Regional selective deposition method for thin film using atomic layer deposition method, and substrate for selectively forming thin film

The regional selective atomic layer deposition method using organic thiol small molecule inhibitors addresses the limitations of miniaturization in semiconductor manufacturing by forming thin films with varying thicknesses on metal, silicon dioxide, and nitride substrates, improving precision and reducing costs in semiconductor device production.

CN119096004APending Publication Date: 2024-12-06IND ACADEMIC COOPERATION FOUND UNIV OF INCHEON
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202380034969.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-19
Filing Date
2023-03-16
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing semiconductor manufacturing methods face limitations in accurately patterning devices below 10 nm due to physical constraints and degradation of device performance, necessitating a more precise and reliable thin film deposition method.

Method used

A regional selective atomic layer deposition method using organic thiol small molecule inhibitors is employed to form thin films with varying thicknesses on substrates containing metal, silicon dioxide, and nitride, overcoming the limitations of self-assembled monolayers by ensuring excellent surface sensitivity and adsorption selectivity, allowing for dense monolayer formation without repeated lithography and etching processes.

Benefits of technology

The method enables the formation of thin films with distinct thicknesses on different substrate surfaces, enhancing manufacturing precision and reducing undesirable side effects while minimizing costs, thus addressing the challenges of miniaturization in semiconductor device production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119096004A_ABST
    Figure CN119096004A_ABST
Patent Text Reader

Abstract

The present invention relates to a method for selectively depositing a thin film using a regioselective atomic layer deposition method, and a substrate for selectively forming a thin film, and more particularly, to a method for selectively depositing a thin film using a regioselective atomic layer deposition method, substrates comprising metals such as copper (Cu), substrates comprising silicon dioxide (SiO2), and substrates comprising metals such as titanium nitride (TiN) by using organic thiol small molecule inhibitors The present invention relates to a method for selectively depositing a thin film using a regioselective atomic layer deposition method and a substrate for selectively forming a thin film, wherein thin films having different thicknesses are formed on the surface of a substrate made of a nitride, etc.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for selectively depositing a thin film using a regional selective atomic layer deposition method and a substrate for selectively forming a thin film. More specifically, the present invention relates to a method for selectively depositing a thin film using a regional selective atomic layer deposition method and a substrate for selectively forming a thin film by passivating the surfaces of three or more substrates, i.e., a substrate including a metal, a substrate including silicon dioxide (SiO2), and a substrate including a nitride, using an organic thiol small molecule inhibitor to form a thin film having different thicknesses. Background Art

[0002] With the development of semiconductor industry technology, the size of semiconductor devices has been continuously reduced to meet the needs of the semiconductor market, and currently the size is required to be below 10nm.

[0003] For this reason, existing top-down semiconductor device manufacturing methods including repeated lithography and etching processes have physical limitations when manufacturing semiconductor devices with dimensions below 10 nm, such as lack of accurate device patterning or degradation of device performance and reliability due to misalignment of patterned features during device layering.

[0004] Atomic layer deposition (ALD) is a thin film deposition technology that has significant advantages over other thin film deposition methods in terms of uniformity, thickness control, and coating properties (conformality).

[0005] Due to the self-limiting surface characteristics of the atomic layer deposition process, in addition to thin film deposition and area selective deposition (ASD), other advantages can be provided. Specifically, by using appropriate chemical treatment to control the surface chemical reactivity in a vacuum environment, local deposition can be performed in area selective deposition. Through the area selective deposition as described above, it is possible to transfer it from bottom to top using a suitable pattern on the original surface without repeated lithography and etching processes. In addition, it can also be used to create additional patterns inside the 3D pattern, which is impossible to achieve in the prior art. Furthermore, another advantage is that it can minimize the undesirable side effects that may occur in the current complex process and reduce manufacturing costs.

[0006] Area-selective atomic layer deposition (AS-ALD) is a deposition method with excellent reliability in the ALD method. In addition, the use of inhibitors in the area-selective ALD method is an effective surface functionalization method. The inhibitor is selectively adsorbed on the surface to passivate during the ALD method, performing the function of inducing selective regional inactivation. In the prior art, self-assembled monolayers (SAM), small molecule inhibitors (SMI) and precursor inhibitors (Pis) are used as such inhibitors.

[0007] SAM is a self-assembled molecule that inhibits growth by adsorption due to its surface sensitivity and surface selectivity. However, as the size of semiconductor devices becomes smaller and smaller, thermal stability is low, and there are physical limitations when using SAMs of a certain size for semiconductor device manufacturing processes.

[0008] SMIs are generally nanoscale molecules with characteristic chemical adsorption reaction areas and have adsorption selectivity similar to that of SAMs. This adsorption selectivity is determined by inert ligands. By using nanoscale SMIs for regional selective deposition, the difficulties faced by SAMs in high-volume manufacturing can be overcome. In addition, SMIs do not require the adsorption process of wet chemical methods that SAMs must perform. In short, as an inhibitor, SMIs are proposed to be a better method than the previously widely used SAMs. Summary of the invention

[0009] Technical issues

[0010] The object of the present invention is to provide a selective deposition method of a thin film using a regional selective atomic layer deposition method and a substrate for selectively forming a thin film, which uses an organic thiol small molecule inhibitor that has surface sensitivity and surface selectivity like SAM and is adsorbed on the surface of the substrate, so that the vapor pressure is excellent, the chamber transfer is easy, and a dense monolayer can be formed in a short time.

[0011] In addition, another object of the present invention is to provide a method for selective deposition of a thin film using a regional selective atomic layer deposition method and a substrate for selectively forming a thin film, which respectively uses organic thiol small molecule inhibitors adsorbed at different concentrations on the surfaces of a substrate including metal, a substrate including silicon dioxide, and a substrate including nitride, thereby forming thin films with different thicknesses on the surfaces of a substrate including metal, a substrate including silicon dioxide, and a substrate including nitride.

[0012] Solutions to the problem

[0013] In order to solve the above problems, the selective deposition method of a thin film using a regional selective atomic layer deposition method of the present invention may include: a first step, preparing a substrate in which a first substrate including a metal, a second substrate including silicon dioxide and a third substrate including a nitride are arranged in parallel and integrated; a second step, exposing the above substrate to an organic thiol small molecule inhibitor; and a third step, using a regional selective atomic layer deposition method (AS-ALD) to form a thin film on the surface of the substrate exposed to the above organic thiol small molecule inhibitor. The metal of the first substrate according to the present invention can be selected from the group consisting of copper (Cu), cobalt (Co), ruthenium (Ru), molybdenum (Mo) and tungsten (W), preferably, it can be copper. In addition, the nitride of the third substrate according to the present invention can be selected from the group consisting of titanium nitride, molybdenum nitride, tungsten nitride and silicon nitride, preferably, it can be titanium nitride. In addition, the thin film formed according to the present invention can be a thin film selected from the group consisting of metals, metal oxides and silicon dielectric materials, preferably, it can be a hafnium oxide (HfO2) film.

[0014] In a preferred embodiment of the present invention, the thickness of the thin film formed on the surface of the first substrate, the thickness of the thin film formed on the surface of the second substrate, and the thickness of the thin film formed on the surface of the third substrate may be different.

[0015] In a preferred embodiment of the present invention, the method for selective deposition of a thin film using area selective atomic layer deposition of the present invention can satisfy the following condition (1).

[0016] (1)A <B<C

[0017] In the above condition (1), A represents the thickness of the thin film formed on the surface of the first substrate, B represents the thickness of the thin film formed on the surface of the second substrate, and C represents the thickness of the thin film formed on the surface of the third substrate.

[0018] In a preferred embodiment of the present invention, the organic thiol small molecule inhibitor may include a compound represented by the following Chemical Formula 1.

[0019] [Chemical formula 1]

[0020]

[0021] In the above chemical formula 1, R 1 and R 2 Each is independently a C1-C12 straight-chain alkyl group, a C3-C12 branched-chain alkyl group or a C6-C12 aryl group. 1 and R 2 It is a C1-C12 straight chain alkyl group, and more preferably a C1-C3 straight chain alkyl group.

[0022] In a preferred embodiment of the present invention, the second step in the method for selective deposition of a thin film using the area selective atomic layer deposition method of the present invention may include: step 2-1, after drying the above-mentioned substrate, placing the above-mentioned substrate in a chamber with an internal temperature of about 300°C to about 500°C and a vacuum base pressure condition and maintaining it for about 1 minute to about 20 minutes; step 2-2, purging the above-mentioned chamber, while maintaining the internal temperature of the chamber at about 200°C to about 500°C, placing an organic thiol small molecule inhibitor into the chamber, so that the substrate is exposed to the organic thiol small molecule inhibitor for about 1 second to about 100 seconds; and step 2-3, cooling the substrate exposed to the above-mentioned organic thiol small molecule inhibitor to a temperature of about 15°C to about 35°C.

[0023] In a preferred embodiment of the present invention, in the second step of the selective deposition method of a thin film using the area selective atomic layer deposition method of the present invention, the water contact angle of the first substrate surface exposed to the organic thiol small molecule inhibitor can be about 90° to about 100°, and the water contact angle of the second substrate surface exposed to the organic thiol small molecule inhibitor can be about 70° to about 80°.

[0024] In a preferred embodiment of the present invention, in the second step of the thin film selective deposition method of the area selective atomic layer deposition method of the present invention, the organic thiol small molecule inhibitor introduced into the chamber undergoes thermal dissociation and is separated into alkylsulfanyl and alkyl, respectively. The alkylsulfanyl can be adsorbed on the surface of the first substrate, and the alkyl can be adsorbed on the surface of the second substrate. At this time, the alkylsulfanyl is preferably ethylsulfanyl, and the alkyl is preferably ethyl.

[0025] In a preferred embodiment of the present invention, the third step of the method for selective deposition of a thin film using regional selective atomic layer deposition of the present invention may include: step 3-1, placing the substrate exposed to the organic thiol small molecule inhibitor into a chamber and heating it at about 200°C to about 350°C; and step 3-2, performing regional selective atomic layer deposition by placing a thin film deposition precursor into the above-mentioned chamber, exposing it for about 1 second to about 10 seconds, then purging for about 50 seconds to about 70 seconds, placing the relative reactant into the chamber and exposing it for about 1 second to about 5 seconds, and then purging for about 50 seconds to about 70 seconds.

[0026] In a preferred embodiment of the present invention, the thin film deposition precursor may be a volatile precursor including Group 3 to Group 16 compounds such as titanium compounds, hafnium compounds, zirconium compounds, tantalum compounds, vanadium compounds, niobium compounds, molybdenum compounds or silicon compounds.

[0027] In a preferred embodiment of the present invention, the thin film deposition precursor may include at least one selected from the group consisting of a compound represented by the following Chemical Formula 2, a compound represented by the following Chemical Formula 3, a compound represented by the following Chemical Formula 4, and a compound represented by the following Chemical Formula 5.

[0028] [Chemical formula 2]

[0029] (L1) n M(NR 3 R 4 ) 4-n

[0030] In the above chemical formula 2, L1 is a ligand selected from the group consisting of cyclopentadienyl and C1-C12 alkyl-substituted cyclopentadienyl, M is a metal selected from the group consisting of titanium, hafnium and zirconium, and R 3 and R 4 Each is independently a C1-C12 straight-chain alkyl group or a C3-C12 branched-chain alkyl group, and n is 0, 1 or 2.

[0031] [Chemical formula 3]

[0032] R 5 m M(OR 6 ) 3-m

[0033] In the above chemical formula 3, M is a metal selected from the group consisting of aluminum, hafnium and zirconium, and R 5 and R 6 Each is independently a C1-C12 straight-chain alkyl group or a C3-C12 branched-chain alkyl group, and m is 1 to 3.

[0034] [Chemical formula 4]

[0035] (L2)pMR7(OR 8 ) 3-p

[0036] In the above chemical formula 4, L2 is a ligand selected from the group consisting of cyclopentadienyl and C1-C12 alkyl-substituted cyclopentadienyl, M is a metal selected from the group consisting of titanium, hafnium and zirconium, R 7 and R 8 Each is independently a C1-C12 straight-chain alkyl group or a C3-C12 branched-chain alkyl group, and p is 1 or 2.

[0037] [Chemical formula 5]

[0038] (R 9 N) q M(NR 10 R 11 ) 4-q

[0039] In the above chemical formula 5, M is a metal selected from the group consisting of vanadium, niobium, tantalum, molybdenum and tungsten, and R 9 , R 10 and R 11 Each is independently a C1-C12 straight-chain alkyl group or a C3-C12 branched-chain alkyl group, and q is 1 or 2.

