range from 0 to 25000 ppm, more preferably in the range from 0 to 20000 ppm, calculated as elemental Na, preferably determined according to Reference Example 8.

[0109] Preferably, the particulate alumina has a diameter of from 30 to 150 μm. 2 / g, preferably in the range of 40 to 140 m 2 The BET specific surface area in the range of 1000 Å / g is preferably measured according to Reference Example 4.

[0110] Preferably, the particulate alumina has a total pore volume in the range from 0.5 to 1.5 ml / g, more preferably in the range from 0.7 to 1.3 ml / g, more preferably in the range from 0.8 to 1.2 ml / g, preferably determined according to Reference Example 5.

[0111] Preferably, the particulate alumina has a relative particle attrition in the range from 0 wt-% to 2 wt-%, preferably determined according to Reference Example 9.

[0112] Preferably, the particulate alumina is in the form of spheres.

[0113] Still further, the present invention relates to a particulate aluminum oxide having a lateral compressive strength in the range of from 9 to 25 N / mm and a relative humidity in the range of from 0.45 to 0.55 g / cm 3 The filling apparent bulk density is within the range of , wherein the lateral compression strength is preferably measured according to Reference Example 2, and wherein the filling apparent bulk density is preferably measured according to Reference Example 3.

[0114] Preferably, the particulate alumina has a lateral compressive strength in the range from 10 to 19 N / mm, more preferably in the range from 11 to 18 N / mm, more preferably in the range from 12 to 17 N / mm, preferably measured according to Reference Example 2.

[0115] Preferably, the particulate alumina has a particle size in the range from 2.0 to 3.0 mm, more preferably in the range from 2.5 to 3.0 mm, preferably according to Reference Example 6.

[0116] Preferably, the micronized alumina has a particle size of from 0.48 to 0.52 g / cm 3 In the range of from 0.49 to 0.51 g / cm 3 The filling apparent bulk density is within the range of, preferably measured according to Reference Example 3.

[0117] Preferably, the particulate alumina comprises Na in an amount in the range from 0 to 25000 ppm, more preferably in the range from 0 to 20000 ppm, calculated as elemental Na.

[0118] Preferably, the particulate alumina has a diameter of from 30 to 150 μm. 2 / g, more preferably in the range of 40 to 140 m 2 The BET specific surface area in the range of 1000 Å / g is preferably measured according to Reference Example 4.

[0119] Preferably, the particulate alumina has a total pore volume in the range from 0.5 to 1.5 ml / g, more preferably in the range from 0.7 to 1.3 ml / g, more preferably in the range from 0.8 to 1.2 ml / g, preferably determined according to Reference Example 5.

[0120] Preferably, the particulate alumina has a relative particle attrition in the range from 0 wt-% to 2 wt-%, preferably determined according to Reference Example 9.

[0121] Preferably, the particulate alumina is in the form of spheres.

[0122] Still further, the present invention relates to the use of the microparticle alumina according to any one of the embodiments disclosed herein as a catalyst or catalyst support, preferably as a catalyst support for a metal selected from the group consisting of Fe, Ru, Os, Co, Rh, Ir, Ni, Pd, Pt, Cu, Ag, Au and a mixture of two or more thereof, more preferably as a catalyst support for a metal selected from the group consisting of Pd, Ag and a mixture thereof.

[0123] The present invention is further illustrated by the following groups of examples and combinations of examples obtained by dependencies and back-references as shown. In particular, it should be noted that in each case where a series of examples is mentioned, for example in the context of a term such as "a method as described in any one of Examples 1 to 4", each embodiment in this series is intended to be disclosed explicitly to the skilled person, i.e. the wording of this term should be understood by the skilled person as synonymous with "a method as described in any one of Examples 1, 2, 3 and 4".

[0124] In addition, it is explicitly pointed out that the following embodiment group is not a claim group for determining the scope of protection, but represents a suitable structural part of the present description related to general and preferred aspects of the present invention.

[0125] 1. A method for preparing microparticle aluminum oxide, comprising:

[0126] (i) preparing a mixture comprising water and one or more alumina sources;

[0127] (ii) spraying the mixture obtained in (i) to form droplets;

[0128] (iii) heating the droplets obtained in (ii) in a non-polar organic solvent system to a temperature ranging from 85° C. to 100° C. to obtain precursor particles;

[0129] (iv) heating the precursor particles obtained in (iii) in an aqueous solution S2 to a temperature ranging from 85° C. to 110° C. to obtain particulate aluminum oxide, wherein the pH of the aqueous solution S2 is ranging from 12 to 14.

[0130] 2. The method according to embodiment 1, wherein preparing the mixture in (i) comprises cooling the mixture to a temperature in the range of from 0°C to 15°C, preferably in the range of from 2°C to 10°C, more preferably in the range of from 3°C to 7°C.

[0131] 3. The method according to embodiment 1 or 2, wherein (i) comprises

[0132] (i.1) cooling the water to a temperature in the range of from 0°C to 15°C, preferably in the range of from 2°C to 10°C, more preferably in the range of from 3°C to 7°C;

[0133] (i.2) mixing one or more alumina sources with the water cooled in (i.1); to obtain a mixture comprising water and the one or more alumina sources.

[0134] 4. The method of any one of embodiments 1 to 3, wherein preparing the mixture in (i) comprises stirring, preferably with a spiral stirrer, wherein preparing the mixture in (i) preferably comprises stirring at 200 to 300 rpm, more preferably at 225 to 275 rpm.

