Crystalline glass and method for producing same
By controlling the heat treatment temperature and optimizing the components, the semi-transparent glass with small crystal size is prepared, which solves the energy consumption and irreversibility problems of high-temperature firing, and realizes a controllable transformation from translucent to transparent, reducing energy consumption and avoiding burning Burn damage.
Patent Information
- Application Number
- CN202380036815.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-06-13
- Filing Date
- 2023-06-07
- Publication Date
- 2024-12-06
AI Technical Summary
In the prior art, when preparing translucent crystal glass, high temperature firing leads to high energy consumption and damage to the firing furnace, and the crystallization process is irreversible, making it difficult to restore from the translucent state to the transparent state.
By controlling the heat treatment temperature during crystallization, the crystallization stops in the initial stage, ensuring a large difference in refractive index between the crystallization and the glass phase, semi-transparent glass with a small crystal size is prepared, and it becomes transparent through further heat treatment. Specific processes include heat treatment below the glass transition temperature, optimized component ratios such as SiO2 45-75%, Al2O3 15-35%, Li2O 0-4%, Na2O 0-6%, TiO2 0-1.4%, and ZrO2 0.5% or more , P2O5/(ZrO2+TiO2)≤0.4, Pt+Rh is less than 7ppm, and MoO3 is more than 0%, avoiding As and Pb components.
Crystal glass with the desired translucency and can easily achieve transparency as needed is achieved, reducing energy consumption and avoiding furnace damage.
Smart Images

Figure CN119095808A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a crystallized glass with a translucent appearance. Background Art
[0002] In the past, translucent glass and glass ceramic products were used in windows, doors, etc. for the purpose of both privacy protection and lighting performance. Frosted glass is a type of translucent glass, which is obtained by roughening the surface of the glass by sandblasting, etc., and is mainly used as window glass. However, although frosted glass is effective in protecting privacy, it has a problem that its mechanical strength is easily reduced and it is easily damaged by external impacts, etc. due to its significantly rough surface.
[0003] Therefore, as a translucent glass, a crystallized glass obtained by precipitating coarse crystals in glass has been proposed so far. For example, in Patent Document 1, a Li2O-Al2O3-SiO2 glass is heat-treated at a high temperature to be crystallized, thereby precipitating a β-spodumene solid solution having an average particle size of 150 nm or more into the glass matrix, thereby achieving translucency.
[0004] Similarly, in patent document 2, it is also shown that the optical transparency is changed due to the crystal size and seed crystal of precipitation. The patent document records that by making the β-spodumene solid solution (thermal quartz) with an average particle size greater than 100nm, a translucent or opaque colored crystalline glass can be manufactured. Specifically, by reducing the content of nucleating components to increase the crystal size, a translucent glass ceramic can be prepared.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2003-300752
[0008] Patent Document 2: Japanese Patent Application Publication No. 2005-325018 Summary of the invention
[0009] Technical problem to be solved by the invention
[0010] The method of excessively growing crystals under high temperature conditions as disclosed in Patent Document 1 is not preferred from the perspective of energy consumption, and there is also the problem of increased damage to the firing furnace caused by high temperature firing. Moreover, the crystal growth process as described above is irreversible, so once crystallized, the semi-transparent crystallized glass can basically not be restored to transparency.
[0011] As described in Patent Document 2, although translucent crystallized glass can be produced by changing the composition, it is difficult to generate a dense crystalline phase from glass with significantly less nucleating components. Therefore, it is difficult to obtain transparent crystallized glass by changing the firing conditions with the same composition.
[0012] An object of the present invention is to provide a crystallized glass which has desired translucency and can be easily made transparent as needed.
[0013] Technical solutions for solving technical problems
[0014] The crystallized glass of the present invention is characterized in that the average haze at a wavelength of 380 to 780 nm is greater than 0 and less than 30% when converted to a wall thickness of 4 mm, and the average particle size of the main crystal is 1 to 100 nm.
[0015] The crystallization in the crystallized glass has a tendency that the larger its size is, the stronger the light scattering intensity is. And, there is a tendency that the refractive index difference between the crystallization and the glass phase around it is larger and the light scattering intensity is stronger. For example, as mentioned above, the translucent product of the existing Li2O-Al2O3-SiO2 crystallized glass is ensured translucency by enlarging the crystal size and separating out the β-spodumene solid solution inconsistent with the refractive index of the glass phase. However, the precipitation process of the β-spodumene solid solution that the crystal size is large is irreversible, and therefore, once it becomes a translucent product, it is difficult to restore it to a transparent product.
[0016] After in-depth research, the inventor of the present invention found that by precipitating crystals smaller than existing translucent products, a translucent crystallized glass was achieved. As described later, the crystallized glass can be prepared by controlling the heat treatment temperature during crystallization. Although the detailed mechanism is still under study, the inventor considers the following.
[0017] When the amorphous precursor glass is heat treated to crystallize it, the difference in refractive index between the crystal and the remaining glass phase changes from the initial stage of crystallization to the final stage of crystallization. Specifically, in the initial stage of crystallization, the difference in refractive index between the crystal and the glass phase is large, and as crystallization proceeds, the difference in refractive index becomes smaller. Therefore, if the heat treatment temperature during crystallization is controlled so that it stops at the initial stage of crystallization, the difference in refractive index between the crystal and the remaining glass phase becomes large, and based on the difference in refractive index, a translucent appearance can be obtained. It should be noted that, although in the initial stage of crystallization, the average particle size of the crystal is as small as 1 to 100 nm, even if the heat treatment is directly further performed to promote crystallization to a certain extent, the average particle size of the crystal does not change substantially. On the other hand, since the difference in refractive index between the crystal and the glass phase gradually decreases (even when the difference in refractive index is close to zero, or becomes zero), the crystallized glass can be made transparent. In this way, the crystallized glass of the present invention can be easily transparentized from a translucent state by further heat treatment.