[0040] In a preferred embodiment of the present invention, specifically, the compound represented by the above chemical formula 2 can be tetrakis(dimethylamino)hafnium (TDMAH), tetrakis(diethylamino)hafnium (TDEAH), tetrakis(ethylmethylamino)hafnium (TEMAH), cyclopentadienyltris(dimethylamino)hafnium (CpHf(NMe2)3), methylcyclopentadienyltris(dimethylamino)hafnium ((MeCp)Hf(NMe2)3), ethylcyclopentadienyltris(dimethylamino)hafnium ((EtCp)Hf(NMe2)3), (n-propylcyclopentadienyl)tris(dimethylamino)hafnium (NMeEt)3), methylcyclopentadienyltris(methylethylamino)hafnium ((MeCp)Hf(NMeEt)3), ethylcyclopentadienyltris(methylethylamino)hafnium ((EtCp)Hf(NMeEt)3), cyclopentadienyltris(diethylamino)hafnium (CpHf(NEt2)3, methylcyclopentadienyltris(diethylamino)hafnium ((MeCp)Hf(NEt2)3), ethylcyclopentadienyltris(diethylamino)hafnium ((EtCp)Hf(NMeEt)3), cyclopentadienyltris(diethylamino)hafnium (CpHf(NEt2)3), methylcyclopentadienyltris(diethylamino)hafnium ((MeCp)Hf(NEt2)3), bis(cyclopentadienyl)bis(dimethylamino)hafnium ((EtCp)Hf(NEt2)3), bis(cyclopentadienyl)bis(dimethylamino)hafnium (Cp2Hf(NMe2)2), bis(methylcyclopentadienyl)bis(dimethylamino)hafnium ((MeCp)2Hf(NMe2)2), bis(ethylcyclopentadienyl)bis(dimethylamino)hafnium ((EtCp)2Hf(NMe2)2), bis(cyclopentadienyl)bis(methylethylamino)hafnium (Cp2Hf(NMeEt)2), bis(methylcyclopentadienyl)bis(methylethylamino)hafnium ((MeCp)2Hf(NMeEt )2), bis(ethylcyclopentadienyl)bis(methylethylamino)hafnium ((EtCp)2Hf(NMeEt)2), bis(cyclopentadienyl)bis(diethylamino)hafnium (Cp2Hf(NEt2)2), bis(methylcyclopentadienyl)bis(diethylamino)hafnium ((MeCp)2Hf(NEt2)3), bis(ethylcyclopentadienyl)bis(diethylamino)hafnium ((EtCp)2Hf(NEt2)2) or (n-propylcyclopentadienyl)tris(dimethylamino)zirconium ((n-PrCp)Zr(NMe2)3), but are not limited thereto.

[0041] In a preferred embodiment of the present invention, specifically, the compound represented by the above Chemical Formula 3 may be trimethylaluminum, triethylaluminum, dimethylaluminum isopropoxide or diethylaluminum isopropoxide, but is not limited thereto.

[0042] In a preferred embodiment of the present invention, specifically, the compound represented by the above Chemical Formula 4 can be CpHfMe(OMe)2, CpZrMe(OMe)2, (MeCp)HfMe(OMe)2, (MeCp)ZrMe(OMe)2, (EtCp)HfMe(OMe)2 or (EtCp)ZrMe(OMe), but is not limited thereto.

[0043] In a preferred embodiment of the present invention, the compound represented by the above chemical formula 5 may be tert-butyliminotris(diethylamino)tantalum (TBTDET), tert-butyliminotris(dimethylamino)tantalum (TBTDMT), tert-butyliminotris(ethylmethylamino)tantalum (TBTEMT), ethyliminotris(diethylamino)tantalum (EITDET), ethyliminotris(dimethylamino)tantalum (EITDMT), ethyliminotris(ethylmethylamino)tantalum (EITEMT), tert-amyltris(dimethylamino)tantalum (TAIMAT), tert-amyliminotris(diethylamino)tantalum, penta(dimethylamino)tantalum, tert-amyliminotris(ethylmethylamino)tantalum, bis(tert-butylimino)bis(dimethylamino)tungsten (BTBMW), bis(tert-butylimino)bis(diethylamino)tungsten or bis(tert-butylimino)bis(ethylmethylamino)tungsten, but is not limited thereto.

[0044] In a preferred embodiment of the present invention, the thin film deposition precursor may include a compound represented by the following Chemical Formula 2-1.

[0045] [Chemical formula 2-1]

[0046]

[0047] In the above chemical formula 2-1, R 3 and R 4 Each is independently a C1-C12 straight-chain alkyl group or a C3-C12 branched-chain alkyl group.

[0048] In a preferred embodiment of the present invention, the relative reactants may include one or more selected from deionized water and hydrogen peroxide (H2O2).

[0049] In a preferred embodiment of the present invention, the above-mentioned area selective atomic layer deposition method may be cycled for about 2 to about 100 times.

[0050] In a preferred embodiment of the present invention, in the above-mentioned area selective atomic layer deposition method, each cycle can form a layer with a thickness of about to about At this time, preferably, the film can be a hafnium oxide film.

[0051] In a preferred embodiment of the present invention, in the above-mentioned area selective atomic layer deposition method, each cycle can form a layer with a thickness of about to about At this time, preferably, the film can be a hafnium oxide film.

[0052] In a preferred embodiment of the present invention, in the above-mentioned area selective atomic layer deposition method, a layer with a thickness of about to about At this time, preferably, the film can be a hafnium oxide film.

[0053] On the other hand, the substrate for selectively forming a thin film of the present invention may include: a substrate in which a first substrate including a metal, a second substrate including silicon dioxide, and a third substrate including a nitride are arranged in parallel and integrated; and a thin film formed on the surface of the above-mentioned substrate. At this time, the metal of the first substrate may be selected from the group consisting of copper, cobalt, ruthenium, molybdenum and tungsten, preferably, it may be copper. In addition, the nitride of the third substrate according to the present invention may be selected from the group consisting of titanium nitride, molybdenum nitride, tungsten nitride and silicon nitride, preferably, it may be titanium nitride. In addition, the thin film formed on the surface of the substrate may be a thin film selected from the group consisting of metals, metal oxides and silicon dielectric materials, preferably, it may be a hafnium oxide thin film.

[0054] In a preferred embodiment of the present invention, the alkylthio group may be adsorbed on the surface of the first substrate.

[0055] In a preferred embodiment of the present invention, the alkylthio group may be an ethylthio group.

[0056] In a preferred embodiment of the present invention, the alkyl group may be adsorbed on the surface of the second substrate.

[0057] In a preferred embodiment of the present invention, the alkyl group may be an ethyl group.

[0058] In a preferred embodiment of the present invention, in the substrate for selectively forming a thin film of the present invention, the thickness of the thin film formed on the surface of the first substrate, the thickness of the thin film formed on the surface of the second substrate, and the thickness of the thin film formed on the surface of the third substrate may be different.

[0059] In a preferred embodiment of the present invention, the substrate for selectively forming a thin film of the present invention can satisfy the following condition (1).

[0060] (1)A <B<C

[0061] In the above condition (1), A represents the thickness of the thin film formed on the surface of the first substrate, B represents the thickness of the thin film formed on the surface of the second substrate, and C represents the thickness of the thin film formed on the surface of the third substrate.

[0062] Effects of the Invention

[0063] The method for selectively depositing a thin film using the area selective atomic layer deposition method of the present invention can form thin films having different thicknesses on surfaces of three or more substrates, ie, a substrate including a metal, a substrate including silicon dioxide, and a substrate including a nitride. BRIEF DESCRIPTION OF THE DRAWINGS

[0064] Figure 1 A schematic diagram showing that when a substrate is exposed to an organic thiol small molecule inhibitor in the second step of the method for selectively depositing a thin film using an area selective atomic layer deposition method, a dissociated organic thiol small molecule inhibitor is adsorbed on the surface of a substrate.

[0065] Figure 2 1 is a schematic diagram showing that hafnium oxide thin films having different thicknesses are formed on a surface of a substrate by area selective atomic layer deposition in a third step of a method for selectively depositing a thin film using area selective atomic layer deposition.

[0066] Figure 3 The graph shows the measurement results of the water contact angle of each of the copper substrate, the silicon dioxide substrate and the titanium nitride (TiN) substrate exposed to the organic thiol small molecule inhibitor in Preparation Examples 1 to 3 according to the exposure time (DES Exposure Time) of the organic thiol small molecule inhibitor.

[0067] Figure 4 The figure shows the S-2p XPS spectrum obtained by performing X-ray photoelectron spectroscopy (XPS) analysis on each of the copper substrate, silicon dioxide substrate and titanium nitride substrate exposed to the organic thiol small molecule inhibitor in Preparation Examples 1 to Preparation Examples 3 while maintaining the internal temperature of the chamber at 400°C.

[0068] Figure 5 This is a graph showing S-2p XPS spectra obtained by XPS analysis of the copper substrate exposed to the organic thiol small molecule inhibitor in the state where the chamber internal temperature was maintained at 200° C. and 300° C. in Preparation Example 1.

[0069] Figure 6A chart showing Fourier transform infrared spectroscopy (FT-IR) analysis of each of a silica substrate (=DES / SiO2) exposed to an organic thiol small molecule inhibitor for 30 seconds while maintaining the internal temperature of the chamber at 400°C in Preparation Example 2 and a silica substrate (=Bare SiO2) not exposed to the organic thiol small molecule inhibitor.

[0070] Figure 7 Schematic diagram showing the adsorption mechanism of organothiol small molecule inhibitor (DES) on the surface of silica substrate.

[0071] Figure 8 The graphs show the measurements of the homogeneous selectivity according to the number of cycles of the area selective atomic layer deposition method between the copper substrate in Comparative Example 1 and the copper substrate in Example 1, between the silicon dioxide substrate in Comparative Example 2 and the silicon dioxide substrate in Example 2, and between the titanium nitride substrate in Comparative Example 3 and the titanium nitride substrate in Example 3.

[0072] Fig. 9 The graphs show the measurements of the heterogeneous selectivity between the copper substrate in Example 1 and the silicon dioxide substrate in Example 2, between the silicon dioxide substrate in Example 2 and the titanium nitride substrate in Example 3, and between the titanium nitride substrate in Example 3 and the copper substrate in Example 1 according to the number of cycles of the area selective atomic layer deposition method.

[0073] Fig.10 A graph showing the thickness of the hafnium oxide film formed on the copper substrate in Example 1, the thickness of the hafnium oxide film formed on the silicon dioxide substrate in Example 2, and the thickness of the hafnium oxide film formed on the titanium nitride substrate in Example 3, respectively, according to the number of cycles of the area selective atomic layer deposition method.

[0074] Fig.11 The chart shows the analysis using field-emission scanning electron microscopy (FE-SEM) on the titanium nitride substrate with a silicon dioxide pattern formed in Preparation Example 1, the titanium nitride substrate with a silicon dioxide pattern formed in Comparative Preparation Example 1, the titanium nitride substrate with a copper pattern formed in Preparation Example 2, and the titanium nitride substrate with a copper pattern formed in Comparative Preparation Example 2.

[0075] Fig.12This is a graph showing analysis of the titanium nitride substrate on which the silicon dioxide-copper pattern was formed in Preparation Example 3 by Auger electron spectroscopy (AES). DETAILED DESCRIPTION

[0076] Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings so that a person skilled in the art can easily implement the present invention. The present invention can be implemented in a variety of different embodiments and is not limited to the embodiments described in this specification. Throughout the specification, the same or similar structural elements are given the same reference numerals.

[0077] In the present specification, the term "substantially free of" is defined as a content of less than 0.001 weight % (wt%) and including 0.000 weight % (wt%). In addition, the term "free of" means 0.000 weight %.

[0078] In the present specification, the term "about" is intended to correspond to ±5% of the defined figure.

[0079] The method for selectively depositing a thin film using the area selective atomic layer deposition method of the present invention includes first to third steps.

[0080] First, in the first step of the method for selective deposition of a thin film using the area selective atomic layer deposition method of the present invention, a substrate is prepared in which the first substrate, the second substrate and the third substrate are arranged in parallel and integrated. At this time, the first substrate, the second substrate and the third substrate can be substrates containing different materials, the first substrate can include a metal, preferably, a metal selected from the group consisting of copper, cobalt, ruthenium, molybdenum and tungsten, and particularly preferably, copper, the second substrate can include silicon dioxide, and the third substrate can include a nitride, preferably, a nitride selected from the group consisting of titanium nitride, molybdenum nitride, tungsten nitride and silicon nitride, and particularly preferably, titanium nitride.

[0081] Next, in the second step of the method for selectively depositing a thin film using the area selective atomic layer deposition method of the present invention, the substrate prepared in the first step may be exposed to an organic thiol small molecule inhibitor.

[0082] At this time, the organic thiol small molecule inhibitor may include a compound represented by Chemical Formula 1 below.