[0135] 5. The method according to any one of embodiments 1 to 4, wherein the total amount of the one or more alumina sources in the mixture obtained in (i), calculated as Al2O3, is in the range from 40 wt.-% to 65 wt.-%, preferably in the range from 45 wt.-% to 60 wt.-%, more preferably in the range from 50 wt.-% to 55 wt.-%, more preferably in the range from 52 wt.-% to 53 wt.-%, based on the weight of the mixture obtained in (i).

[0136] 6. A method according to any one of embodiments 1 to 6, wherein the one or more alumina sources comprise, preferably consist of, one or more of aluminum hydroxide, Al2O3·0.5H2O, ρ-alumina and sodium aluminate, preferably one or more of gibbsite (α-aluminum hydroxide), bayerite (β-aluminum hydroxide), nordstrandite (γ-aluminum hydroxide), pseudo-amorphous aluminum hydroxide, Al2O3·0.5H2O, ρ-alumina and sodium aluminate, wherein the one or more alumina sources more preferably comprise, more preferably consist of, one or more of sodium aluminate, Al2O3·0.5H2O and ρ-alumina.

[0137] 7. The method according to any one of embodiments 1 to 6, wherein the one or more alumina sources comprise sodium aluminate, and wherein preparing the mixture according to (i) comprises adding an aqueous solution of sodium aluminate in an amount in the range from 0.05 volume-% to 1.5 volume-%, preferably in the range from 0.1 volume-% to 1.0 volume-%, based on the volume of the mixture obtained in (i).

[0138] 8. The method according to embodiment 7, wherein the aqueous sodium aluminate solution comprises from 32 wt-% to 44 wt-%, preferably from 36 wt-% to 40 wt-%, more preferably from 37 wt-% to 39 wt-% of sodium aluminate, based on the weight of the aqueous sodium aluminate solution.

[0139] 9. The method according to any one of embodiments 1 to 8, wherein the one or more alumina sources contained in the mixture obtained in (i) are ground, preferably ball-milled, hammer-milled or jet-milled, more preferably ball-milled.

[0140] 10. A method according to any one of embodiments 1 to 9, wherein one or more of the one or more alumina sources contained in the mixture obtained in (i) is solid, wherein the one or more alumina solid sources in the mixture obtained in (i) have a volume-based particle size D50 value in the range from 1 to 11 microns, preferably in the range from 2 to 8 microns, more preferably in the range from 3 to 7 microns, preferably determined according to Reference Example 7.

[0141] 11. The method according to any one of embodiments 1 to 10, wherein the mixture obtained in (i) has a viscosity in the range from 700 to 900 mPa·s, preferably in the range from 750 to 850 mPa·s, more preferably in the range from 790 to 810 mPa·s.

[0142] 12. The method according to any one of embodiments 1 to 11, wherein the mixture obtained in (i) comprises sodium hydroxide in an amount in the range from 0 mol-% to 1 mol-%, preferably in the range from 0 mol-% to 0.1 mol-%, preferably in the range from 0 mol-% to 0.01 mol-%, calculated as Al2O3, based on the total amount of the one or more alumina sources.

[0143] 13. The process according to any one of embodiments 1 to 12, wherein the mixture obtained in (i) is sprayed in (ii) through a nozzle, preferably under vibration of the nozzle.

[0144] 14. The method according to embodiment 13, wherein the nozzle comprises a hole with a diameter in the range from 1.0 to 1.4 mm, preferably in the range from 1.1 to 1.3 mm.

[0145] 15. The method according to embodiment 13 or 14, wherein the nozzle is arranged to allow spraying the mixture obtained in (i) in the falling direction of the formed droplets.

[0146] 16. The method according to any one of embodiments 1 to 15, wherein the mixture obtained in (i) is sprayed through the nozzle according to (ii) with a frequency in the range of 1 to 5 drops / second, preferably in the range of from 1 to 3 drops / second.

[0147] 17. The method according to any one of embodiments 1 to 16, wherein the mixture obtained in (i) is sprayed through the nozzle according to (ii) to obtain droplets having an average diameter in the range from 1 to 5 mm, preferably in the range from 2 to 4 mm, more preferably in the range from 2.5 to 3.5 mm.

[0148] 18. The method according to any one of embodiments 1 to 17, wherein spraying the mixture obtained in (i) according to (ii) comprises applying at a depth of from 50 to 80 cm 3 / min, preferably in the range of from 55 to 75 cm 3 / min, more preferably in the range of from 60 to 70 cm / min 3 The flow rate is in the range of 1000 / min.

[0149] 19. The method according to any one of embodiments 1 to 18, wherein spraying the mixture obtained in (i) according to (ii) comprises applying an overpressure in the range from 0.1 to 0.8 bar, preferably in the range from 0.2 to 0.7 bar, more preferably in the range from 0.3 to 0.6 bar.

[0150] 20. The method of any one of embodiments 1 to 19, wherein the method further comprises after (ii) and before (iii)

[0151] causing the droplets obtained in (ii) to fall through the atmosphere,

[0152] wherein the atmosphere has a temperature in the range from 10° C. to 60° C., preferably in the range from 15° C. to 50° C.,

[0153] The atmosphere preferably comprises one or more of nitrogen and oxygen, and more preferably the atmosphere is air.

[0154] 21. The method according to any one of embodiments 1 to 20, wherein in (iii) the droplets obtained in (ii) are heated for a duration in the range of from 10 to 50 s, preferably in the range of from 14 to 40 s, more preferably in the range of from 15 to 30 s, more preferably in the range of from 20 to 25 s, more preferably in the range of from 21 to 22 s.