[0018] In this specification, the "average haze" refers to the arithmetic mean of the haze obtained by using the following formula for the total light transmittance and diffuse transmittance of the glass at a specific wavelength obtained using an integrating sphere.
[0019] Haze = diffuse transmittance / total light transmittance
[0020] The crystallized glass of the present invention preferably contains the following components in mass %. In this way, desired translucent crystallized glass can be easily obtained.
[0021] SiO2 45~75%,
[0022] Al2O3 15~35%,
[0023] Li2O 0~4%,
[0024] Na2O 0~6%,
[0025] K2O 0~10%,
[0026] TiO2 0~1.4%,
[0027] SnO2 0~3%,
[0028] P2O5 0~2%,
[0029] ZrO2 0.5% or more,
[0030] P2O5 / (ZrO2+TiO2)≤0.4.
[0031] In addition, in this specification, "x+y+..." means the sum of the contents of each component, and "x / y" means the value obtained by dividing the content of x by the content of y.
[0032] The crystallized glass of the present invention preferably has β-OH [mm -1 ] and the total amount of ZrO2 and TiO2 in mass % satisfy β-OH / (ZrO2+TiO2)≤0.14. In this way, a dense crystalline phase is easily obtained. Among them, "β-OH / (ZrO2+TiO2)" refers to the value of β-OH divided by the total amount of ZrO2 and TiO2. It should be noted that β-OH refers to the value obtained by measuring the transmittance of glass using FT-IR (Fourier transform infrared spectrophotometer) and using the following formula.
[0033] β-OH=(1 / X)log(T1 / T2)
[0034] X: glass wall thickness (mm),
[0035] T1: Reference wavelength 3846cm -1 Transmittance (%),
[0036] T2: Hydroxyl absorption wavelength 3600cm -1 Minimum transmittance (%) near .
[0037] The crystallized glass of the present invention preferably has a Pt+Rh content of less than 7 ppm.
[0038] The crystallized glass of the present invention preferably contains more than 0% MoO3.
[0039] The crystallized glass of the present invention preferably contains substantially no As component and Pb component. It should be noted that in this specification, "substantially contains no" means that it is not intentionally contained as a raw material, and unavoidable impurities are not excluded. Objectively speaking, it means that the content is less than 0.1% by mass%.
[0040] The crystallized glass of the present invention preferably has a crystallinity of 1 to 99%.
[0041] The crystallized glass of the present invention preferably precipitates at least one selected from the group consisting of a β-quartz solid solution, a β-spodumene solid solution, and zirconium oxide.
[0042] The method for manufacturing the crystallized glass of the present invention is a method for manufacturing the above-mentioned crystallized glass, characterized in that it includes: a step of preparing a precursor glass; and a step of heat-treating the precursor glass at a temperature below the glass transition temperature of the precursor glass + 200° C. to crystallize the precursor glass. It should be noted that the glass transition temperature refers to the temperature at the point (inflection point) where the slope of the thermal expansion curve changes.
[0043] Effects of the Invention
[0044] According to the present invention, it is possible to provide a crystallized glass which has desired translucency and can be easily made transparent as needed. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 This is a photograph of the crystallized glass sample obtained in No. 3 in Example. DETAILED DESCRIPTION
[0046] The crystallized glass of the present invention is characterized in that the average haze at a wavelength of 380 to 780 nm is greater than 0 and less than 30% when converted to a wall thickness of 4 mm, and the average particle size of the main crystal is 1 to 100 nm.
[0047] The larger the average particle diameter of the main crystallization is, the easier it is for the crystallized glass to present a translucent outward appearance. Therefore, the average particle diameter of the main crystallization is preferably more than 1nm, more than 5nm, more than 10nm, more than 20nm, and more than 30nm is particularly preferred. On the other hand, in the case where the average particle diameter of the main crystallization is too large, even if crystallization is carried out by the heat treatment process again, the refractive index difference between the crystalline phase and the glass phase is reduced, and the light scattering intensity at the interface of the two cannot become sufficiently small, and it is difficult to recover into a transparent product. Consider from such a viewpoint, the average particle diameter of the main crystallization is as small as possible, specifically preferably less than 100nm, less than 90nm, less than 80nm, less than 70nm, less than 60nm, and more preferably less than 50nm.
[0048] It should be noted that the more the content of crystal in the crystallized glass, the larger the interface of the crystal phase and the glass phase, the easier light scattering occurs, and therefore the easier it becomes translucent. Therefore, in order to obtain desired translucency, the crystallinity is preferably more than 1%, more than 5%, more than 10%, more than 20%, more than 30%, and particularly preferably more than 40%. On the other hand, when there is too high a crystallinity, the tendency of the refractive index difference between the crystal phase and the glass phase to decrease, therefore, in this case, sometimes desired translucency cannot be obtained. Considering from such a viewpoint, the crystallinity is preferably a low value, specifically preferably less than 99%, less than 95%, less than 90%, less than 85%, less than 80%, less than 75%, less than 70%, and particularly preferably less than 60%.
