Method for purifying ferrous materials
By using fluorine-containing leaching liquid and controlling pH, the problem of difficulty in removing impurities in the iron-containing materials in the prior art is solved, and high-performance and low-cost iron material purification is achieved, and electrodes suitable for long-term energy storage batteries are suitable for use in electrodes. Materials improve the storage capacity and stability of electrochemical batteries.
Patent Information
- Application Number
- CN202380030991.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-05-25
- Filing Date
- 2023-02-06
- Publication Date
- 2024-12-06
AI Technical Summary
The prior art is difficult to remove impurities such as silica, alumina, magnesium oxide, calcium oxide and manganese oxide from iron-containing materials at low cost and highly scalable, making it difficult to realize high-performance and low-cost iron materials, affecting iron. Long-term energy storage performance of basic electrochemical systems.
Using fluorine-containing leaching solutions, such as ammonium fluoride (NH4F) or ammonium hydrogen fluoride (NH4HF2), selectively dissolve or precipitate impurities through alkali or acid leaching techniques, using fluxes such as NaBO2 and LiBO2, as well as controlling pH values and adding corrosion inhibition to purify iron-containing materials.
It effectively removes impurities, improves the purity and performance of iron materials, reduces production costs, and is suitable for electrode materials for long-term and ultra-long-term energy storage batteries, improving the storage capacity and stability of electrochemical batteries.
Smart Images

Figure CN119095989A_ABST
Abstract
Description
[0001] Related Applications
[0002] This application claims priority to U.S. Provisional Patent Application No. 63 / 307,462, filed on February 7, 2022, entitled “Method for Purifying Iron-Containing Materials” and U.S. Provisional Patent Application No. 63 / 365,297, filed on May 25, 2022, entitled “Method for Purifying Iron-Containing Materials”, the entire contents of both patent applications are incorporated herein by reference for all purposes. Background Art
[0003] Energy storage technologies play an increasingly important role in the electric grid; at the most basic level, these storage assets provide smoothing to better match generation and demand on the grid. The services provided by energy storage devices benefit the grid at multiple time scales (from milliseconds to years). Today, energy storage technologies exist that can support time scales from milliseconds to hours, but long-duration and ultra-long-duration (in general, >8 hours) energy storage systems are needed.
[0004] Iron-based negative electrode electrochemical systems (or iron-based anode electrochemical systems in another way) are attractive options for electrochemical energy storage. However, iron-based negative electrodes may be difficult to achieve high performance, especially at lower discharge rates, such as discharge rates associated with full discharge times greater than about 8 hours (such as 8 hours, more than 8 hours, 8-16 hours, 16 hours, more than 16 hours, 16-24 hours, 24 hours, more than 24 hours, 24-30 hours, 30 hours, more than 30 hours, etc.). In view of the cost of sponge iron, sponge iron is an excellent candidate material for iron-based negative electrodes, but despite the promising material properties of sponge iron, electrodes made of sponge iron still face challenges in achieving performance improvements.
[0005] Iron-based alkaline electrochemical systems are attractive options for grid-scale, long-duration energy storage due to the low equity cost of iron and alkaline electrolyte components. Grid-scale energy storage requires the use of raw materials that are lower in cost and therefore lower in purity than conventional iron electrode materials. Impurities can be detrimental to the performance of iron electrodes. It is difficult to remove some of these impurities from iron-containing materials in a low-cost and highly scalable manner to obtain high-performance, low-cost iron materials.
[0006] Therefore, there is a need to remove impurities from iron-containing materials in a cost-effective and highly scalable manner to obtain high-performance, low-cost iron materials. Some specific impurities that need to be removed are silicon dioxide (SiO2) (also known as silicon oxide), aluminum oxide (Al2O3) (also known as aluminum oxide), magnesium oxide (MgO) (also known as magnesium oxide), calcium oxide (CaO) (also known as calcium oxide), and manganese oxide.
[0007] This background technology section is intended to introduce various aspects of the art that may be relevant to the embodiments of the present invention. Therefore, the foregoing discussion in this section provides a framework for a better understanding of the present invention and should not be regarded as an admission of the prior art. Summary of the invention
[0008] Various embodiments include methods for purifying and / or preparing iron-containing materials. Various embodiments include the purification and / or preparation of iron ore, iron and intermediates thereof. Various embodiments include methods for purifying iron-containing materials comprising leaching one or more soluble impurities from the iron-containing material using a fluorine-containing leachate.
[0009] Various embodiments include methods for removing impurities such as silicon dioxide, aluminum oxide, magnesium oxide, manganese oxide, and / or calcium oxide from iron-containing materials. Various embodiments may include one or more materials and / or methods for leaching soluble species from iron-based materials.
[0010] Various embodiments may include alkaline leaching techniques for dissolving impurities in iron-containing materials.
[0011] Various embodiments may include acid leaching techniques for dissolving impurities in iron-containing materials.
[0012] Various embodiments for purifying iron-containing materials may include the use of fluxes, such as NaBO2, LiBO2, Li2B2O7, and the like.
[0013] Various embodiments may include techniques for dissolving silica using ammonium bifluoride (NH4HF2) to dissolve impurities in iron-containing materials.
[0014] Ammonium fluoride (NH4F) or ammonium bifluoride (NH4HF2) or acidic ammonium fluoride (3NH4 . HF2) or mixtures, solutions and derivatives thereof, hereinafter collectively referred to as AF, can be used to selectively dissolve silicates from iron-containing ores and minerals, iron and its partially processed intermediates. Without being bound by any particular scientific explanation, the inventors believe that AF is capable of dissolving or partially dissolving solid silicon-containing compounds. Compared with other chemical reagents that can dissolve silicates in target iron-containing materials, such as hydrofluoric acid (HF), alkali metal hydroxides (including NaOH and KOH) and high-temperature melts (such as molten chlorides or fluorides or oxides), AF has the following advantages: lower toxicity and higher safety than HF, and higher reactivity at lower temperatures and lower concentrations than alkali metal hydroxides or high-temperature melts.
[0015] Various embodiments may include modifying impurities in iron-containing materials into benign compounds.
[0016] Various embodiments may include methods of purifying and / or preparing iron-containing materials at one or more stages of processing iron ore for one or more purposes, such as for processing iron ore into sponge iron-based battery components. In various embodiments, one or more stages of processing iron ore may include before, during, and / or after grinding, mixing, adding a binder, adding a flux, filtering, pelletizing, hardening, forming iron ore pellets (IOPs), reducing, crushing, powdering, heating, hot pressing, and / or forming battery components (e.g., electrodes).
[0017] Various embodiments may include methods for preventing or limiting stannate precipitation, such as methods for preventing or limiting stannate precipitation for long life, high performance iron electrodes. Various embodiments may provide methods for removing CaO and / or MgO from iron electrode materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate exemplary embodiments of the claims and, together with the general description given above and the detailed description given below, serve to explain features of the claims.
[0019] Figure 1A is a schematic diagram of an electrochemical cell according to various embodiments of the present disclosure.
[0020] Figure 1B Exemplary steps in an exemplary battery pack assembly production method according to various embodiments are shown.
[0021] Figure 2A A graph showing the corrosion rate and corrosion intensity of iron in the presence of an agitated aqueous solution.
[0022] Figure 2B A graph showing the results of a silica dissolution experiment at different pH.
[0023] Figure 3 Figure 2 is a graph of the pH dependence of the silica dissolution experiment.
[0024] Figure 4 is a block diagram illustrating processing operations and apparatus for processing iron ore into battery components (eg, electrodes), and opportunities for removing impurities (eg, removing silica) during iron ore processing, according to various embodiments.
[0025] Figure 5-Figure 11 Exemplary methods of removing impurities such as silicon dioxide, aluminum oxide, calcium oxide, magnesium oxide, and / or manganese oxide from iron-containing materials are shown according to various embodiments.
[0026] Figure 12A-12Cis a Pourbaix diagram showing the pH range where calcium and magnesium based aqueous solutions begin to have high solubility for calcium and magnesium and a comparison with the solubility of iron.
[0027] Figure 13-Figure 21 Various exemplary systems are shown in which one or more aspects of various embodiments may be used as part of a bulk energy storage system. DETAILED DESCRIPTION
[0028] The following examples are provided to illustrate various embodiments of the systems and methods of the present invention. These examples are for illustrative purposes, may be prophetic, should not be considered limiting, and do not otherwise limit the scope of the present invention.
[0029] A number of embodiments will be described in detail with reference to the accompanying drawings. Where possible, the same reference numerals will be used throughout the drawings to refer to the same or similar parts. Reference to specific examples and embodiments is for illustrative purposes and is not intended to limit the scope of the claims. The following description of the embodiments of the invention is not intended to limit the invention to these embodiments, but is intended to enable those skilled in the art to make and use the invention. Unless otherwise noted, the drawings are not drawn to scale.
[0030] As used herein, room temperature is 25° C. unless otherwise specified. Also, standard temperature and pressure are 25° C. and 1 atmosphere. Unless otherwise expressly stated, all tests, test results, physical properties and values related to temperature, pressure, or both are provided at standard ambient temperature and pressure.
[0031] In general, unless otherwise indicated, the term "about" and the symbol "~" as used herein are intended to encompass a variance or range of ±10%, the experimental or instrument error associated with obtaining the stated value, and preferably the greater of these.
[0032] As used herein, recitation of ranges of values herein is merely intended to serve as a shorthand method of referring individually to each separate value falling within the range, unless otherwise indicated herein. Unless otherwise indicated herein, each separate value within a range is incorporated into the specification as if it were individually recited herein.
[0033] It should be noted that it is not necessary to provide or address the theoretical basis for the novel and groundbreaking methods, materials, performances, or other beneficial features and characteristics that are the subject of or related to the embodiments of the present invention. However, a variety of theories are provided in this specification to further advance the technology in this field. Unless otherwise expressly stated, the theories proposed in this specification in no way limit, restrict, or narrow the scope of protection provided by the claimed invention. These theories may not be necessary or practical to use the present invention. It should also be understood that the present invention may lead to new and heretofore unknown theories to explain the functional characteristics of the embodiments of the methods, articles, materials, devices, and systems of the present invention; these later developed theories should not limit the scope of protection provided by the present invention.
[0034] The multiple embodiments of the systems, devices, techniques, methods, activities and operations described in this specification can be used in a variety of other activities and other fields beyond those described herein. In addition, these embodiments can be used together with the following, for example: other devices or activities that may be developed in the future; and existing devices or activities that are partially modified based on the teachings of this specification. In addition, the multiple embodiments and examples described in this specification can be used in whole or in part with each other, and can be used in different and multiple combinations. Therefore, the configurations provided in the multiple embodiments of this specification can be used together with each other. For example, according to the teachings of this specification, components of the embodiments with A, A' and B and components of the embodiments with A", C and D can be used together with each other in multiple combinations, such as A, C, D and A, A", C and D, etc. Therefore, the scope of protection provided by the present invention should not be limited to specific embodiments, or the configurations or arrangements described in the embodiments in specific embodiments, examples or specific drawings.
[0035] Electrochemical cells, such as batteries, store electrochemical energy by using an electrochemical potential difference to create a voltage difference between a positive and negative electrode. This voltage difference generates an electric current if the electrodes are connected by a conductive element. In a battery, the negative and positive electrodes are connected in series by external and internal resistive elements. Generally, the external element conducts electrons and the internal element (electrolyte) conducts ions. Because a charge imbalance cannot be maintained between the negative and positive electrodes, the two streams must provide ions and electrons at the same rate. In operation, the current can be used to drive external devices. Rechargeable batteries can be recharged by applying a reverse voltage difference, which drives the current and ion current to flow in the opposite direction of the discharged battery in use.
[0036] Embodiments of the present invention include long-term, and ultra-long-term, low-cost energy storage devices, systems and methods. In this article, "long-term" and / or "ultra-long-term" may refer to an energy storage period of 8 hours or longer, such as an energy storage period of 8 hours, an energy storage period of 8 hours to 20 hours, an energy storage period of 20 hours to 24 hours, an energy storage period of 24 hours, an energy storage period of 24 hours to a week, an energy storage period of one week to a year (e.g., from a few days to a few weeks to a few months), etc. In other words, a "long-term" and / or "ultra-long-term" energy storage battery may refer to an electrochemical cell that can be configured to store energy over a time span of several days, weeks, or seasons. For example, an electrochemical cell may be configured to store energy generated by a solar cell in the summer months when the sun is abundant and solar power generation exceeds the grid demand, and release the stored energy in the winter months when the sun may not be enough to meet the grid demand.
[0037] Typically, in one embodiment, the long-term energy storage battery can be a long-term electrochemical battery. Typically, such a long-term electrochemical battery can store electricity generated by a power generation system when: (i) the power source or fuel used to generate electricity is available, abundant, cheap, and combinations and variations of these; (ii) the energy requirements or power demand of the power grid, customers or other users are less than the amount of electricity generated by the power generation system, and the price paid for providing such energy to the power grid, customers or other users is lower than the economic efficiency point of generating such energy (for example, the cost of generating electricity exceeds the market price of electricity), and combinations and variations of these; and (iii) combinations and variations of (i) and (ii) and other reasons. The electricity stored in the long-term electrochemical battery can then be distributed to the power grid, customers or other users when economically or otherwise needed. For example, the electrochemical battery can be configured to store energy generated by solar cells in summer months when sunlight is abundant and solar power generation exceeds grid demand, and release the stored energy in winter months when sunlight may not be sufficient to meet grid demand.
[0038] According to other embodiments, the present invention includes devices, systems and methods for storing energy for shorter periods of time, less than about 8 hours. For example, an electrochemical cell can be configured to store energy generated by a solar cell during a diurnal cycle, where solar power generation may exceed grid demand at noon, and release the stored energy in the evening when sunlight may not be sufficient to meet grid demand. As another example, the invention can include energy storage for use as a backup power source when the power supplied by the grid is insufficient, for facilities including homes, commercial buildings, factories, hospitals or data centers, where the required discharge duration can range from a few minutes to several days.