[0083] [Chemical formula 1]

[0084]

[0085] In the above chemical formula 1, R 1 and R 2Each is independently a C1-C12 straight-chain alkyl group, a C3-C12 branched-chain alkyl group or a C6-C12 aryl group, preferably a C1-C12 straight-chain alkyl group, and more preferably a C1-C3 straight-chain alkyl group.

[0086] In addition, the weight average molecular weight of the organic mercaptan low molecular weight inhibitor may be about 300 or less, preferably, about 30 to about 150, and more preferably, about 60 to about 95.

[0087] Specifically, refer to Figure 1 The second step of the method for selectively depositing a thin film using the area selective atomic layer deposition method of the present invention may include steps 2-1 to 2-3.

[0088] First, in step 2-1 of the method for selective deposition of a thin film using the area selective atomic layer deposition method of the present invention, after drying the substrate prepared in the first step, the substrate can be placed in a chamber having an internal temperature of about 300° C. to about 500° C., preferably about 350° C. to about 450° C. and having a vacuum minimum pressure condition and maintained for about 1 minute to about 20 minutes, preferably, about 5 minutes to about 15 minutes. If the internal temperature is lower than about 300° C., there may be problems with the adsorption of the organic thiol small molecule inhibitor, and if the internal temperature exceeds about 500° C., there may be problems with the desorption and decomposition of the organic thiol small molecule inhibitor.

[0089] Secondly, in step 2-2 of the method for selective deposition of a thin film using the area selective atomic layer deposition method of the present invention, the chamber can be purged to maintain the internal temperature of the chamber at about 200°C to about 500°C, preferably about 350°C to about 450°C, and more preferably about 390°C to about 410°C. In this state, the organic thiol small molecule inhibitor is put into the chamber to expose the substrate to the organic thiol small molecule inhibitor for about 1 second to about 100 seconds, preferably about 30 seconds to about 90 seconds, and more preferably about 30 seconds to about 60 seconds. If the internal temperature is lower than about 200°C, the problem of low adsorption efficiency of the organic thiol small molecule inhibitor may occur, and if the internal temperature exceeds about 500°C, the problem of desorption and decomposition of the organic thiol small molecule inhibitor may occur.

[0090] Finally, in step 2-3 of the method for selective deposition of a thin film using area selective atomic layer deposition, the substrate exposed to the organic thiol small molecule inhibitor in step 2-2 can be cooled to a temperature of about 15°C to about 35°C, preferably about 20°C to about 30°C.

[0091] On the other hand, in the second step of the method for selectively depositing a thin film using area selective atomic layer deposition of the present invention, the water contact angle of the first substrate surface exposed to the organic thiol small molecule inhibitor may be about 90° to about 100°.

[0092] Also, in the second step of the method for selectively depositing a thin film using area selective atomic layer deposition of the present invention, the water contact angle of the second substrate surface exposed to the organic thiol small molecule inhibitor may be about 70° to about 80°.

[0093] In addition, in step 2-2 of the thin film selective deposition method of the area selective atomic layer deposition method of the present invention, the organic thiol small molecule inhibitor introduced into the chamber undergoes thermal dissociation and is separated into alkylthio groups and alkyl groups, respectively. The alkylthio groups can be adsorbed on the surface of the first substrate, and the alkyl groups can be adsorbed on the surface of the second substrate. Specifically, the alkylthio groups can be ethylthio groups, and the alkyl groups can be ethyl groups.

[0094] Finally, in the third step of the thin film selective deposition method of the area selective atomic layer deposition method of the present invention, a thin film may be formed on the substrate surface exposed to the organic thiol small molecule inhibitor in the second step using area selective atomic layer deposition.

[0095] At this time, the thickness of the thin film formed on the surface of the first substrate, the thickness of the thin film formed on the surface of the second substrate, and the thickness of the thin film formed on the surface of the third substrate may be different, and preferably, the following condition (1) may be satisfied.

[0096] (1)A <B<C

[0097] In the above condition (1), A represents the thickness of the thin film formed on the surface of the first substrate, B represents the thickness of the thin film formed on the surface of the second substrate, and C represents the thickness of the thin film formed on the surface of the third substrate.

[0098] Specifically, refer to Figure 2 To explain, the third step of the thin film selective deposition method of the area selective atomic layer deposition method of the present invention may include step 3-1 and step 3-2.

[0099] First, in step 3-1 of the method for selective deposition of a thin film using the area selective atomic layer deposition method of the present invention, the substrate exposed to the organic thiol small molecule inhibitor in the second step can be put into a chamber and heated at about 200° C. to about 350° C., preferably about 250° C. to about 300° C. If the temperature of the substrate exposed to the organic thiol small molecule inhibitor is lower than about 200° C., the adsorption efficiency of the organic thiol small molecule inhibitor may be low, and if the temperature of the substrate exceeds about 350° C., the organic thiol small molecule inhibitor may be decomposed.

[0100] Secondly, in step 3-2 of the method for selective deposition of a thin film using the regional selective atomic layer deposition method of the present invention, the regional selective atomic layer deposition method can be carried out by placing a precursor for thin film deposition into the above-mentioned chamber and exposing it for about 1 second to about 10 seconds, preferably about 2 seconds to about 6 seconds, and then purging it for about 50 seconds to about 70 seconds, preferably about 55 seconds to about 65 seconds, placing a relative reactant into the chamber and exposing it for about 1 second to about 5 seconds, preferably about 1 second to about 3 seconds, and then purging it for about 50 seconds to about 70 seconds, preferably about 55 seconds to about 65 seconds.

[0101] The thin film deposition precursor may include one or more selected from the group consisting of a compound represented by the following Chemical Formula 2, a compound represented by the following Chemical Formula 3, a compound represented by the following Chemical Formula 4, and a compound represented by the following Chemical Formula 5.

[0102] [Chemical formula 2]

[0103] (L1) n M(NR 3 R 4 ) 4-n

[0104] In the above chemical formula 2, L1 is a ligand selected from the group consisting of cyclopentadienyl and C1-C12 alkyl-substituted cyclopentadienyl, M is a metal selected from the group consisting of titanium, hafnium and zirconium, and R 3 and R 4 Each is independently a C1-C12 straight-chain alkyl group or a C3-C12 branched-chain alkyl group, and n is 0, 1 or 2.

[0105] [Chemical formula 3]

[0106] R 5 m M(OR 6 ) 3-m

[0107] In the above chemical formula 3, M is a metal selected from the group consisting of aluminum, hafnium and zirconium, and R 5 and R 6 Each is independently a C1-C12 straight-chain alkyl group or a C3-C12 branched-chain alkyl group, and m is 1 to 3.

[0108] [Chemical formula 4]

[0109] (L2)pMR7(OR 8 ) 3-p

[0110] In the above chemical formula 4, L2 is a ligand selected from the group consisting of cyclopentadienyl and C1-C12 alkyl-substituted cyclopentadienyl, M is a metal selected from the group consisting of titanium, hafnium and zirconium, R 7 and R8 Each is independently a C1-C12 straight-chain alkyl group or a C3-C12 branched-chain alkyl group, and p is 1 or 2.

[0111] [Chemical formula 5]

[0112] (R 9 N) q M(NR 10 R 11 ) 4-q

[0113] In the above chemical formula 5, M is a metal selected from the group consisting of vanadium, niobium, tantalum, molybdenum and tungsten, and R 9 , R 10 and R 11 Each is independently a C1-C12 straight-chain alkyl group or a C3-C12 branched-chain alkyl group, and q is 1 or 2.

[0114] Specifically, the compound represented by the above Chemical Formula 2 may be tetrakis(dimethylamino)hafnium (TDMAH), tetrakis(diethylamino)hafnium (TDEAH), tetrakis(ethylmethylamino)hafnium (TEMAH), cyclopentadienyltris(dimethylamino)hafnium (CpHf(NMe2)3), methylcyclopentadienyltris(dimethylamino)hafnium ((MeCp)Hf(NMe2)3), ethylcyclopentadienyltris(dimethylamino)hafnium ((EtCp)Hf(NMe2)3), (n-propylcyclopentadienyl)tris(dimethylamino)hafnium ((n- PrCp)Hf(NMe2)3), cyclopentadienyl tris(methylethylamino) hafnium (CpHf(NMeEt)3), methylcyclopentadienyl tris(methylethylamino) hafnium ((MeCp)Hf(NMeEt)3), ethylcyclopentadienyl tris(methylethylamino) hafnium ((EtCp)Hf(NMeEt)3), cyclopentadienyl tris(diethylamino) hafnium (CpHf(NEt2)3, methylcyclopentadienyl tris(diethylamino) hafnium ((MeCp)Hf(NEt2)3), ethylcyclopentadienyl tris(diethylamino) hafnium ((EtCp)Hf(NMeEt)3), tCp)Hf(NEt2)3), bis(cyclopentadienyl)bis(dimethylamino)hafnium (Cp2Hf(NMe2)2), bis(methylcyclopentadienyl)bis(dimethylamino)hafnium ((MeCp)2Hf(NMe2)2), bis(ethylcyclopentadienyl)bis(dimethylamino)hafnium ((EtCp)2Hf(NMe2)2), bis(cyclopentadienyl)bis(methylethylamino)hafnium (Cp2Hf(NMeEt)2), bis(methylcyclopentadienyl)bis(methylethylamino)hafnium ((MeCp)2Hf(NMeEt)2) , bis(ethylcyclopentadienyl)bis(methylethylamino)hafnium ((EtCp)2Hf(NMeEt)2), bis(cyclopentadienyl)bis(diethylamino)hafnium (Cp2Hf(NEt2)2), bis(methylcyclopentadienyl)bis(diethylamino)hafnium ((MeCp)2Hf(NEt2)3), bis(ethylcyclopentadienyl)bis(diethylamino)hafnium ((EtCp)2Hf(NEt2)2) or (n-propylcyclopentadienyl)tris(dimethylamino)zirconium ((n-PrCp)Zr(NMe2)3), but are not limited thereto.

[0115] And, specifically, the compound represented by the above Chemical Formula 3 may be trimethylaluminum, triethylaluminum, dimethylaluminum isopropoxide, or diethylaluminum isopropoxide, but is not limited thereto.

[0116] And, specifically, the compound represented by the above Chemical Formula 4 may be CpHfMe(OMe)2, CpZrMe(OMe)2, (MeCp)HfMe(OMe)2, (MeCp)ZrMe(OMe)2, (EtCp)HfMe(OMe)2 or (EtCp)ZrMe(OMe), but is not limited thereto.

[0117] Furthermore, the compound represented by the above Chemical Formula 5 may be tert-butyliminotris(diethylamino)tantalum (TBTDET), tert-butyliminotris(dimethylamino)tantalum (TBTDMT), tert-butyliminotris(ethylmethylamino)tantalum (TBTEMT), ethyliminotris(diethylamino)tantalum (EITDET), ethyliminotris(dimethylamino)tantalum (EITDMT), ethyliminotris(ethylmethylamino)tantalum (EITEMT), tert-amyltris(dimethylamino)tantalum (TAIMAT), tert-amyliminotris(diethylamino)tantalum, penta(dimethylamino)tantalum, tert-amyliminotris(ethylmethylamino)tantalum, bis(tert-butylimino)bis(dimethylamino)tungsten (BTBMW), bis(tert-butylimino)bis(diethylamino)tungsten or bis(tert-butylimino)bis(ethylmethylamino)tungsten, but is not limited thereto.

[0118] Most preferably, the thin film deposition precursor may include a compound represented by the following Chemical Formula 2-1.

[0119] [Chemical formula 2-1]

[0120]

[0121] In the above chemical formula 2-1, R 3 and R 4 Each is independently a C1-C12 straight-chain alkyl group or a C3-C12 branched-chain alkyl group, preferably a C1-C12 straight-chain alkyl group, and more preferably a C1-C3 straight-chain alkyl group.

[0122] Furthermore, the relative reactant may include one or more selected from deionized water and hydrogen peroxide, and preferably, may include deionized water.

[0123] On the other hand, the cycle of the area selective atomic layer deposition method can be performed about 2 times to about 100 times, preferably about 10 times to about 25 times, and more preferably about 10 times to about 15 times.

[0124] In addition, in the area selective atomic layer deposition method, each cycle can form a layer with a thickness of about to about Preferred about to about of film.

[0125] In addition, in the area selective atomic layer deposition method, each cycle can form a layer with a thickness of about to about Preferred about to about of film.

[0126] In addition, in the area selective atomic layer deposition method, a layer with a thickness of about to about Preferred about to about of film.

[0127] On the other hand, the thin film formed on the surface of the substrate may be a thin film selected from the group consisting of metal, metal oxide and silicon dielectric material, and preferably, may be a hafnium oxide thin film.

