Core and heat transfer device

By using the core of nanofibers and two-dimensional material in the heat transfer device, the problem of slow liquid-state working fluid delivery speed in the prior art is solved, and more efficient heat transfer performance is achieved.

CN119096108AInactive Publication Date: 2024-12-06MURATA MFG CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202380039461.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-05-13
Filing Date
2023-05-12
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the existing heat transfer devices, the liquid state working fluid is transported slowly by the capillary force of the core, which limits the heat transfer performance.

Method used

Materials containing nanofibers and/or two-dimensional substances are used as cores. By configuring these materials in the shell, the high volume density and hydrophilic surfaces are used to improve the conveying speed of working fluid in liquid state.

Benefits of technology

The conveying speed of the working fluid in liquid state is significantly improved, and the heat transfer performance and maximum heat transfer volume of the heat transfer device are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119096108A_ABST
    Figure CN119096108A_ABST
Patent Text Reader

Abstract

A core for heat transfer, the core comprising a material comprising a nanofiber and / or a two-dimensional substance of a material represented by the formula: MQaOb (in the formula, M is at least one element selected from the group consisting of groups 3, 4, 5, 6 and 7, Q is at least one element selected from the group consisting of groups 12, 13, 14, 15 and 16 (excluding O), a is 0-2, and b is greater than 0 and 2 or less).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a core and a heat transport device, and more particularly to a core used for heat transport and a heat transport device using phase change of a working fluid. Background Art

[0002] Conventionally, there are known heat transfer devices that utilize phase change (more specifically, evaporation and condensation) of a working fluid, such as heat pipes and vapor chambers. In such heat transfer devices, a core is used that transports a working fluid in a liquid state by means of capillary force (attractive force generated by capillary phenomena).

[0003] For example, Patent Document 1 describes the use of a sintered body of metal particles having an average particle size of 20 μm or more and 200 μm or less as a core body. Also, for example, Patent Document 2 describes the use of a fiber-containing porous body in which at least a portion of a fiber structure including carbon fibers and / or oxidized fibers is filled with a carbonaceous porous body as a core body, wherein the fiber-containing porous body has at least one peak in a region of pore diameters of 10 μm or less in the pore size distribution of the carbonaceous porous body.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2022-27310

[0007] Patent Document 2: Japanese Patent Application Publication No. 2020-112326

[0008] Non-patent literature

[0009] Non-patent document 1: Hussein O. Badr, et al., "Bottom-up, scalable synthesis of anatase nanofilament-based two-dimensional titanium carbo-oxide flakes", Materials Today (2021)

[0010] https: / / doi.org / 10.1016 / j.mattod.2021.10.033 Summary of the invention

[0011] Problems to be solved by the invention

[0012] The heat transfer device as described above has the following structure: a shell having at least partial thermal conductivity is used, a core is arranged in the shell, and a working fluid is sealed. In the shell, the working fluid evaporates in a relatively high temperature portion to which heat is supplied from the outside, and the working fluid in a gaseous state moves in the shell, condenses in a relatively low temperature portion, thereby releasing heat to the outside, and the working fluid in a liquid state is transported to the relatively high temperature portion (return) by the capillary force of the core.

[0013] In recent years, due to the miniaturization of electronic devices that can be assembled with heat transport devices, etc., heat transport devices are required to further improve heat transport performance. In the past, the speed at which the working fluid in a liquid state is transported by the capillary force of the core is generally lower than the speed at which the working fluid in a gas state moves in the housing, and the heat transport performance of the heat transport device may be limited by the speed at which the working fluid in a liquid state is transported by the capillary force of the core. In order to improve the heat transport performance of the heat transport device, it is preferred that the transport speed of the working fluid in a liquid state in the core is greater.

[0014] An object of the present invention is to provide a novel core having a high conveying speed for a working fluid in a liquid state. Another object of the present invention is to provide a novel heat transport device using the core.

[0015] Means for solving problems

[0016] According to one subject of the present invention, there is provided a core for heat transfer, wherein the core comprises a material including nanofibers and / or a two-dimensional substance.

[0017] The nanofibers and / or two-dimensional materials are represented by the following formula: MQ a O b express,

[0018] (wherein, M is at least one element selected from Groups 3, 4, 5, 6 and 7,

[0019] Q is at least one element selected from Groups 12, 13, 14, 15 and 16 (excluding O),

[0020] a is greater than or equal to 0 and less than or equal to 2,

[0021] b is greater than 0 and less than 2).

[0022] According to another aspect of the present invention, there is provided a heat transport device which utilizes the phase change of a working fluid, the heat transport device comprising:

[0023] a housing having a space therein;

[0024] The core is disposed in the shell; and

[0025] A working fluid is sealed in the housing in a state where the working fluid can come into contact with the core.

[0026] Effects of the Invention

[0027] According to the present invention, there is provided a novel core having a high conveying speed of a working fluid in a liquid state. In addition, according to the present invention, there is provided a novel heat transport device using the core. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is a schematic cross-sectional view of a heat transport device according to one embodiment of the present invention.

[0029] Figure 2 The XRD spectrum of the material (TiCO) produced in Example 1 is shown.

[0030] Figure 3 The FE-SEM image of the material (TiCO) produced in Example 1 is shown. DETAILED DESCRIPTION

[0031] Hereinafter, the core and the heat transport device in the embodiments of the present invention will be described in detail, but the present invention is not limited to these embodiments.