[0039] In some embodiments, the electrochemical cell comprises a negative electrode, a positive electrode, an electrolyte, and a separator (e.g., Figure 1A shown). Figure 1AAn exemplary electrochemical cell 100, such as a battery, is shown, including a negative electrode and electrolyte 102, which are separated from a positive electrode and electrolyte 103 by a separator 104. The separator 104 can be supported by a polypropylene mesh 105 and a polyethylene frame 108 of the cell 100. A current collector 107 can be associated with the respective electrodes of the negative electrode 102 and the positive electrode 103 and supported by a polyethylene backing 106. In some embodiments, the temperature of the electrochemical cell 100 can be controlled, such as by insulation around the cell 100 and / or a heater 150. For example, the heater 150 can increase the temperature of the cell 100 and / or specific components of the cell, such as the electrolytes 102, 103. Figure 1A The configuration of the electrochemical cell 100 in is merely an example of one electrochemical cell configuration according to various embodiments and is not intended to be limiting. Other configurations, such as electrochemical cells with different types of mesh and / or without polypropylene mesh 105, electrochemical cells with different types of frames and / or without polyethylene frames 108, electrochemical cells with different types of current collectors and / or without current collectors, electrochemical cells with different types of backsheets and / or without polyethylene backsheets 106, electrochemical cells with different types of insulation and / or without insulation, and / or electrochemical cells with different types of heaters and / or without heaters 150 may be substituted. Figure 1A An exemplary configuration of electrochemical cell 100 is shown, and other configurations are consistent with various embodiments.
[0040] In some embodiments, multiple Figure 1A The electrochemical cells 100 in the embodiment can be electrically connected in series to form a battery stack. In certain other embodiments, multiple electrochemical cells 100 can be electrically connected in parallel. In certain other embodiments, the electrochemical cells 100 are connected in a mixed series-parallel electrical configuration to achieve a favorable combination of delivered current and voltage.
[0041] According to different embodiments, the negative electrode comprises a pelletized, briquette, pressed or sintered iron-containing compound. Such iron-containing compounds may include one or more forms of iron, from highly reduced (more metallic) iron to highly oxidized (more ionic) iron. In multiple embodiments, the iron-containing compound may include a variety of iron phases, such as iron oxides, hydroxides, sulfides, carbides or combinations thereof. In multiple embodiments, the negative electrode may be a sintered iron agglomerate with a variety of shapes. In some embodiments, atomized iron powder or sponge iron powder may be used as a raw material for forming a sintered iron electrode. In some embodiments, the green body may also include a binder, such as a polymer or an inorganic clay-like material. In multiple embodiments, the sintered iron agglomerate may be formed in a furnace (such as a continuously fed calciner, a batch-fed calciner, a shaft furnace, a rotary calciner, a rotary hearth furnace, etc.). In other embodiments, iron ore may be directly fed into a reduction furnace (such as in, for example, a variety of sponge iron manufacturing methods or a fluidized bed reactor) without heat treatment. In various embodiments, the iron active material feedstock may include a reduced and / or sintered iron-containing precursor known to those skilled in the art as direct reduced iron (DRI), and / or its byproduct materials. Various embodiments may include treating the iron active material feedstock, such as DRI pellets, using electrical, electrochemical, mechanical, chemical and / or thermal treatments prior to introducing the iron active material feedstock into an electrochemical cell.
[0042] Discussed are multiple embodiments related to the use of an iron active material feedstock (e.g., direct reduced iron (DRI) (also known as sponge iron)) as a material in a battery (or cell), as a component of a battery (or cell), and combinations and variations thereof. In multiple embodiments, the iron active material feedstock (e.g., DRI) may be produced from a material obtained from the reduction of a natural or processed iron ore without reaching the melting temperature of iron, or may be a material obtained from the reduction of a natural or processed iron ore. In multiple embodiments, the iron ore may be taconite or magnetite or hematite or goethite, etc. In multiple embodiments, the iron active material feedstock (e.g., DRI) may be in the form of pellets, which may be spherical or substantially spherical. In multiple embodiments, the iron active material feedstock (e.g., DRI) may be in a form other than pellets that may not be spherical, such as fines, granules, briquettes, fragments, discs, lumps, powders, dusts, etc. In multiple embodiments, the iron active material feedstock (e.g., DRI) may be porous, containing open and / or closed internal pores. In various embodiments, the iron active material feedstock (e.g., DRI) may include material that has been further processed by hot briquetting or cold briquetting. In various embodiments, the iron active material feedstock (e.g., DRI) may be produced by reducing iron ore form factors (e.g., iron ore pellets, briquettes, etc.) to form a more metallic (more reduced, less oxidized) material, such as iron metal (Fe 0 ), pyrite (FeO) or a composite form comprising iron metal and residual oxide phases (e.g., composite pellets, composite briquette ore, etc.). In multiple non-limiting embodiments, the iron active material raw material (e.g., DRI) can be reduced iron ore taconite, directly reduced ("DR") taconite, reduced "blast furnace (BF) grade" pellets, reduced "electric arc furnace (EAF) grade" pellets, "cold direct reduced iron (CDRI)" pellets, direct reduced iron ("DRI") pellets, hot briquette iron (HBI), or any combination thereof. In the iron and steelmaking industries, DRI is sometimes referred to as "sponge iron"; this usage is particularly common in the Indian or pressing and sintering powder metallurgy industries.
[0043] According to various embodiments, an electrochemical cell, e.g. Figure 1A The battery 100 includes a negative electrode (also called an anode), a positive electrode (also called a cathode), and an electrolyte. The negative electrode can be an iron material. The electrolyte can be an aqueous solution. In some embodiments, the electrolyte can be an alkaline solution (pH>10). In some embodiments, the electrolyte can be a near-neutral solution (10>pH>4).
[0044] Various embodiments include methods for purifying iron-containing materials. Various embodiments include purification of iron ore, iron, and intermediates thereof. Various embodiments include methods for preparing iron-containing materials. Various embodiments include preparation of iron ore, iron, and intermediates thereof. Various embodiments may include methods for purifying and / or preparing iron-containing materials for a variety of purposes, such as for battery applications or any other purpose.
[0045] Various embodiments include methods for removing impurities such as silicon dioxide, aluminum oxide, calcium oxide, magnesium oxide, and / or manganese oxide from iron-containing materials.
[0046] Various embodiments may include methods for purifying iron-containing materials, such as by removing impurities including silica, alumina, CaO, and / or MgOa, which may occur at one or more steps in a method of forming any type of iron-containing material, such as at one or more steps in producing DRI pellets, at one or more steps in producing DRI fines, at one or more steps in an electrolytic iron production process, etc. Various embodiments may include methods for purifying iron-containing materials, such as by removing impurities including silica, alumina, calcium oxide, magnesium oxide, and / or manganese oxide, which may occur at one or more steps in a method of forming any type of iron-containing material for use in a battery, such as a method of making electrodes or other battery components using pelletized DRI, a method of making electrodes or other battery components using DRI fines, a method of making electrodes or other battery components using electrolytic iron, etc. As an example, Figure 1B Exemplary steps in a battery assembly production method 152 using pelletized DRI, exemplary steps in a battery assembly production method 154 using fine-particle-based DRI, and exemplary steps in a battery assembly production method 156 using electrolytic iron are shown. The steps in methods 152-156 are merely exemplary, and various embodiments may include other methods and / or other steps.
[0047] As an example, methods 152-156 can begin with a mining step, in which iron is mined and rocks or other materials associated with the iron ore deposit are extracted. In various embodiments, the embodiment methods of purifying iron-containing materials discussed herein, such as by removing impurities including silica, alumina, calcium oxide, magnesium oxide, and / or manganese oxides, can be performed during and / or after mining in methods 152-156. In methods 152-156, a crushing and grinding step can be after mining, in which the mined rock is crushed and / or ground into smaller fragments. Crushing and grinding can reduce the mined rock to smaller fragments than the originally mined rock, and can begin to separate the desired iron ore from the gangue material in the mined rock. In various embodiments, the embodiment methods of purifying iron-containing materials discussed herein, such as by removing impurities including silica, alumina, calcium oxide, magnesium oxide, and / or manganese oxides, can be performed before, during, and / or after the crushing and grinding steps in methods 152-156. In methods 152-156, beneficiation can be performed after crushing and grinding, and can include chemically and / or physically separating gangue materials from the iron ore. In multiple embodiments, the embodiment methods of purifying iron-containing materials discussed herein, for example by removing impurities including silica, alumina, calcium oxide, magnesium oxide and / or manganese oxides, can be performed before, during and / or after beneficiation in methods 152-156. The crushing and grinding and / or beneficiation steps can produce a concentrate. In methods 152 and 154, an optional silica removal step can be performed after beneficiation. For example, the silica removal step can remove silica and / or other substances from the concentrate. In multiple embodiments, the embodiment methods of purifying iron-containing materials discussed herein, for example by removing impurities including silica, alumina, calcium oxide, magnesium oxide and / or manganese oxides, can be performed before, during and / or after the optional silica removal step in methods 152 and 154. In method 152, a pelleting step may be performed after the beneficiation and / or optional silica removal step. In various embodiments, the embodiment methods of purifying iron-containing materials discussed herein, for example by removing impurities including silica, alumina, calcium oxide, magnesium oxide, and / or manganese oxides, may be performed before, during, and / or after the pelletizing step in method 152. In method 152, a hardening (or sintering) step may be performed after pelletizing. In various embodiments, the embodiment methods of purifying iron-containing materials discussed herein, for example by removing impurities including silica, alumina, calcium oxide, magnesium oxide, and / or manganese oxides, may be performed before, during, and / or after the hardening step in method 152.In methods 152 and 154, a direct reduction step may be performed (e.g., after hardening in method 152 or after optional silica removal in method 154), wherein the iron ore may be reduced by heating that does not reach the melting temperature of iron. In various embodiments, the embodiment methods of purifying iron-containing materials discussed herein, such as by removing impurities including silica, alumina, calcium oxide, magnesium oxide, and / or manganese oxides, may be performed before, during, and / or after the direct reduction step in methods 152 and 154. In method 152, the resulting DRI pellets may be powdered to reduce their size and / or produce DRI fines. In various embodiments, the embodiment methods of purifying iron-containing materials discussed herein, such as by removing impurities including silica, alumina, calcium oxide, magnesium oxide, and / or manganese oxides, may be performed before, during, and / or after the powdering step in method 152. In method 156, after beneficiation, digestion and purification of the iron ore may be performed, followed by electrodeposition and drying. In various embodiments, the embodiment methods of purifying iron-containing materials discussed herein, for example by removing impurities including silica, alumina, calcium oxide, magnesium oxide, and / or manganese oxides, can be performed before, during, and / or after digestion and purification in method 156. In various embodiments, the embodiment methods of purifying iron-containing materials discussed herein, for example by removing impurities including silica, alumina, calcium oxide, magnesium oxide, and / or manganese oxides, can be performed before, during, and / or after electrodeposition in method 156. In various embodiments, the embodiment methods of purifying iron-containing materials discussed herein, for example by removing impurities including silica, alumina, calcium oxide, magnesium oxide, and / or manganese oxides, can be performed before, during, and / or after drying in method 156. The iron material obtained by powdering in method 152, direct reduction in method 154, and / or drying in method 156 can be placed in a mold and heated in methods 152-156. In various embodiments, the embodiment methods of purifying iron-containing materials discussed herein, for example by removing impurities including silica, alumina, calcia, magnesia, and / or manganese oxides, can be performed before, during, and / or after filling the mold in methods 152-156. In various embodiments, the embodiment methods of purifying iron-containing materials discussed herein, for example by removing impurities including silica, alumina, calcia, magnesia, and / or manganese oxides, can be performed before, during, and / or after reheating in methods 152-156. In methods 152 and 154, an optional decarburization step can be performed after reheating the filled mold.In various embodiments, the embodiment methods of purifying iron-containing materials discussed herein, for example by removing impurities including silica, alumina, calcium oxide, magnesium oxide, and / or manganese oxides, can be performed before, during, and / or after decarburization in methods 152 and 154. In methods 152-156, the iron material in the mold can be hot pressed and then cooled to form a battery component, such as an iron electrode. In various embodiments, the embodiment methods of purifying iron-containing materials discussed herein, for example by removing impurities including silica, alumina, calcium oxide, magnesium oxide, and / or manganese oxides, can be performed before, during, and / or after hot pressing in methods 152-156. In various embodiments, the embodiment methods of purifying iron-containing materials discussed herein, for example by removing impurities including silica, alumina, calcium oxide, magnesium oxide, and / or manganese oxides, can be performed before, during, and / or after cooling in methods 152-156.
[0048] Various embodiments may provide methods for purifying iron-containing materials in one or more different steps, such as when the iron is in a concentrate step (e.g., after obtaining (e.g., mining) the iron ore, and after the iron ore is ground and beneficiated), when the iron is in an iron ore pellet step, when the iron is in a high purity iron ore fines or iron ore pellet fragments (e.g., less than 6 mm) step, when the iron is in a direct reduced iron step, when the iron is part of a complete anode, before and / or after adding a binder, etc. Table 1 lists a number of exemplary steps / iron-containing materials and considerations for each step.
[0049] Table 1
[0050]
[0051]
[0052]
[0053] Various embodiments may provide methods for purifying iron-containing materials that produce concentrates having a selected range of soluble silica contents. The soluble silica content may be defined as the amount of silica that is soluble in an alkaline environment once the material is incorporated into an alkaline battery. The specifications for soluble silica are essentially the same for iron ore pellets and iron concentrates, as the specifications for silica are given on a per weight %-iron basis and the amount of silica. The soluble silica content may be measured by leaching the material for a long period of time (≥2 weeks) at an elevated temperature close to the boiling point of the alkaline leachate (≥90°C). After the leaching process, the soluble silica may be measured by one of two measurement techniques: 1) subsequent analysis of the amount of Si remaining in the material by techniques known in the art for quantifying the mass fraction of silica, including, for example, inductively coupled plasma in combination with suitable spectroscopy techniques. If the silicon content is defined relative to the amount of Fe remaining in the material, the total iron content of the material can be analyzed by techniques known in the art for quantifying the total iron content (e.g., ISO 2597), and the contents of Si and Fe in the material before and after the leaching operation can be compared; or 2) directly measuring the silicon leached into the alkaline leachate in the form of silicates. The mass fraction of dissolved silicates can be measured by any technique known in the art for detecting silicates in alkaline solutions, including but not limited to ICP-OES. The alkaline leachate can be a solution of 7M KOH. In the case where the solubility of silica in the electrolyte used in the electrochemical cell using the Fe active material is significantly different, the soluble silica leaching process can be performed in the electrolyte to be used in the electrochemical cell instead. The inventors have experimentally found that ≥2 weeks at 90°C is generally sufficient to measure the soluble silica content in the Fe active material. However, in some cases, the dissolution of silica from the Fe active material may be very slow, and a longer time or a different dissolution temperature may be required to achieve complete dissolution of silica. In some cases, the Fe active material may need to be electrochemically cycled to release all the silica. In the case where the Fe active material may need to be electrochemically cycled to release all of the silica, the soluble silica content may be measured by sampling the electrolyte and / or Fe active material collected from the cycling electrochemical cell. Various embodiments may provide methods for purifying iron-containing materials that may produce a concentrate having a selected range of soluble silica content, wherein the soluble silica content specified range is the weight percent (wt %) of SiO2 relative to the wt % Fe, e.g., 0<0.01x<0.85, 0<0.01x<0.65, 0<0.01x<0.33, 0<0.01x<0.16, 0<0.01x<0.11, etc.