[0128] Furthermore, the substrate for selectively forming a thin film of the present invention may include: a substrate in which a first substrate including a metal, a second substrate including silicon dioxide, and a third substrate including a nitride are arranged in parallel and integrated; and a thin film formed on the surface of the above substrate. In this case, an alkylthio group may be adsorbed on the surface of the first substrate, preferably, an ethylthio group may be adsorbed on the surface of the first substrate. In addition, an alkyl group may be adsorbed on the surface of the second substrate, preferably, an ethyl group may be adsorbed on the surface of the second substrate.

[0129] On the other hand, the metal of the first substrate may be selected from the group consisting of copper, cobalt, ruthenium, molybdenum and tungsten, and preferably, may be copper.

[0130] In addition, the nitride of the third substrate according to the present invention may be selected from the group consisting of titanium nitride, molybdenum nitride, tungsten nitride and silicon nitride, and preferably may be titanium nitride.

[0131] In addition, the thin film formed on the surface of the substrate may be a thin film selected from the group consisting of metal, metal oxide and silicon dielectric material, and preferably, may be a hafnium oxide thin film.

[0132] Furthermore, in the substrate for selectively forming a thin film of the present invention, the thickness of the thin film formed on the surface of the first substrate, the thickness of the thin film formed on the surface of the second substrate, and the thickness of the thin film formed on the surface of the third substrate may be different, and preferably, the following condition (1) may be satisfied.

[0133] (1)A <B<C

[0134] In the above condition (1), A represents the thickness of the thin film formed on the surface of the first substrate, B represents the thickness of the thin film formed on the surface of the second substrate, and C represents the thickness of the thin film formed on the surface of the third substrate.

[0135] The present invention has been described above with examples as the center, but this is only an example and does not limit the examples of the present invention. A person skilled in the art of the present invention should understand that the present invention can be subjected to various deformations and applications not illustrated in the above description within the scope of the essential characteristics of the present invention. For example, the various structural elements specifically shown in the examples of the present invention can be changed to implement the invention. Moreover, the differences related to such deformations and applications should be interpreted as belonging to the scope of the present invention specified in the scope of the invention claims.

[0136] Preparation Example 1: Exposure of Copper Substrate to Organothiol Small Molecule Inhibitor

[0137] (1) The copper substrate was ultrasonically cleaned for 10 minutes using acetone, isopropyl alcohol, and deionized water in that order.

[0138] (2) After drying the cleaned copper substrate with nitrogen (N2 gas), the substrate was placed in a chamber with an internal temperature of 400° C. and a minimum vacuum pressure condition and maintained for 10 minutes.

[0139] (3) A stainless-steel canister was prepared which was kept at an internal temperature of 25° C. and stored an organic thiol small molecule inhibitor. At this time, a compound represented by the following Chemical Formula 1 was used as the organic thiol small molecule inhibitor.

[0140] [Chemical formula 1]

[0141]

[0142] In the above chemical formula 1, R 1 and R 2 It is ethyl.

[0143] (4) The stainless steel tank and the substrate are connected so that the copper substrate is exposed to the compound represented by the above Chemical Formula 1.

[0144] (5) The chamber was purged with nitrogen gas, and the copper substrate was exposed to the compound represented by the chemical formula 1 for 0 seconds, 15 seconds, 30 seconds, 60 seconds, and 90 seconds, respectively, while the temperature inside the chamber was maintained at 200° C., 300° C., and 400° C., respectively.

[0145] (6) The copper substrate exposed to the compound represented by the above Chemical Formula 1 was cooled to a temperature of 25°C.

[0146] Preparation Example 2: Exposure of Silica Substrate to Organothiol Small Molecule Inhibitor

[0147] (1) The silicon dioxide substrate was ultrasonically cleaned for 10 minutes using acetone, isopropyl alcohol, and deionized water in that order.

[0148] (2) After the cleaned silicon dioxide substrate was dried with nitrogen gas, the substrate was placed in a chamber having an internal temperature of 400° C. and a vacuum minimum pressure condition and maintained therein for 10 minutes.

[0149] (3) A stainless steel tank was prepared for storing an organic thiol small molecule inhibitor at an internal temperature of 25° C. At this time, a compound represented by the following Chemical Formula 1 was used as the organic thiol small molecule inhibitor.

[0150] [Chemical formula 1]

[0151]

[0152] In the above chemical formula 1, R 1 and R 2 It is ethyl.

[0153] (4) The stainless steel tank and the substrate are connected so that the silicon dioxide substrate is exposed to the compound represented by the chemical formula 1.

[0154] (5) The chamber was purged with nitrogen gas, and the silicon dioxide substrate was exposed to the compound represented by the chemical formula 1 for 0 seconds, 15 seconds, 30 seconds, 60 seconds, and 90 seconds, respectively, while the temperature inside the chamber was maintained at 200° C., 300° C., and 400° C., respectively.

[0155] (6) The silicon dioxide substrate exposed to the compound represented by the above Chemical Formula 1 was cooled to a temperature of 25°C.

[0156] Preparation Example 3: Exposure of Titanium Nitride Substrate to Organic Thiol Small Molecule Inhibitor

[0157] (1) The titanium nitride substrate was ultrasonically cleaned for 10 minutes using acetone, isopropanol, and deionized water in that order.

[0158] (2) After the cleaned titanium nitride substrate was dried with nitrogen gas, the substrate was placed in a chamber with an internal temperature of 400° C. and a vacuum minimum pressure condition and maintained for 10 minutes.

[0159] (3) A stainless steel tank was prepared which was kept at an internal temperature of 25° C. and stored an organic thiol small molecule inhibitor. At this time, a compound represented by the following Chemical Formula 1 was used as the organic thiol small molecule inhibitor.

[0160] [Chemical formula 1]

[0161]

[0162] In the above chemical formula 1, R1 and R 2 It is ethyl.

[0163] (4) The stainless steel tank and the substrate are connected to expose the titanium nitride substrate to the compound represented by the chemical formula 1.

[0164] (5) The chamber was purged with nitrogen gas, and the titanium nitride substrate was exposed to the compound represented by the chemical formula 1 for 0 seconds, 15 seconds, 30 seconds, 60 seconds, and 90 seconds, respectively, while the temperature inside the chamber was maintained at 200° C., 300° C., and 400° C., respectively.

[0165] (6) The titanium nitride substrate exposed to the compound represented by the above Chemical Formula 1 was cooled to a temperature of 25°C.

[0166] Experimental Example 1: Water contact angle measurement

[0167] The water contact angle of each of the copper substrate, silicon dioxide substrate and titanium nitride substrate exposed to the organic thiol small molecule inhibitor in Preparation Examples 1 to 3 was measured, and the results are as follows: Figure 3 Specifically, Figure 3 The left graph shows the water contact angle of the copper substrate of Preparation Example 1 according to the exposure time of the organic thiol small molecule inhibitor. Figure 3 The middle graph shows the water contact angle of the silicon dioxide substrate of Preparation Example 2 according to the exposure time of the organic thiol small molecule inhibitor. Figure 3 The right graph of FIG. 3 shows the water contact angle of the titanium nitride substrate of Preparation Example 3 according to the exposure time of the organic thiol small molecule inhibitor. In addition, the water contact angle was measured using a contact angle meter (SDL200TEZD, Femtobiomed Co., Ltd.), using deionized water as the measurement source, and the droplet size was limited to 100 μm during the measurement.

[0168] from Figure 3It can be confirmed from the left graph that the water contact angle on the surface of the copper substrate gradually increases from 55°. In addition, it can be confirmed that the copper substrate exposed to the organic thiol small molecule inhibitor while maintaining the internal temperature of the chamber at 200°C increases with the exposure time of the organic thiol small molecule inhibitor, and reaches a saturated state at a water contact angle of about 75°. In addition, it can be confirmed that the copper substrate exposed to the organic thiol small molecule inhibitor while maintaining the internal temperature of the chamber at 300°C increases the water contact angle from 55° to about 68° after being exposed to the organic thiol small molecule inhibitor for 15 seconds, and reaches a saturated state at a water contact angle of about 80° after being exposed to the organic thiol small molecule inhibitor for 60 seconds. In addition, it can be confirmed that the copper substrate exposed to the organic thiol small molecule inhibitor while maintaining the internal temperature of the chamber at 400°C increases the water contact angle from 55° to about 95° after being exposed to the organic thiol small molecule inhibitor for 15 seconds, and reaches a saturated state at a water contact angle of about 98° after being exposed to the organic thiol small molecule inhibitor for 30 seconds. These results confirm that the gradual increase in the water contact angle of the copper substrate at chamber internal temperatures of 200°C and 300°C is due to the limited adsorption of the organic thiol small molecule inhibitor at low temperatures.

[0169] from Figure 3 In the middle graph of , it can be confirmed that the water contact angle of the silica substrate exposed to the organic thiol small molecule inhibitor increased from 44° to about 55° after 30 seconds of exposure to the organic thiol small molecule inhibitor while the internal temperature of the chamber was maintained at 200°C, and reached a saturation state at a water contact angle of about 62° after 60 seconds of exposure to the organic thiol small molecule inhibitor. In addition, it can be confirmed that the water contact angle of the silica substrate exposed to the organic thiol small molecule inhibitor increased from 44° to about 65° after 30 seconds of exposure to the organic thiol small molecule inhibitor, reaching a saturation state. In addition, it can be confirmed that the water contact angle of the silica substrate exposed to the organic thiol small molecule inhibitor increased from 44° to about 76° after 15 seconds of exposure to the organic thiol small molecule inhibitor while the internal temperature of the chamber was maintained at 400°C, and reached a saturation state at a water contact angle of about 80° after 30 seconds of exposure to the organic thiol small molecule inhibitor.

[0170] from Figure 3 As can be seen from the right graph of the results, no significant increase in the water contact angle was observed for the titanium nitride substrate exposed to the organic thiol small molecule inhibitor while the chamber internal temperature was maintained at 300°C and 400°C, respectively, even when the exposure time to the organic thiol small molecule inhibitor increased. These results confirm that the organic thiol small molecule inhibitor cannot change the surface properties of the titanium nitride substrate.

[0171] Experimental Example 2: XPS Analysis

[0172] X-ray photoelectron spectroscopy (XPS) analysis was performed on each of the copper substrate (exposed for 30 seconds), silicon dioxide substrate (exposed for 30 seconds), and titanium nitride substrate (exposed for 30 seconds) exposed to the organic thiol small molecule inhibitor in the state where the internal temperature of the chamber was maintained at 400° C. in Preparation Examples 1 to 3. The results are as follows: Figure 4 Specifically, in order to confirm the presence of small molecule inhibitors of organic thiol on copper substrates, silicon dioxide substrates and titanium nitride substrates, the S-2p peak was confirmed. Figure 4 The left graph of shows the S-2p XPS spectrum of the copper substrate exposed to the organic thiol small molecule inhibitor in the state where the internal temperature of the chamber is maintained at 400° C. in Preparation Example 1. Figure 4 The middle graph of shows the S-2p XPS spectrum of the silicon dioxide substrate exposed to the organic thiol small molecule inhibitor while the chamber internal temperature was maintained at 400° C. in Preparation Example 2. Figure 4 The right graph of shows the S-2p XPS spectrum of the titanium nitride substrate exposed to the organic thiol small molecule inhibitor while the chamber internal temperature was maintained at 400° C. in Preparation Example 3. In addition, XPS analysis was performed by an XPS system (PHI-5000Versa Probe II, ULVAC, Physical Electronics Co., Ltd.) using monochromatic Al Kα rays as a source.

[0173] from Figure 4 It can be confirmed in the left graph that the S-2p peak is clearly observed in the S-2p XPS spectrum of the copper substrate exposed to the organic thiol small molecule inhibitor while maintaining the internal temperature of the chamber at 400°C in Preparation Example 1. Specifically, a core electron peak can be confirmed in the S-2p region. The S-2p peak is in the range of 159eV to 164eV. After deconvolution of the S-2p peak, two chemical bonds of S-2p can be confirmed, including the S2p at 161.0eV. 3 / 2 and S2p of 162.5 eV 1 / 2 The binding energy of is equivalent to the spin-orbit splitting of sulfur, that is, it represents the interaction between sulfur and carbon. It is judged that the S-2p peak confirms that the thiol group of the organic thiol small molecule inhibitor is adsorbed on the surface of the copper substrate. At high temperatures, the organic thiol small molecule inhibitor undergoes thermal dissociation and separates into ethylthio groups. Due to the alkalinity of the copper substrate, only the acidic ethylthio group can be adsorbed on the copper substrate. In short, it can be confirmed that the ethylthio group is adsorbed and bound to the copper substrate exposed to the organic thiol small molecule inhibitor in the state where the internal temperature of the chamber is maintained at 400°C in Preparation Example 1. On the other hand, it can be confirmed that the ethylthio group makes the surface of the copper substrate hydrophobic by adsorption, thereby passivating the surface of the copper substrate.