[0032] (Implementation 1: Core)

[0033] This embodiment relates to a core. In the present invention, a "core" refers to a member for heat transfer. More specifically, a "core" refers to a member capable of transporting a working fluid in a liquid state by capillary force.

[0034] In the present embodiment, the core contains a material containing nanofibers and / or a two-dimensional substance. In the present invention, when simply referred to as a "material", it refers to a "material containing nanofibers and / or a two-dimensional substance" (in other words, a material containing at least any one of nanofibers and two-dimensional substances). In the present embodiment, the material containing nanofibers and / or a two-dimensional substance representatively refers to a material that is a solid component and does not contain a binder, etc. (such as a polymer). The material containing nanofibers and / or a two-dimensional substance can refer to a material that is essentially composed of at least any one of nanofibers and two-dimensional substances in a narrow sense (which may include: other objects, impurities, etc. that may be inevitably mixed in). However, the material containing nanofibers and / or two-dimensional substances is not limited to these.

[0035] The material contained in the core of the present embodiment is a nanofiber (or nanowire, hereinafter the same) and / or a two-dimensional substance of a predetermined material (substance). The predetermined material that can be used in the present embodiment is represented by the following formula (1).

[0036] MQ a Ob ···(1)

[0037] (wherein, M is at least one element selected from Groups 3, 4, 5, 6 and 7, and may include so-called early transition metals, such as at least one element selected from Sc, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo and Mn, and may preferably include at least one element selected from Ti, V, Cr, Mo and Mn,

[0038] Q is at least one element selected from Groups 12, 13, 14, 15 and 16 (excluding O), for example, at least one element selected from B, C, N, Si, P and S,

[0039] a is greater than or equal to 0 and less than or equal to 2,

[0040] b is greater than 0 and less than 2)

[0041] Hereinafter, the above-mentioned material is also referred to as "MQO". Examples of MQO include materials represented by formulas such as TiO2, TiCO, TiCON, VO2, VCO, VCON, CrO2, CrCO, CrCON, MoO2, MoCO, MoCON, MnO2, MnCO, and MnCON. For example, in formula (1), the above-mentioned M may be Ti, and the above-mentioned Q may be C. In addition, for example, in formula (1), the above-mentioned a may not be 0.

[0042] The above-mentioned predetermined material may typically have a peak in a range of a diffraction angle 2θ of 2° to 10° in an X-ray diffraction (XRD) spectrum.

[0043] MQO has a crystal structure different from the hexagonal system. The present embodiment is not limited by any theory, but the crystal structure of MQO can be considered to be anatase or lepidocrocite type or a mixture thereof. For example, the crystal structure of MQO can be lepidocrocite type.

[0044] MQO can be produced, for example, using a first raw material and a second raw material as follows: The first raw material contains at least the above-mentioned M, and the second raw material contains at least the above-mentioned Q. The first raw material and the second raw material can react in a protic solvent to produce MQO.

[0045] As the first raw material, a material represented by the following formula (2) can be used.

[0046] M c A 1 d ···(2)

[0047] (Where M is as described above,

[0048] A1 is at least one element selected from Groups 12, 13, 14, 15 and 16, for example, it may contain at least one element selected from B, C, N, O, Si, P and S,

[0049] c and d are each independently 1 or more and 5 or less)

[0050] The material represented by formula (2) needs to be different from the product MQO. The material represented by formula (2) may be a material that does not have a peak in the range of a diffraction angle 2θ of 2° to 10° in an X-ray diffraction (XRD) spectrum.

[0051] Examples of the first raw material represented by formula (2) include TiB2, TiB, TiC, TiN, TiO2, Ti5Si3, Ti2SbP, VO2, V2O4, NbC, Nb2O5, MoO2, MoO3, MoS2, MnO2, Mn3O4, MnCO3, etc. MnO2 that can be used as the first raw material has a peak near 2θ=13° in the XRD spectrum, and has no peak in the range of 2θ being greater than 2° and less than 10°.

[0052] Alternatively, or in addition to the above, as the first raw material, a material represented by the following formula (3) (hereinafter, also referred to as “MAX phase” or “MAX raw material”) may be used.

[0053] M m A 2 X n ···(3)

[0054] (Where M is as described above,

[0055] X is at least one element selected from C and N,

[0056] n is greater than or equal to 1 and less than or equal to 4,

[0057] m is greater than n and less than 5,

[0058] A 2 It is at least one element selected from Groups 12, 13, 14, 15 and 16, usually an element of Group A, typically Group IIIA and Group IVA, and more specifically, it may include at least one selected from Al, Ga, In, Tl, Si, Ge, Sn, Pb, P, As, S and Cd, preferably Al)

[0059] The MAX phase has the following crystal structure: 2 The atomic layer is located at M m X nThe MAX phase has a repeating unit in which layers of X atoms are arranged one after another between layers of n+1 layers of M atoms (these layers are collectively referred to as "M". m X n Layer”), and configure A 2 Atomic layers (“A 2 atomic layer") as the next layer of the layer of the n+1th M atom. However, the MAX phase is not limited to this.

[0060] Examples of the first raw material represented by formula (3) include Ti 3 AlC 2 , Ti 3 GaC 2 , and Ti 3 SiC 2 .

[0061] As the first raw material, the material represented by formula (2) and the material represented by formula (3) may be used together (for example, in the form of a mixture).

[0062] As the second raw material, an ionic bonding substance having a carbon-containing group can be used. The ionic bonding substance having a carbon-containing group contains C. Examples of the ionic bonding substance include ammonium salts, phosphates, and sulfates.