[0049] As the type of main crystal, in the case of Li2O-Al2O3-SiO2 crystallized glass, Li2O-Al2O3-SiO2 system crystals and zirconium oxide such as β-quartz solid solution or β-spodumene solid solution can be cited. Crystallization can be only one kind, or two or more kinds can be precipitated. Since the refractive index difference between β-quartz solid solution and β-spodumene solid solution and glass phase is small, according to the above mechanism, by crystallization, translucent products can be transformed into transparent products. Among them, β-spodumene solid solution makes the particle size easy to increase due to the stability of crystallization itself. Therefore, crystallized glass containing β-spodumene solid solution is easily transformed into translucent products. However, based on the above reasons, when β-spodumene solid solution is excessively precipitated, it is difficult to recover to transparent products by subsequent heat treatment. Therefore, in the case of Li2O-Al2O3-SiO2 crystallized glass, the main crystal is preferably β-quartz solid solution. Note that zirconium oxide has an effect of making it easy for other crystals to precipitate densely, and thus it is easy to obtain crystallized glass having a homogeneous appearance.
[0050] When the haze of the crystallized glass is too low, the transparency becomes high and it is difficult to obtain the desired translucent appearance. Therefore, when converted to a wall thickness of 4 mm, the average haze of the crystallized glass of the present invention at a wavelength of 380 to 780 nm is preferably more than 0%, more than 0.1%, more than 0.2%, more than 0.3%, more than 0.4%, more than 0.5%, more than 0.5%, more than 0.6%, more than 0.7%, more than 0.8%, more than 0.9%, more than 1%, more than 2%, more than 3%, more than 5%, more than 10%, and particularly preferably more than 15%. On the other hand, when the haze of the crystallized glass is too high, the transmittance becomes too low, and when used for window glass, for example, there is a tendency to lose lighting. Therefore, the average haze is preferably less than 30%, less than 28%, and particularly preferably less than 25%.
[0051] Next, a preferred example of the composition of the crystallized glass of the present invention is described. The crystallized glass of the present invention preferably contains the following components in mass %. The reasons for limiting the composition as described below are described below. It should be noted that in the following description, unless otherwise specified, "%" and "ppm" are "mass %" references.
[0052] SiO2 45~75%,
[0053] Al2O3 15~35%,
[0054] Li2O 0~4%,
[0055] Na2O 0~6%,
[0056] K2O 0~10%,
[0057] TiO2 0~1.4%,
[0058] SnO2 0~3%,
[0059] P2O5 0~2%,
[0060] ZrO2 0.5% or more,
[0061] P2O5 / (ZrO2+TiO2)≤0.4.
[0062] SiO2 is a component that forms the glass skeleton. The content of SiO2 is preferably 45-75%, 50-75%, 55-70%, 60-70%, and particularly preferably 65-70%. When the content of SiO2 is too little, the thermal expansion coefficient tends to increase, and it is difficult to obtain a crystallized glass with excellent heat shock resistance. Moreover, there is a tendency for chemical durability to decrease. On the other hand, when the content of SiO2 is too much, the solubility of the glass decreases, or the viscosity of the glass melt increases and becomes difficult to become clear, or the glass is difficult to form and the productivity is easily reduced. Moreover, the time required for crystallization becomes longer, and the productivity is easily reduced.
[0063] Al2O3 is a component that forms the glass skeleton. Moreover, Al2O3 is also a component that coordinates around the crystal nucleus to form a core-shell structure. When forming a core-shell structure, it is not easy to supply the crystal nucleus component from the outside of the shell, so the crystal nucleus is not easy to become larger, and it is easy to form many tiny crystal nuclei. As a result, fine crystals can be uniformly precipitated in the glass matrix. Moreover, Al2O3 is also a component that increases the refractive index of the crystallized glass. The content of Al2O3 is preferably 15-35%, 20-30%, and particularly preferably 20-25%. When the content of Al2O3 is too little, there is a tendency for the thermal expansion coefficient to increase, and it is difficult to obtain a crystallized glass with excellent thermal shock resistance. And, there is a tendency for chemical durability to decrease. Moreover, the crystal nucleus becomes larger, and accordingly, coarse crystals are easily precipitated. On the other hand, when the content of Al2O3 is too much, the solubility of the glass decreases, or the viscosity of the glass melt increases and it is difficult to become clear, or the glass is difficult to form and the productivity is easily reduced. Furthermore, mullite crystals tend to precipitate and cause devitrification of the glass, and as a result, the crystallized glass is easily broken.
[0064] Li2O is a component that has a great influence on crystallinity. By containing Li2O, desired crystals such as Li2O-Al2O3-SiO2 system crystals are easily precipitated, and the precipitation of undesirable crystals such as mullite crystals can be suppressed. Li2O is a component that reduces the viscosity of glass and improves the solubility and formability of glass. It is also a component that easily reduces the refractive index of crystallized glass. The content of Li2O is preferably 0-4%, 1-4%, 2-4%, 3-4%, and particularly preferably 3.5-4%. When the content of Li2O is too much, the crystallinity becomes too strong, the glass tends to lose transparency easily, and the crystallized glass becomes easily broken.