[0054] The amount of soluble silica allowable in a cell may alternatively or additionally be defined based on the amount of silica entering the electrolyte. The dissolved silica may be measured by sampling the electrolyte from the cell, or by performing a leaching experiment outside the cell as described above, and converting the silica content to an equivalent silica concentration, which would be measured in the cell by appropriately adjusting the leached Fe active material ratio (e.g., in mL lixiviant / g Fe active material) relative to the electrolyte to Fe active material ratio (e.g., in mL electrolyte / g Fe active material). The soluble silica content should be <400 mM silicate, <200 mM silicate, <100 mM silicate, <50 mM silicate, <25 mM silicate, <10 mM silicate, and most preferably <5 mM silicate.
[0055] A plurality of embodiments can provide a method for purifying iron-containing materials, which can produce iron ore pellets (IOP) with a selected range of soluble silica content. Many other metrics related to the ability to process, transport and reduce iron oxide pellets in a variety of reduction technologies can be collected. The IOP material properties listed here are only examples that may be critical to the performance of auxiliary storage systems (secondary storage systerm). The IOP can be designed in other ways to allow the IOP to be properly processed (e.g., reduced) in downstream steps. Strength, other impurity levels, etc. are all related to processing success, but are also related to the details of the processing performed. The open porosity in the pellet specifically refers to the open porosity. The open porosity can be measured by measuring the shell (envelope) density of the pellet and the skeleton density of the pellet, thereby deriving the porosity in the pellet. This can be measured by a variety of techniques known in the art for measuring the porosity of porous bodies, including helium pycnometer method or mercury porosimetry method for true density, and immersion density method or helium pycnometer method for shell density. Various embodiments may provide methods for purifying iron-containing materials, the methods may produce iron ore pellets (IOP) having a selected range of soluble silica content, wherein the specified range of soluble silica content is the weight percentage (wt%) of SiO2 relative to the weight % iron, such as 0<0.01x<0.85, 0<0.01x<0.65, 0<0.01x<0.33, 0<0.01x<0.16, 0<0.01x<0.11, etc. Various embodiments may provide methods for purifying iron-containing materials, the methods may produce iron ore pellets (IOP) having a selected range of intra-pellet open porosity, such as 20-50 volume percent (vol%), 25-45 vol%, 29-42 vol%, less than 50 vol%, greater than 20 vol%, etc. Various embodiments may provide methods for purifying iron-containing materials that may produce iron ore pellets (IOPs) having a selected total iron content (eg, greater than 62%, greater than 65%, greater than 67%, etc.).
[0056] Multiple embodiments can provide a method for purifying iron-containing materials, which can produce DRI (or similar sponge iron) with a selected range of soluble silica content. Many other metrics related to the ability to process, transport and reduce DRI in a variety of reduction technologies can be collected. The DRI material properties listed here are only examples that may be critical to the performance of the auxiliary storage system. DRI can be designed in other ways so that DRI can be properly processed in downstream steps or incorporated into the battery pack. Strength, other impurity levels, etc. may all be related to successful processing and incorporation into the battery, but also to the details of the processing performed. The open porosity of the pellets in DRI specifically refers to the open porosity. The open porosity can be measured by measuring the shell density of the DRI pellets and the skeleton density of the DRI pellets, thereby deriving the porosity in the DRI pellets. This can be measured by a variety of techniques known in the art for measuring the porosity of porous bodies, including helium pycnometers or mercury porosimetry for true density, and immersion density or helium pycnometers for shell density. Various embodiments may provide methods for purifying iron-containing materials, which methods may produce DRI (or similar sponge iron) having a selected range of soluble silica content, such as DRI pellets, wherein the soluble silica content specified range is the weight percentage (wt%) of SiO2 relative to the weight % iron, such as 0<0.01x<0.85, 0<0.01x<0.65, 0<0.01x<0.33, 0<0.01x<0.16, 0<0.01x<0.11, etc. Various embodiments may provide methods for purifying iron-containing materials, which methods may produce DRI (or similar sponge iron) having a selected range of DRI inner pellet open porosity, such as DRI pellets, wherein the DRI inner pellet open porosity range is, for example, 50-75 volume percent (vol%), 55-72 vol%, 57-67 vol%, less than 75 vol%, greater than 50 vol%, etc. Various embodiments may provide methods for purifying iron-containing materials that may produce DRI (or similar sponge iron), such as DRI pellets, having a selected total iron content (e.g., greater than 85%, greater than 90%, greater than 92%, etc.).
[0057] A number of embodiments can provide methods for purifying iron-containing materials that can produce high purity iron ore fines or iron ore pellet (IOP) fragments (e.g., less than 6 mm) having a selected range of soluble silica content. For some iron ores, the porosity within the ore does not need to be very high or specifically defined. The mineralogy of the ore allows the ore to be reduced to a highly metallized state with a large amount of measurable porosity prior to the reduction process. The open porosity within the pellet of the IOP fragment specifically refers to the open porosity. The open porosity can be measured by measuring the shell density of the IOP fragment and the skeleton density of the IOP fragment, thereby deriving the porosity within the IOP fragment. This can be measured by a variety of techniques known in the art for measuring the porosity of porous bodies, including helium pycnometer or mercury porosimetry for true density, and immersion density or helium pycnometer for shell density. Various embodiments may provide methods for purifying iron-containing materials, which may produce high purity iron ore fines or iron ore pellets (IOP) fragments (e.g., less than 6 mm) having a selected range of soluble silica content, wherein the specified range of soluble silica content is the weight percentage (wt %) of SiO2 relative to the wt % iron, such as 0<0.01x<0.85, 0<0.01x<0.65, 0<0.01x<0.33, 0<0.01x<0.16, 0<0.01x<0.11, etc. Multiple embodiments may provide a method for purifying iron-containing materials, the method being capable of producing high-purity iron ore fines or iron ore pellet (IOP) fragments (e.g., less than 6 mm) having a selected range of intra-pellet open porosity (for IOP fragments), the DRI intra-pellet open porosity range being, for example, 20-50 volume percent (vol %), 24-45 vol %, 29-42 vol %, less than 50 vol %, greater than 20 vol %, etc. Multiple embodiments may provide a method for purifying iron-containing materials, the method being capable of producing high-purity iron ore fines or iron ore pellet (IOP) fragments (e.g., less than 6 mm) having a selected total iron content (e.g., greater than 62%, greater than 65%, greater than 67%, etc.).
[0058] Multiple embodiments may provide methods for purifying iron-containing materials, the methods may produce materials that have been made into electrodes for electrochemical systems, the materials having a selected range of soluble silica content. The geometric density of the active material-containing region of the electrode may be defined as the mass of the electrode active material relative to the volume occupied by the active material (including the porosity inside and between the active material particles). The electrode geometric density should exclude the weight and volume of the current collector or other parts of the electrode design that do not contain active materials. Multiple embodiments may provide methods for purifying iron-containing materials, the methods may produce materials that have been made into electrodes for electrochemical systems, the materials having a selected range of soluble silica content, wherein the specified range of soluble silica content is the weight percentage (wt %) of SiO2 relative to the wt % iron, for example 0<0.01x<0.85, 0<0.01x<0.65, 0<0.01x<0.33, 0<0.01x<0.16, 0<0.01x<0.11, etc. Various embodiments may provide methods for purifying iron-containing materials, which methods may produce materials that have been fabricated into electrodes for use in electrochemical systems, the materials having a selected geometric density range of the electrode active area, such as 1.2-4 grams per cubic centimeter (g / cc), 1.5-4 g / cc, 1.8-2.6 g / cc, 1.9-2.5 g / cc, less than 4 g / cc, greater than 1.2 g / cc, etc. Various embodiments may provide methods for purifying iron-containing materials, which methods may produce materials that have been fabricated into electrodes for use in electrochemical systems, the materials having a selected total iron content of iron-based active species, such as greater than 85%, greater than 90%, greater than 92%, etc.
[0059] Various embodiments for purifying iron-containing materials may include a leaching process. A leaching process may be considered any process in which 1) a material is exposed to a leachate and 2) components of the material exposed to the leachate are partially or fully dissolved in the leachate. In the context of the present disclosure, etching and leaching may be considered synonymous. In other words, instances of the term "etching" or "etch" in connection with a process in the present disclosure may be considered synonymous with the term "leaching" or "leach" in connection with the process, and the method should be understood as a "leaching process" as defined in this paragraph.
[0060] Various embodiments for purifying iron-containing materials may include an alkaline leaching process. Various embodiments include a method for purifying iron-containing materials, the method comprising leaching one or more soluble impurities from the iron-containing material using a fluorine-containing leachate.
[0061] Various embodiments may include one or more processes for leaching soluble species from iron-based materials. Various embodiments may include alkaline leaching techniques for dissolving impurities from iron-containing materials. Dissolution-based methods are attractive because they can purify iron-containing materials to very low impurity concentrations.
[0062] In some alkaline leaching processes, concentrated alkali (e.g., NaOH and / or KOH) can be used to leach alkali-soluble substances from iron-containing materials. It is known that higher concentrations of alkali accelerate the leaching kinetics of silicon dioxide and aluminum oxide. Leachates with concentrations of 0.1 to 10M may be relevant to industry. In various embodiments, the molar concentration of the fluorine-containing component of the leachate may be or be greater than about 100 parts per million (ppm), such as about 100 ppm, 100 ppm to 10000 ppm, about 100 ppm to 500 ppm, about 500 ppm, 100 ppm to 5000 ppm, about 500 ppm to 5000 ppm, greater than 500 ppm, 500 ppm to 5000 ppm, about 5000 ppm, greater than 5000 ppm, about 5000 ppm to 10000 ppm, about 10000 ppm, etc. In various embodiments, the molar concentration of the fluorine-containing component of the leachate is 500 ppm to 5000 ppm.
[0063] In some processes, the leachate is washed and reconcentrated to recover expensive leaching chemicals in the leachate. In such processes, the concentration of the leachate can be selected so that the concentration of the reconcentrated leachate is similar or identical to the concentration of the leaching bath, so that leaching can be carried out in a closed loop with little need to update the composition of the solution.
[0064] In general, the leaching process can make more efficient use of the leachate if the major leaching impurities are removed from the leachate so that the leachate is not saturated with dissolved impurities. In some leaching processes, impurity removal chemicals can be added to the leachate to prevent the solution from being saturated. The two main impurities removed from iron-containing materials are silica and alumina. Dissolved silica and alumina can be effectively removed from alkaline solutions by calcium hydroxide or related chemicals such as calcium oxide (which can be converted to calcium oxide when hydrated). Therefore, in some leaching processes, the leachate can be contacted with a material containing calcium hydroxide so that the silica and alumina do not saturate the solution. In some leaching processes, the calcium hydroxide-containing material (or related precursors) can be continuously added and removed so that a continuous leaching process can be performed without saturating the leaching bath.
[0065] In some leaching processes, the leach bath may be heated to accelerate the dissolution of silica and alumina so that the material is leached on a practical and cost-effective time scale. The temperature of the leach bath required varies depending on the ore microstructure and the phase of the silica- and alumina-containing impurities, but in general, temperatures between 30°C and the boiling point of the leachate are preferred.
[0066] In some leaching processes, it may be more efficient to remove dissolved impurities at a temperature different from the optimum temperature for leaching impurities from the iron-containing material. In such cases, different processes may be performed at different temperatures. For example, silicate-based materials may be dissolved in an alkaline solution at a high temperature and precipitated from solution by calcium hydroxide or magnesium hydroxide materials at a low temperature.
[0067] The solubility and dissolution rate of silica-based materials in alkali are closely related to the silica phase. In some leaching processes, iron-containing materials can be selected to make the silica-based materials fast dissolving materials. In some embodiments, ores or other iron sources containing fast dissolving materials can be used to simplify processing and reduce costs. For example, relative to the slowest dissolving quartz phase, faster dissolving materials such as amorphous silica and / or tridymite / cristobalite may be preferred.