[0063] More specifically, as the second raw material, a quaternary ammonium salt can be used. Examples of quaternary ammonium salts include tetramethylammonium hydroxide (TMAH), tetraethylammonium hydroxide (TEAH), tetrapropylammonium hydroxide (TPAH), tetrabutylammonium hydroxide (TBAH or TBAOH), benzyltrimethylammonium hydroxide, tetrabutylammonium fluoride (TBAF), tetrabutylammonium chloride (TBACl), tetrabutylammonium bromide (TBAB), tetrabutylammonium iodide (TBAI), benzyltriethylammonium chloride (BTEAC), hexadecyltrimethylammonium bromide, cetyltrimethylammonium bromide (CTAB), benzethonium chloride, benzalkonium chloride, hexadecylpyridinium chloride (CPC), etc. Among them, TMAH and TBAOH are preferred.

[0064] Alternatively or in addition to the above, other ionic bonding substances containing P and / or S etc. may be used as the second raw material.

[0065] The protic solvent may be any solvent capable of at least partially dissolving the first raw material and the second raw material, and may be an aqueous solvent in particular. As the protic solvent, water, alcohol (e.g., ethanol, 1-propanol, isopropanol), carboxylic acid (e.g., acetic acid, formic acid), etc. may be used. The aqueous solvent may be composed of water and a liquid substance compatible with water (e.g., a protic solvent other than water) as appropriate, and is preferably water.

[0066] The first raw material and the second raw material are reacted in a protic solvent. The second raw material may be added to the protic solvent in advance. The ratio of the second raw material to the total of the protic solvent and the second raw material may be, for example, 5% by mass or more, particularly 20% by mass or more, and / or, for example, 80% by mass or less, particularly 50% by mass or less. The first raw material may be further added to the protic solvent to which the second raw material is added and mixed. In this mixture, a reaction to generate MQO is performed. The temperature (reaction temperature) of the mixture (which may include the reaction product) may be, for example, 15° C. or more, particularly 40° C. or more, and / or, for example, 100° C. or less, particularly 80° C. or less. The mixing time (reaction time) may be, for example, 1 day or more, particularly 2 days or more, and / or, for example, 10 days or less, particularly 7 days or less. The mixing may be performed, for example, by using a hot plate stirrer and a warm water bath to maintain the reaction temperature while using a magnetic stirrer to rotate and stir the magnetic stirrer put into the container. However, the treatment operation and conditions (temperature, time, etc.) that enable the reaction to proceed are not limited to the above and can be appropriately selected depending on the first raw material, second raw material, and protic solvent used.

[0067] MQO is generated by the above reaction, and eventually it can grow into MQO nanofibers, and then grow into MQO nanosheets. The present invention is not limited, but the obtained MQO nanofibers can be in the form of nanobelts extending with a nanometer-level width. In addition, a plurality of MQO nanofibers (such as nanobelts) can be combined with each other and / or integrated to grow into nanosheets extending in a two-dimensional shape. In addition, a plurality of MQO nanosheets can overlap each other (for example, by van der Waals forces) to form a laminate. The present invention is not limited by any theory, but the generation and growth of this MQO can be considered to be a bottom-up synthesis reaction (for example, refer to non-patent document 1).

[0068] In the present invention, MQO is a solid component. MQO may be representatively in the form of particles (or powder).

[0069] The mixture after the reaction (also referred to as a reaction mixture) may be subjected to a post-treatment as appropriate, such as washing, applying impact (including applying shear force), drying (such as freeze drying, heat drying), pulverization, etc.

[0070] The washing can be carried out using a protic solvent. The same description as above can be applied to the protic solvent, and the protic solvent can be washed, for example, with water or alcohol. After washing, a separation operation (centrifugation and / or decantation) can be performed. The washing and separation operations can be repeatedly performed until the pH of the supernatant after centrifugation becomes, for example, below 8.

[0071] Depending on the situation, the cleaning may be performed using an aqueous solution of a metal salt instead of or in addition to the above cleaning. The metal salt may be, for example, a halide (fluoride, chloride, bromide, iodide) of an alkali metal (Li, Na, K, etc.), typically LiCl, NaCl, KCl, etc. Specifically, for example, a 1 to 10 molar concentration of a metal salt aqueous solution may be used for cleaning. After cleaning, a separation operation (centrifugation and / or decantation) may be performed. In this case, the cleaning and separation operations may also be repeated as needed until the pH of the supernatant after centrifugation becomes, for example, below 8.

[0072] During and / or after cleaning, shocks such as vibration and / or ultrasound can be applied. This can promote the dispersion of MQO particles (such as nanofibers / nanoflakes, the same below). In the case where MQO particles are agglomerated, they can be broken up. This effect can be significantly achieved when shocks are applied during cleaning with an aqueous solution of a metal salt (it can be considered that metal cations from the metal salt can enter the gaps between the agglomerates and break them up). The shock can be applied, for example, using any one or more of a hand shaker (Japanese: ハンドシェイク), an automatic shaker, a mechanical oscillator, a vortex mixer, a homogenizer, and an ultrasonic bath.