[0065] Na2O is a component that can be dissolved in the crystals in the crystallized glass. It has a great influence on the crystallinity, reduces the viscosity of the glass, and improves the meltability and formability of the glass. Moreover, it is also a component used to adjust the thermal expansion coefficient and refractive index of the crystallized glass. It should be noted that the more Na2O content, the easier it is for the refractive index of the crystallized glass to become lower. The content of Na2O is preferably 0-6%, 0-5%, 0-4%, 0-3%, 0-2%, and particularly preferably 0-1%. When the content of Na2O is too much, the crystallinity becomes too strong, the glass is easy to lose transparency, and the crystallized glass becomes easy to break. Moreover, the ionic radius of the Na cation is large and it is relatively difficult to enter the crystal, so the Na cation is also easy to remain in the glass phase (glass matrix) after crystallization. Therefore, when the content of Na2O is too much, it is easy to produce a refractive index difference between the crystal phase and the residual glass phase, and the crystallized glass tends to become excessively turbid. However, since Na2O is easily mixed into glass as an impurity, when it is desired to completely remove Na2O, the raw material batch becomes expensive and the manufacturing cost tends to increase. Therefore, from the viewpoint of suppressing the increase in manufacturing cost, the lower limit of the content of Na2O is preferably 0.0003% or more, 0.0005% or more, and particularly preferably 0.001% or more.
[0066] K2O is a component that can be dissolved in the crystals in the crystallized glass. It has a great influence on the crystallinity, reduces the viscosity of the glass, and improves the meltability and formability of the glass. Moreover, it is also a component used to adjust the thermal expansion coefficient and refractive index of the crystallized glass. It should be noted that the more K2O content, the easier it is for the refractive index of the crystallized glass to become lower. The content of K2O is preferably 0-10%, 0-8%, 0-6%, 0-5%, 0-4%, 0-3%, 0-2%, and particularly preferably 0-1%. When the content of K2O is too much, the crystallinity becomes too strong, the glass is easy to lose transparency, and the crystallized glass becomes easy to break. Moreover, the ionic radius of the K cation is large and it is relatively difficult to enter the crystal, so the K cation is also easy to remain in the residual glass phase after crystallization. Therefore, when the content of K2O is too much, it is easy to produce a refractive index difference between the crystal phase and the residual glass phase, and the crystallized glass tends to become excessively turbid. However, since K2O is easily mixed into glass as an impurity, when it is desired to completely remove K2O, the raw material batch becomes expensive and the manufacturing cost tends to increase. Therefore, from the viewpoint of suppressing the increase in manufacturing cost, the lower limit of the content of K2O is preferably 0.0003% or more, 0.0005% or more, and particularly preferably 0.001% or more.
[0067] TiO2 is a nucleating component used to precipitate crystals in the crystallization process. On the other hand, when it is contained in large quantities, the coloring of the glass is significantly enhanced. In particular, zirconium titanate crystals containing ZrO2 and TiO2 act as crystallization nuclei, but electrons transition (LMCT transition) from the valence electron band of oxygen as a ligand to the conduction band of zirconium oxide and titanium as the central metal, participating in the coloring of the crystallized glass. Moreover, in the case where titanium remains in the residual glass phase after crystallization, LMCT transitions from the valence electron band of the SiO2 skeleton to the conduction band of tetravalent titanium in the residual glass phase may occur. Moreover, trivalent titanium in the residual glass phase undergoes dd transitions, participating in the coloring of the crystallized glass. Moreover, in the case where titanium and iron coexist, a coloring similar to ilmenite (FeTiO3) is exhibited. Moreover, it is known that in the case where titanium and tin coexist, yellow color will be enhanced. Therefore, the content of TiO2 is preferably less than 1.4%, less than 1%, less than 0.5%, less than 0.2%, and particularly preferably less than 0.1%. It should be noted that the lower limit of TiO2 content is not particularly limited, can be 0%, but as mentioned above, TiO2 may become crystal nuclei, therefore when adding in the glass, has the tendency of easily separating out crystal nuclei in the crystallization process.And TiO2 is easy to sneak into the glass with impurity form, therefore, when wanting to remove TiO2 fully, has the tendency that raw material batch becomes expensive and manufacturing cost increases.Consider from such reason, TiO2 the lower limit of content is preferably above 0%, more than 0.0003%, more than 0.0005%, more than 0.001%, more than 0.005%, particularly preferably more than 0.01%.
[0068] SnO2 is a component that acts as a clarifier. Moreover, it is also a component used to efficiently precipitate crystals in the crystallization process. Specifically, by containing SnO2, it is easy to form crystal nuclei, suppress excessive turbidity caused by the precipitation of coarse crystals, and as a result, it is possible to suppress the breakage of glass. On the other hand, when SnO2 is contained in large quantities, it is also a component that significantly enhances the coloring of glass. The content of SnO2 is preferably 0% or more, 0.01% or more, 0.1% or more, 0.2% or more, 0.5% or more, and particularly preferably 1% or more. When the content of SnO2 is too much, it is possible to enhance the coloring of crystallized glass. Moreover, there is a tendency to increase the evaporation amount of SnO2 during melting and increase the environmental load. Therefore, the content of SnO2 is preferably 3% or less, 2% or less, and particularly preferably 1.5% or less. Moreover, when SnO2 is added to glass, the refractive index of the remaining glass phase tends to become higher, so it can also be used for adjusting translucency.
[0069] P2O5 is a component that inhibits the precipitation of coarse ZrO2 crystals. When coarse ZrO2 crystals are precipitated, the glass is easily devitrified and becomes easily broken. The content of P2O5 is preferably 0% or more, 0.01% or more, 0.1% or more, 0.2% or more, and particularly preferably 0.3% or more. On the other hand, when the content of P2O5 is too much, crystallization can be inhibited, and it is difficult to obtain a crystalline glass with the desired translucency. Therefore, the content of P2O5 is preferably 2% or less, 1.5% or less, and particularly preferably 1% or less.