[0155] 22. The method according to any one of embodiments 1 to 21, wherein the droplets obtained in (ii) are heated in (iii) to a temperature in the range from 90°C to 98°C, preferably in the range from 94°C to 96°C.

[0156] 23. The method according to any one of embodiments 1 to 22, wherein the droplets obtained in (ii) are heated in a column in (iii).

[0157] 24. The method according to embodiment 23, wherein the column has a length in the range from 0.5 to 5 m, preferably in the range from 1 to 4 m, more preferably in the range from 2 to 3 m.

[0158] 25. The method according to embodiment 23 or 24, wherein the column has a diameter in the range from 30 to 70 mm, preferably in the range from 45 to 55 mm.

[0159] 26. The method according to any one of embodiments 1 to 25, wherein heating the droplets obtained in (ii) according to (iii) comprises keeping the droplets suspended in the non-polar organic solvent, preferably by letting the droplets fall through the non-polar organic solvent system.

[0160] 27. The method according to any one of embodiments 1 to 26, wherein the non-polar organic solvent system comprises S in an amount in the range from 0 wt-% to 0.2 wt-%, preferably in the range from 0 wt-% to 0.1 wt-%, based on the weight of the non-polar organic solvent system, wherein the amount of S is preferably determined according to DIN EN ISO 14596.

[0161] 28. The method according to any one of embodiments 1 to 27, wherein the non-polar organic solvent system has a density in the range of from 850 to 880 g / ml, preferably in the range of from 860 to 870 g / ml, wherein the density is preferably determined at a temperature of 20° C., wherein the density is preferably determined according to DIN 51757 Test Procedure 3 (German DIN 51757 Verf 3).

[0162] 29. The method of any one of embodiments 1 to 28, wherein the non-polar organic solvent system has a molecular weight of from 4.8 to 5.6 mm 2 / s, preferably in the range of from 5.0 to 5.4 mm 2 The kinematic viscosity is preferably in the range of 100° C. to 200° C., wherein the kinematic viscosity is preferably determined in accordance with DIN EN ISO 3104.

[0163] 30. The method according to any one of embodiments 1 to 29, wherein the non-polar organic solvent system has a refractive index in the range from 1.4763 to 1.4769, preferably in the range from 1.4765 to 1.4767, wherein the refractive index is preferably determined at a temperature of 100° C., wherein the refractive index is preferably determined according to DIN 51423-02.

[0164] 31. The method according to any one of embodiments 1 to 30, wherein the non-polar organic solvent system comprises aromatic hydrocarbons in an amount in the range from 2 wt-% to 4 wt-%, preferably in the range from 2.5 wt-% to 3.5 wt-%, based on the weight of the non-polar organic solvent system, wherein the amount of aromatic hydrocarbons is preferably determined according to calculation method U of DIN 51378.

[0165] 32. The method according to any one of embodiments 1 to 31, wherein the non-polar organic solvent system comprises cycloalkanes in an amount in the range from 28 wt-% to 34 wt-%, preferably in the range from 30 wt-% to 32 wt-%, based on the weight of the non-polar organic solvent system, wherein the amount of cycloalkanes is preferably determined according to calculation method U of DIN 51378.

[0166] 33. The method according to any one of embodiments 1 to 32, wherein the non-polar organic solvent system comprises paraffins in an amount in the range from 61 wt-% to 69 wt-%, preferably in the range from 63 wt-% to 67 wt-%, based on the weight of the non-polar organic solvent system, wherein the amount of paraffins is preferably determined according to calculation method U of DIN 51378.

[0167] 34. The method according to any one of embodiments 1 to 33, wherein the non-polar organic solvent system has a viscosity index in the range from 97 to 103, preferably in the range from 99 to 101, wherein the viscosity index is preferably determined according to DIN ISO 2909.

[0168] 35. The method according to any one of embodiments 1 to 34, wherein heating the droplets obtained in (ii) according to (iii) comprises applying a flow of the non-polar organic solvent system opposite to the falling direction of the droplets.

[0169] 36. The method of any one of embodiments 1 to 35, further comprising collecting the precursor particles in aqueous solution S1 after (iii) and before (iv).

[0170] 37. The method according to embodiment 36, wherein the pH of the aqueous solution S1 is in the range from 11.0 to 14.0, preferably in the range from 12.0 to 13.7, more preferably in the range from 13.0 to 13.5.

[0171] 38. The method according to embodiment 36 or 37, wherein the precursor particles are collected in the aqueous solution S1 in a column, wherein more preferably the precursor particles are collected in the same column in which the droplets obtained in (ii) are heated according to (iii).

[0172] 39. The method according to any one of embodiments 36 to 38, wherein heating the droplets obtained in (ii) in the non-polar organic solvent system according to (iii) and collecting the droplets in the aqueous solution S1 is performed in a column, wherein the column comprises the non-polar organic solvent system and the aqueous solution S1,

[0173] wherein the droplets obtained in (ii) are heated according to (iii) before being collected in the aqueous solution S1,

[0174] Therein the process preferably comprises passing the droplets obtained in (ii) through the non-polar organic solvent system before being collected in the aqueous solution S1.

[0175] 40. The method according to any one of embodiments 1 to 39, wherein the precursor particles obtained in (iii) in the aqueous solution S2 are heated in a container according to (iv).