[0073] Since the particles of MQO are solid components, in order to remove the unnecessary liquid components when they are present, a separation operation can be performed at any appropriate time. As the final separation operation, for example, a drying operation can be performed, representative of which is freeze drying or heat drying. Freeze drying can be performed, for example, by freezing a mixture of particles containing MQO and a liquid component at any appropriate temperature (for example, -40°C) and then drying it under a reduced pressure atmosphere. Heat drying can be performed, for example, by drying a mixture of particles containing MQO and a liquid component at a temperature of 25°C or above (for example, below 200°C) under normal pressure or a reduced pressure atmosphere. There is no particular limitation on crushing, and for example, it can be performed using a combination of a mortar and pestle, or an IKA mill, etc. Crushing can be performed after drying.

[0074] Thus, MQO particles can be obtained as a material containing MQO. As MQO particles, for example, nanofibers (and aggregates of MQO nanofibers, such as MQO nanosheets, which are also collectively referred to as "MQO nanofibers, etc.") can be obtained.

[0075] MQO is represented by formula (1), but the material containing MQO (representatively, particles of MQO) does not need to be composed only of the constituent elements of formula (1). The present invention is not limited, but the material containing MQO may contain protons and / or metal cations as needed. In addition, the present invention is not limited, but the material containing MQO may have at least one selected from hydroxyl groups, chlorine atoms, oxygen atoms, hydrogen atoms, and nitrogen atoms as a modification or terminal T present on its surface as needed. In addition, the material containing MQO (representatively, particles of MQO) may have two or more layers, and at least one selected from ammonium ions (e.g., quaternary ammonium cations) and metal cations (e.g., alkali metal ions, alkaline earth metal ions) may exist between these layers.

[0076] Materials containing MQO, such as MQO nanofibers, may contain unreacted first raw material and / or second raw material as impurities, and may also contain substances from the first raw material, the second raw material and / or protic solvents. For example, when a quaternary ammonium salt is used as the second raw material, N may exist (remain) in any form in materials containing MQO, such as MQO nanofibers. This embodiment is not limited, but the material containing MQO may contain ammonium ions and tetramethylammonium ions. In addition, for example, when a MAX raw material is used as the first raw material, in the present invention, the material containing MQO may contain residual A atoms in a smaller amount, for example, less than 10% by mass relative to the original A atoms. The residual amount of A atoms may preferably be less than 8% by mass, and more preferably less than 6% by mass. However, even if the residual amount of A atoms exceeds 10% by mass, there is sometimes no problem depending on the conditions of use.

[0077] In order to obtain MQO nanofibers and other materials containing MQO with higher purity, it is preferred to repeatedly perform multiple washing and centrifugal separation, and recover the supernatant after the final centrifugal separation. The supernatant can be directly or appropriately diluted with a liquid medium, or mixed with a liquid medium after drying to prepare a slurry of MQO particles such as MQO nanofibers containing MQO.

[0078] The core of the present embodiment can be manufactured by shaping (forming, cutting, etc.) a material containing MQO such as MQO nanofibers into a desired shape and size using any appropriate method. Representatively, the core of the present embodiment can be a fiber structure formed using MQO nanofibers, etc. The fiber structure can be manufactured, for example, by applying a slurry of nanofibers containing MQO to a substrate by any appropriate method (such as filtering, spraying, rod coating, spin coating, dipping, etc.), drying it, and then removing the substrate. The liquid medium contained in the above slurry can be appropriately selected, for example, a protic solvent (the same description as above can be applied), a non-protic solvent (such as tetrahydrofuran, dichloromethane, acetonitrile, acetone, N,N-dimethylformamide, dimethyl sulfoxide, etc.), a non-polar solvent (such as hexane, benzene, toluene, diethyl ether, chloroform, ethyl acetate), etc. can be used.

[0079] In this way, the core body of the present embodiment can be obtained. The shape and size of the core body of the present embodiment can be appropriately selected according to the desired use.

[0080] As described above, the material containing MQO may typically have a peak in the range of a diffraction angle 2θ of 2° to 10° in an X-ray diffraction (XRD) spectrum. The present invention is not limited by any theory, but it is considered that the fact that the material containing MQO has a peak in the range of 2θ=2° to 10° in the XRD spectrum means that the MQO has a crystal structure different from that of known metal oxides.

[0081] It should be noted that in the present invention, the XRD spectrum is a spectrum (the vertical axis is intensity and the horizontal axis is 2θ) obtained by scanning in the θ-axis direction using an XRD analysis device using CuKα rays (= about 1.54Å) as characteristic X-rays, and can also be called an "XRD curve". The peaks in the XRD spectrum can be identified visually or using software used in conjunction with the XRD analysis device. In order to measure the XRD spectrum as accurately as possible in the low-angle region of 2θ, it is preferred to set a c-axis oriented MQO film in the XRD analysis device (for example, as in the embodiment described later, for the self-supporting film obtained by removing the filter after suction filtration, the surface in contact with the filter is arranged on the lower side) for measurement.

[0082] This embodiment is not limited to this. For example, the material of this embodiment (more specifically, MQO) may have a Raman shift of at least 275 to 295 cm in a Raman spectrum using a laser beam having a wavelength of 514 nm. -1 、435~455cm -1 and 665~745cm -1 The position has a peak.

[0083] This embodiment is not limited to this. For example, the material of this embodiment (more specifically, MQO) may have a Raman shift of 140 to 160 cm in a Raman spectrum using a laser beam having a wavelength of 514 nm. -1 、275~295cm -1 、435~455cm -1 and 665~745cm -1 It should be noted that the peak is between 140 and 160 cm -1 It is an anatase type peak.

[0084] The present embodiment is not limited, and for example, the material of the present embodiment (more specifically, MQO) has an anatase type or lepidocrocite type crystal structure or a mixture thereof, and more preferably has a lepidocrocite type crystal structure.