[0174] And, from Figure 4 As can be confirmed from the left graph of , the XPS spectrum of the copper substrate exposed to the organic thiol small molecule inhibitor while the chamber internal temperature was maintained at 400° C. in Preparation Example 1 shows that there is no sulfur oxide such as sulfonate having a binding energy higher than 166 eV.

[0175] from Figure 4 It can be confirmed from the middle graph that no S-2p characteristic peak is observed in the S-2p XPS spectrum of the silica substrate exposed to the organic thiol small molecule inhibitor while maintaining the internal temperature of the chamber at 400°C in Preparation Example 2, which indicates that there is no thiol group on the surface of the silica substrate.

[0176] In addition, from Figure 4 It can be confirmed from the right graph that no S-2p characteristic peak is observed in the S-2p XPS spectrum of the titanium nitride substrate exposed to the organic thiol small molecule inhibitor while maintaining the internal temperature of the chamber at 400°C in Preparation Example 3, which also indicates that there are no thiol groups on the surface of the titanium nitride substrate.

[0177] In addition, the S-2p XPS spectra of the copper substrate exposed to the organic thiol small molecule inhibitor for 30 seconds in the state where the chamber internal temperature was maintained at 200° C. and 300° C. in Preparation Example 1 are as follows: Figure 5 shown.

[0178] from Figure 5 It was confirmed that no S-2p peak was observed in the S-2p XPS spectra of the copper substrates exposed to the organic thiol small molecule inhibitor in Preparation Example 1 while the chamber internal temperature was maintained at 200° C. and 300° C., respectively.

[0179] Experimental Example 3: FT-IR Analysis

[0180] Fourier transform infrared spectroscopy (FT-IR) analysis was performed on each of the silicon dioxide substrate (=DES / SiO2) exposed to the organic thiol small molecule inhibitor for 30 seconds while maintaining the internal temperature of the chamber at 400°C in Preparation Example 2 and the silicon dioxide substrate (=Bare SiO2) not exposed to the organic thiol small molecule inhibitor. The results are as follows: Figure 6 shown.

[0181] In addition, a Bruker spectrometer (VERTEX 80V, HYPERION 2000) was used in the attenuated total reflection (ATR) mode at 8000 cm -1 Up to 800cm -1 The FT-IR absorption spectrum was measured and analyzed at a wave number of .

[0182] from Figure 6 It can be confirmed that in the spectrum of the silica substrate exposed to the organic thiol small molecule inhibitor while the chamber internal temperature was maintained at 400°C in Preparation Example 2, the 2975 cm-1 wavelength indicating the presence of CH stretching vibration (CH stretching) -1 There is a peak at 945 cm, which indicates the existence of CH bending vibration. -1 The above two peaks are peaks not observed in the silica substrate that was not exposed to the organic thiol small molecule inhibitor, indicating that alkyl groups exist on the surface of the silica substrate exposed to the organic thiol small molecule inhibitor while the chamber internal temperature was maintained at 400°C in Preparation Example 2. From the above results, it can be confirmed that the organic thiol small molecule inhibitor is thermally dissociated and separated into ethyl groups at high temperatures, and the separated ethyl groups are adsorbed and bonded to the surface of the silica substrate.

[0183] on the other hand, Figure 7 The adsorption mechanism of the organic thiol small molecule inhibitor on the surface of the silica substrate is shown, which shows that when the silica substrate is exposed to the organic thiol small molecule inhibitor while the temperature inside the high-temperature chamber is maintained at 400°C, the organic thiol small molecule inhibitor is thermally dissociated and separated into ethylthio and ethyl groups, and the dissociated ethyl groups are adsorbed to -OH groups present on the surface of the silica substrate.

[0184] Example 1: Formation of a hafnium oxide film on a copper substrate exposed to an organic thiol small molecule inhibitor

[0185] A hafnium oxide thin film was formed on the copper substrate exposed to an organic thiol small molecule inhibitor for 30 seconds while the chamber internal temperature was maintained at 400° C. in Preparation Example 1 by using an area selective atomic layer deposition method. In the area selective atomic layer deposition method, a compound represented by the following chemical formula 2-1 was used as a precursor for thin film deposition, and deionized water was used as a relative reactant.

[0186] [Chemical formula 2-1]

[0187]

[0188] In the above chemical formula 2-1, R 3 and R 4 It is methyl.

[0189] Specifically, a stainless steel tank with an internal temperature of 50° C. and storing a precursor for thin film deposition and a glass tank with an internal temperature of 22° C. and storing a relative reactant were connected to a chamber including a copper substrate, and the area selective atomic layer deposition method was performed while the copper substrate was heated to 275° C. In addition, in the area selective atomic layer deposition method, nitrogen gas was used for purging at a flow rate of 10 sccm and controlled by a mass flow controller (MFC).

[0190] On the other hand, the area selective atomic layer deposition method is performed by introducing a precursor for thin film deposition into a chamber including a copper substrate, exposing for 4 seconds, purging for 60 seconds, and then introducing a relative reactant into a chamber including a copper substrate, exposing for 2 seconds, and purging for 60 seconds in a cycle.

[0191] Furthermore, the cycle of the area selective atomic layer deposition method was performed 2 times, 10 times, 25 times, 50 times and 100 times respectively.

[0192] Example 2: Formation of a hafnium oxide film on a silicon dioxide substrate exposed to an organic thiol small molecule inhibitor

[0193] A hafnium oxide thin film was formed on a silicon dioxide substrate exposed to an organic thiol small molecule inhibitor for 30 seconds while maintaining the internal temperature of the chamber at 400° C. in Preparation Example 2 by using a regioselective atomic layer deposition method. In the regioselective atomic layer deposition method, a compound represented by the following chemical formula 2-1 was used as a precursor for thin film deposition, and deionized water was used as a relative reactant.

[0194] [Chemical formula 2-1]

[0195]

[0196] In the above chemical formula 2-1, R 3 and R 4 It is methyl.

[0197] Specifically, a stainless steel tank with an internal temperature of 50° C. and storing a precursor for thin film deposition and a glass tank with an internal temperature of 22° C. and storing a relative reactant were connected to a chamber including a silicon dioxide substrate, and the area selective atomic layer deposition method was performed while the silicon dioxide substrate was heated to 275° C. In addition, in the area selective atomic layer deposition method, nitrogen gas was used for purging at a flow rate of 10 sccm and controlled by a mass flow controller.

[0198] On the other hand, area selective atomic layer deposition is performed by introducing a precursor for thin film deposition into a chamber including a silicon dioxide substrate, exposing for 4 seconds, purging for 60 seconds, and then introducing a relative reactant into a chamber including a silicon dioxide substrate, exposing for 2 seconds, and purging for 60 seconds in a cycle.

[0199] Furthermore, the cycle of the area selective atomic layer deposition method was performed 2 times, 10 times, 25 times, 50 times and 100 times respectively.

[0200] Example 3: Formation of a hafnium oxide film on a titanium nitride substrate exposed to an organic thiol small molecule inhibitor

[0201] A hafnium oxide thin film was formed on the titanium nitride substrate exposed to an organic thiol small molecule inhibitor for 30 seconds while the chamber internal temperature was maintained at 400° C. in Preparation Example 3 using the area selective atomic layer deposition method. In the area selective atomic layer deposition method, a compound represented by the following chemical formula 2-1 was used as a precursor for thin film deposition, and deionized water was used as a relative reactant.

[0202] [Chemical formula 2-1]

[0203]

[0204] In the above chemical formula 2-1, R 3 and R 4 It is methyl.

[0205] Specifically, a stainless steel tank with an internal temperature of 50° C. and storing a precursor for thin film deposition and a glass tank with an internal temperature of 22° C. and storing a relative reactant were connected to a chamber including a titanium nitride substrate, and the area selective atomic layer deposition method was performed while the titanium nitride substrate was heated to 275° C. In addition, in the area selective atomic layer deposition method, nitrogen gas was used for purging at a flow rate of 10 sccm and controlled by a mass flow controller.

[0206] On the other hand, area selective atomic layer deposition is performed by introducing a precursor for thin film deposition into a chamber including a titanium nitride substrate, exposing for 4 seconds, purging for 60 seconds, and then introducing a relative reactant into a chamber including a titanium nitride substrate, exposing for 2 seconds, and purging for 60 seconds in a cycle.

[0207] Furthermore, the cycle of the area selective atomic layer deposition method was performed 2 times, 10 times, 25 times, 50 times and 100 times respectively.

[0208] Comparative Example 1: Formation of a hafnium oxide thin film on a copper substrate

[0209] A hafnium oxide thin film was formed on a copper substrate using an area selective atomic layer deposition method, wherein the compound represented by the following chemical formula 2-1 was used as a thin film deposition precursor and deionized water was used as a relative reactant.

[0210] [Chemical formula 2-1]

[0211]

[0212] In the above chemical formula 2-1, R 3 and R 4 It is methyl.

[0213] Specifically, a stainless steel tank with an internal temperature of 50° C. and storing a precursor for thin film deposition and a glass tank with an internal temperature of 22° C. and storing a relative reactant were connected to a chamber including a copper substrate, and the area selective atomic layer deposition method was performed while the copper substrate was heated to 275° C. In addition, in the area selective atomic layer deposition method, nitrogen gas was used for purging at a flow rate of 10 sccm and controlled by a mass flow controller.

[0214] On the other hand, the area selective atomic layer deposition method is performed by introducing a precursor for thin film deposition into a chamber including a copper substrate, exposing for 4 seconds, purging for 60 seconds, and then introducing a relative reactant into a chamber including a copper substrate, exposing for 2 seconds, and purging for 60 seconds in a cycle.

[0215] Furthermore, the cycle of the area selective atomic layer deposition method was performed 2 times, 10 times, 25 times, 50 times and 100 times respectively.

[0216] Comparative Example 2: Formation of a hafnium oxide thin film on a silicon dioxide substrate

[0217] A hafnium oxide thin film is formed on a silicon dioxide substrate by using an area selective atomic layer deposition method, wherein the compound represented by the following chemical formula 2-1 is used as a thin film deposition precursor and deionized water is used as a relative reactant.

[0218] [Chemical formula 2-1]

[0219]

[0220] In the above chemical formula 2-1, R 3 and R 4 It is methyl.

[0221] Specifically, a stainless steel tank with an internal temperature of 50° C. and storing a precursor for thin film deposition and a glass tank with an internal temperature of 22° C. and storing a relative reactant were connected to a chamber including a silicon dioxide substrate, and the area selective atomic layer deposition method was performed while the silicon dioxide substrate was heated to 275° C. In addition, in the area selective atomic layer deposition method, nitrogen gas was used for purging at a flow rate of 10 sccm and controlled by a mass flow controller.

[0222] On the other hand, area selective atomic layer deposition is performed by introducing a precursor for thin film deposition into a chamber including a silicon dioxide substrate, exposing for 4 seconds, purging for 60 seconds, and then introducing a relative reactant into a chamber including a silicon dioxide substrate, exposing for 2 seconds, and purging for 60 seconds in a cycle.

[0223] Furthermore, the cycle of the area selective atomic layer deposition method was performed 2 times, 10 times, 25 times, 50 times and 100 times respectively.

[0224] Comparative Example 3: Formation of a hafnium oxide thin film on a titanium nitride substrate

[0225] A hafnium oxide thin film is formed on a titanium nitride substrate using an area selective atomic layer deposition method, wherein the compound represented by the following chemical formula 2-1 is used as a thin film deposition precursor and deionized water is used as a relative reactant.

[0226] [Chemical formula 2-1]

[0227]

[0228] In the above chemical formula 2-1, R 3 and R 4 It is methyl.

[0229] Specifically, a stainless steel tank with an internal temperature of 50° C. and storing a precursor for thin film deposition and a glass tank with an internal temperature of 22° C. and storing a relative reactant were connected to a chamber including a titanium nitride substrate, and the area selective atomic layer deposition method was performed while the titanium nitride substrate was heated to 275° C. In addition, in the area selective atomic layer deposition method, nitrogen gas was used for purging at a flow rate of 10 sccm and controlled by a mass flow controller.

[0230] On the other hand, area selective atomic layer deposition is performed by introducing a precursor for thin film deposition into a chamber including a titanium nitride substrate, exposing for 4 seconds, purging for 60 seconds, and then introducing a relative reactant into a chamber including a titanium nitride substrate, exposing for 2 seconds, and purging for 60 seconds in a cycle.

[0231] Furthermore, the cycle of the area selective atomic layer deposition method was performed 2 times, 10 times, 25 times, 50 times and 100 times respectively.

[0232] Experimental Example 4: Selective measurement of the number of cycles according to area-selective atomic layer deposition

[0233] The selectivity was calculated by the following Equation 1 based on the difference in atomic concentration between the growth area (GS) and the non-growth area (NGS).