[0068] If a metallized iron-containing material is used in a purification process, the metallic iron may be oxidized during the etching process. This is generally undesirable, so corrosion inhibitors may be introduced into the feed and / or leachate to slow down the oxidation of the iron while removing impurities. In one aspect, sulfides or silicates may be introduced into the solution to slow down the corrosion of the metallic iron. In some embodiments, corrosion inhibitors used in the field of iron and steel metallurgy to inhibit aqueous corrosion may be used to slow down the corrosion of the metallic iron. Exemplary corrosion inhibitors that may be introduced into the feed and / or leachate in various embodiments may be selected from the non-limiting group of sodium thiosulfate, sodium thiocyanate, polyethylene glycol (PEG) 1000, trimethylsulfoxide iodide, zincate (by dissolving ZnO in NaOH), hexanethiol, decanethiol, sodium chloride, sodium permanganate, lead (IV) oxide, lead (II) oxide, magnesium oxide, sodium chlorate, sodium nitrate, sodium acetate, ferric phosphate, phosphoric acid, sodium phosphate, ammonium sulfate, ammonium thiosulfate, lithopone, magnesium sulfate, iron (III) acetylacetonate, hydroquinone monomethyl ether, sodium metavanadate, sodium chromate, pentanediol, sodium sulfoxide ... Acid, dimethyl phthalate, methyl methacrylate, methylpentynol, adipic acid, allyl urea, citric acid, thiomalic acid, N-(2-aminoethyl)-3-aminopropyl trimethoxysilane, propylene glycol, trimethoxysilylpropyl diethylene, aminopropyl trimethoxysilane, dimethyl butynedioate (DMAD), 1,3-diethylthiourea, N,N'-diethylthiourea, aminomethyl propanol, methyl butynol, amino-modified organosilane, succinic acid, isopropanolamine, phenoxyethanol, dipropylene glycol, benzoic acid, N-(2-aminoethyl)-3-aminopropyl, behenamide, 2-phosphonobutanetricarboxylic acid, boric acid (mipa borate), 3-methacryloxypropyl trimethoxysilane, 2-ethylhexanoic acid, isobutyl alcohol, tert-butylaminoethyl methacrylate, diisopropanolamine, propylene glycol n-propyl ether, sodium benzotriazole, pentasodium aminotrimethylenephosphonate, sodium cocoyl sarcosinate, lauryl pyridinium chloride, stearyltrimethylammonium chloride, stearalkonium chloride, calcium montanate, quaternary ammonium-18 chloride, sodium hexametaphosphate, dicyclohexylamine nitrite, lead stearate, calcium dinonylnaphthalenesulfonate, iron (II) sulfide, sodium hydrogen sulfide, pyrite, sodium nitrite, complex alkyl phosphates (e.g. RA 600 emulsifier), 4-mercaptobenzoic acid, ethylenediaminetetraacetic acid, ethylenediaminetetraacetic acid (EDTA), 1,3-propylenediaminetetraacetic acid (PDTA), nitrilotriacetic acid (NTA), ethylenediamine disuccinic acid (EDDS), diethylenetriaminepentaacetic acid (DTPA) and other aminopolycarboxylates (APC), ethylenetriaminepentaacetic acid, 2-methylbenzenethiol, 1-octanethiol, manganese dioxide, manganese (III) oxide, manganese (II) oxide, manganese hydroxide, manganese (II) hydroxide, manganese (III) hydroxide, bismuth sulfide, bismuth oxide, antimony (III) sulfide, antimony (III) oxide, antimony (V) oxide, selenium bismuth, antimony selenide, selenium sulfide, selenium (IV) oxide, propargyl alcohol, 5-hexyn-1-ol, 1-hexyn-3-ol, N-allylthiourea, thiourea, 4-methylcatechol, trans-cinnamaldehyde, iron (III) sulfide, calcium nitrate, hydroxylamine, benzotriazole, furfurylamine, quinoline, tin (II) chloride, ascorbic acid, 8-hydroxyquinoline, pyrogallol, tetraethylammonium hydroxide, calcium carbonate, magnesium carbonate, antimony dialkyl dithiophosphates, potassium stannate, sodium stannate, tannic acid, gelatin, saponin, agar, 8-hydroxyquinoline, bismuth stannate, potassium gluconate, lithium molybdenum oxide, potassium molybdenum oxide, hydrotreated light petroleum, heavy naphthenic petroleum (e.g., 631), antimony sulfate, antimony acetate, bismuth acetate, hydrotreated heavy naphtha (e.g. for sale), tetramethylammonium hydroxide, NaSb tartrate, urea, D-glucose, C6Na2O6, potassium antimony tartrate, hydrazine sulfate, silica gel, triethylamine, potassium antimonate trihydrate, sodium hydroxide, 1,3-di-o-tolyl-2-thiourea, 1,2-diethyl-2-thiourea, 1,2-diisopropyl-2-thiourea, N-phenylthiourea, N,N'-diphenylthiourea, sodium L-antimony tartrate, disodium rhodamine, sodium selenate, potassium sulfide, and combinations thereof.
[0069] In various embodiments, concentrates from different sources, such as fluxes, etc., may be added to the iron-containing material to change the phase of impurities, such as the silica phase, the alumina phase, the phase of silica and alumina, etc., so that the impurities (e.g., silica, alumina, calcium oxide, magnesium oxide and / or manganese oxides, etc.) are more soluble, insoluble, or more easily mechanically separated. For example, during the mixing stage of the pelletizing process, concentrates from different sources, fluxes, etc. may be added to change the phase of silica, alumina, calcium oxide, magnesium oxide and / or manganese oxides, so that the silica, alumina, calcium oxide, magnesium oxide and / or manganese oxides are more soluble, insoluble, or more easily mechanically separated. As a specific example, dolomitic lime (MgO-CaO) may be added to the concentrate during the hardening process, and the silica may be combined with the dolomitic lime to form a SiO2-MgO-CaO phase, which may be amorphous. In another example, alumina (e.g., in the form of bauxite or other minerals of alumina) can be added in combination with CaO or MgO to produce a low melting point, amorphous SiO2-Al2O3-(CaO or MgO) phase.
[0070] Various embodiments for purifying iron-containing materials may include acid leaching.
[0071] Various embodiments may include one or more materials and / or processes for leaching soluble species from iron-based materials. Various embodiments may include acid leaching techniques for dissolving impurities from iron-containing materials.
[0072] Silica is soluble in acids such as hydrofluoric acid (HF). However, a first problem may be that it may be difficult to replicate the dissolution rate of silica by using HF. A second problem may be that iron oxides are unstable in acidic environments; they may dissolve in acidic solutions to form soluble iron-containing species, such as Fe2+.
[0073] In a first embodiment, the first etch rate of the iron oxide is adjusted to be much slower than the second etch rate of the impurity (silicon dioxide) that is desired to be dissolved or otherwise removed from the iron-containing material. In another example of the first embodiment, for an etchant comprising HF, the first etch rate of the iron oxide is very slow, while the second etch rate of the silicon dioxide is very fast.
[0074] In a second embodiment, the iron-containing material is immersed in a buffered hydrofluoric acid solution. A first example of a buffered hydrofluoric acid solution includes ammonium bifluoride (NH4HF2). A second example of a buffered hydrofluoric acid solution includes potassium difluoride (KHF2).
[0075] In a third embodiment, the iron-containing material is immersed in an acid mixture. The acid mixture may include HF, hydrochloric acid, sulfuric acid, and nitric acid.
[0076] Multiple embodiments for purifying iron-containing materials can include leaching soluble substances from iron-based materials, such as by dissolving silicon dioxide with ammonium bifluoride (NH4HF2). For example, ammonium bifluoride (NH4HF2) can be used to dissolve silicon dioxide-based impurities in iron-containing materials, more specifically, silicon dioxide is exposed to ammonium fluoride in an aqueous medium or a mixture of ammonium fluoride and acidic ammonium fluoride to produce ammonium fluorosilicate. Ammonium fluorosilicate can then be precipitated to produce precipitated silicon dioxide, and it is possible to achieve recycling of ammonium bifluoride etchant, thereby achieving a closed-loop etching process by dissolving and precipitating silicon dioxide. In multiple embodiments, other etchants other than ammonium bifluoride and hydrogen fluoride can also be used to remove silicon dioxide from iron-containing materials. For example, such etchants contain fluorine, F. Several such etchants are discussed in Konstantinos D. Demadis et al. 2012, Additive-Driven Dissolution Enhancement of Colloidal Silica. 3. Fluorine-Containing Additives (referred to herein as Demadis et al.) and Ehrlich et al. 2010 Modern Views on Desilicification: Biosilica and Abiotic Silica Dissolution in Natural and Artificial Environments, both of which are incorporated herein in their entirety as part of this disclosure for all purposes, and which describe a variety of etchants, any of which may be examples of etchants for dissolving silicon-based impurities in iron-containing materials in various embodiments. Of particular interest are etchants that produce solubility and high etch rates with minimal safety risks and etching selectivity for silicon dioxide, aluminum oxide, calcium oxide, magnesium oxide, and / or manganese oxide relative to iron. One such etchant is sodium fluorophosphate Na2PO3F.
[0077] Various embodiments for purifying iron-containing materials may include methods for controlling the reaction of the iron-containing material with the etching solution by controlling the pH to reduce or minimize corrosion. In some embodiments, the pH of the etching solution can be effectively controlled so that the iron-containing material is stable or corrodes at a very low rate in the solution of interest. This method is applicable when the etchant can achieve a fast etching rate in a pH range that minimizes corrosion of the iron-containing material. In general, corrosion of iron can be minimized in a mild to moderate alkaline environment with a pH of 8-13 (see, e.g., Figure 2A(Diagram reproduced from the Electrochemical Equilibrium Atlas by Marcel Pourbaix). An example of such an etchant that exhibits high etching activity at these pHs is Na2PO3F. Figure 2B Data from Demadis et al. are reproduced, demonstrating the high solubility of silicon dioxide in aqueous solutions at pH 7 and 9. In general, there are a number of such fluorine-containing buffered etching solutions, any of which may be used in a variety of embodiments, and the pH of the solution may be adjusted to co-optimize iron reactivity and silicon dioxide dissolution rate.
[0078] Various embodiments of purifying iron-containing materials may include methods for controlling the reaction of the iron-containing material with the etching solution to inhibit or eliminate corrosion by controlling the etchant chemistry. In some embodiments, the solubility of silicon dioxide (and the associated etching rate) may be a strong function of pH. Generally, etchants have higher solubility and faster etching kinetics for silicon dioxide at pHs far from neutral. For example, in the case of HF and ammonium bifluoride etching, silicon dioxide etchants are most effective at more acidic pHs. Figure 3 The data shown reproduces the data of Demadis et al., illustrating this point. In general, etching in acid is incompatible with preserving iron-containing materials in the solid state, since iron and many of its compounds are known to be soluble in acidic solutions. To inhibit or eliminate this risk, soluble iron ions can be added to the etchant. The presence of these ions reduces the driving force for the iron to dissolve into the solution. In some embodiments, the iron can be effectively dissolved to its solubility limit in the etchant, thereby completely eliminating the driving force for the iron to dissolve.
[0079] In some embodiments, the dissolved iron ions may be provided by dissolving a portion of the iron-containing material. The etching solution may be recirculated in a closed loop to maximize the amount of iron-containing material retained during the etching process.
[0080] In some embodiments, dissolved iron ions can be provided by adding a suitable soluble iron salt to the etchant, such as FeSO4: ferrous sulfate; iron (II) sulfate FeCl2: ferrous chloride; iron (II) chloride Fe(NO3)3: ferric nitrate; iron (III) nitrate Fe(SO4)3: ferric sulfate; iron (III) sulfate FeCl3: ferric chloride; and / or iron (III) chloride.
[0081] Various embodiments for purifying iron-containing materials may include ammonium bifluoride (NH4HF2) etching.
[0082] Various embodiments may include one or more materials and / or methods for leaching soluble species from iron-based materials. Various embodiments may include a technique for dissolving silica with ammonium bifluoride (NH4HF2) for dissolving impurities from iron-containing materials.
[0083] Ammonium bifluoride can be used to dissolve silica-based impurities in iron-containing materials, more specifically, exposing silica to ammonium fluoride or a mixture of ammonium fluoride and acidic ammonium fluoride in an aqueous medium to produce ammonium fluorosilicate. The ammonium fluorosilicate can then be precipitated to produce precipitated silica and potentially enable the ammonium bifluoride etchant to be recycled, thereby enabling a closed-loop etching process through dissolution and precipitation of silica.
[0084] Ammonium fluoride (NH4F) or ammonium bifluoride (NH4HF2) or acidic ammonium fluoride (3NH4 . HF2) or mixtures, solutions and derivatives thereof, hereinafter collectively referred to as AF, can be used to selectively dissolve silicates from iron-containing ores and minerals, iron and partially processed intermediates thereof. Without being bound by any particular scientific explanation, the inventors believe that AF is capable of dissolving or partially dissolving solid silicon-containing compounds. Compared with other chemical reagents that can dissolve silicates in target iron-containing materials, such as hydrofluoric acid (HF), alkali metal hydroxides (including NaOH and KOH) and high-temperature melts (such as molten chlorides or fluorides or oxides), AF has the following advantages: lower toxicity and higher safety advantages than HF, and higher reactivity at lower temperatures and lower concentrations than alkali metal hydroxides or high-temperature melts.
[0085] As described herein, AF may comprise a solid compound or a mixture of solid compounds, a molten or partially molten form of the solid compound, or AF dissolved in a liquid, the liquid comprising water, a polar solvent, a non-polar solvent, or a mixture of the solvents. The dissolved concentration of AF in the liquid solvent may be in the range of a lower limit of 0.001M to an upper limit of 20M, preferably in the range of 0.01M to 10M, and still more preferably, in the range of 0.01M to 5M.
[0086] In some embodiments, the AF used to treat the iron-containing material is used once and discarded or repaired or recycled after use. However, in a preferred embodiment, a closed loop process is used in which the AF is regenerated and reused, reducing or eliminating the need to provide additional AF to treat new materials. An example of such a closed loop process is now described, which can be performed in a batch mode or as a continuous process.
[0087] Considering the use of NH4F as the AF, the multi-stage reactor may have a first stage of dissolving the silica. Without being bound by any particular scientific explanation, the dissolution reaction is a reaction that produces ammonia as a product, for example according to the following reaction:
[0088] SiO2+6NH4F → (NH4)2SiF6+2H2O+4NH3 (1)
[0089] Such reactions can be carried out at a temperature range of about 25° C. to about 110° C. In order to promote the forward reaction, the activity of the ammonia reaction product should be reduced. This can be achieved by separating ammonia from water by well-known methods, such as by distillation utilizing the higher vapor pressure of ammonia.
[0090] In the second stage of the reactor, reaction (1) is reversed by increasing the activity of ammonia. The ideal stoichiometric ratio of ammonia to ammonium fluorosilicate is more than 4:1. As a result, SiO2 is reprecipitated and NH4F is produced. The solid precipitated SiO2 can then be separated from the liquid, for example by filtration or centrifugation, and discarded or used beneficially for another application.
[0091] Another possible reaction with a similar reaction scheme is:
[0092] SiO2+6NH4F → H2SiF6+2H2O+6NH3 (2)
[0093] As another example, consider using ammonium bifluoride, NH4HF2, in a similar scheme. Ammonium bifluoride can dissolve silica according to the following reaction:
[0094] SiO2+4NH4HF2 → (NH4)2SiF6+2NH4F+2H2O (3)
[0095] or:
[0096] SiO2+4NH4HF2 → SiF4+4NH4F+2H2O (4)
[0097] or:
[0098] SiO2+3NH4HF2 → H2SiF6+3NH3+2H2O (5)
[0099] Via reaction 5, a reaction scheme similar to that described above for ammonium fluoride can be used to dissolve and then precipitate SiO2, thereby removing it from iron-containing materials.