[0176] 41. A method according to any one of embodiments 1 to 40, wherein in (iv), the weight ratio of the precursor particles calculated as the sum of the weights of the precursor particles to the aqueous solution S2 calculated as the weight of the aqueous solution S2 is in the range of from 1:2 to 1:20, preferably in the range of from 1:4 to 1:15, and more preferably in the range of from 1:6 to 1:10.

[0177] 42. The method according to any one of embodiments 1 to 41, wherein the aqueous solution S2 comprises one or more of sodium aluminate (NaAlO2), ammonia and sodium hydroxide (NaOH), preferably sodium aluminate (NaAlO2) and sodium hydroxide.

[0178] 43. A method according to embodiment 42, wherein the aqueous solution S2 contains, in addition to the aluminum contained in these precursor particles, an amount of aluminum calculated as Al2O3 in the range from 3.00 to 6.50 g / l, preferably in the range from 4.50 to 5.00 g / l, more preferably in the range from 4.65 to 4.80 g / l.

[0179] 44. A method according to embodiment 42 or 43, wherein the aqueous solution S2 contains, in addition to the sodium optionally contained in the precursor particles, sodium in an amount calculated as Na in the range from 2.00 to 5.00 g / l, preferably in the range from 3.40 to 3.80 g / l, more preferably in the range from 3.55 to 3.65 g / l.

[0180] 45. A method according to any one of embodiments 1 to 44, wherein the pH of the aqueous solution S2 according to (iv) is in the range of from 12.2 to 13.9, preferably in the range of from 12.4 to 13.8, more preferably in the range of from 12.6 to 13.7, more preferably in the range of from 12.8 to 13.6, more preferably in the range of from 13.0 to 13.5, wherein the pH is preferably determined according to Reference Example 1.

[0181] 46. ​​A method according to any one of embodiments 1 to 45, wherein the precursor particles obtained in (iii) are heated to a temperature in the range of from 87°C to 105°C, preferably in the range of from 89°C to 102°C, more preferably in the range of from 90°C to 100°C according to (iv).

[0182] 47. The method according to any one of embodiments 1 to 46, wherein the precursor particles obtained in (iii) are heated according to (iv) for a duration in the range from 3 to 25 h, preferably in the range from 4 to 20 h, more preferably in the range from 5 to 17 h.

[0183] 48. The method of any one of embodiments 1 to 47, further comprising

[0184] (v) separating the particulate alumina obtained in (iv) from the aqueous solution S2, wherein the separation preferably comprises filtering or centrifuging the aqueous solution S2.

[0185] 49. The method of any one of embodiments 1 to 48, further comprising

[0186] (vi) washing the particulate alumina obtained in (iv) or (v) with a liquid solvent system,

[0187] wherein the liquid solvent system preferably comprises one or more of water, alcohol, and a mixture of two or more thereof, wherein the particulate alumina is more preferably washed with water, wherein the particulate alumina is more preferably washed with deionized water, wherein the particulate alumina is more preferably washed with deionized water until the conductivity of the washing water is less than 400 μS.

[0188] 50. The method of any one of embodiments 1 to 49, further comprising

[0189] (vii) drying the fine-particle alumina obtained in (iv), (v) or (vi) in an atmosphere.

[0190] 51. The method according to embodiment 50, wherein the atmosphere in (vii) has a temperature in the range from 90°C to 130°C, preferably in the range from 100°C to 120°C, more preferably in the range from 105°C to 115°C.

[0191] 52. The method according to embodiment 50 or 51, wherein the atmosphere in (vii) comprises one or more of oxygen and nitrogen, wherein the atmosphere in (vii) is preferably oxygen or air.

[0192] 53. The method according to any one of embodiments 50 to 52, wherein in (vii) the particulate alumina obtained in (iv), (v) or (vi) is dried in an oven or in a belt dryer, preferably in a belt dryer.

[0193] 54. The method according to any one of embodiments 50 to 53, wherein in (vii) the particulate alumina obtained in (iv), (v) or (vi) is dried for 1 to 5 h, preferably 2 to 3 h.

[0194] 55. The method of any one of embodiments 1 to 54, further comprising

[0195] (viii) pre-calcining the fine-particle alumina obtained in (iv), (v), (vi) or (vii) in an atmosphere.

[0196] 56. The method of embodiment 55, wherein the atmosphere in (viii) has a temperature in the range of from 400°C to 460°C, preferably in the range of from 420°C to 440°C, more preferably in the range of from 425°C to 435°C.

[0197] 57. The method according to embodiment 55 or 56, wherein the precalcination according to (viii) comprises heating the atmosphere with a heating ramp of 3 to 7 K / min, preferably 4 to 6 K / min.

[0198] 58. The method according to any one of embodiments 55 to 57, wherein the atmosphere in (viii) comprises one or more of oxygen and nitrogen, wherein the atmosphere in (viii) is preferably oxygen or air.

[0199] 59. The method according to any one of embodiments 55 to 58, wherein in (viii) the particulate alumina obtained in (iv), (v), (vi) or (vii) is pre-calcined in a rotary calciner.

[0200] 60. The method according to any one of embodiments 55 to 59, wherein the particulate alumina obtained in (iv), (v), (vi) or (vii) is pre-calcined in (viii) for 0.25 to 2 h, preferably 0.5 to 1 h.

[0201] 61. The method of any one of embodiments 1 to 60, further comprising

[0202] (ix) calcining the fine-particle alumina obtained in (iv), (v), (vi), (vii) or (viii) in an atmosphere.

[0203] 62. The method according to embodiment 61, wherein the atmosphere in (ix) has a temperature in the range from 900°C to 1050°C, preferably in the range from 940°C to 980°C, more preferably in the range from 945°C to 975°C.