[0070] ZrO2 is a nucleating component used to precipitate crystals in the crystallization process. The content of ZrO2 is preferably 0.5% or more, 1% or more, 1.5% or more, 2% or more, and particularly preferably 2.5%. When the content of ZrO2 is too little, it may not be possible to fully form crystal nuclei, and coarse crystals will precipitate, making the crystallized glass excessively turbid or broken. On the other hand, although the upper limit is not particularly limited, when the content of ZrO2 is too much, coarse ZrO2 crystals will precipitate, the glass is prone to devitrification, and the crystallized glass is prone to breakage. Therefore, the content of ZrO2 is preferably less than 10%, less than 8%, less than 6%, and particularly preferably less than 4%. Moreover, ZrO2 is also a component that easily increases the refractive index of the residual glass phase, and therefore, it can also be used to adjust translucency.
[0071] As mentioned above, the ratio of ZrO2, TiO2 as nucleating components and P2O5 as crystallization precipitation inhibition component has a great influence on the process from nucleation to main crystal growth. In order to obtain a dense crystalline phase (to precipitate fine crystals homogeneously), in terms of mass ratio, the value of P2O5 / (ZrO2+TiO2) is preferably less than 0.4, less than 0.38, less than 0.36, less than 0.34, less than 0.32, and particularly preferably less than 0.3. The lower limit is not particularly limited, but when the ratio is too small, the devitrification caused by ZrO2 and the generation of coarse ZrO2 crystals are prone to occur, so it is preferably more than 0.01, more than 0.02, more than 0.05, and particularly preferably more than 0.1.
[0072] The crystallized glass of the present invention may contain the following components in addition to the above components.
[0073] Pt is a composition that can be mixed into the glass with the state of ions or colloids, metals, etc., and shows yellow to dark brown coloring. And this tendency tends to be remarkable after crystallization. Therefore, the content of Pt is preferably below 7ppm, below 6ppm, below 5ppm, below 4ppm, below 3ppm, below 2ppm, below 1ppm, below 0.9ppm, below 0.8ppm, below 0.7ppm, below 0.6ppm, below 0.5ppm, below 0.4ppm, particularly preferably below 0.3ppm. Although the mixing of Pt should be avoided as far as possible, in the case of using common melting equipment, in order to obtain homogeneous glass, it is sometimes necessary to use Pt components. Therefore, when wanting to remove Pt completely, there is a tendency that manufacturing cost increases. In the case where the coloring of glass is not adversely affected, in order to suppress the increase of manufacturing cost, the lower limit of the content of Pt is preferably more than 0.0001ppm, more than 0.001ppm, more than 0.01ppm, more than 0.02ppm, more than 0.03ppm, more than 0.04ppm, more than 0.05ppm, more than 0.06ppm, and particularly preferably more than 0.07ppm. And, in the case where coloring is allowed, Pt and ZrO2, TiO2, etc. can also be used as nucleating agents that promote the precipitation of main crystals. In this case, Pt can be used as nucleating agent alone, and can also be formed into nucleating agent by compounding with other components. And, in the case of using Pt as nucleating agent, no special requirements are made to the form (colloid, metal crystal, etc.).
[0074] Rh is a component that can be mixed into the glass in the state of ions, colloids, metals, etc., and like Pt, has a tendency to show yellow to dark brown coloring. Therefore, the content of Rh is preferably below 7ppm, below 6ppm, below 5ppm, below 4ppm, below 3ppm, below 2ppm, below 1ppm, below 0.9ppm, below 0.8ppm, below 0.7ppm, below 0.6ppm, below 0.5ppm, below 0.4ppm, and particularly preferably below 0.3ppm. Although the mixing of Rh should be avoided as far as possible, in the case of using common melting equipment, in order to obtain homogeneous glass, it is sometimes necessary to use Rh components. Therefore, when wanting to remove Rh completely, there is a tendency that manufacturing cost increases. In the case where no adverse effect is produced on coloring, in order to suppress the increase of manufacturing cost, the lower limit of the content of Rh is preferably more than 0.0001ppm, more than 0.001ppm, more than 0.01ppm, more than 0.02ppm, more than 0.03ppm, more than 0.04ppm, more than 0.05ppm, more than 0.06ppm, and more than 0.07ppm is particularly preferred. And, in the case where coloring is allowed, Rh and ZrO2, TiO2, etc. can also be used as nucleating agents. At this time, Rh can be used as nucleating agent alone, and can also be formed into nucleating agent by compounding with other components. And, in the case of nucleating agent for promoting the precipitation of main crystals with Rh, no special requirements are made to the form (colloid, metal crystal, etc.).
[0075] And, based on the above reasons, Pt+Rh is preferably below 7ppm, below 6ppm, below 5ppm, below 4ppm, below 3ppm, below 2ppm, below 1ppm, below 0.9ppm, below 0.8ppm, below 0.7ppm, below 0.6ppm, below 0.5ppm, below 0.4ppm, particularly preferably below 0.3ppm. It should be noted that, although the mixing of Pt and Rh should be avoided as far as possible, in the case of using common melting equipment, in order to obtain homogeneous glass, it is sometimes necessary to use Pt and Rh components. Therefore, when wanting to remove Pt and Rh completely, there is a tendency that manufacturing cost increases. In the case of not having a negative impact on coloring, in order to suppress the increase of manufacturing cost, the lower limit of Pt+Rh is preferably more than 0.0001ppm, more than 0.001ppm, more than 0.01ppm, more than 0.02ppm, more than 0.03ppm, more than 0.04ppm, more than 0.05ppm, more than 0.06ppm, particularly preferably more than 0.07ppm.