[0234] [Equation 1]

[0235]

[0236] In the above equation 1, It represents atomic concentration.

[0237] The uniform selectivity according to the number of cycles of the area selective atomic layer deposition method was measured between the copper substrate on which the hafnium oxide thin film was formed in Comparative Example 1 and the copper substrate on which the hafnium oxide thin film was formed in Example 1. The results are as follows: Figure 8 (indicated by =Cu w / &w / oDES).

[0238] from Figure 8 It can be confirmed that the uniform selectivity of the copper substrate on which the hafnium oxide thin film is formed is measured to be 100% at 2 cycles, 99.8% at 10 cycles, 98% at 25 cycles, 55% at 50 cycles, and 24.8% at 100 cycles.

[0239] In addition, the uniform selectivity according to the number of cycles of the area selective atomic layer deposition method was measured between the silicon dioxide substrate on which the hafnium oxide thin film was formed in Comparative Example 2 and the silicon dioxide substrate on which the hafnium oxide thin film was formed in Example 2. The results are as follows: Figure 8 (represented by =SiO2 w / &w / o DES).

[0240] In addition, the uniform selectivity according to the number of cycles of the area selective atomic layer deposition method was measured between the titanium nitride substrate on which the hafnium oxide film was formed in Comparative Example 3 and the titanium nitride substrate on which the hafnium oxide film was formed in Example 3. The results are as follows: Figure 8 (indicated by =TiN w / &w / o DES).

[0241] from Figure 8It can be confirmed that the uniform selectivity of the silicon dioxide substrate on which the hafnium oxide film is formed is measured to be 61% at 2 cycles, 27% at 10 cycles, 19% at 25 cycles, 9% at 50 cycles, and 6% at 100 cycles.

[0242] In addition, it was confirmed that there was no uniform selectivity between the titanium nitride substrate on which the hafnium oxide thin film was formed in Comparative Example 3 and the titanium nitride substrate on which the hafnium oxide thin film was formed in Example 3.

[0243] Based on these results, it can be confirmed that the uniform selectivity of the copper substrate surface on which the hafnium oxide film is formed and the silicon dioxide substrate surface on which the hafnium oxide film is formed decreases with the increase in the number of regional selective atomic layer deposition cycles, among which the copper substrate surface on which the hafnium oxide film is formed has better uniform selectivity.

[0244] On the other hand, the heterogeneous selectivity according to the number of cycles of the area selective atomic layer deposition method was measured between the copper substrate on which the hafnium oxide thin film was formed in Example 1 and the silicon dioxide substrate on which the hafnium oxide thin film was formed in Example 2. The results are as follows: Fig. 9 (indicated by =b / w DES on Cu&SiO2).

[0245] Furthermore, the heterogeneous selectivity according to the number of cycles of the area selective atomic layer deposition method was measured between the silicon dioxide substrate on which the hafnium oxide film was formed in Example 2 and the titanium nitride substrate on which the hafnium oxide film was formed in Example 3. The results are as follows: Fig. 9 (indicated by =b / w DES on Cu&TiN).

[0246] In addition, the heterogeneous selectivity according to the number of area selective atomic layer deposition cycles between the titanium nitride substrate on which the hafnium oxide thin film is formed in Example 3 and the copper substrate on which the hafnium oxide thin film is formed in Example 1 was measured, and the results are as follows: Fig. 9 (indicated by =b / w DES on SiO2&TiN).

[0247] from Fig. 9 It can be confirmed that, according to measurements, the heterogeneous selectivity according to the number of cycles of the area selective atomic layer deposition method between the copper substrate on which a hafnium oxide thin film is formed in Example 1 and the silicon dioxide substrate on which a hafnium oxide thin film is formed in Example 2 is 100% from 2 cycles to 25 cycles, 52.4% at 50 cycles, and 47.6% at 100 cycles.

[0248] Furthermore, the heterogeneous selectivity according to the number of cycles of the area selective atomic layer deposition method between the silicon dioxide substrate on which the hafnium oxide film is formed in Example 2 and the titanium nitride substrate on which the hafnium oxide film is formed in Example 3 is 100% at 2 cycles, 99.2% at 10 cycles, 98.1% at 25 cycles, 31.7% at 50 cycles, and 25.2% at 100 cycles.

[0249] In addition, the heterogeneous selectivity according to the number of cycles of the area selective atomic layer deposition method between the titanium nitride substrate on which the hafnium oxide film is formed in Example 3 and the copper substrate on which the hafnium oxide film is formed in Example 1 is 68.5% at 2 cycles, 42.1% at 10 cycles, 35.9% at 25 cycles, 25.8% at 50 cycles, and 21.2% at 100 cycles.

[0250] Experimental Example 5: Thickness measurement of hafnium oxide film according to the number of cycles of area selective atomic layer deposition

[0251] According to the number of cycles of the area selective atomic layer deposition method, the thickness of the hafnium oxide film formed on the copper substrate in Example 1 (expressed by =HfO2 / DES / CuO), the thickness of the hafnium oxide film formed on the silicon dioxide substrate in Example 2 (expressed by =HfO2 / DES / SiO2), and the thickness of the hafnium oxide film formed on the titanium nitride substrate in Example 3 (expressed by =HfO2 / DES / TiN) were measured, and the results are shown as follows: Fig.10 shown.

[0252] like Fig.10 It was confirmed that the formation of the hafnium oxide film on the copper substrate was delayed until 25 cycles, and the hafnium oxide film was formed when the cycle exceeded 25. From these results, it was confirmed that the formation of the hafnium oxide film on the copper substrate was delayed until 25 cycles by the organic thiol small molecule inhibitor adsorbed on the surface of the copper substrate, and this delay effect disappeared when the cycle exceeded 25.

[0253] On the other hand, the phenomenon of delayed formation of hafnium oxide film which occurs on copper substrate was not observed on silicon dioxide substrate and titanium nitride substrate. The phenomenon of delayed formation of hafnium oxide film as described above was most excellent on copper substrate, followed by silicon dioxide substrate and titanium nitride substrate. In particular, the effect of delayed formation of hafnium oxide film was not observed on titanium nitride substrate.

[0254] Specifically, it was measured that the thickness of the hafnium oxide thin film formed on the copper substrate in Example 1 was 0 nm at 2 cycles, 0 nm at 10 cycles, 0 nm at 25 cycles, 2.95 nm at 50 cycles, and 5.91 nm at 100 cycles.

[0255] In addition, it was measured that the thickness of the hafnium oxide film formed on the silicon dioxide substrate in Example 2 was 0.35 nm at 2 cycles, 1.37 nm at 10 cycles, 2.43 nm at 25 cycles, 5.56 nm at 50 cycles, and 9.90 nm at 100 cycles.

[0256] In addition, it was measured that the thickness of the hafnium oxide film formed on the titanium nitride substrate in Example 3 was 2.43 nm at 2 cycles, 4.25 nm at 10 cycles, 5.16 nm at 25 cycles, 9.43 nm at 50 cycles, and 16.66 nm at 100 cycles.

[0257] Preparation Example 1: Formation of a hafnium oxide thin film on a titanium nitride substrate having a silicon dioxide pattern formed thereon

[0258] (1) A silicon dioxide pattern was formed on a titanium nitride substrate by drop casting. At this time, a 0.1 M solution of silicon dioxide powder dispersed in 50 ml of ethanol was used to form the silicon dioxide pattern, and the remaining solution after the silicon dioxide pattern was formed was evaporated at 22°C.

[0259] (2) The titanium nitride substrate on which the silicon dioxide pattern was formed was ultrasonically cleaned for 10 minutes using acetone, isopropyl alcohol, and deionized water in that order.

[0260] (3) After the cleaned titanium nitride substrate on which the silicon dioxide pattern was formed was dried with nitrogen gas, the substrate was placed in a chamber having an internal temperature of 400° C. and a vacuum minimum pressure condition and maintained therein for 10 minutes.

[0261] (4) A stainless steel tank was prepared for storing an organic thiol small molecule inhibitor, the internal temperature of which was maintained at 25° C. At this time, a compound represented by the following Chemical Formula 1 was used as the organic thiol small molecule inhibitor.

[0262] [Chemical formula 1]

[0263]

[0264] In the above chemical formula 1, R 1 and R 2 It is ethyl.

[0265] (5) The stainless steel tank and the substrate are connected so that the titanium nitride substrate on which the silicon dioxide pattern is formed is exposed to the compound represented by the chemical formula 1.

[0266] (6) The chamber was purged with nitrogen gas, and the titanium nitride substrate having the silicon dioxide pattern formed thereon was exposed to the compound represented by the chemical formula 1 for 30 seconds while the temperature inside the chamber was maintained at 400° C.

[0267] (7) The titanium nitride substrate on which the silicon dioxide pattern was formed and which was exposed to the compound represented by the above Chemical Formula 1 was cooled to a temperature of 25°C.

[0268] (8) A hafnium oxide thin film is formed on a titanium nitride substrate having a silicon dioxide pattern and exposed to an organic thiol small molecule inhibitor using a regioselective atomic layer deposition method, wherein the compound represented by the following chemical formula 2-1 is used as a precursor for thin film deposition, and deionized water is used as a relative reactant.

[0269] [Chemical formula 2-1]

[0270]

[0271] In the above chemical formula 2-1, R 3 and R 4 It is methyl.

[0272] Specifically, a stainless steel tank with an internal temperature of 50° C. and storing a precursor for thin film deposition and a glass tank with an internal temperature of 22° C. and storing a relative reactant were connected to a chamber including a titanium nitride substrate with a silicon dioxide pattern formed thereon, and the area selective atomic layer deposition method was performed while the titanium nitride substrate with a silicon dioxide pattern formed thereon was heated to 275° C. In addition, in the area selective atomic layer deposition method, nitrogen gas was used for purging at a flow rate of 10 sccm and controlled by a mass flow controller.

[0273] On the other hand, the area selective atomic layer deposition method was performed by introducing a thin film deposition precursor into a chamber including a titanium nitride substrate formed with a silicon dioxide pattern, exposing for 4 seconds, purging for 60 seconds, and then introducing a relative reactant into a chamber including a titanium nitride substrate formed with a silicon dioxide pattern, exposing for 2 seconds, and purging for 60 seconds. In addition, the cycle of the area selective atomic layer deposition method was performed 10 times.

[0274] Preparation Example 2: Formation of a hafnium oxide thin film on a titanium nitride substrate having a copper pattern formed thereon

[0275] (1) A copper pattern was formed on a titanium nitride substrate using a drop casting method. At this time, the copper pattern was formed using a 0.1 M solution in which copper powder was dispersed in 50 ml of ethanol, and the remaining solution after the copper pattern was formed was evaporated at 22°C.

[0276] (2) The titanium nitride substrate having the copper pattern formed thereon was ultrasonically cleaned for 10 minutes using acetone, isopropyl alcohol, and deionized water in that order.

[0277] (3) After the cleaned titanium nitride substrate on which the copper pattern was formed was dried with nitrogen gas, the substrate was placed in a chamber having an internal temperature of 400° C. and a vacuum minimum pressure condition and maintained therein for 10 minutes.

[0278] (4) A stainless steel tank was prepared for storing an organic thiol small molecule inhibitor, the internal temperature of which was maintained at 25° C. At this time, a compound represented by the following Chemical Formula 1 was used as the organic thiol small molecule inhibitor.

[0279] [Chemical formula 1]

[0280]

[0281] In the above chemical formula 1, R 1 and R 2 It is ethyl.

[0282] (5) The stainless steel can and the substrate are connected so that the titanium nitride substrate on which the copper pattern is formed is exposed to the compound represented by the above Chemical Formula 1.

[0283] (6) The chamber was purged with nitrogen gas, and the titanium nitride substrate having the copper pattern formed thereon was exposed to the compound represented by the chemical formula 1 for 30 seconds while the temperature inside the chamber was maintained at 400° C.

[0284] (7) The titanium nitride substrate on which the copper pattern was formed and which was exposed to the compound represented by the above Chemical Formula 1 was cooled to a temperature of 25°C.

[0285] (8) A hafnium oxide thin film is formed on a titanium nitride substrate having a copper pattern formed thereon and exposed to an organic thiol small molecule inhibitor using a regioselective atomic layer deposition method, wherein the compound represented by the following chemical formula 2-1 is used as a precursor for thin film deposition, and deionized water is used as a relative reactant when performing the regioselective atomic layer deposition method.

[0286] [Chemical formula 2-1]

[0287]

[0288] In the above chemical formula 2-1, R 3 and R 4 It is methyl.