[0100] Embodiments of the present invention include the above-mentioned methods for dissolving and reprecipitating silicates from the iron-containing material. The present invention also includes a multi-stage reactor for performing a dissolution reaction, removing and capturing the products of the dissolution reaction, and providing them to a subsequent precipitation reactor. The present invention also includes a system for implementing this method, which includes an iron-containing material source and an AF source, one or more reactors and subsystems for implementing the dissolution and reprecipitation processes, the subsystems being used to separate the treated solid siliceous material from the liquid and optionally drying the solid, and optionally delivering the treated iron to the manufacturing operations of various products (including but not limited to iron, steel, and electrochemical cells using the iron-containing material). Such systems can be operated in whole or in part using renewable energy sources (including low-carbon electricity sources).
[0101] The siliceous material present in the iron-containing material (called "gangue") may not be pure silica, and may include other components that are soluble in acid or alkali, as well as silica that is soluble when reacted with AF. An example is calcium silicate, in which the calcium component is soluble in acid (such as HCl or HNO3 or H2SO4), and the silica is soluble in AF. Generally, the leaching or dissolution of one phase will also accelerate the leaching or dissolution of the other phase. Therefore, an acidic solution that also contains AF can be used to simultaneously leach or react the calcium silicate. Optionally, a sequential process can be used when there are phases that are each preferentially leached by one of the reactants. For example, in the example of calcium silicate, the iron can first react with the acid to dissolve or partially dissolve the calcium component, and then react with AF to dissolve or partially dissolve the silica component, or the order of operations can be reversed.
[0102] According to some embodiments, any chemical dissolution reaction described herein can be supplemented with mechanical energy, such as by grinding or milling. For example, iron ore material leached with AF solution or acid can be simultaneously ground using, for example, ball milling or attritor milling to increase the efficiency or rate of the chemical reaction.
[0103] Various embodiments may include one or more materials and / or methods for leaching soluble species from iron-based materials. Various embodiments may include dissolving silica with chemical reagent techniques other than AF to dissolve impurities from iron-containing materials, such as using hydrofluoric acid (HF), alkali metal hydroxides (including NaOH and KOH), and / or high temperature melts (e.g., molten chlorides or fluorides or oxides) to dissolve silica and / or remove other impurities from iron-containing materials.
[0104] Various embodiments for purifying iron-containing materials may include the use of fluxes such as NABO2, LiBO2, Li2B2O7, and the like.
[0105] Various embodiments may include one or more materials and / or methods for leaching soluble species from iron-based materials. Various embodiments may include dissolving silica by adding a flux (e.g., a glass flux). An example of a flux is a metaborate.
[0106] In a first embodiment, a flux is added to an iron material, the iron material comprising silicon dioxide. The silicon dioxide in the iron material forms a molten silicon dioxide material. In a first embodiment, the molten silicon dioxide material is heated to a melting point (liquidus) of the molten silicon dioxide material, which is lower than the melting point of iron. In this way, the molten silicon dioxide material can be separated from the iron material.
[0107] In one embodiment, the molten silica is separated from the iron-rich material by preferentially wicking the silica into a porous matrix having a lower contact angle for the molten silica phase than for the iron-containing material. In this way, the porous matrix can act as a high temperature sponge to absorb the molten silica material. The porous matrix can be a high melting point phase of silica.
[0108] In some embodiments, the iron-based concentrate can be purified by any method described herein to achieve a lower impurity content, with an emphasis on reducing impurities containing silicon dioxide, calcium oxide, and aluminum oxide. Then, the iron-based concentrate can be used directly as an active material to make an electrode, rather than processing iron ore to form a reduced iron substance. In this way, the ore material can be used to make an electrode using a common method in the art for forming an electrode from a non-conductive or semiconductor active material. In some embodiments, the iron-based concentrate can be a magnetite concentrate, thereby effectively utilizing the semiconductor properties of magnetite to facilitate the transmission of electrons through the battery electrodes. In some embodiments, the iron-based concentrate can be combined with any one of a binder and a conductive additive. The binder can be any binder system for making an iron electrode used in an alkaline environment, including carboxymethyl cellulose (CMC), polyacrylic acid, and / or polytetrafluoroethylene (teflon). The conductive additive can be any conductive additive known in the art to enhance the transmission of electrons in alkaline battery electrodes, including but not limited to carbon black or graphite. The formulation can include 94% by weight of an iron ore-based concentrate, 3% by weight of a conductive additive, and 3% by weight of a binder.
[0109] Figure 4 is a block diagram illustrating processing operations and apparatus for processing iron ore into battery components (such as electrodes) according to various embodiments, as well as opportunities for removing silicon dioxide during iron ore processing. For example, Figure 4 Reference can be shown Figure 1B Specific examples of exemplary operations are discussed. Figure 4It is shown that iron ore, for example in the form of blocks and / or fines, can be milled, crushed and / or ground, for example by a ball mill 401. As an example, water can be added to the ball mill 401 to produce a ground iron slurry leaving the ball mill 401. The ground iron ore can be conveyed to a mixing tank 402, where a variety of additives such as binders, clays and / or water can be added to the ground iron ore slurry. The ground iron ore and additives combined in the mixing tank 402 can produce a mixed iron concentrate, which can be filtered in one or more filtering units 403. Filtration can remove unwanted substances and / or liquids from the mixed iron concentrate. Filtration may produce filter cake material. The filter cake material of the mixed iron concentrate can undergo a granulation process 404 to produce green pellets, which can undergo a hardening process 405 to form iron ore pellets (IOPs). The IOP may enter a reduction process 406 and form DRI pellets, which may be crushed and / or powdered in a crushing / powdering process 407. The crushed / powdered DRI may proceed to a heating furnace 408 for heating, and may undergo a hot pressing process 409 to form a battery component, such as one or more electrodes.
[0110] In various embodiments, chemical purification processes such as chemical removal of silica, alumina, calcium oxide, magnesium oxide, and / or manganese oxides may occur at process points 421, 422, 423, 424, 425, and / or 426 during the processing of iron ore into DRI and battery components such as electrodes. For example, process point 421 may be chemical silica removal after wet grinding of the iron ore. For example, process point 422 may be chemical silica removal after mixing and adding a binder and / or flux to the iron concentrate. For example, process point 423 may be chemical removal of silica from IOP. For example, process point 424 may be chemical removal of silica from DRI particles. For example, process point 425 may be chemical removal of silica from crushed / powdered DRI. For example, process point 426 may be chemical removal of silica from a battery component form factor after assembling the battery component, such as chemical removal of silica from an electrode form factor after assembling the electrode.
[0111] Figure 5-Figure 11 Exemplary methods for removing impurities such as silicon dioxide, aluminum oxide, calcium oxide, magnesium oxide, and / or manganese oxide from iron-containing materials according to various embodiments are shown. For example, Figure 5-Figure 11 The process shown in Figure 4 The processing of iron ore into battery components (e.g., electrodes) is performed as part of the processing operations and equipment shown in FIG.
[0112] Figure 5An exemplary operation according to various embodiments is shown in which one or more etchants / leaching agents 501 for removing impurities such as silicon dioxide, aluminum oxide, calcium oxide, magnesium oxide, and / or manganese oxides from iron-containing materials may be introduced into a concentrate mixing tank 402. For example, an acid may be introduced into the tank 402. Introducing one or more etchants / leaching agents 501 into the mixing tank 402 may represent the simplest process modification for removing impurities such as silicon dioxide, aluminum oxide, calcium oxide, magnesium oxide, and / or manganese oxides from iron-containing materials.
[0113] Figure 6 Shown with Figure 5 A similar exemplary operation is shown in which a second filtration step 601 is used to rinse the filter cake with a neutralizer 602. The second filtration step 601 including the neutralizer 602 rinse can avoid diluting the recycle stream. The filtration step 601 can produce a rinse liquid recycle stream 604 and an etchant / leaching agent recycle stream 603.
[0114] In various embodiments, heat can be added to the system to aid in the chemical etching and / or leaching process. For example, heat can be added in the mixing tank 402, after the mixing tank 402 (e.g., in a flow reactor), and / or during the filtration process.
[0115] Fig. 7A Shown with Figure 6 Another similar exemplary configuration. Specifically, Fig. 7A An exemplary operation according to various embodiments is shown, where one or more etchants / leaching agents 501 for removing impurities (e.g., silicon dioxide, aluminum oxide, calcium oxide, magnesium oxide, and / or manganese oxide) from iron-containing materials may be introduced into a concentrate mixing tank 402, and heat may be added to support the etching / leaching chemistry to remove SiO2 without dissolving Fe species. For example, Fig. 7AShown is adding heat upstream of mixing tank 402 (sometimes also referred to as reaction vessel) by plug flow reactor 702. The concentrate stream leaving mixing tank 402 can be heated by heater 701, and the reaction of etchant and / or leaching agent 501 with target SiO2 can occur in plug flow reactor 702. Heat can be added by heater 701 in mixing tank 402, upstream of plug flow reactor 702 after mixing tank 402 and / or directly in plug flow reactor 702. In some embodiments, plug flow reactor 702 can adopt double tube exchanger configuration, wherein the concentrate stream leaving mixing tank 402 passes through internal pipe, and heating medium passes through annular structure. In the case where the reaction of etchant and / or leaching agent requires short and precise duration, this configuration may be preferred. The annular structure can be divided into multiple heating zones and cooling zones. A temperature sensor 703 can be included in the system to monitor the temperature of the concentrate stream in mixing tank 402 before entering plug flow reactor 702 and / or after leaving plug flow reactor 702.
[0116] Figure 7B Shown with Fig. 7A Similarly, another exemplary configuration is provided in which the plug flow reactor 702 is replaced by a pseudo-plug flow reactor 750 formed by a series of stirred vessels 751 (e.g., one or more stirred vessels 751, three stirred vessels 751, more than three stirred vessels 751, etc.). Each stirred vessel may include its own heating coil and may controllably provide heat to the concentrate stream as it passes through the vessel 751. The pseudo-plug flow reactor 750 may provide less precise heating than a true plug flow reactor 702, but the pseudo-plug flow reactor 750 is still able to add heat to the concentrate stream to support the etching / leaching chemistry to remove SiO2 without dissolving Fe species.
[0117] Figure 8 A drum filter and rinse process 802 is shown, which may be combined with a filtration operation such as the above-described filtration operations 403 and / or 601. By means of the drum filter and rinse process 802, the etch / leaching solution may be diluted, but the potential for recycling may not be reduced.
[0118] Fig. 9 A two-step filtering process 902 is shown, which may be combined with filtering operations (e.g., filtering operations 403 and / or 601 described above). Fig. 9As shown, a neutralizing agent can be added in the rinsing step. In this embodiment, a two-step filtering process is adopted. The first filtration 903 removes most of the etching / leaching solution for recycling. The filter cake can then be mixed with a neutralizing rinsing solution in a mixing tank 905. The second filtration 904 removes the rinsing solution and prepares a concentrate for granulation. A ceramic disc filter can be an example of a filter that can be used for the first filter 903 and / or the second filter 904. Ceramic disc filters are preferably used in this embodiment due to their increased production capacity. However, in multiple embodiments, other filter media and / or filtering processes can also be used to replace ceramic disc filters.
[0119] In the embodiment where iron is purified in a larger form, in the IOP, DRI pellets, crushed DRI or electrode plate stage of the production line, all or part of an immersion process, such as a single-stage bath or multi-stage bath, a fixed bed silo, a screw conveyor and / or other types of processes, can be used to apply etching and / or leaching liquid to the iron material. For example, a bath with an immersion conveyor can be used to expose the iron material to an etchant. A bath with an immersion conveyor that moves at a controlled speed can achieve excellent duration accuracy. As another example, a screw conveyor can be used to move the iron material through a liquid etchant so that the iron material is exposed to the etchant. As another example, a fixed bed silo can be used to expose the iron material to the etchant. In multiple embodiments, water rinsing can be incorporated into the process to rinse the iron material after the iron material is removed from the etching solution. In multiple embodiments, the etching solution, such as an etching solution bath, a screw conveyor, a fixed bed silo, etc., may or may not be heated. In various embodiments, a fully or partially submerged process, such as a single or multiple bath, fixed bed silo, screw conveyor, and / or other type of process, may be used to generate a Figure 5 The etchant and / or leachate is applied to the ferrous material during or after any of the described processes 404-409. In various embodiments, the etchant / leachate can be continuously or intermittently circulated in a full or partial immersion process such as a single or multiple baths, fixed bed silos, screw conveyors, and / or other types of processes, through a regeneration process that can precipitate the etched or leached material (e.g., silicon dioxide, aluminum oxide, calcium oxide, magnesium oxide, and / or manganese oxide) from the etchant / leachate to reload the etchant / leachate.
[0120] Fig.10 An exemplary etchant batch process is shown, wherein IOP pellets on a conveyor (e.g., IOP pellets having a size of about 5 mm to about 15 mm) are immersed in an etchant bath through a conveyor path and rinsed with water after leaving the etchant bath. The speed of the conveyor belt can be controlled to ensure the precise duration of exposure of the IOP pellets to the etchant bath.
[0121] Fig.11An exemplary etchant batch process is shown, wherein crushed and / or powdered DRI pellets (e.g., DRI pellets having a size of about 2 mm to about 5 mm) on a conveyor are immersed in an etchant bath through a conveyor path and rinsed with water after leaving the etchant bath. The DRI pellets may pass through a second neutralization and rinsing step, which may be separated from the etchant bath. The speed of the conveyor belt may be controlled to ensure the precise duration of exposure of the DRI pellets to the etchant bath. The etchant bath may be continuously circulated from the bath by a regeneration process that may precipitate silicon dioxide from the etchant bath.
[0122] Stannate can be a performance enhancing additive for iron anodes. In some cases, the performance enhancing effect of stannate requires that the stannate is soluble. In order to improve the performance of iron anodes in alkaline media, a stannate concentration of 1-300 mM is generally required.
[0123] Some impurities in the iron electrode active material or other parts of the battery may precipitate the stannate, making the solubility of the stannate lower than that required to enhance electrochemical performance. Additionally or alternatively, the precipitation of the stannate from a soluble state to an insoluble state may result in an increase in the cost of the stannate-containing additive to obtain the same level of performance as in the absence of stannate precipitation.
[0124] Various embodiments include methods for limiting or eliminating precipitation of stannate from an electrolyte.
[0125] In addition to the motivation for targeting stannates, these approaches also need to address a more general problem. The more general problem is that whenever impurities are present in an electrochemical cell, they have the potential to react with the electrolyte or electrodes, leading to deviations in electrochemical performance. Therefore, it is generally desirable to control the composition of all materials in the cell and / or to ensure that the impurities do not react with the rest of the cell.