[0085] The present embodiment is not limited thereto. For example, the material of the present embodiment (more specifically, MQO) may be such that in a Raman spectrum using a laser beam having a wavelength of 514 nm, at least a Raman shift of 275 to 295 cm -1 、435~455cm -1 and 665~745cm -1 There is a peak at the position of , and when the intensity of each peak is represented by X, Y, and Z, X is the largest.

[0086] The present embodiment is not limited thereto, but it is more preferable that the material of the present embodiment (more specifically, MQO) has a Raman shift of at least 180 to 200 cm in a Raman spectrum using a laser beam having a wavelength of 514 nm. -1 、275~295cm -1 、375~395cm -1 、435~455cm -1 and 665~745cm -1 There is a peak at the position of , and when the intensity of each peak is defined as V, X, Y, Z, and W, X is the largest.

[0087] It should be noted that, in the present invention, Raman spectrum is a spectrum measured by a Raman spectrometer using a laser with a wavelength of 514 nm as an excitation light source (the vertical axis is intensity and the horizontal axis is Raman shift). The peaks in the Raman spectrum can be identified visually or using software used with the Raman spectrometer.

[0088] The particle size of MQO particles may be, for example, 0.01 nm or more, particularly 0.1 nm or more, and further 1 nm or more, and / or may be, for example, less than 1000 nm, particularly less than 100 nm, and further less than 50 nm. Such particles may also be referred to as nanoparticles.

[0089] The MQO particles are in the form of nanofibers and / or two-dimensional materials. The two-dimensional materials include one or more of nanosheets and nanosheet stacks. In the present embodiment, the two-dimensional materials are not limited to nanosheets and nanosheet stacks.

[0090] According to the present embodiment, a core is provided that includes a material containing MQO, typically particles of MQO (e.g., nanofibers / nanoflakes), such as nanofibers of MQO (and, depending on the situation, aggregates of nanofibers of MQO, such as nanoflakes of MQO). For example, the nanofibers of MQO have a hydrophilic surface and have nanometer-scale cross-sectional dimensions. The core that includes the nanofibers of MQO has a large force (e.g., suction force) to attract a working fluid in a liquid state through a capillary phenomenon, and therefore, can transport the working fluid in a liquid state at a relatively high speed (e.g., suction). It is believed that the reason for this is that, due to the nanometer-scale cross-sectional dimensions, the volume density of the nanofibers in the core is high, a narrow space (flow path of the working fluid) is formed through the gaps between the nanofibers, and the total surface area of ​​the nanofibers that can contact the working fluid in a liquid state becomes larger; due to the hydrophilic surface, the working fluid in a liquid state (representatively, water, but not limited to this) can easily wet and spread relative to the surface of the nanofibers of MQO.

[0091] In the present invention, the "nanofiber" of MQO refers to a solid object extending in the length direction, and the outer dimensions of the cross section perpendicular to the length direction (cross-sectional outer dimensions) are nanometer-level (i.e., greater than 1nm and less than 1000nm) or smaller than the sub-nanometer level (less than 1nm, for example, greater than 0.1nm and less than 1nm). The length of the nanofiber of MQO in the length direction is not particularly limited. That is, the length of the nanofiber in the length direction is not limited to the nanometer level (i.e., greater than 1nm and less than 1000nm), and may also be micrometer-level (greater than 1μm and less than 1000μm). The cross-sectional outer dimensions of the nanofiber may be, for example, greater than 0.1nm, particularly greater than 1nm, for example, less than 100nm, particularly less than 50nm, and preferably less than 15nm. A core body including nanofibers of MQO having such a small cross-sectional outer dimension can transport a working fluid in a liquid state at a greater speed. This embodiment is not limited, but according to the above-mentioned manufacturing method, nanofibers of MQO having such a small cross-sectional outer dimension can be achieved.

[0092] In the present invention, the cross-sectional dimensions of the nanofiber of MQO refer to the shortest distance through the center in the cross section that crosses the length direction of the nanofiber of MQO. The shape of the cross section of the nanofiber of MQO is not particularly limited, for example, it can be approximately rectangular (rectangular, square, etc.), elliptical (flat circle, perfect circle, etc.). In the case where the nanofiber of MQO is in the form of a nanobelt, the shape of its cross section can be approximately rectangular, and the cross-sectional dimensions can be equivalent to the short side length of the rectangle. In the case where the nanofiber of MQO is in the form of a nanowire, the shape of its cross section can be approximately flat circle, and the cross-sectional dimensions can be equivalent to the short diameter length of the flat circle.

[0093] The BET specific surface area of ​​a material including MQO, such as MQO nanofibers, is not particularly limited, and may be, for example, 10 m 2 / g and above and 500m 2 The BET specific surface area is calculated by the BET formula based on the isothermal adsorption curve of nitrogen or the above-mentioned other gas at liquid nitrogen temperature (77K) by using the adsorption method of nitrogen or other appropriate gas (such as krypton (Kr) gas, etc.).