[0076] MoO3 is an element that a trace amount will have an impact on the color of crystallization or crystallized glass. The inventor believes that in the case of Li2O-Al2O3-SiO2 crystallized glass, there is an effect of suppressing the precipitation of the β-spodumene solid solution that is easy to form coarse crystals. Therefore, in order to make the translucent product easily return to the transparent product, a trace amount of MoO3 can be added. The content of MoO3 is preferably more than 0%, more than 0%, more than 0.1ppm, more than 0.2ppm, and more than 0.3ppm is particularly preferred. On the other hand, when excessively added, there is a situation where the crystallized glass is colored and the design is impaired. Therefore, the content of MoO3 is preferably less than 100ppm, less than 80ppm, less than 60ppm, less than 40ppm, and more preferably less than 20ppm.
[0077] As components (As2O3, etc.) and Pb components (PbO, etc.) are components that function as clarifiers or nucleating agents, but they are highly toxic and may pollute the environment during the glass manufacturing process or waste glass treatment. Therefore, As2O3 and PbO are preferably less than 2%, less than 1%, less than 0.7%, less than 0.7%, less than 0.6%, less than 0.5%, less than 0.4%, less than 0.3%, less than 0.2%, less than 0.1%, and are particularly preferably substantially free of them.
[0078] In the crystallized glass of the present invention, as long as it does not have an adverse effect on translucency, the crystallized glass of the present invention can contain a total amount of up to 10% of SO3, MnO, Cl2, Y2O3, La2O3, WO3, HfO2, Ta2O5, Nd2O3, Nb2O5, RfO2, etc. However, since the raw materials of the above-mentioned components are relatively expensive, there is a tendency to increase the manufacturing cost, so if there is no special situation, it is not necessary to add. In particular, the raw material cost of HfO2 is relatively high, and Ta2O5 sometimes becomes a conflict mineral, so the total amount of these components is preferably less than 5%, less than 4%, less than 3%, less than 2%, less than 1%, less than 0.5%, less than 0.4%, less than 0.3%, less than 0.2%, less than 0.1%, less than 0.05%, less than 0.05%, less than 0.049%, less than 0.048%, less than 0.047%, less than 0.046%, and particularly preferably less than 0.045%.
[0079] Moreover, as long as the translucency is not adversely affected, in addition to the above-mentioned components, the crystallized glass of the present invention may also contain trace components such as H2, CO2, CO, H2O, He, Ne, Ar, N2, etc., each of which is up to 0.1%. In addition, when Ag, Au, Pd, Ir, V, Cr, Sc, Ce, Pr, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, Ac, Th, Pa, U, etc. are intentionally added to the glass, there is a tendency to increase the cost of raw materials. On the other hand, when the glass containing Ag, Au, etc. is subjected to light irradiation or heat treatment, agglomerates of these components can be formed, and crystallization can be promoted with this as a starting point. In addition, Pd, etc. have various catalytic effects, and by containing these materials, special functions can be given to the crystallized glass. In view of this situation, when the purpose is to promote crystallization or impart other functions, the above-mentioned components can be contained in an amount of less than 1%, less than 0.5%, less than 0.3%, or less than 0.1%, respectively. If not, it is preferably less than 500 ppm, less than 300 ppm, or less than 100 ppm, and particularly preferably less than 10 ppm.
[0080] β-OH, an indicator of the amount of water in the glass, has a significant impact on the crystallization process. When β-OH is too large, it will promote excessive growth of crystals, so it may be difficult to restore the translucent product to a transparent product through heat treatment. Although the reason why β-OH promotes crystal growth is not clear, the inventor predicts that one of the reasons is that β-OH weakens the bonding of the glass skeleton, thereby reducing the viscosity of the glass. The preferred range of β-OH is 0 to 2 mm -1 , 0.1~1.5mm -1 , 0.15~1mm -1 , 0.18~0.5mm -1 , particularly preferably 0.2 to 0.4 mm -1 It should be noted that, similar to the relationship between P2O5, ZrO2 and TiO2, by properly controlling the relationship between β-OH, ZrO2 and TiO2, a dense crystalline phase can be obtained. Specifically, the ratio of β-OH / (ZrO2+TiO2) is preferably less than 0.14, less than 0.13, less than 0.12, less than 0.11, and particularly preferably less than 0.105. The lower limit is not particularly limited and can be 0, but in reality it is greater than 0.01.
[0081] β-OH varies according to the raw materials used, the melting atmosphere, the melting temperature, the melting time, etc., and therefore, these conditions can be changed as needed to adjust β-OH. For example, β-OH can be increased by increasing the amount of hydroxide in the raw materials, or by heating with a burner for melting, or by increasing the melting temperature. Moreover, β-OH can be increased by extending the melting time under closed conditions or by shortening the melting time under non-closed conditions.
[0082] The crystallized glass of the present invention can be prepared by preparing a precursor glass before crystallization and heat treating the precursor glass to crystallize it. It should be noted that the precursor glass can be obtained by melting a batch of raw materials prepared to obtain a desired glass composition at a temperature of, for example, 1500 to 1700° C. and molding the obtained molten glass. The shape of the precursor glass is not particularly limited, and is usually plate-shaped. The precursor glass is preferably amorphous, and a portion of crystals may also be precipitated.