[0126] Various embodiments include methods and systems for removing impurities from materials entering an electrochemical cell. Various embodiments include methods and systems for passivating or reacting with impurities so that the impurities cannot interact with the rest of the cell.
[0127] In the presence of tin in alkaline solution, stannates can be precipitated on the material to form stable compounds. As described below, sometimes such stable compounds can be used to effectively suppress the loss of stannates. However, other elements may also form compounds with tin in alkaline solutions, so that the amount of tin in the solution is permanently reduced. In the presence of stannates, calcium, magnesium, aluminum and manganese can all form stable compounds. More specifically, CaO, MgO, Al2O3 and Mn-based oxides can all react with stannates to produce metal-stannate compounds with low solubility in alkaline solutions relative to the desired concentration for enhancing the performance of iron electrodes.
[0128] It is often useful to remove impurities from electrode materials to prevent deleterious interactions with the electrochemical behavior of the battery. For example, in some cases it is useful to remove impurities that cause stannate precipitation when using an iron anode in an alkaline solution.
[0129] In the event that the electrode active material contains these impurities, removal of these impurities may be achieved by dissolving the impurities or otherwise treating the material prior to contacting the electrode active material with the stannate-containing solution.
[0130] Various embodiments may include removing impurities by dissolution.
[0131] Ca and Mg are usually present as impurities in low-cost iron materials, usually in the form of CaO / MgO and / or their hydroxides (Ca(OH)2 and Mg(OH)2). Since the oxides CaO and MgO are converted into their hydroxides in aqueous solution, the inventors' experience is that the oxides (CaO, MgO) can be treated in the same manner as the hydroxides with respect to their dissolution / reaction behavior in aqueous solution.
[0132] CaO and MgO are alkaline oxides that dissolve readily in acid. Therefore, acid can be used to remove these species from solution. If acid is used to dissolve these oxides from the iron-containing active material, the acid solution may need to be appropriately buffered so that CaO and MgO are selectively leached out with the acid while retaining most of the iron-containing active material. Ca(OH)2 begins to dissolve even at highly alkaline pH values (low solubility requires a pH of about 13 and high solubility requires a pH of 11.5), but an acidic component of the etching solution is required to promote dissolution. Similarly, Mg(OH)2 is soluble at a pH below about 11 and is highly soluble at a pH below about 8.
[0133] Similar considerations apply to the removal of other acid-soluble impurities such as Al2O3 and Mn-based oxides. Therefore, the various acid-based embodiments discussed below in connection with the removal of CaO and MgO and / or their hydroxides (Ca(OH)2 and Mg(OH)2) can be applied to the removal of other impurities such as Al2O3 and Mn-based oxides. Therefore, in the various embodiments discussed below regarding the removal of impurities CaO and MgO and / or their hydroxides (Ca(OH)2 and Mg(OH)2), other impurities such as Al2O3 and Mn-based oxides can replace CaO and MgO and / or their hydroxides (Ca(OH)2 and Mg(OH)2), and various embodiments can be used to remove these other impurities.
[0134] Figure 12A-12CPourbaix diagram showing the pH range in which calcium and magnesium based aqueous solutions begin to have high solubility of calcium and magnesium and a comparison with the solubility of iron.
[0135] Various embodiments may include an etching solution to remove impurities, such as one or more of CaO and MgO and / or one or more of their hydroxides (Ca(OH)2 and Mg(OH)2).
[0136] Ideally, the solution used to treat the iron active material will have limited reactivity with the iron active material being treated while exhibiting rapid reaction with and high solubility for the impurities being removed. Depending on the iron active material being treated, a number of solution configurations are possible. Figure 12A-12C As shown in the Pourbaix diagram in , iron will dissolve in low pH solutions (< about 5), which are generally not preferred solutions for processing iron active materials. However, there is a pH range where iron is passivated and / or corrodes very slowly, which overlaps with the high solubility pH range of magnesium and calcium, particularly pH about 5-10. Those skilled in the art will recognize that the pH ranges given above are approximate and are subject to many considerations surrounding other experimental factors.
[0137] Although many different acids can be used to remove CaO and MgO from iron electrode materials, there are preferred acid chemicals for carrying out this dissolution process. Specifically, it is necessary to produce a weak acid or buffered acid chemical with a preferred pH range of 5-10. The anion used for the acid should be selected to minimize the corrosion of iron and be compatible with the electrochemical cell when some small contamination occurs. For example, if etching is performed on iron concentrate, an acid (such as nitric acid) that can be volatilized in a furnace in subsequent processing is preferred. Hydrochloric acid is generally not ideal because contamination by chloride ions is generally harmful to the performance of the iron electrode and the performance of the electrochemical cell. Sulfuric acid etching can be used for active materials that are etched before entering the electrochemical cell because a small amount of sulfate ions is generally harmless to the performance of the iron electrode. In all cases, the material should be rinsed or purified after the etching process to ensure that other impurities do not enter the battery. The buffer selected for etching will vary depending on the target pH range, but some examples may include carbonic acid / bicarbonate, acetic acid, C6H 13 NO4S and any of a number of other buffers commonly found in the art.
[0138] Various embodiments may include controlling the amount of dissolved iron to extend the stability domain of the iron.
[0139] The pH range over which the iron etch / corrosion rate is low is a function of the amount of dissolved iron in the solution, where higher concentrations of dissolved iron expand the pH range of passivation and reduce the corrosion rate of iron. Therefore, iron ions can be intentionally added to expand the pH range over which iron is not appreciably etched, thereby speeding up the etching kinetics of magnesium and calcium-based compounds by operating the dissolution process at lower pH. The concentration of dissolved iron required to enhance passivation increases exponentially with a linear decrease in pH.
[0140] Various embodiments may include adding corrosion inhibitors to reduce the corrosion rate of iron.
[0141] In many practical cases, impurities can be removed from iron in a solution that is nominally corrosive to iron, albeit at a slower rate. In such cases, a corrosion inhibitor can be added to the etching bath to stabilize the iron against corrosion. Additionally or alternatively, the iron material to be treated can be treated with a corrosion inhibitor prior to allowing the iron material to contact the etching solution. Depending on the chemistry of the solution, a number of corrosion inhibitors can be used, including thioureas, sulfides (such as sodium sulfide), silicates or other thiolated organics (such as hexyl mercaptan, heptyl mercaptan, octyl mercaptan, etc.).
[0142] A plurality of embodiments may include the recycling of etching solution. In some cases, the etching agent can be purified and continuously reused. For example, the etching agent can be exposed to a material that can precipitate the impurities to be removed. In some cases, magnesium and calcium can be precipitated by exposure to carbonate ions (formed by bubbling CO2 in the etching agent), thereby forming calcium carbonate and magnesium carbonate. In other cases, impurities may be precipitated by exposure to other counter ions of low solubility that cause dissolved impurities, such as fluoride ions or phosphate ions. In other cases, the solution can be used for selectively removing ions by any other process known in the art, including the use of reverse osmosis and ion selective membranes.
[0143] Various embodiments may include passivating impurities.
[0144] In some cases, impurities may be passivated or reacted so that they can no longer react with the electrolyte, thereby limiting the ability of impurities to adversely affect electrochemical performance. In one example, impurities may be treated with low-solubility passivating ions. In the case of calcium and magnesium, fluoride ions and phosphate ions are treated to form low Ksp (solubility product) compounds, which have very low or no solubility and are highly stable, thereby preventing these materials from reacting with other components of the electrochemical cell. In some cases, the treatment process may be performed before the impurities enter the battery. In other cases, the material may be treated by including a treatment material in the electrolyte or otherwise added to the battery when it enters the battery.
[0145] In some cases, passivation of the impurity particle surface can be achieved by adsorption of substances that do not form low Ksp compounds. For example, aluminates or silicates can be added to the solution to form a passivating film on Ca and Mg by forming a surface layer of calcium silicate hydrate or magnesium silicate hydrate. Importantly, the CaO or MgO particles do not need to be fully reacted to be effectively passivated.
[0146] Various embodiments may include reacting an impurity that may cause precipitation with a compound that preferentially reacts with the impurity such that the stannate is retained in solution.
[0147] In some cases, precipitation of the stannate may be prevented by causing another reaction to occur instead of the stannate precipitation. This may be accomplished by adding a co-additive with the stannate so that the calcium or magnesium reacts preferentially with the co-additive rather than the stannate. Fluoride ions, phosphate ions, and carbonate ions may all be used to form stable compounds with magnesium and calcium in solution. The added material that preferentially reacts with Ca may be added at the start of use of the battery cell, or may be dosed or otherwise slowly introduced during operation to allow the reaction to occur without the instantaneous concentration of the co-additive in the electrolyte being too high.
[0148] Various embodiments may include a method for purifying an iron-containing material, comprising: leaching one or more soluble impurities from the iron-containing material, wherein the leaching comprises leaching using a fluorine-containing leachate. In various embodiments, the leachate comprises ammonium fluoride (NH4F) or acidic ammonium fluoride (3NH4 .HF2), or a mixture thereof. In various embodiments, the leachate comprises ammonium bifluoride (NH4HF2). In various embodiments, leaching comprises dissolving impurities using hydrofluoric acid (HF), alkali metal hydroxides (e.g., NaOH and KOH) and / or high temperature melts (e.g., molten chlorides or fluorides or oxides). In various embodiments, the leachate comprises sodium fluorophosphate (Na2PO3F). In various embodiments, the fluorine-containing component of the leachate has a molar concentration of 100 ppm to 10000 ppm. In various embodiments, the fluorine-containing component of the leachate has a molar concentration of 500 ppm to 5000 ppm. In various embodiments, the iron-containing material is iron ore, iron and / or their intermediates. Various embodiments may also include controlling the pH of the leachate. In various embodiments, the pH is controlled in the range of 8 to 13. In various embodiments, the pH is controlled in the range of 7 to 9. In various embodiments, the pH is controlled in the range of 5 to 10. Various embodiments may also include adding soluble iron salts to the leachate. In various embodiments, the iron salt comprises one or more of ferrous sulfate, iron (II) sulfate, ferrous chloride, ferric nitrate, ferric sulfate and / or ferric chloride. Various embodiments may also include adding iron ions to the leachate. Various embodiments may also include adding one or more corrosion inhibitors to the leachate. Various embodiments may also include recycling the leachate. Various embodiments may include a method for purifying an iron-containing material, comprising: leaching one or more soluble impurities from the iron-containing material, wherein the leaching comprises dissolving by adding a flux. Various embodiments may also include using the purified iron-containing material to form an electrode of a battery. Various embodiments may also include providing the battery to a large-capacity energy storage system. In various embodiments, the large-capacity energy storage system is a long-duration energy storage (LODES) system. Various embodiments may include a battery and / or a large-capacity energy storage system, comprising at least one electrode formed at least in part according to the operation of the method of this paragraph.
[0149] Multiple embodiments may include a method for improving the harmful effects of impurities in an iron electrode, comprising: passivating impurities in an iron-containing material so that the passivated impurities no longer react with the electrolyte of a battery in which the iron-containing material will be used. Multiple embodiments may include a method for improving the harmful effects of impurities in an iron electrode, comprising: adding a co-additive to the iron-containing material that preferentially reacts with impurities in the iron-containing material rather than stannate added to the iron-containing material. In multiple embodiments, the impurities include calcium or magnesium. In multiple embodiments, the co-additive includes fluoride ions, phosphate ions, and / or carbonate ions. In multiple embodiments, the method discussed in this paragraph may be performed in combination with one or more of the methods discussed in the previous paragraph. In multiple embodiments, the purification of the iron-containing material is performed at one or more stages in the processing of iron ore for forming a battery component. In multiple embodiments, one or more stages include grinding, mixing, adding a binder, adding a flux, filtering, granulating, hardening, forming iron ore pellets (IOP), reducing, forming direct reduced iron (DRI) pellets, crushing, powdering, heating, hot pressing, and / or forming a battery component before, during, and / or after. In multiple embodiments, the battery component is an electrode. In various embodiments, purification includes adding an etchant and / or a leaching agent to a concentrate mixing tank, rinsing the filter cake with a neutralizing agent, heating the concentrate stream to which the etchant and / or the leaching agent has been added, drum filtering, two-step filtering, partially immersing the iron material in the etching and / or leaching solution, completely immersing the iron material in the etching and / or leaching solution, and / or regenerating the etching and / or leaching solution. Various embodiments may include using the purified iron-containing material to form electrodes of a battery pack. Various embodiments may also include using the purified iron-containing material to form electrodes of a battery pack. Various embodiments may also include providing the battery pack to a large-capacity energy storage system. In various embodiments, the large-capacity energy storage system is a long-duration energy storage (LODES) system. Various embodiments may include a battery pack and / or a large-capacity energy storage system, which includes at least one electrode formed at least in part according to the operation of the method of this paragraph.
[0150] Various embodiments may include a method for purifying an iron-containing material, comprising: etching and / or leaching one or more soluble impurities from the iron-containing material, wherein the impurities include silicon dioxide, aluminum oxide, magnesium oxide, manganese oxide, and / or calcium oxide. In various embodiments, leaching comprises alkaline leaching. In various embodiments, leaching comprises acid leaching. In various embodiments, leaching comprises dissolving by adding a flux. In various embodiments, leaching comprises using ammonium fluoride (NH4F) or ammonium bifluoride (NH4HF2) or acidic ammonium fluoride (3NH4 .HF2) or its mixtures, solutions and derivatives (hereinafter collectively referred to as AF) to dissolve impurities. In various embodiments, leaching includes using hydrofluoric acid (HF), alkali metal hydroxides (e.g., NaOH and KOH) and / or high temperature melts (e.g., molten chlorides or fluorides or oxides) to dissolve impurities. In various embodiments, the iron-containing material is iron ore, iron and / or their intermediates. In various embodiments, etching includes etching with ammonium bifluoride (NH4HF2). In various embodiments, etching includes etching with an etchant containing fluorine. In various embodiments, etching includes etching with sodium fluorophosphate (Na2PO3F). Various embodiments may also include controlling the pH of the etching solution. In various embodiments, the pH is controlled in the range of 8 to 13. In various embodiments, the pH is controlled in the range of 7 to 9. In various embodiments, the pH is controlled in the range of 5 to 10. Various embodiments may also include adding soluble iron salts to the etching solution. In various embodiments, the iron salt comprises one or more of ferrous sulfate, iron (II) sulfate, ferrous chloride, ferric nitrate, ferric sulfate, and / or ferric chloride. Various embodiments may further include adding iron ions to the etching solution. Various embodiments may further include adding one or more corrosion inhibitors to the etching solution. Various embodiments may further include recycling the etching solution. Various embodiments may include a method for purifying an iron-containing material, comprising: modifying an impurity species in the iron-containing material to a benign compound. In various embodiments, the impurity is silicon dioxide, and the modification comprises adding an additive to convert the silicon dioxide into a silicon compound. In various embodiments, the additive is dolomite lime. Various embodiments may include a method for purifying an iron-containing material, comprising: passivating the impurities in the iron-containing material so that the passivated impurities no longer react with the electrolyte of a battery in which the iron-containing material will be used. Various embodiments may include a method for purifying an iron-containing material, comprising: adding a co-additive to the iron-containing material that preferentially reacts with the impurities in the iron-containing material rather than the stannate added to the iron-containing material. In various embodiments, the impurity comprises calcium or magnesium. In various embodiments, the co-additive comprises fluoride ions, phosphate ions and / or carbonate ions. In various embodiments, the purification of the iron-containing material is carried out at one or more stages in the processing of iron ore for forming battery components. In various embodiments, one or more stages include grinding, mixing, adding a binder, adding a flux, filtering, granulating, hardening, forming iron ore pellets (IOP), reducing, forming direct reduced iron (DRI) pellets, crushing, powdering, heating, hot pressing and / or forming battery components before, during and / or after. Various embodiments may also include using the purified iron-containing material to form the electrodes of the battery. Various embodiments may also include providing the battery to a large-capacity energy storage system. In various embodiments, the large-capacity energy storage system is a long-duration energy storage (LODES) system.Various embodiments may include a battery and / or bulk energy storage system comprising at least one electrode formed at least in part according to the operations of the method of this paragraph.