[0204] 63. The method according to embodiment 61 or 62, wherein the calcining according to (ix) comprises heating the atmosphere with a heating ramp of 3 to 7 K / min, preferably 4 to 6 K / min.

[0205] 64. The method according to any one of embodiments 61 to 63, wherein the atmosphere in (ix) comprises one or more of oxygen and nitrogen, wherein the atmosphere in (ix) is preferably oxygen or air.

[0206] 65. The method according to any one of embodiments 61 to 64, wherein in (ix) the particulate alumina obtained in (iv), (v), (vi), (vii) or (viii) is calcined in a rotary calciner.

[0207] 66. The method according to any one of embodiments 61 to 65, wherein the particulate alumina obtained in (iv), (v), (vi), (vii) or (viii) is calcined in (ix) for 0.25 to 2 h, preferably 0.5 to 1 h.

[0208] 67. A particulate alumina as obtained and / or obtainable by the method according to any one of embodiments 1 to 66.

[0209] 68. The particulate alumina according to Example 67 has a lateral compressive strength in the range of from 9 to 25 N / mm, preferably in the range of from 10 to 19 N / mm, more preferably in the range of from 11 to 18 N / mm, more preferably in the range of from 12 to 17 N / mm, preferably measured according to Reference Example 2.

[0210] 69. The particulate alumina according to embodiment 67 or 68, having a particle size in the range of from 2.0 to 3.0 mm, preferably in the range of from 2.5 to 3.0 mm, preferably according to reference example 6.

[0211] 70. The micronized alumina of any one of embodiments 67 to 69 having a relative humidity of from 0.45 to 0.55 g / cm 3 In the range of 0.48 to 0.52 g / cm 3 In the range of from 0.49 to 0.51 g / cm 3 The filling apparent bulk density is within the range of, preferably measured according to Reference Example 3.

[0212] 71. The microparticle alumina according to any one of embodiments 67 to 70, comprising Na in an amount in the range from 0 to 25000 ppm, preferably in the range from 0 to 20000 ppm, calculated as elemental Na, preferably determined according to Reference Example 8.

[0213] 72. The particulate alumina of any one of embodiments 67 to 71 having a particle size of from 30 to 150 m 2 / g, preferably in the range of 40 to 140 m 2 The BET specific surface area in the range of 1000 Å / g is preferably measured according to Reference Example 4.

[0214] 73. The microparticle alumina according to any one of Examples 67 to 72, having a total pore volume in the range from 0.5 to 1.5 ml / g, preferably in the range from 0.7 to 1.3 ml / g, more preferably in the range from 0.8 to 1.2 ml / g, preferably determined according to Reference Example 5.

[0215] 74. The microparticle alumina of any one of embodiments 67 to 73, having a relative particle attrition in the range from 0 wt-% to 2 wt-%, preferably determined according to Reference Example 9.

[0216] 75. The particulate alumina of any one of embodiments 67 to 74 in the form of spheres.

[0217] 76. A particulate alumina having a lateral compressive strength in the range of from 9 to 25 N / mm and a relative humidity in the range of from 0.45 to 0.55 g / cm 3 The filling apparent bulk density is within the range of , wherein the lateral compression strength is preferably measured according to Reference Example 2, and wherein the filling apparent bulk density is preferably measured according to Reference Example 3.

[0218] 77. The microparticle alumina according to Example 76 has a lateral compressive strength in the range of from 10 to 19 N / mm, preferably in the range of from 11 to 18 N / mm, more preferably in the range of from 12 to 17 N / mm, preferably measured according to Reference Example 2.

[0219] 78. The particulate alumina according to embodiment 76 or 77, having a particle size in the range of from 2.0 to 3.0 mm, preferably in the range of from 2.5 to 3.0 mm, preferably according to reference example 6.

[0220] 79. The micronized alumina of any one of embodiments 76 to 78 having a relative humidity of from 0.48 to 0.52 g / cm 3 In the range of from 0.49 to 0.51 g / cm 3 The filling apparent bulk density is within the range of, preferably measured according to Reference Example 3.

[0221] 80. The particulate alumina according to any one of embodiments 76 to 79, comprising Na in an amount in the range from 0 to 25000 ppm, preferably in the range from 0 to 20000 ppm, calculated as elemental Na.

[0222] 81. The particulate alumina of any one of embodiments 76 to 80 having a particle size of from 30 to 150 m 2 / g, preferably in the range of 40 to 140 m 2The BET specific surface area in the range of 1000 Å / g is preferably measured according to Reference Example 4.

[0223] 82. The microparticle alumina according to any one of Examples 76 to 81, having a total pore volume in the range of from 0.5 to 1.5 ml / g, preferably in the range of from 0.7 to 1.3 ml / g, more preferably in the range of from 0.8 to 1.2 ml / g, preferably determined according to Reference Example 5.

[0224] 83. The microparticle alumina of any one of embodiments 76 to 82, having a relative particle attrition in the range from 0 wt-% to 2 wt-%, preferably determined according to Reference Example 9.

[0225] 84. The particulate alumina of any one of embodiments 76 to 83 in the form of spheres.

[0226] 85. A use of the microparticle alumina according to any one of embodiments 67 to 84 as a catalyst or catalyst support, preferably as a catalyst support for a metal selected from the group consisting of Fe, Ru, Os, Co, Rh, Ir, Ni, Pd, Pt, Cu, Ag, Au and mixtures of two or more thereof, more preferably as a catalyst support for a metal selected from the group consisting of Pd, Ag and mixtures thereof.