[0289] Specifically, a stainless steel tank with an internal temperature of 50° C. and storing a precursor for thin film deposition and a glass tank with an internal temperature of 22° C. and storing a relative reactant were connected to a chamber including a titanium nitride substrate with a copper pattern formed thereon, and the area selective atomic layer deposition method was performed while the titanium nitride substrate with a copper pattern formed thereon was heated to 275° C. In addition, in the area selective atomic layer deposition method, nitrogen gas was used for purging at a flow rate of 10 sccm and controlled by a mass flow controller.

[0290] On the other hand, the region selective atomic layer deposition method was performed by placing a thin film deposition precursor into a chamber including a titanium nitride substrate formed with a copper pattern, exposing for 4 seconds, purging for 60 seconds, and then placing a relative reactant into a chamber including a titanium nitride substrate formed with a copper pattern, exposing for 2 seconds, and purging for 60 seconds. In addition, the region selective atomic layer deposition method was repeated 10 times.

[0291] Comparative Preparation Example 1: Formation of a Hafnium Oxide Thin Film on a Titanium Nitride Substrate with a Silicon Dioxide Pattern

[0292] (1) A silicon dioxide pattern was formed on a titanium nitride substrate using a drop casting method. At this time, a 0.1 M solution of silicon dioxide powder dispersed in 50 ml of ethanol was used to form the silicon dioxide pattern, and the remaining solution after the silicon dioxide pattern was formed was evaporated at 22°C.

[0293] (2) The titanium nitride substrate on which the silicon dioxide pattern was formed was ultrasonically cleaned for 10 minutes using acetone, isopropyl alcohol, and deionized water in that order.

[0294] (3) After the cleaned titanium nitride substrate on which the silicon dioxide pattern was formed was dried with nitrogen gas, the substrate was placed in a chamber with an internal temperature of 25° C. and kept there for 10 minutes.

[0295] (4) A hafnium oxide thin film is formed on a titanium nitride substrate having a silicon dioxide pattern by using an area selective atomic layer deposition method, wherein the compound represented by the following chemical formula 2-1 is used as a precursor for thin film deposition, and deionized water is used as a relative reactant.

[0296] [Chemical formula 2-1]

[0297]

[0298] In the above chemical formula 2-1, R 3 and R 4 It is methyl.

[0299] Specifically, a stainless steel tank with an internal temperature of 50° C. and storing a precursor for thin film deposition and a glass tank with an internal temperature of 22° C. and storing a relative reactant were connected to a chamber including a titanium nitride substrate with a silicon dioxide pattern formed thereon, and the area selective atomic layer deposition method was performed while the titanium nitride substrate with a silicon dioxide pattern formed thereon was heated to 275° C. In addition, in the area selective atomic layer deposition method, nitrogen gas was used for purging at a flow rate of 10 sccm and controlled by a mass flow controller.

[0300] On the other hand, the area selective atomic layer deposition method was performed by introducing a thin film deposition precursor into a chamber including a titanium nitride substrate formed with a silicon dioxide pattern, exposing for 4 seconds, purging for 60 seconds, and then introducing a relative reactant into a chamber including a titanium nitride substrate formed with a silicon dioxide pattern, exposing for 2 seconds, and purging for 60 seconds. In addition, the cycle of the area selective atomic layer deposition method was performed 10 times.

[0301] Comparative Preparation Example 2: Formation of a Hafnium Oxide Thin Film on a Titanium Nitride Substrate with a Copper Pattern

[0302] (1) A copper pattern was formed on a titanium nitride substrate using a drop casting method. At this time, the copper pattern was formed using a 0.1 M solution in which copper powder was dispersed in 50 ml of ethanol, and the remaining solution after the copper pattern was formed was evaporated at 22°C.

[0303] (2) The titanium nitride substrate having the copper pattern formed thereon was ultrasonically cleaned for 10 minutes using acetone, isopropyl alcohol, and deionized water in that order.

[0304] (3) After the cleaned titanium nitride substrate on which the copper pattern was formed was dried with nitrogen gas, the substrate was placed in a chamber with an internal temperature of 25° C. and kept there for 10 minutes.

[0305] (4) A hafnium oxide thin film is formed on a titanium nitride substrate having a copper pattern by using an area selective atomic layer deposition method, wherein the compound represented by the following chemical formula 2-1 is used as a precursor for thin film deposition, and deionized water is used as a relative reactant.

[0306] [Chemical formula 2-1]

[0307]

[0308] In the above chemical formula 2-1, R 3 and R 4 It is methyl.

[0309] Specifically, a stainless steel tank with an internal temperature of 50° C. and storing a precursor for thin film deposition and a glass tank with an internal temperature of 22° C. and storing a relative reactant were connected to a chamber including a titanium nitride substrate with a copper pattern formed thereon, and the area selective atomic layer deposition method was performed while the titanium nitride substrate with a copper pattern formed thereon was heated to 275° C. In addition, in the area selective atomic layer deposition method, nitrogen gas was used for purging at a flow rate of 10 sccm and controlled by a mass flow controller.

[0310] On the other hand, the region selective atomic layer deposition method was performed by placing a thin film deposition precursor into a chamber including a titanium nitride substrate formed with a copper pattern, exposing for 4 seconds, purging for 60 seconds, and then placing a relative reactant into a chamber including a titanium nitride substrate formed with a copper pattern, exposing for 2 seconds, and purging for 60 seconds. In addition, the region selective atomic layer deposition method was repeated 10 times.

[0311] Experimental Example 6: FE-SEM Analysis

[0312] The titanium nitride substrate with a silicon dioxide pattern formed thereon in Preparation Example 1 was analyzed using a field emission scanning electron microscope (FE-SEM). Fig.11 As shown in part (a) of FIG. 1 , the titanium nitride substrate having a silicon dioxide pattern formed thereon in Comparative Preparation Example 1 was analyzed using FE-SEM, and the results are as follows Fig.11 As shown in part (b) of the present invention, the titanium nitride substrate having a copper pattern formed thereon in Preparation Example 2 was analyzed using FE-SEM, and the results are as follows: Fig.11 As shown in part (c) of FIG. 1 , the titanium nitride substrate having a copper pattern formed thereon in Comparative Preparation Example 2 was analyzed using FE-SEM, and the results are as follows: Fig.11 As the analytical instrument, a JEOL JSM-7800F instrument (JEOL Ltd.) was used.

[0313] pass Fig.11 Part (a) and Fig.11 The comparison of part (b) of FIG. 1 shows that the roughness of the silica particles on the titanium nitride substrate with a silica pattern formed in Comparative Example 1 is greater than that of the silica particles on the titanium nitride substrate with a silica pattern formed in Comparative Example 1, and thus it can be seen that the hafnium oxide film on the titanium nitride substrate with a silica pattern formed in Comparative Example 1 is formed thicker. In addition, it can be confirmed that the formation of the hafnium oxide film on the titanium nitride substrate with a silica pattern formed in Comparative Example 1 is suppressed by the adsorbed organic thiol small molecule inhibitor.

[0314] In addition, through Fig.11 Part (c) and Fig.11The comparison of part (d) of FIG. 2 shows that the roughness of the copper particles of the titanium nitride substrate with a copper pattern formed in Comparative Example 2 is greater than the roughness of the silicon dioxide particles of the titanium nitride substrate with a copper pattern formed in Comparative Example 2, which shows that the hafnium oxide film formed on the titanium nitride substrate with a copper pattern formed in Comparative Example 2 is thicker. In addition, it can be confirmed that the formation of the hafnium oxide film on the titanium nitride substrate with a copper pattern formed in Comparative Example 2 is suppressed by the adsorbed organic thiol small molecule inhibitor.

[0315] Preparation Example 3: Formation of a hafnium oxide thin film on a titanium nitride substrate having a silicon dioxide-copper pattern formed thereon

[0316] (1) A silicon dioxide-copper pattern was formed on a titanium nitride substrate using a drop casting method. At this time, a 0.1 M solution of silicon dioxide powder and copper powder dispersed in 50 ml of ethanol was used to form the silicon dioxide-copper pattern, and the remaining solution after forming the silicon dioxide-copper pattern was evaporated at 22°C.

[0317] (2) The titanium nitride substrate on which the silicon dioxide-copper pattern was formed was ultrasonically cleaned for 10 minutes using acetone, isopropyl alcohol, and deionized water in that order.

[0318] (3) After the cleaned titanium nitride substrate on which the silicon dioxide-copper pattern was formed was dried with nitrogen gas, the substrate was placed in a chamber having an internal temperature of 400° C. and a vacuum minimum pressure condition and maintained therein for 10 minutes.

[0319] (4) A stainless steel tank was prepared for storing an organic thiol small molecule inhibitor, the internal temperature of which was maintained at 25° C. At this time, a compound represented by the following Chemical Formula 1 was used as the organic thiol small molecule inhibitor.

[0320] [Chemical formula 1]

[0321]

[0322] In the above chemical formula 1, R 1 and R 2 It is ethyl.

[0323] (5) The stainless steel tank and the substrate are connected so that the titanium nitride substrate on which the silicon dioxide-copper pattern is formed is exposed to the compound represented by the above Chemical Formula 1.

[0324] (6) The chamber was purged with nitrogen gas, and the titanium nitride substrate having the silicon dioxide-copper pattern formed thereon was exposed to the compound represented by the chemical formula 1 for 30 seconds while the temperature inside the chamber was maintained at 400° C.

[0325] (7) The titanium nitride substrate on which the silicon dioxide-copper pattern was formed and which was exposed to the compound represented by the above Chemical Formula 1 was cooled to a temperature of 25°C.

[0326] (8) A hafnium oxide thin film is formed on a titanium nitride substrate having a silicon dioxide-copper pattern and exposed to an organic thiol small molecule inhibitor using a regioselective atomic layer deposition method, wherein the compound represented by the following chemical formula 2-1 is used as a precursor for thin film deposition, and deionized water is used as a relative reactant.

[0327] [Chemical formula 2-1]

[0328]

[0329] In the above chemical formula 2-1, R 3 and R 4 It is methyl.

[0330] Specifically, a stainless steel tank with an internal temperature of 50° C. and storing a precursor for thin film deposition and a glass tank with an internal temperature of 22° C. and storing a relative reactant were connected to a chamber including a titanium nitride substrate with a silicon dioxide-copper pattern formed thereon, and the area selective atomic layer deposition method was performed while the titanium nitride substrate with the silicon dioxide-copper pattern formed thereon was heated to 275° C. In addition, in the area selective atomic layer deposition method, nitrogen gas was used for purging at a flow rate of 10 sccm and controlled by a mass flow controller.

[0331] On the other hand, area selective atomic layer deposition is performed by introducing a thin film deposition precursor into a chamber including a titanium nitride substrate formed with a silicon dioxide-copper pattern, exposing for 4 seconds, purging for 60 seconds, and then introducing a relative reactant into a chamber including a titanium nitride substrate formed with a silicon dioxide-copper pattern, exposing for 2 seconds, and purging for 60 seconds in a cycle.

[0332] Also, the cycles of the area selective atomic layer deposition method were performed 10 times and 25 times, respectively.

[0333] Experimental Example 7: AES Analysis

[0334] The titanium nitride substrate with a silicon dioxide-copper pattern formed in Preparation Example 3 was analyzed by Auger electron spectroscopy (AES). Fig.12 As the analysis instrument, a PHI 700TM device (Scanning Auger Nanoprobe) was used. For line scanning and mapping methods, the beam size was 20 nm, based on an analysis area of ​​20×20 μm. 2 Two-point scan.

[0335] Fig.12 Parts (a) and (d) of FIG. 3 are AES images of the silicon dioxide-copper pattern used for mapping the profile and line scan. In addition, Fig.12Part (b) shows the mapping profile after 10 cycles of area selective atomic layer deposition. Fig.12 Part (e) is the mapping profile after 25 cycles of area selective atomic layer deposition. Fig.12 Part (c) is a line scan after 10 cycles of area selective atomic layer deposition. Fig.12 Part (f) is a line scan after area-selective atomic layer deposition was performed with 25 cycles.

[0336] Fig.12 Part (b) shows the RGB superimposed mapping profile of red oxygen, green copper and blue hafnium, from which it can be confirmed that copper patches are observed between purple patches. The purple patches show that oxygen from silicon dioxide and hafnium oxide overlaps with blue hafnium. It can be seen that hafnium oxide does not exist on the copper wire of the pattern. Through these results, it can be confirmed that after 10 cycles of area selective atomic layer deposition, copper has a complete blocking selectivity for silicon dioxide.

[0337] Fig.12 Part (c) shows a line scan for the same pattern, but no hafnium concentration is observed in the copper profile, and only the oxide profile is observed. In the silicon dioxide line, there are oxides contained in silicon dioxide and oxides contained in hafnium oxide, so a greater oxygen intensity is observed in the silicon dioxide line.