[0094] In the present invention, "two-dimensional material" refers to a solid material having a two-dimensionally extended surface (also referred to as a plane, a two-dimensional sheet plane) and a thickness that is smaller than the maximum size of the surface (corresponding to the "in-plane size" of the particle), and a thickness of nanometer level (i.e., 1 nm or more and less than 1000 nm) or a sub-nanometer level (less than 1 nm, for example, 0.1 nm or more and less than 1 nm) smaller than it. The above-mentioned in-plane size is not limited to the nanometer level (i.e., 1 nm or more and less than 1000 nm), and may also be micrometer level (1 μm or more and less than 1000 μm). Two-dimensional materials include one or more of the nanosheets and nanosheet stacks as described above. Nanosheets may also be referred to as nanosheets or two-dimensional (nano) sheets. The thickness of a layer of nanosheets may be, for example, 0.01 nm or more, particularly 0.8 nm or more, for example, 20 nm or less, particularly 3 nm or less. The in-plane size of the nanosheet may be, for example, 0.1 μm or more, particularly 1 μm or more, for example, 200 μm or less, particularly 40 μm or less. Nanosheets can be constructed by agglomeration of nanofibers.

[0095] The stack of nanosheets may also be referred to as multilayer MQO. The distance (interlayer distance or gap size) between two adjacent nanosheets (or two adjacent layers of MQO) is not particularly limited.

[0096] It should be noted that the above-mentioned dimensions (processed by methods such as focused ion beam (FIB) when necessary) can be obtained as the number average size (the number average of at least 40) based on the photographs observed by scanning electron microscope (SEM), transmission electron microscope (TEM) or atomic force microscope (AFM), or the distance in the actual space calculated from the position in the reciprocal lattice space of the (002) plane measured by X-ray diffraction (XRD) method. In the present invention, for example, the cross-sectional external dimensions of the MQO nanofibers are obtained as follows: the cross-section of the core of the MQO nanofibers is exposed by methods such as focused ion beam (FIB), the exposed cross-section is photographed by scanning electron microscope (SEM) and transmission electron microscope (TEM), and in the obtained image, at least 40 MQO nanofibers that appear in the cross-section in the length direction of the MQO nanofibers are extracted, thereby obtaining the number average of the cross-sectional external dimensions of the MQO nanofibers.

[0097] However, it should be noted that in the present invention, the MQO is not limited to the above-mentioned form, but may have any suitable form.

[0098] (Embodiment 2: Heat Transfer Device)

[0099] This embodiment relates to a heat transfer device. In the present invention, a "heat transfer device" refers to a device that transfers heat by using the phase change of a working fluid. The phase change of a working fluid refers to evaporation and condensation.

[0100] Reference Figure 1 The heat transport device 20 of this embodiment includes:

[0101] A housing 1 having a space therein;

[0102] a core 3 disposed in the housing 1; and

[0103] A working fluid (not shown) is sealed in the housing 1 in a state where it can come into contact with the core 3 .

[0104] The core 3 used is the core described in Embodiment 1.

[0105] This embodiment is not limited to Figure 1The heat transfer device 20 is exemplarily shown as a ring-type heat pipe. In the example shown in the figure, the housing 1 includes an evaporator 11, a condenser 13, and a gas flow path 15 and a liquid flow path 17 respectively connecting them. The evaporator 11, the condenser 13, the gas flow path 15 and the liquid flow path 17 integrally constitute the internal space of the housing 1. The core 3 is arranged in the evaporator 11. The working fluid (not shown) is sealed in the internal space of the housing 1. The housing 1 is made of a material having thermal conductivity (for example, metal) at least in the evaporator 11 and the condenser 13.

[0106] In the shell 1, the working fluid evaporates in the evaporator 11 (relatively high temperature portion) supplied with heat from the outside (heat source), and the working fluid in a gaseous state moves in the gas flow path 15, condenses in the condenser 13 (relatively low temperature portion) and releases heat to the outside, and the working fluid in a liquid state is transported (returned) to the evaporator 11 through the liquid flow path 17 by the capillary force of the core 3. Thus, the working fluid circulates in the shell 1 while undergoing phase change. Figure 1 In the figure, the flow of the working fluid is schematically indicated by the dotted arrows, and the supply of heat from the outside (heat input) and the heat dissipation to the outside (heat output) are schematically indicated by the wavy arrows.

[0107] According to this embodiment, in the heat transport device 20, since the core 3 described in Embodiment 1 is used, the working fluid in a liquid state can be transported at a higher speed, a higher heat transport performance can be obtained, and the maximum heat transport amount of the heat transport device 20 is improved.

[0108] exist Figure 1 In the example shown, the heat transfer device 20 is a ring-type heat pipe, but in addition to using the core 3 described in Embodiment 1, the heat transfer device of this embodiment can also apply a known heat transfer device having a core (such as a tubular heat pipe, a heat spreader, etc.).

[0109] The core and the heat transport device in one embodiment of the present invention are described in detail above, but the present invention can be modified in various ways. It should be noted that the core of the present invention can also be manufactured by a method different from the manufacturing method in the above embodiment.

[0110] Example

[0111] (Example 1)

[0112] Example 1 relates to the core of Embodiment 1, which is a core using TiCO nanofibers.