[0083] In the crystallization process of the precursor glass, by performing heat treatment at a relatively low temperature, it also has the advantages of slowing down the progress of crystallization, not being easy to precipitate large crystals excessively, and being able to suppress the excessive precipitation of undesirable crystals. Moreover, heat treatment at a relatively low temperature is also preferred because it can suppress energy consumption and damage to the firing furnace. Specifically, the heat treatment temperature (the highest temperature of the temperature distribution in the crystallization process) is based on the glass transition temperature Tg of the precursor glass, preferably below +200°C, below +180°C, below +160°C, below +155°C, below +150°C, below +145°C, and particularly preferably below +140°C. It should be noted that when the heat treatment temperature is too low, it is difficult to produce the desired crystallization. Moreover, the crystallization takes too much time, so compared to the case of firing at high temperature, the result may lead to increased energy consumption. Therefore, the heat treatment temperature (the highest temperature of the temperature distribution in the crystallization process) is preferably above +60°C, above +65°C, above +70°C, above +75°C, and particularly preferably above 80°C, based on the glass transition temperature Tg of the precursor glass.
[0084] The heat treatment time is, for example, preferably 0.1 to 100 hours, 0.5 to 60 hours, and particularly preferably 1 to 40 hours. When the heat treatment time is too short, it is difficult to produce the desired crystallization. On the other hand, when the heat treatment time is too long, it is possible to make the crystallization excessively proceed and become transparent, or excessively turbid, and the desired translucent product cannot be obtained.
[0085] It should be noted that, according to the crystallization process, before maintaining the maximum temperature for a certain period of time, it is also possible to maintain the temperature at a lower temperature for a certain period of time to promote the precipitation of crystal nuclei (crystallization nucleation process). In this way, a dense crystalline phase is easily obtained. The temperature of the crystallization nucleation process is based on the glass transition temperature Tg of the precursor glass, preferably above +10°C, above +20°C, particularly preferably above +30°C, preferably below +80°C, below +70°C, and particularly preferably below +60°C. In addition, the time of the crystallization nucleation process is preferably 0.1 to 30 hours, 0.5 to 15 hours, and particularly preferably 1 to 10 hours. In this way, crystal nuclei can be fully formed in the glass.
[0086] Example
[0087] Hereinafter, the present invention will be described based on examples, but the present invention is not limited to the following examples.
[0088] Table 1 shows the composition and properties of the glasses prepared in the examples. Tables 2 to 4 show the examples (No. 1 to 12).
[0089] [Table 1]
[0090]
[0091] [Table 2]
[0092]
[0093] [Table 3]
[0094]
[0095] [Table 4]
[0096]
[0097] (Example 1)
[0098] In order to obtain a glass having the composition described in Table 1, each raw material is prepared in the form of oxides, hydroxides, carbonates, nitrates, etc., to obtain a glass batch. The obtained glass batch is melted at a temperature of 1500 to 1700°C and roll-formed into a thickness of 4 to 5 mm to obtain a glass sample (precursor glass). It should be noted that the composition described in Table 1 is the analysis value of the glass sample actually produced by the following method. The melting is carried out using a melting furnace commonly used in glass manufacturing.
[0099] The contents of Pt and Rh in the glass sample were analyzed according to the following steps. First, the prepared glass sample was crushed, moistened with pure water, and then dissolved by adding perchloric acid, nitric acid, sulfuric acid, hydrofluoric acid, etc. For the obtained solution, an ICP-MS (inductively coupled plasma mass spectrometry) device (Agilent 8800 manufactured by Agilent Technology) was used to measure the contents of Pt and Rh in the glass sample. It should be noted that the measurement was performed based on a calibration curve prepared using a pre-prepared Pt solution and Rh solution with known concentrations. The measurement mode was set to Pt:He gas / HMI (low mode), Rh:HEHe gas / HMI (medium mode), and the mass numbers were set to Pt: 198 and Rh: 103.
[0100] The Li2O content in the glass sample was analyzed using an atomic absorption spectrometer (ContrAA600 manufactured by Analytik Jena). The analysis was performed in the same manner as the Pt and Rh analysis, including the melting method of the glass sample and the use of a calibration curve.
[0101] As for other components, similar to Pt, Rh and Li2O, ICP-MS or atomic absorption spectrometry is used for measurement, or a glass sample with a known concentration previously studied using ICP-MS or atomic absorption spectrometry is used as a calibration curve sample, and a calibration curve is prepared using an XRF (fluorescent X-ray) analyzer (ZSX Primus IV manufactured by RIGAKU), and then the content of each component is obtained from the XRF analysis value of the measured sample based on the calibration curve. In XRF analysis, the tube voltage, tube current, exposure time, etc. are adjusted at any time according to the analyzed component.
[0102] The glass transition temperature was evaluated by measuring a thermal expansion curve using a glass sample processed into 20 mm×Φ3.8 mm and calculating the inflection point. The measurement was performed using a Dilatometer manufactured by NETZSCH.