[0227] The present invention is further illustrated by the following Reference Examples, Examples and Comparative Examples.

[0228] Examples

[0229] Reference Example 1: Determination of pH value

[0230] The pH was measured with a pH 3310 pH meter from WTW. Before each use, the pH electrode was calibrated at room temperature using standard solutions for calibration with pH = 7 and pH = 10, respectively. The pH of the starting solution was measured at room temperature. To monitor the pH during the synthesis, repeated sampling was performed and measured at room temperature. The temperature dependence of the pH value was taken into account.

[0231] Reference Example 2: Determination of lateral compression strength

[0232] The lateral compression strength is measured by placing the spherical particles between two parallel plates of a testing machine such as the Schleuniger 6D manufactured by Schleuniger Pharmatron. The amount of force required to crush the particles is measured in Newtons. A sufficient number of particles (35) are crushed to obtain a statistically significant estimate of the total population. Mean values ​​are calculated from individual results. The amount of force required to crush the particles can be converted to N / mm by dividing the amount of force required to crush the particles by the size of the particles measured as described in Reference Example 6.

[0233] Reference Example 3: Determination of Apparent Bulk Density of Filling

[0234] The apparent bulk density of the fill was measured using a Dr. Schleuniger Pharmatron AG tap density tester JV-2000.

[0235] General description of the assay method:

[0236] Fill the graduated cylinder with sample in 5 steps, 250 ml sample in total. Perform 200 taps after each filling step. Finally, perform another 200 taps. Thus obtain the filled catalyst bed. When the graduated cylinder is filled, read the volume and determine the net weight of the graduated cylinder. The weight / volume ratio is PABD.

[0237] Detailed determination method:

[0238] 1. Determine the tare weight of the measuring cylinder to the nearest 0.1 gram (T, g).

[0239] 2. Fill the graduated cylinder with approximately 50 ml of sample.

[0240] 3. Place the measuring cylinder on the impression and secure it with the appropriate bayonet fitting.

[0241] 4. If necessary, use the function keys to select the appropriate method.

[0242] 5. Use the numeric keys to enter 200 to set the number of taps.

[0243] 6. Press start. Then, apply 200 taps.

[0244] 7. Fill the cylinder with another 50 ml of sample and press start (tap 200 more times).

[0245] 8. Repeat step 73 more times (a total of 5 fillings and 1000 taps).

[0246] 9. Then, vibrate another 200 times, for a total of 1200 resonances.

[0247] 10. Read the final volume (V, ml).

[0248] 11. Determine the weight of the filled cylinder (G, grams).

[0249] 12. Calculate the apparent bulk density of the fill according to the following formula:

[0250] PABD=(GT) / V.

[0251] Reference Example 4: Determination of BET specific surface area

[0252] The BET specific surface area was determined via nitrogen physical adsorption at 77 K according to the method disclosed in ISO 9277:2010.

[0253] Reference Example 5: Determination of total pore volume

[0254] The total pore volume is determined by mercury intrusion porosimetry according to standard ASTM D 4284-12.

[0255] Reference Example 6: Determination of particle diameter

[0256] Particle size was measured using a sliding micrometer apparatus.

[0257] Reference Example 7: Determination of volume-based particle size distribution

[0258] The volume-based particle size distribution (PSD) is measured on a sample in powder form. It is measured by laser diffraction with a Malvernmastersizer device. First, the sample is dispersed in water. For the measurement, the sample is then placed in a measuring chamber. The intensity of the scattered light is then measured by a detector, and the particle size distribution is then calculated from this intensity. (Malvern Panalytical, 2019)

[0259] Reference Example 8: Determination of Na content

[0260] The Na content of the samples was determined using an iCE3000AA atomic absorption spectrometer (Thermo Scientific).

[0261] General description of the assay method:

[0262] After the metal is placed in the solution, this solution is atomized in a flame. The metal absorbs a portion of the wavelength of light specific to it, which is emitted by a hollow cathode lamp specific to the element. The amount of light absorbed is measured using a photomultiplier tube and is a measure of the concentration. In addition to absorption, emission can also be measured with this device. The radiation emitted from the element to be measured is measured with a photomultiplier tube. A radiation buffer is added to prevent ionization.

[0263] Calibration method:

[0264] 1. AAS calibration was performed using a 10 mg / L sodium solution as a reference. The reference solution was made from a certified standard of 1000 ppm sodium.

[0265] 2. Measure the reference solution as follows. Perform a reference measurement after every 5 measurements.

[0266] Draw a calibration curve for the determination of sodium:

[0267] 1. Based on 1000 mg / l Na stock solution, generate a calibration curve according to the table below.

[0268]

[0269] 2. Fill the flask with demineralized water and homogenize.

[0270] 3. Enter the default line according to the procedure. As indicated above, the calibration standard is 10 mg / l.

[0271] Detailed determination method:

[0272] 1. Connect the equipment and open the acetylene and air valves.

[0273] 2. In the gas chamber, set the acetylene pressure to 0.75 bar.

[0274] 3. Set the air pressure on the panel to 2.9 bar

[0275] 4. Turn on the spectrometer

[0276] 5. Launch the software

[0277] 7. Turn on the lights

[0278] 8. Select the correct light in the menu and set the status to ON. Allow the light to stabilize for half an hour.

[0279] 9. Choose the analysis method

[0280] 10. Create a new result file

[0281] 11. Check the burner height. When the unit is switched on, the burner height will be approximately 16.3 mm. Use the knob to set the burner height to approximately 7 mm

[0282] 12. Open the burner compartment with the knob on the right.