[0113] Preparation of slurry containing TiCO nanofibers

[0114] First, add 1 g of titanium diboride (TiB2, manufactured by AlfaAesar) and 30 mL of a 25% by mass aqueous solution of tetramethylammonium hydroxide (TMAH) (manufactured by Tokyo Chemical Industry Co., Ltd.) to a container (100 mL IBOY (trade name)). Add a stirring piece of approximately the same length (35 mm) as the inner diameter of the circular bottom of the container. While keeping the container at 50°C in a water bath, stir the mixture in the container with a stirring piece and maintain it for 120 hours to allow the reaction to proceed. Next, use a stainless steel spatula to transfer the reaction mixture in the container (without adding liquid media such as ethanol and water) to a 50 mL centrifuge tube. Use a centrifuge to centrifuge at 3500G and 5 minutes to settle the solid component. (i) After centrifugation, discard the supernatant, (ii) add 40 mL of ethanol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) to the sediment remaining in the centrifuge tube, and manually shake (repulp) for 5 minutes, (iii) centrifuge under the same conditions as above. Repeat the operations (i) to (iii) until the pH of the supernatant becomes less than 8. After repeating 3 times, the pH of the supernatant becomes less than 8, so the supernatant is discarded and the repeated operations are terminated. Add 40 mL of pure water to the sediment remaining in the centrifuge tube and vibrate and stir for 15 minutes using an automatic vibrator. Then, use a centrifuge to centrifuge at 3500G and 30 minutes, and recover the supernatant as a sample slurry. The obtained sample slurry corresponds to a slurry containing TiCO nanofibers (refer to the following analysis results).

[0115] ·Core production

[0116] The sample slurry prepared above was filtered overnight using a suction filter. The filter used for the filtration was a membrane filter (Durapore, pore size 0.45 μm, manufactured by Merck Co., Ltd.). After the filtration, the precursor film on the filter was dried overnight at 80°C in a vacuum oven, and the filter was removed to obtain a self-supporting film. The obtained self-supporting film was cut into a rectangle to obtain a core sample with a width (W) of 1 cm, a length (L) of 2 cm, and a thickness (T) of 100 μm.

[0117] Core evaluation

[0118] The core sample prepared above was placed in a petri dish filled with water in a vertically upright state with the WT surface (1 cm × 100 μm) as the upper and lower end surfaces, and immersed in water at a depth of about 1 mm. As a result, water was sucked up to the upper end surface at a speed of 4 mm / s. According to the results, the volume of water sucked up per unit area per unit time of the core sample was 4×10 -3 m 3 / (m 2·s), therefore, the mass of water sucked up per unit area per unit time is 4kg / (m 2 ·s) (Specific gravity of water: 1000kg / m 3 ). The heat of evaporation of water per unit mass at 25°C is 2442 kJ / kg, so the heat taken away by the core sample due to the evaporation of water at 25°C is calculated to be 9768 kW / m 2 That is, the water transport speed of the core sample of Example 1 is 4 mm / s, and the heat transfer performance of water at 25°C is about 10 4 kW / m 2 .

[0119] ·analyze

[0120] The self-supporting film obtained in the same manner as above was analyzed by X-ray photoelectron spectroscopy (XPS), and peaks corresponding to Ti2p, C1s, O1s, and N1s were observed in the obtained XPS spectrum, and thus Ti, C, O, and N were detected. N is considered to be a residual component of TMAH of the raw material, and thus the material of the self-supporting film is considered to be composed of Ti, C, and O.

[0121] In addition, the self-supporting film obtained in the same manner as above was measured using an XRD device (MiniFlex manufactured by Rigaku Corporation) to obtain an XRD curve (characteristic X-ray: CuKα=1.54Å). The obtained XRD spectrum is shown in FIG. Figure 2 .according to Figure 2 It can be appreciated that this material has a peak at 2θ=7.26°.

[0122] In addition, 0.01 g of the slurry containing TiCO nanofibers obtained in the same manner as above and 1 g of pure water were added to a centrifuge tube, and the mixture was vibrated and stirred for 5 minutes using an automatic vibrator. The obtained slurry was dropped onto an alumina porous substrate (manufactured by Cytiva), and the TiCO nanofibers were observed using a FE-SEM (S-4800, manufactured by Hitachi High-Tech Co., Ltd.). Figure 3 , showing the FE-SEM image. Figure 3 It will be appreciated that the material has a cross-sectional dimension of approximately 5 nm.

[0123] (Comparative Example 1)

[0124] Comparative Example 1 relates to a core using MXene particles, which are a type of two-dimensional material.

[0125] Preparation of MAX particles (precursor of MXene particles)

[0126] TiC powder, Ti powder and Al powder (all made by Kojun Chemical Research Institute Co., Ltd.) were put into a ball mill with zirconium oxide balls at a molar ratio of 2:1:1 and mixed for 24 hours. The obtained mixed powder was fired at 1350°C for 2 hours under Ar atmosphere. The fired body (block) thus obtained was crushed with an end mill to a maximum size of less than 40μm. Thus, Ti3AlC2 particles as MAX particles were obtained.

[0127] · Precursor etching (ACID method)

[0128] The Ti 3 AlC 2 particles (powder) prepared by the above method were used and etching was performed under the following etching conditions to obtain a solid-liquid mixture (slurry) containing a solid component derived from the Ti 3 AlC 2 powder.

[0129] (Etching conditions)

[0130] Precursor: Ti3AlC2 (sieved with 45μm mesh)

[0131] Etching solution composition: 49% HF 6mL

[0132] H2O 18mL

[0133] HCl (12M) 36mL

[0134] Precursor input amount: 3.0g

[0135] Etching container: 100mL IBOY

[0136] Etching temperature: 35°C

[0137] Etching time: 24h

[0138] Stirrer speed: 400rpm

[0139] Post-etching cleaning

[0140] The slurry was divided into two parts, each of which was inserted into two 50 mL centrifuge tubes. After centrifugation at 3500G using a centrifuge, the supernatant was discarded. 40 mL of pure water was added to the remaining precipitate in each centrifuge tube, and centrifugation was performed again at 3500G to separate and remove the supernatant. This operation was repeated 11 times. After the final centrifugation, the supernatant was discarded to obtain Ti3C2T x - Moisture medium clay.