[0338] On the other hand, Fig.12 In parts (e) and (f) of Figure 3, hafnium is observed in the copper wire. These results confirm that the copper wire has hafnium barrier properties and interferes with atomic layer deposition. Fig.12 In part (e), small green patches can still be observed, indicating that the small patches of copper are still not covered with hafnium oxide. Fig.12 The presence of hafnium can be seen in the scan area of ​​part (f), but a higher hafnium concentration is observed in the silica lines.

[0339] In conclusion, AES analysis confirmed that the organothiol small molecule inhibitor effectively blocked copper in the SiO2-Cu pattern until 10 cycles of area-selective ALD.

Claims

1. A method for selective deposition of a thin film using area selective atomic layer deposition, characterized in that: include: The first step is to prepare a substrate in which a first substrate including metal, a second substrate including silicon dioxide and a third substrate including nitride are arranged in parallel and integrated; The second step is to expose the substrate to an organic thiol small molecule inhibitor; and The third step is to form a thin film on the surface of the substrate exposed to the organic thiol small molecule inhibitor by using a regional selective atomic layer deposition method; The thickness of the thin film formed on the surface of the first substrate, the thickness of the thin film formed on the surface of the second substrate, and the thickness of the thin film formed on the surface of the third substrate are different.

2. The method for selective deposition of a thin film using area selective atomic layer deposition according to claim 1, characterized in that: The metal is selected from the group consisting of copper, cobalt, ruthenium, molybdenum and tungsten, The nitride is selected from the group consisting of titanium nitride, molybdenum nitride, tungsten nitride and silicon nitride. The thin film is a thin film selected from the group consisting of metal, metal oxide and silicon dielectric material.

3. The method for selective deposition of a thin film using area selective atomic layer deposition according to claim 1, characterized in that: The above metal is copper, The above nitride is titanium nitride, The above-mentioned thin film is a hafnium oxide thin film.

4. The method for selective deposition of a thin film using area selective atomic layer deposition according to claim 1, characterized in that: The following conditions (1) are met: (1)A <B<C In the above condition (1), A represents the thickness of the thin film formed on the surface of the first substrate, B represents the thickness of the thin film formed on the surface of the second substrate, and C represents the thickness of the thin film formed on the surface of the third substrate.

5. The method for selective deposition of a thin film using area selective atomic layer deposition according to claim 1, characterized in that: The above-mentioned organic thiol small molecule inhibitor includes a compound represented by the following chemical formula 1: [Chemical formula 1] In the above chemical formula 1, R 1 and R 2 Each is independently a C1-C12 straight-chain alkyl group, a C3-C12 branched-chain alkyl group or a C6-C12 aryl group.

6. The method for selective deposition of a thin film using area selective atomic layer deposition according to claim 1, characterized in that: The second step includes: Step 2-1, after drying the substrate, placing the substrate in a chamber with an internal temperature of 300° C. to 500° C. and a minimum vacuum pressure condition and maintaining the chamber for 1 minute to 20 minutes; In step 2-2, the chamber is purged, and an organic thiol small molecule inhibitor is introduced into the chamber while maintaining the internal temperature of the chamber at 200° C. to 500° C., so that the substrate is exposed to the organic thiol small molecule inhibitor for 1 second to 100 seconds; and In step 2-3, the substrate exposed to the organic thiol small molecule inhibitor is cooled to a temperature of 15°C to 35°C.

7. The method for selective deposition of a thin film using area selective atomic layer deposition according to claim 1, characterized in that: In the second step above, The water contact angle of the first substrate surface exposed to the organic thiol small molecule inhibitor is 90° to 100°, The water contact angle of the second substrate surface exposed to the organic thiol small molecule inhibitor is 70° to 80°.

8. The method for selective deposition of a thin film using area selective atomic layer deposition according to claim 6, characterized in that: The organic thiol small molecule inhibitor introduced into the above chamber undergoes thermal dissociation and separates into alkylthio and alkyl groups. The alkylthio group is adsorbed on the surface of the first substrate, and the alkyl group is adsorbed on the surface of the second substrate.

9. The method for selective deposition of a thin film using area selective atomic layer deposition according to claim 8, characterized in that: The above-mentioned alkylthio group is ethylthio group, The above-mentioned alkyl group is ethyl group.

10. The method for selective deposition of a thin film using area selective atomic layer deposition according to claim 1, characterized in that: The third step includes: In step 3-1, the substrate exposed to the organic thiol small molecule inhibitor is placed in a chamber and heated at 200° C. to 350° C.; and In step 3-2, a regional selective atomic layer deposition method is performed by introducing a thin film deposition precursor into the above-mentioned chamber, exposing it for 1 second to 10 seconds, then purging it for 50 seconds to 70 seconds, introducing a relative reactant into the chamber and exposing it for 1 second to 5 seconds, and then purging it for 50 seconds to 70 seconds.

11. The method for selective deposition of a thin film using area selective atomic layer deposition according to claim 10, characterized in that: The thin film deposition precursor includes at least one compound selected from the group consisting of a compound represented by the following chemical formula 2, a compound represented by the following chemical formula 3, a compound represented by the following chemical formula 4, and a compound represented by the following chemical formula 5: [Chemical formula 2] (L1) n M(NR 3 R 4 ) 4-n In the above chemical formula 2, L1 is a ligand selected from the group consisting of cyclopentadienyl and C1-C12 alkyl-substituted cyclopentadienyl, M is a metal selected from the group consisting of titanium, hafnium and zirconium, and R 3 and R 4 Each is independently a C1-C12 straight chain alkyl or a C3-C12 branched chain alkyl, and n is 0, 1 or 2; [Chemical formula 3] R 5 m M(OR 6 ) 3-m In the above chemical formula 3, M is a metal selected from the group consisting of aluminum, hafnium and zirconium, and R 5 and R 6 Each is independently a C1-C12 straight chain alkyl or a C3-C12 branched chain alkyl, and m is 1 to 3; [Chemical formula 4] (L2)pMR7(OR 8 ) 3-p In the above chemical formula 4, L2 is a ligand selected from the group consisting of cyclopentadienyl and C1-C12 alkyl-substituted cyclopentadienyl, M is a metal selected from the group consisting of titanium, hafnium and zirconium, R 7 and R 8 Each is independently a C1-C12 straight-chain alkyl group or a C3-C12 branched-chain alkyl group, and p is 1 or 2; [Chemical formula 5] (R 9 N) q M(NR 10 R 11 ) 4-q In the above chemical formula 5, M is a metal selected from the group consisting of vanadium, niobium, tantalum, molybdenum and tungsten, and R 9 , R 10 and R 11 Each is independently a C1-C12 straight-chain alkyl group or a C3-C12 branched-chain alkyl group, and q is 1 or 2.

12. The method for selective deposition of a thin film using area selective atomic layer deposition according to claim 11, characterized in that: The compound represented by the above chemical formula 2 is tetrakis(dimethylamino)hafnium (TDMAH), tetrakis(diethylamino)hafnium (TDEAH), tetrakis(ethylmethylamino)hafnium (TEMAH), cyclopentadienyltris(dimethylamino)hafnium (CpHf(NMe2)3), methylcyclopentadienyltris(dimethylamino)hafnium ((MeCp)Hf(NMe2)3), ethylcyclopentadienyltris(dimethylamino)hafnium ((EtCp)Hf(NMe2)3), (n-propylcyclopentadienyl)tris(dimethylamino)hafnium ((n-PrC p)Hf(NMe2)3), cyclopentadienyl tris(methylethylamino) hafnium (CpHf(NMeEt)3), methylcyclopentadienyl tris(methylethylamino) hafnium ((MeCp)Hf(NMeEt)3), ethylcyclopentadienyl tris(methylethylamino) hafnium ((EtCp)Hf(NMeEt)3), cyclopentadienyl tris(diethylamino) hafnium (CpHf(NEt2)3, methylcyclopentadienyl tris(diethylamino) hafnium ((MeCp)Hf(NEt2)3), ethylcyclopentadienyl tris(diethylamino) hafnium ((E tCp)Hf(NEt2)3), bis(cyclopentadienyl)bis(dimethylamino)hafnium (Cp2Hf(NMe2)2), bis(methylcyclopentadienyl)bis(dimethylamino)hafnium ((MeCp)2Hf(NMe2)2), bis(ethylcyclopentadienyl)bis(dimethylamino)hafnium ((EtCp)2Hf(NMe2)2), bis(cyclopentadienyl)bis(methylethylamino)hafnium (Cp2Hf(NMeEt)2), bis(methylcyclopentadienyl)bis(methylethylamino)hafnium ((MeCp)2Hf(NMeEt )2), bis(ethylcyclopentadienyl)bis(methylethylamino)hafnium ((EtCp)2Hf(NMeEt)2), bis(cyclopentadienyl)bis(diethylamino)hafnium (Cp2Hf(NEt2)2), bis(methylcyclopentadienyl)bis(diethylamino)hafnium ((MeCp)2Hf(NEt2)3), bis(ethylcyclopentadienyl)bis(diethylamino)hafnium ((EtCp)2Hf(NEt2)2) or (n-propylcyclopentadienyl)tris(dimethylamino)zirconium ((n-PrCp)Zr(NMe2)3), The compound represented by the above chemical formula 3 is trimethylaluminum, triethylaluminum, dimethylaluminum isopropoxide or diethylaluminum isopropoxide, The compound represented by the above Chemical Formula 4 is CpHfMe(OMe)2, CpZrMe(OMe)2, (MeCp)HfMe(OMe)2, (MeCp)ZrMe(OMe)2, (EtCp)HfMe(OMe)2 or (EtCp)ZrMe(OMe); The compound represented by the above Chemical Formula 5 is tert-butyliminotris(diethylamino)tantalum (TBTDET), tert-butyliminotris(dimethylamino)tantalum (TBTDMT), tert-butyliminotris(ethylmethylamino)tantalum (TBTEMT), ethyliminotris(diethylamino)tantalum (EITDET), ethyliminotris(dimethylamino)tantalum (EITDMT), ethyliminotris(ethylmethylamino)tantalum (EITEMT), tert-amyltris(dimethylamino)tantalum (TAIMAT), tert-amyliminotris(diethylamino)tantalum, penta(dimethylamino)tantalum, tert-amyliminotris(ethylmethylamino)tantalum, bis(tert-butylimino)bis(dimethylamino)tungsten (BTBMW), bis(tert-butylimino)bis(diethylamino)tungsten or bis(tert-butylimino)bis(ethylmethylamino)tungsten.

13. The method for selective deposition of a thin film using area selective atomic layer deposition according to claim 11, characterized in that: The thin film deposition precursor includes a compound represented by the following chemical formula 2-1: [Chemical formula 2-1] In the above chemical formula 2-1, R 3 and R 4 Each is independently a C1-C12 straight-chain alkyl group or a C3-C12 branched-chain alkyl group.

14. The method for selective deposition of a thin film using area selective atomic layer deposition according to claim 10, characterized in that: The above-mentioned counter reactants include at least one selected from deionized water and hydrogen peroxide.

15. The method for selective deposition of a thin film using area selective atomic layer deposition according to claim 10, characterized in that: The above-mentioned area selective atomic layer deposition method is cycled 2 to 100 times.

16. The method for selective deposition of a thin film using area selective atomic layer deposition according to claim 10, characterized in that: In the above-mentioned area selective atomic layer deposition method, Each cycle forms a layer with a thickness of to film, Each cycle forms a layer with a thickness of to film, Each cycle forms a layer with a thickness of to of film.

17. A substrate for selectively forming a thin film, characterized in that: include: A substrate in which a first substrate including metal, a second substrate including silicon dioxide and a third substrate including nitride are arranged in parallel to form an integrated structure; and A thin film formed on the surface of the substrate; wherein the alkylthio group is adsorbed on the surface of the first substrate, and the alkyl group is adsorbed on the surface of the second substrate. The thickness of the thin film formed on the surface of the first substrate, the thickness of the thin film formed on the surface of the second substrate, and the thickness of the thin film formed on the surface of the third substrate are different.

18. The substrate for selectively forming a thin film according to claim 17, characterized in that: The following conditions (1) are met: (1)A <B<C In the above condition (1), A represents the thickness of the thin film formed on the surface of the first substrate, B represents the thickness of the thin film formed on the surface of the second substrate, and C represents the thickness of the thin film formed on the surface of the third substrate.

19. The substrate for selectively forming a thin film according to claim 17, characterized in that: The above-mentioned alkylthio group is ethylthio group, The above-mentioned alkyl group is ethyl group.

20. The substrate for selectively forming a thin film according to claim 17, characterized in that: The metal of the first substrate is copper. The nitride of the third substrate is titanium nitride. The above-mentioned thin film is a hafnium oxide thin film.

Citation Information

Cited By

  • Initiation type molecular layer deposition method and regioselective deposition regulation and control method