[0283] 13. Use a test block to check whether the light beam is shining tightly on the burner opening.

[0284] 14. If necessary, correct the lateral adjustment by turning the left knob on the outside near the suction hose. The door must be closed for this. The button must be pressed in order to turn.

[0285] 15. Remove the test piece from the burner

[0286] 16. Close the burner compartment and check that the white button on the left is flashing.

[0287] 17. Light the flame by briefly pressing the white button on the left until the burner lights.

[0288] 18. Start the method and then perform the analysis.

[0289] 19. When measuring with AAS, start with demineralized water. The device regulates the height of the burner itself.

[0290] 20. Continue to follow the on-screen instructions.

[0291] 21. After measuring, switch off the burner using the red button on the left side of the device.

[0292] 22. Turn off lights and gas taps.

[0293] Reference Example 9: Determination of relative particle abrasion

[0294] Abrasion was measured according to ASTM D4058-7.

[0295] An attrition resistant Rotab AS / S having a rotating drum equipped with a baffle and a 20 mesh (0.850 mm) screen was used.

[0296] Detailed description of the assay:

[0297] 1. Open the Rotab door and unscrew the drum

[0298] 2. Weigh approximately 100 grams of sample and place in a 600 ml beaker in the powder cabinet.

[0299] 3. Carefully sieve this sample to remove any "fines" that may be present

[0300] 4. Weigh the sample to the nearest 0.01 g (A, g)

[0301] 5. Place the sample in the baffle drum and close it. Make sure the 8 bolts are tightened crosswise. It is also important to tighten the bolts properly. This ensures that no powder is released during the rotation.

[0302] 6. Open the door of the Rotab and place the drum. Make sure that the opening of the drum falls exactly on the axis of rotation. With the help of a special wrench, tighten the screws on the drum. Close the door. The counter is set to 1800 by default. The top line must be set to 0. The speed is set to 60rpm by default

[0303] 7. After 30 minutes, remove the sample from the drum and sieve on a 20 mesh screen. Use acrylic gloves and sleeve protectors.

[0304] 8. Weigh the material retained on the sieve in the powder cabinet to the nearest 0.01 g (B, g)

[0305] 9. Calculate the wear (%) according to the following formula:

[0306] (AB) / A*100

[0307] Example 1: Method for preparing micro-alumina

[0308] In a container, 655 g of deionized water were cooled to 5° C. Then, 740 g of alumina (p-alumina, amorphous Al2O3·0.5H2O; ball-milled to a volume-based particle size D50 of 5 microns) were added while stirring with a spiral stirrer at 250 rpm to obtain a mixture containing 52.5 wt-% alumina. The alumina was added over about 30 minutes. The resulting slurry was stirred overnight. The slurry then had a viscosity of about 800 mPa·s.

[0309] To form the droplets, a vibrating nozzle is used which implements a laminar jet breakup mechanism to generate droplets from the slurry.

[0310] The droplets formed by dispersing the slurry through the nozzle fall about 10 cm in the air into the oil contained in the forming tower. The forming tower comprises a steel column with a total length of 3 m and a diameter of 50 mm. The forming tower is filled with oil over a length of 2.5 m of the column, and with water over a length of 0.5 m of the column. Thus, the column comprises an oil phase and an aqueous phase. The oil phase is heated to a temperature of 90° C. In addition, a flow of oil opposite to the falling direction of the precursor particles is established. For this purpose, a sinus pump is used. The residence time of the droplets in the oil is about 21 s. During the time, precursor particles are formed. The precursor particles are then collected in the aqueous phase, wherein the pH of the aqueous phase is adjusted to 11 by adding NaOH.

[0311] The collected precursor particles are then conveyed in a stream of water into a collection container. The precursor particles are then aged in the collection container. To this end, the pH of the mixture comprising water and precursor particles is adjusted to 13 by adding sodium aluminate (NaAlO2). The weight ratio of precursor particles to water is 1:8. The mixture is then heated to a temperature of 100°C and the precursor particles are aged overnight at said temperature.

[0312] The obtained particulate alumina was then washed with deionized water. Subsequently, the washed particulate alumina was dried in an oven at 110° C. in air for 2 to 3 hours. Finally, the dried particulate alumina was calcined in an oven in air according to the procedure outlined in Table 1 below.

[0313] Table 1

[0314] Calcination procedure for calcining the obtained particulate alumina.

[0315] temperature Keep Target 110℃ 5h Heating ramp 5℃ / min Target 430℃ 0.75h Heating ramp 5℃ / min Target 970℃ 0.75h

[0316] The average particle size of the obtained micro-alumina was 2.7 mm, the lateral compression strength was 44 N (N / particle, average value for 35 alumina particles), the packing apparent bulk density was 0.50 g / ml, the Na content was 12500 ppm, and the BET specific surface area was 136 m 2 / g, and the total pore volume is 0.86 ml / g.

[0317] Table 2

[0318] The pore distribution of Example 1 measured according to Reference Example 5.

[0319]

[0320]

[0321]

[0322] Example 2: Method for preparing micro-alumina

[0323] Example 1 was repeated except that the pH of the mixture comprising water and precursor particles used for aging was adjusted to 13.5 (instead of 13).

[0324] The average particle size of the obtained micro-alumina was 2.7 mm, the lateral compression strength was 51 N (N / particle, average value for 35 alumina particles), the packing apparent bulk density was 0.51 g / ml, the Na content was 18411 ppm, and the BET specific surface area was 121 m 2 / g, and the total pore volume is 0.83 ml / g.