[0103] The obtained glass sample was heat treated under the conditions described in Tables 2 to 4. Specifically, after heat treatment under the conditions of the first temperature and the first time described in Tables 2 to 4 to form nuclei, it was further heat treated under the conditions of the second temperature and the second time to grow the crystals, thereby achieving crystallization. The temperature was then lowered to room temperature at 400°C / h. In this way, a crystallized glass sample was obtained. The obtained sample was evaluated for β-OH value, haze, precipitated crystal seeds, grain size of the main crystal, crystallinity, refractive index (nd), and density. It should be noted that the photograph of the crystallized glass sample No. 3 is shown in Figure 1 middle.
[0104] The transmittance of β-OH was measured by FT-IR Frontier (manufactured by Perkin Elmer) and was determined using the above formula. It should be noted that during the measurement, the scanning speed was set to 100 μm / min and the sampling interval was set to 1 cm. -1 , the number of scans was set to 5 scans per measurement.
[0105] The haze is calculated from the transmittance data obtained by measuring the total light transmittance and the diffuse transmittance using the following method. Each transmittance is evaluated by measuring a crystallized glass plate (30 mm square) with both sides optically polished to a wall thickness of 4 mm using a spectrophotometer. The measurement was performed using a spectrophotometer V-670 manufactured by JASCO Corporation. It should be noted that the V-670 is equipped with an integrating sphere unit "ISN-723", and the measured transmittance is equivalent to the total light transmittance. In addition, the measurement wavelength range is set to 380 to 780 nm, the scanning speed is set to 200 nm / minute, the sampling interval is set to 1 nm, and the bandwidth is set to 5 nm. Before the measurement, a baseline correction (corresponding to 100%) and a dark area measurement (corresponding to 0%) are performed. When measuring the dark area, the barium sulfate plate attached to the ISN-723 is removed. The diffuse transmittance of the crystallized glass was measured by using the same model of equipment as described above, with the measurement sample set in a state where the barium sulfate plate attached to ISN-723 was removed.
[0106] The precipitated crystals were evaluated using an X-ray diffraction device (Aeris, a desktop X-ray diffraction device manufactured by Malvern Panalytical). The measurement range was set to 5-60°, the measurement step was set to 0.01°, and the scanning speed was set to 1.5° / minute. The main crystals were identified using analysis software, and the average particle size was evaluated. As precipitated crystal seeds identified as the main crystals, β-quartz solid solution was recorded as "β-Q" and β-spodumene solid solution was recorded as "β-S" and shown in the table. In addition, the average particle size of the main crystals was calculated based on the Debye-Scherrer method using the measured X-ray diffraction peaks. The degree of crystallinity is obtained based on the ratio of the integrated intensity of the amorphous peak to the crystalline peak.
[0107] The refractive index was measured using a precision refractometer on a crystallized glass plate (30 mm square) with a wall thickness of 4 mm. The measurement was performed using a Kalnew precision refractometer KPR-2000 manufactured by Shimadzu Corporation. The measurement was performed using the V-block method, where the crystallized glass plate with both sides polished to a right angle was placed on the prism of the device, and the refractive index of the d line (587.6 nm) was measured. In addition, in order to reduce the light scattering between the prism surface and the sample surface to improve the measurement accuracy, the measurement was performed in a state where an immersion liquid with a refractive index nd of 1.53 was present between the prism and the sample.
[0108] The density was evaluated using the Archimedean method.
[0109] As shown in Tables 2 to 4, the crystallized glasses of Examples No. 1 to 12 all satisfy the desired characteristics that the average particle size of the main crystal is 100 nm or less and the average haze is 0.5 to 22.2%. Figure 1 As shown, the crystallized glass No. 3 precipitated crystals with an average crystal size of 43nm, which is significantly smaller than the crystallized glass in the above patent document, but showed a translucent appearance with an average haze of 22.2%. It was also confirmed that the haze was reduced by reheating the crystallized glass at a temperature of 860°C, and the average haze at a wavelength of 380 to 780nm changed to less than 0.5%.
Claims
1. A crystallized glass, characterized in that: When converted to a wall thickness of 4 mm, the average haze at a wavelength of 380 to 780 nm is greater than 0 and is 30% or less, and the average particle size of the main crystal is 1 to 100 nm.
2. The crystallized glass according to claim 1, wherein: The following components are contained in mass %, P2O5 / (ZrO2+TiO2)≤0.
4.
3. The crystallized glass according to claim 1 or 2, characterized in that: The value of β-OH and the total amount of ZrO2 and TiO2 in mass % satisfy β-OH / (ZrO2+TiO2)≤0.14, where the unit of β-OH is mm -1 .
4. The crystallized glass according to claim 1 or 2, characterized in that: Pt+Rh is less than 7ppm.
5. The crystallized glass according to claim 1 or 2, characterized in that: MoO3 is greater than 0%.
6. The crystallized glass according to claim 1 or 2, characterized in that: It contains substantially no As or Pb components.
7. The crystallized glass according to claim 1 or 2, characterized in that: The crystallinity is 1 to 99%.
8. The crystallized glass according to claim 1 or 2, characterized in that: The crystallized glass precipitates at least one selected from β-quartz solid solution, β-spodumene solid solution and zirconium oxide.
9. A method for manufacturing crystallized glass, wherein the crystallized glass is the crystallized glass according to claim 1 or 2, wherein the method comprises: A process for preparing a precursor glass; and A step of heat-treating the precursor glass at a temperature lower than the glass transition temperature of the precursor glass + 200° C. to crystallize the precursor glass.
Citation Information
Patent Citations
Fire-proof glass article
JP2003300752A
Translucent or opaque colored glass ceramic product used as cooking surface and its use
JP2005325018A