[0151] The various embodiments described and illustrated herein may provide apparatus and / or methods for large-capacity energy storage systems such as long-duration energy storage (LODES) systems, short-duration energy storage (SDES) systems, and the like. As an example, various embodiments may provide battery packs (e.g., battery pack 200) for large-capacity energy storage systems, such as battery packs for LODES. Renewable energy sources are becoming increasingly common and cost-effective. However, many renewable energy sources face intermittent issues that hinder the adoption of renewable energy sources. The impact of the intermittent trend of renewable energy sources can be mitigated by pairing renewable energy sources with large-capacity energy storage systems such as LODES systems, SDES systems, and the like. In order to support the use of a combination of power generation, transmission, and storage systems (e.g., a power plant with a renewable power generation source paired with a large-capacity energy storage system and a transmission facility located in either the power plant and / or the large-capacity energy storage system), it is necessary to support the design and operation of such a combination of power generation, transmission, and storage systems. Apparatus and methods, such as the apparatus and methods of the various embodiments described herein.
[0152] The combination of power generation, transmission and storage systems can be a power plant including one or more power generation sources (e.g., one or more renewable energy power generation sources, one or more non-renewable energy power generation sources, a combination of renewable energy and non-renewable energy power generation sources, etc.), one or more transmission facilities, and one or more large-capacity energy storage systems. The transmission facilities in any of the power plant and / or large-capacity energy storage system can be optimized together with the power generation and storage system, or restrictions can be imposed on the design and operation of the power generation and storage system. The combination of power generation, transmission and storage systems can be configured to meet a variety of output targets under a variety of design and operating constraints.
[0153] Figure 13-Figure 21 Various exemplary systems are shown, wherein one or more aspects of various embodiments can be used as part of a bulk energy storage system such as a LODES system, a SDES system, etc. For example, reference is made herein to Figure 1A-Figure 12CThe described multiple embodiments can be used as a battery pack for a large-capacity energy storage system such as a LODES system, a SDES system, etc., and / or, the multiple electrodes described herein can be used as components of a large-capacity energy storage system. As used herein, the term "LODES system" can refer to a large-capacity energy storage system configured to have a rated duration (energy / power ratio) of 24 hours (h) or longer, such as a duration of 24h, a duration of 24h to 50h, a duration greater than 50 hours, a duration of 24h to 150h, a duration greater than 150h, a duration of 24h to 200h, a duration greater than 200h, a duration of 24h to 500h, a duration greater than 500h, etc.
[0154] Fig.13An exemplary system is shown in which one or more aspects of multiple embodiments can be used as part of a large-capacity energy storage system. As a specific example, a large-capacity energy storage system incorporating one or more aspects of multiple embodiments can be a LODES system 2404. As an example, the LODES system 2404 can include a battery pack of multiple embodiments described herein, multiple electrodes described herein, and the like. The LODES system 2404 can be electrically connected to a wind farm 2402 and one or more transmission facilities 2406. The wind farm 2402 can be electrically connected to the transmission facility 2406. The transmission facility 2406 can be electrically connected to a power grid 2408. The wind farm 2402 can generate electricity, and the wind farm 2402 can output the generated electricity to the LODES system 2404 and / or the transmission facility 2406. The LODES system 2404 can store electricity received from the wind farm 2402 and / or the transmission facility 2406. The LODES system 2404 can output the stored electricity to the transmission facility 2406. The transmission facility 2406 may output power received from one or both of the wind farm 2402 and the LODES system 2404 to the grid 2408, and / or may receive power from the grid 2408 and output the power to the LODES system 2404. The wind farm 2402, the LODES system 2404, and the transmission facility 2406 may together constitute a power plant 2400, which may be a combination of power generation, transmission, and storage systems. The power generated by the wind farm 2402 may be supplied directly to the grid 2408 via the transmission facility 2406, or may be first stored in the LODES system 2404. In some cases, the power supplied to the grid 2408 may come entirely from the wind farm 2402, entirely from the LODES system 2404, or from a combination of the wind farm 2402 and the LODES system 2404. The power dispatch of the power plant 2400, which is a combination of wind farm 2402 and LODES system 2404, can be controlled according to a determined long-term (multi-day or even multi-year) plan, or can be controlled according to the day-ahead (24-hour forecast) market conditions, or can be controlled according to the market conditions of the previous hour, or can be controlled in response to real-time pricing signals.
[0155] As an example of the operation of power plant 2400, LODES system 2404 can be used to adjust and "fix" the electricity generated by wind farm 2402. In one such example, wind farm 2402 can have a peak power generation output (capacity) of 260 megawatts (MW) and a capacity factor (CF) of 41%. LODES system 2404 can have a rated power (capacity) of 106MW, a rated duration (energy / power ratio) of 150 hours (h), and an energy efficiency of 15,900 megawatt hours (MWh). In another such example, wind farm 2402 can have a peak power generation output (capacity) of 300MW and a capacity factor (CF) of 41%. LODES system 2404 can have a rated power of 106MW, a rated duration (energy / power ratio) of 200h, and an energy efficiency of 21,200MWh. In another such example, wind farm 2402 can have a peak power generation output (capacity) of 176MW and a capacity factor (CF) of 53%. The LODES system 2404 may have a rated power (capacity) of 88 MW, a rated duration (energy / power ratio) of 150 h, and an energy efficiency of 13,200 MWh. In another such example, the wind farm 2402 may have a peak power generation output (capacity) of 277 MW and a capacity factor (CF) of 41%. The LODES system 2404 may have a rated power (capacity) of 97 MW, a rated duration (energy / power ratio) of 50 h, and an energy efficiency of 4,850 MWh. In another such example, the wind farm 2402 may have a peak power generation output (capacity) of 315 MW and a capacity factor (CF) of 41%. The LODES system 2404 may have a rated power (capacity) of 110 MW, a rated duration (energy / power ratio) of 25 h, and an energy efficiency of 2,750 MWh.
[0156] Fig.14 An exemplary system is shown in which one or more aspects of the various embodiments can be used as part of a bulk energy storage system. As a specific example, a bulk energy storage system incorporating one or more aspects of the various embodiments can be a LODES system 2404. As an example, the LODES system 2404 can include a battery pack of the various embodiments described herein, a plurality of electrodes described herein, etc. The system of FIG. 24 can be similar to Fig.132402. The LODES system 2404 may be electrically connected to the PV farm 2502 and one or more transmission facilities 2406. The PV farm 2502 may be electrically connected to the transmission facility 2406. The transmission facility 2406 may be electrically connected to the grid 2408. The PV farm 2502 may generate electricity and the PV farm 2502 may output the generated electricity to the LODES system 2404 and / or the transmission facility 2406. The LODES system 2404 may store the electricity received from the PV farm 2502 and / or the transmission facility 2406. The LODES system 2404 may output the stored electricity to the transmission facility 2406. The transmission facility 2406 may output the electricity received from one or both of the PV farm 2502 and the LODES system 2404 to the grid 2408, and / or may receive electricity from the grid 2408 and output the electricity to the LODES system 2404. PV farm 2502, LODES system 2404, and transmission facility 2406 together may constitute power plant 2500, which may be a combination of power generation, transmission, and storage systems. The power generated by PV farm 2502 may be directly supplied to grid 2408 via transmission facility 2406, or may be first stored in LODES system 2404. In some cases, the power supplied to grid 2408 may come entirely from PV farm 2502, entirely from LODES system 2404, or from a combination of PV farm 2502 and LODES system 2404. The power dispatch of power plant 2500, which is a combination of PV farm 2502 and LODES system 2404, may be controlled according to a determined long-term (multi-day or even multi-year) plan, or may be controlled according to day-ahead (24-hour forecast) market conditions, or may be controlled according to market conditions one hour earlier, or may be controlled in response to real-time pricing signals.
[0157] As an example of the operation of power plant 2500, LODES system 2404 can be used to adjust and "fix" the electricity generated by PV farm 2502. In one such example, PV farm 2502 can have a peak power generation output (capacity) of 490MW and a capacity factor (CF) of 24%. LODES system 2404 can have a rated power (capacity) of 340MW, a rated duration (energy / power ratio) of 150h, and an energy efficiency of 51,000MWh. In another such example, PV farm 2502 can have a peak power generation output (capacity) of 680MW and a capacity factor (CF) of 24%. LODES system 2404 can have a rated power (capacity) of 410MW, a rated duration (energy / power ratio) of 200h, and an energy efficiency of 82,000MWh. In another such example, PV farm 2502 can have a peak power generation output (capacity) of 330MW and a capacity factor (CF) of 31%. The LODES system 2404 may have a rated power (capacity) of 215 MW, a rated duration (energy / power ratio) of 150 h, and an energy efficiency of 32,250 MWh. In another such example, the PV farm 2502 may have a peak power generation output (capacity) of 510 MW and a capacity factor (CF) of 24%. The LODES system 2404 may have a rated power (capacity) of 380 MW, a rated duration (energy / power ratio) of 50 h, and an energy efficiency of 19,000 MWh. In another such example, the PV farm 2502 may have a peak power generation output (capacity) of 630 MW and a capacity factor (CF) of 24%. The LODES system 2404 may have a rated power (capacity) of 380 MW, a rated duration (energy / power ratio) of 25 h, and an energy efficiency of 9,500 MWh.
[0158] Fig.15 An exemplary system is shown in which one or more aspects of multiple embodiments can be used as part of a bulk energy storage system. As a specific example, a bulk energy storage system incorporating one or more aspects of multiple embodiments can be a LODES system 2404. As an example, the LODES system 2404 can include a battery pack of multiple embodiments described herein, multiple electrodes described herein, etc. Fig.15 The system can be similar to Fig.13 and Fig.14system, except that wind farm 2402 and photovoltaic (PV) farm 2502 can all be generators working together in power plant 2600. PV farm 2502, wind farm 2402, LODES system 2404 and transmission facility 2406 together can constitute power plant 2600, which can be a combination of power generation, transmission and storage systems. The electricity generated by PV farm 2502 and / or wind farm 2402 can be directly supplied to grid 2408 through transmission facility 2406, or can be first stored in LODES system 2404. In some cases, the electricity supplied to grid 2408 can come entirely from PV farm 2502, entirely from wind farm 2402, entirely from LODES system 2404, or from a combination of PV farm 2502, wind farm 2402 and LODES system 2404. The power dispatch of the power plant 2600, which is a combination of wind farm 2402, PV farm 2502 and LODES system 2404, can be controlled according to a determined long-term (multi-day or even multi-year) plan, or can be controlled according to the day-ahead (24-hour forecast) market conditions, or can be controlled according to the market conditions of the previous hour, or can be controlled in response to real-time pricing signals.
[0159] As an example of the operation of power plant 2600, LODES system 2404 can be used to adjust and "fix" the electricity generated by wind farm 2402 and PV farm 2502. In one such example, wind farm 2402 can have a peak power generation output (capacity) of 126MW and a capacity factor (CF) of 41%, and PV farm 2502 can have a peak power generation output (capacity) of 126MW and a capacity factor (CF) of 24%. LODES system 2404 can have a rated power (capacity) of 63MW, a rated duration (energy / power ratio) of 150h, and an energy efficiency of 9,450MWh. In another such example, wind farm 2402 can have a peak power generation output (capacity) of 170MW and a capacity factor (CF) of 41%, and PV farm 2502 can have a peak power generation output (capacity) of 110MW and a capacity factor (CF) of 24%. LODES system 2404 may have a rated power (capacity) of 57 MW, a rated duration (energy / power ratio) of 200 h, and an energy efficiency of 11,400 MWh. In another such example, wind farm 2402 may have a peak power generation output (capacity) of 105 MW and a capacity factor (CF) of 51%, and PV farm 2502 may have a peak power generation output (capacity) of 70 MW and a capacity factor (CF) of 31. LODES system 2404 may have a rated power (capacity) of 61 MW, a rated duration (energy / power ratio) of 150 h, and an energy efficiency of 9,150 MWh. In another such example, wind farm 2402 may have a peak power generation output (capacity) of 135 MW and a capacity factor (CF) of 41%, and PV farm 2502 may have a peak power generation output (capacity) of 90 MW and a capacity factor (CF) of 24%. LODES system 2404 may have a rated power (capacity) of 68 MW, a rated duration (energy / power ratio) of 50 h, and an energy efficiency of 3,400 MWh. In another such example, wind farm 2402 may have a peak power generation output (capacity) of 144 MW and a capacity factor (CF) of 41%, and PV farm 2502 may have a peak power generation output (capacity) of 96 MW and a capacity factor (CF) of 24%. LODES system 2404 may have a rated power (capacity) of 72 MW, a rated duration (energy / power ratio) of 25 h, and an energy efficiency of 1,800 MWh.