[0325] Table 3

[0326] The pore distribution of Example 2 was measured according to Reference Example 5.

[0327]

[0328]

[0329] Example 3: Method for preparing micro-alumina

[0330] Example 1 was repeated except that the mixture was heated to a temperature of 95°C during aging.

[0331] The average particle size of the obtained micro-alumina was 2.77 mm, the lateral compression strength was 79.9 N (N / particle, average value for 35 alumina particles), the Na content was 2120 ppm, and the BET specific surface area was 150 m 2 / g, and the total pore volume is 0.87 ml / g.

[0332] Table 4

[0333] The pore distribution of Example 3 was measured according to Reference Example 5.

[0334]

[0335] Comparative Example 3: Method for preparing micro-alumina according to the prior art

[0336] Example 1 was repeated except that the pH of the mixture comprising water and precursor particles used for aging was adjusted to 11 (instead of 13).

[0337] The average particle size of the obtained micro-alumina was 2.7 mm, the lateral compression strength was 18.4 N (N / particle, average value for 35 alumina particles), the packing apparent bulk density was 0.47 g / ml, the Na content was 410 ppm, and the BET specific surface area was 122 m 2 / g, and the total pore volume is 0.96 ml / g.

[0338] Comparative Example 4: Method for preparing micro-alumina according to the prior art

[0339] Example 1 was repeated except that the pH of the mixture comprising water and precursor particles used for aging was adjusted to 7 (instead of 13).

[0340] The average particle size of the obtained micro-alumina was 2.8 mm, the lateral compression strength was 18.8 N (N / particle, average value for 35 alumina particles), the packing apparent bulk density was 0.49 g / ml, the Na content was 2180 ppm, and the BET specific surface area was 128 m 2 / g, and the total pore volume is 0.95 ml / g.

[0341] As can be seen from Examples 1-2 according to the invention, the method of the invention allows the preparation of microparticle alumina having excellent physical integrity, as shown in particular by a relatively high lateral compressive strength.

[0342] -US 7090825 B2

[0343] -US 4065407 A

[0344] -US 4169874 A

[0345] -US 6197073 B1

[0346] -US 4318896 A

[0347] -US 4542113 A

[0348] -EP 0 153674 A2

[0349] -US 3223483 A

[0350] -US 4279779 A

[0351] -US 4411771 A

[0352] -US 4315839 A

[0353] -US 10232346 B2

[0354] -US 4390456 A

Claims

1. A method for preparing microparticle aluminum oxide, comprising: (i) preparing a mixture comprising water and one or more alumina sources; (ii) spraying the mixture obtained in (i) to form droplets; (iii) heating the droplets obtained in (ii) in a non-polar organic solvent system to a temperature ranging from 85° C. to 100° C. to obtain precursor particles; (iv) heating the precursor particles obtained in (iii) in an aqueous solution S2 to a temperature ranging from 85° C. to 110° C. to obtain particulate aluminum oxide, wherein the pH of the aqueous solution S2 is ranging from 12 to 14.

2. The method according to claim 1, wherein: The total amount of the one or more alumina sources in the mixture obtained in (i) is in the range from 40 wt-% to 65 wt-% calculated as Al2O3, based on the weight of the mixture obtained in (i).

3. The method according to claim 1 or 2, wherein: The one or more alumina sources include one or more of aluminum hydroxide, Al2O3·0.5H2O, rho-alumina and sodium aluminate.

4. The method according to any one of claims 1 to 3, wherein: In (ii), the mixture obtained in (i) is sprayed through a nozzle.

5. The method according to any one of claims 1 to 4, wherein: Heating the droplets obtained in (ii) according to (iii) comprises keeping the droplets suspended in the non-polar organic solvent system, preferably by letting the droplets fall through the non-polar organic solvent system.

6. The method according to any one of claims 1 to 5, further comprising collecting the precursor particles in an aqueous solution S1 after (iii) and before (iv).

7. The method according to claim 6, wherein: The pH of the aqueous solution S1 is in the range from 11.0 to 14.

0.

8. The method according to claim 6 or 7, wherein: heating the droplets obtained in (ii) in the non-polar organic solvent system according to (iii) and collecting the droplets in the aqueous solution S1 is carried out in a column, wherein the column comprises the non-polar organic solvent system and the aqueous solution S1, Therein the droplets obtained in (ii) are heated according to (iii) before being collected in the aqueous solution S1.

9. The method according to any one of claims 1 to 8, wherein: In (iv), a weight ratio of the precursor particles calculated as the sum of the weights of the precursor particles to the aqueous solution S2 calculated as the weight of the aqueous solution S2 ranges from 1:2 to 1:

20.

10. Particulate aluminium oxide as obtained and / or obtainable by a method according to any one of claims 1 to 9.

11. A particulate aluminum oxide having a lateral compressive strength in the range of from 9 to 25 N / mm and a relative humidity in the range of from 0.45 to 0.55 g / cm 3 The filling apparent bulk density is within the range of .

12. The particulate alumina according to claim 11, having a particle size ranging from 2.0 to 3.0 mm.

13. The particulate alumina according to claim 11 or 12, having a particle size of from 30 to 150 m 2 / g in the range of BET specific surface area.

14. Particulate alumina according to any one of claims 11 to 13 having a total pore volume in the range from 0.7 to 1.5 ml / g.

15. Use of the microparticle aluminum oxide according to any one of claims 10 to 14 as a catalyst or catalyst support.