[0160] Fig.16An exemplary system is shown in which one or more aspects of multiple embodiments can be used as part of a large-capacity energy storage system. As a specific example, a large-capacity energy storage system incorporating one or more aspects of multiple embodiments can be a LODES system 2404. As an example, the LODES system 2404 can include a battery pack of multiple embodiments described herein, multiple electrodes described herein, etc. The LODES system 2404 can be electrically connected to one or more transmission facilities 2406. In this way, the LODES system 2404 can operate in a "stand-alone" manner to arbitrate energy around market prices and / or avoid transmission constraints. The LODES system 2404 can be electrically connected to one or more transmission facilities 2406. The transmission facility 2406 can be electrically connected to a power grid 2408. The LODES system 2404 can store electricity received from the transmission facility 2406. The LODES system 2404 can output the stored electricity to the transmission facility 2406. Transmission facility 2406 may output power received from LODES system 2404 to grid 2408 and / or may receive power from grid 2408 and output the power to LODES system 2404 .
[0161] LODES system 2404 and transmission facilities 2406 together can constitute power plant 900. As an example, power plant 900 can be located downstream of transmission restrictions, close to the power consumption end. In such an example where power plant 2700 is located downstream, LODES system 2404 can have a duration of 24h to 500h, and can undergo one or more full discharges per year to support peak power consumption when transmission capacity is insufficient to serve customers. In addition, in such an example where power plant 2700 is located downstream, LODES system 2404 can undergo several shallow discharges (daily or at a higher frequency) to adjudicate the difference between night and daytime electricity prices and reduce the total cost of power service to customers. As another example, power plant 2700 can be located upstream of transmission restrictions, close to the power generation end. In such an example where power plant 2700 is located upstream, LODES system 2404 can have a duration of 24h to 500h, and can undergo one or more full charges per year to absorb excess power generation when transmission capacity is insufficient to distribute power to customers. Additionally, in such an example where the power plant 2700 is located upstream, the LODES system 2404 may undergo several shallow charges and discharges (daily or at a higher frequency) to arbitrate the difference between nighttime and daytime electricity prices and maximize the value of the output of the power generation facility.
[0162] Fig.17An exemplary system is shown in which one or more aspects of multiple embodiments may be used as part of a bulk energy storage system. As a specific example, a bulk energy storage system incorporating one or more aspects of multiple embodiments may be a LODES system 2404. As an example, the LODES system 2404 may include a battery pack of multiple embodiments described herein, multiple electrodes described herein, and the like. The LODES system 2404 may be electrically connected to a commercial and industrial (C&I) customer 2802, such as a data center, a factory, and the like. The LODES system 2404 may be electrically connected to one or more transmission facilities 2406. The transmission facility 2406 may be electrically connected to a power grid 2408. The transmission facility 2406 may receive power from the power grid 2408 and output the power to the LODES system 2404. The LODES system 2404 may store power received from the transmission facility 2406. The LODES system 2404 may output the stored power to a C&I customer 2802. In this manner, LODES system 2404 may operate to adjust power purchased from grid 2408 to match the power usage patterns of C&I customers 2802 .
[0163] LODES system 2404 and transmission facility 2406 may together constitute power plant 2800. As an example, power plant 2800 may be located close to the electricity consumption end, i.e., close to C&I customer 2802, such as between grid 2408 and C&I customer 2802. In such an example, LODES system 2404 may have a duration of 24h to 500h, and may purchase electricity from the market, thereby charging LODES system 2404 when electricity is cheaper. LODES system 2404 may then discharge to provide electricity to C&I customer 2802 when the market price is expensive, thereby offsetting the market purchase of C&I customer 2802. As an alternative configuration, power plant 2800 may be located between renewable energy sources such as PV farms, wind farms, etc., rather than between grid 2408 and C&I customer 2802, and transmission facility 2406 may be connected to the renewable energy source. In such an alternative example, the LODES system 2404 can have a duration of 24 hours to 500 hours, and the LODES system 2404 can be charged when the renewable energy output is available. Then, the LODES system 2404 can be discharged to provide electricity generated by the renewable energy to the C&I customer 2802, thereby meeting part or all of the electricity demand of the C&I customer 2802.
[0164] Fig.18An exemplary system is shown in which one or more aspects of multiple embodiments may be used as part of a bulk energy storage system. As a specific example, a bulk energy storage system incorporating one or more aspects of multiple embodiments may be a LODES system 2404. As an example, the LODES system 2404 may include a battery pack of multiple embodiments described herein, multiple electrodes described herein, and the like. The LODES system 2404 may be electrically connected to a wind farm 2402 and one or more transmission facilities 2406. The wind farm 2402 may be electrically connected to the transmission facility 2406. The transmission facility 2406 may be electrically connected to a C&I customer 2802. The wind farm 2402 may generate electricity, and the wind farm 2402 may output the generated electricity to the LODES system 2404 and / or the transmission facility 2406. The LODES system 2404 may store electricity received from the wind farm 2402.
[0165] The LODES system 2404 may output the stored electricity to a transmission facility 2406. The transmission facility 2406 may output the electricity received from one or both of the wind farm 2402 and the LODES system 2404 to the C&I customer 2802. The wind farm 2402, the LODES system 2404, and the transmission facility 2406 may together constitute a power plant 2900, which may be a combination of power generation, transmission, and storage systems. The electricity generated by the wind farm 2402 may be supplied directly to the C&I customer 2802 via the transmission facility 2406, or may be first stored in the LODES system 2404. In some cases, the electricity supplied to the C&I customer 2802 may come entirely from the wind farm 2402, entirely from the LODES system 2404, or from a combination of the wind farm 2402 and the LODES system 2404. The LODES system 2404 may be used to adjust the electricity generated by the wind farm 2402 to match the consumption pattern of the C&I customer 2802. In one such example, the LODES system 2404 may have a duration of 24 hours to 500 hours and may be charged when the renewable energy generation of the wind farm 2402 exceeds the load of the C&I customer 2802. The LODES system 2404 may then be discharged when the renewable energy generation of the wind farm 2402 does not reach the load of the C&I customer 2802, so as to provide a reliable renewable energy profile to the C&I customer 2802 to offset some or all of the electricity consumption of the C&I customer 2802.
[0166] Fig.19An exemplary system is shown in which one or more aspects of multiple embodiments can be used as part of a large-capacity energy storage system. As a specific example, a large-capacity energy storage system incorporating one or more aspects of multiple embodiments can be a LODES system 2404. As an example, the LODES system 2404 can include a battery pack of multiple embodiments described herein, multiple electrodes described herein, etc. The LODES system 2404 can be part of a power plant 3000, which is used to integrate a large amount of renewable energy generation into a microgrid, and coordinate the renewable energy generation output through, for example, a PV farm 2502 and a wind farm 2402 with the existing thermal power generation output through, for example, a thermal power plant 3002 (e.g., a gas plant, a coal-fired plant, a diesel generator set, etc., or a combination of thermal power generation methods), while renewable energy generation and thermal power generation provide C&I customers 2802 with high-availability loads. Microgrids, such as microgrids formed by power plants 3000 and thermal power plants 3002, can provide 90% or higher availability. The electricity generated by PV farm 2502 and / or wind farm 2402 may be supplied directly to C&I customer 2802 or may first be stored in LODES system 2404 .
[0167] In some cases, the power supplied to C&I customer 2802 may come entirely from PV farm 2502, entirely from wind farm 2402, entirely from LODES system 2404, entirely from thermal power plant 3002, or from any combination of PV farm 2502, wind farm 2402, LODES system 2404, and / or thermal power plant 3002. As an example, LODES system 2404 of power plant 3000 may have a duration of 24 hours to 500 hours. As a specific example, C&I customer 2802 load may have a peak of 100 MW, LODES system 2404 may have a rated power of 14 MW and a duration of 150 hours, the price of natural gas may be $6 per million British thermal units (MMBTU), and the renewable energy share may be 58%. As another specific example, the C&I customer 2802 load may have a peak of 100 MW, the LODES system 2404 may have a rated power of 25 MW and a duration of 150 h, the price of natural gas may be $8 / MMBTU, and the renewable energy share may be 65%.
[0168] Fig. 20An exemplary system is shown in which one or more aspects of multiple embodiments can be used as part of a large-capacity energy storage system. As a specific example, a large-capacity energy storage system incorporating one or more aspects of multiple embodiments can be a LODES system 2404. As an example, the LODES system 2404 can include a battery pack of multiple embodiments described herein, multiple electrodes described herein, etc. The LODES system 2404 can be used to supplement a nuclear power plant 3102 (or other inflexible power generation facilities, such as thermal power plants, biomass power plants, etc., and / or any other type of power plant with a ramp rate of less than 50% of rated power for one hour and a high capacity factor of 80% or more) to increase the flexibility of the combined output of the power plant 3100 consisting of the combination of the LODES system 2404 and the nuclear power plant 3102. The nuclear power plant 3102 can be operated at a high capacity factor and at the highest efficiency point, and the LODES system 2404 can be charged and discharged to effectively adjust the output of the nuclear power plant 3102 to match customer power consumption and / or market electricity prices. As an example, the LODES system 2404 of the power plant 3100 may have a duration of 24 hours to 500 hours. In a specific example, the nuclear power plant 3102 may have a rated output of 1000MW, and due to low market electricity prices, the nuclear power plant 3102 may be forced to be at the lowest stable power generation for a long time or even shut down. The LODES system 2404 can avoid the facility from shutting down and charging when the market price is low; the LODES system 2404 can then discharge and increase the total output power generation when the market pricing is high.
[0169] Fig.21An exemplary system is shown in which one or more aspects of multiple embodiments can be used as part of a large-capacity energy storage system. As a specific example, a large-capacity energy storage system incorporating one or more aspects of multiple embodiments can be a LODES system 2404. As an example, the LODES system 2404 can include a battery pack of multiple embodiments described herein, multiple electrodes described herein, etc. The LODES system 2404 can operate in conjunction with the SDES system 3202. The LODES system 2404 and the SDES system 3202 can together constitute a power plant 3200. As an example, the LODES system 2404 and the SDES system 3202 can be optimized together, whereby the LODES system 2404 can provide a variety of services, including long-term backup and / or bridging multi-day fluctuations (e.g., multi-day fluctuations in market pricing, renewable energy generation, power consumption, etc.), and the SDES system 3202 can provide a variety of services, including fast auxiliary services (e.g., voltage control, frequency regulation, etc.) and / or bridging intraday fluctuations (e.g., intraday fluctuations in market pricing, renewable energy generation, power consumption, etc.). The SDES system 3202 may have a duration of less than 10 hours and a round trip efficiency greater than 80%. The LODES system 2404 may have a duration of 24h to 500h and a round trip efficiency greater than 40%. In one such example, the LODES system 2404 may have a duration of 150 hours and support a customer's power consumption for up to a week of insufficient renewable energy generation. The LODES system 2404 may also support customer power consumption during intraday insufficient power generation events, supplementing the capabilities of the SDES system 3202. In addition, the SDES system 3202 may provide power to customers during intraday insufficient power generation events and provide power regulation and premium services such as voltage control, frequency regulation, etc.
[0170] The foregoing method description is provided only as an illustrative example and is not intended to require or imply that the steps of multiple embodiments must be performed in the order presented. As will be appreciated by those skilled in the art, the order of the steps in the foregoing embodiments can be performed in any order. Words such as "thereafter", "then", "next step" are not necessarily intended to limit the order of steps; these words can be used to guide the reader to understand the description of the method. In addition, singular forms such as using articles ("a", "an" or "the") to mention claim elements should not be interpreted as limiting the element to the singular.
[0171] The foregoing description of the disclosed embodiments is provided to enable any person skilled in the art to make or use the described embodiments. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be applied to other embodiments without departing from the scope of the present disclosure. Therefore, the present invention is not intended to be limited to the embodiments shown herein, but should be given the broadest scope consistent with the appended claims and the principles and novel features disclosed herein.
Claims
1. A method for purifying an iron-containing material, comprising: One or more soluble impurities are leached from an iron-containing material, wherein the leaching comprises leaching with a leachate comprising fluorine.
2. The method according to claim 1, wherein the leachate comprises ammonium fluoride (NH4F) or acidic ammonium fluoride (3NH4 . HF2), or a mixture thereof.
3. The method according to any one of claims 1 to 2, wherein: The leachate contains ammonium bifluoride (NH4HF2).
4. The method according to claim 1, wherein: The leaching includes using hydrofluoric acid (HF), alkali metal hydroxides (eg, NaOH and KOH), and / or high temperature melts (eg, molten chlorides or fluorides or oxides) to dissolve impurities.
5. The method according to any one of claims 1 to 4, wherein: The leachate contains sodium fluorophosphate (Na2PO3F).
6. The method according to any one of claims 1 to 5, wherein: The fluorine-containing component of the leachate has a molar concentration of 100 ppm to 10000 ppm.
7. The method according to claim 6, wherein: The fluorine-containing component of the leachate has a molar concentration of 500 ppm to 5000 ppm.
8. The method according to any one of claims 1 to 7, wherein: The iron-containing material is iron ore, iron and / or intermediates thereof.
9. The method according to any one of claims 1 to 8, further comprising controlling the pH of the leachate.
10. The method according to claim 9, wherein: The pH was controlled in the range of 8 to 13.
11. The method according to claim 10, wherein: The pH was controlled in the range of 7 to 9.
12. The method according to claim 11, wherein: The pH was controlled in the range of 5 to 10.
13. The method according to any one of claims 1 to 12, further comprising adding a soluble iron salt to the leachate.
14. The method of claim 13, wherein the iron salt comprises one or more of ferrous sulfate, iron (II) sulfate, ferrous chloride, ferric nitrate, ferric sulfate and / or ferric chloride.
15. The method according to any one of claims 1 to 14, further comprising adding iron ions to the leachate.
16. The method of any one of claims 1-15, further comprising adding one or more corrosion inhibitors to the leachate.
17. The method of any one of claims 1 to 16, further comprising recycling the leachate.
18. A method for purifying an iron-containing material, comprising: One or more soluble impurities are leached from the iron-containing material, wherein the leaching comprises dissolution by adding a flux.
19. The method of any one of claims 1-18, further comprising using the purified iron-containing material to form an electrode of a battery.
20. The method of claim 19, further comprising providing the battery pack to a bulk energy storage system.
21. The method of claim 20, wherein the bulk energy storage system is a long duration energy storage (LODES) system.
22. A battery and / or bulk energy storage system comprising at least one electrode formed at least in part by operation of the method of claims 1-21.