[0141] Li intercalation

[0142] For Ti3C2T prepared by the above method xThe water-medium clay was subjected to Li intercalation using LiCl as the Li-containing compound under the following conditions and stirring at 20° C. to 25° C. for 12 hours.

[0143] (Conditions for Li intercalation)

[0144] Ti3C2T x - Moisture medium clay (MXene after washing): solid content 0.75g

[0145] LiCl: 0.75g

[0146] Intercalation container: 100mL IBOY

[0147] Temperature: 20°C or higher and 25°C or lower (room temperature)

[0148] Duration: 10h

[0149] Stirrer speed: 800rpm

[0150] ·Delamination

[0151] In the above Ti3C2T x - In the water medium clay, (i) after adding 40 mL of pure water, stir with an oscillator for 15 minutes, (ii) centrifuge at 3500G, and (iii) recover the supernatant as a liquid containing a single layer of MXene. Repeat the operations (i) to (iii) a total of 4 times to obtain a supernatant containing a single layer of MXene. Furthermore, the supernatant was centrifuged at 4300G for 2 hours using a centrifuge, and the supernatant was discarded to obtain a clay containing a single layer and few layers of MXene as a sample containing a single layer and few layers of MXene.

[0152] Preparation of slurry containing MXene particles

[0153] The MXene-containing clay and pure water were mixed in appropriate amounts to prepare a sample slurry having a solid content concentration (MXene particle concentration) of 34 mg / mL. The obtained sample slurry corresponds to a slurry containing MXene particles (MXene-water dispersion).

[0154] ·Core production

[0155] A core sample having a width (W) of 1 cm, a length (L) of 2 cm, and a thickness (T) of 100 μm was obtained in the same manner as in Example 1 except that the sample slurry prepared above was used.

[0156] Core evaluation

[0157] The core sample prepared above was placed in a petri dish filled with water in a vertically upright state with the WT surface (1 cm×100 μm) as the upper and lower end surfaces, and immersed in water at a depth of about 1 mm. As a result, it was completely unable to absorb water (absorption height was zero mm).

[0158] (Comparative Example 2)

[0159] Comparative Example 2 relates to a core body using a sintered body (porous metal sintered body) of metal powder (copper powder).

[0160] ·Core production

[0161] As metal powder, copper powder with an average particle size D50 of 50 μm was used, and acrylic resin (binder) and copper powder were mixed at a volume ratio of 1:1. The obtained mixture was heat-treated at 400°C for 1 hour to burn off the acrylic resin and obtain a porous metal sintered body. The obtained porous metal sintered body was cut to obtain a core sample with a width (W) of 1 cm, a length (L) of 2 cm, and a thickness (T) of 100 μm.

[0162] Core evaluation

[0163] The core sample prepared above was placed in a petri dish filled with water in a vertically upright state with the WT surface (1 cm × 100 μm) as the upper end surface and the lower end surface, and immersed in water at a depth of about 1 mm. As a result, water was sucked up to the upper end surface at a speed of 0.5 mm / s. According to this result, the water transport speed of the core sample of Comparative Example 2 was 0.5 mm / s. By the same calculation as in Example 1, the heat transfer performance of water at 25°C was about 10 3 kW / m 2 .

[0164] (Comparative Example 3)

[0165] Comparative Example 3 relates to a core body of a sintered body (porous metal sintered body) using metal powder (titanium powder).

[0166] ·Core production

[0167] A core sample having a width (W) of 1 cm, a length (L) of 2 cm, and a thickness (T) of 100 μm was obtained in the same manner as in Comparative Example 2 except that titanium powder having an average particle size D50 of 50 μm was used as the metal powder.

[0168] Core evaluation

[0169] The core sample prepared as described above was evaluated in the same manner as in Comparative Example 2. As a result, water was sucked up to the upper end surface at a speed of 0.5 mm / s. According to the results, the water transport speed of the core sample of Comparative Example 3 was 0.5 mm / s, and the heat transfer performance of water at 25°C was about 10 3 kW / m 2 .

[0170] Industrial Applicability

[0171] The core of the present invention can be used to transport the working fluid by capillary force in a heat transport device that utilizes the phase change of the working fluid. The heat transport device of the present invention can be assembled in an electronic device to release (remove) heat from a heat source of the electronic device. However, the core and heat transport device of the present invention can be used not only for these purposes but also for any appropriate purpose.

[0172] <1>

[0173] A core for heat transfer, the core comprising the following formula: MQ a O b Nanofibers of materials represented by

[0174] (Formula MQ a O b wherein M is at least one element selected from Groups 3, 4, 5, 6 and 7,

[0175] Q is at least one element selected from Groups 12, 13, 14, 15 and 16 (excluding O),

[0176] a is greater than or equal to 0 and less than or equal to 2,

[0177] b is greater than 0 and less than 2).

[0178] <2>

[0179] The core according to <1>, wherein the material of the nanofiber has a peak in a range of a diffraction angle 2θ of 2° to 10° in an X-ray diffraction spectrum.

[0180] <3>

[0181] The core according to <1> or <2>, wherein the nanofiber has a cross-sectional outer dimension of 1 nm to 15 nm.

[0182] <4>

[0183] A heat transport device utilizing a phase change of a working fluid, the heat transport device comprising:

[0184] a housing having a space therein;

[0185] The core according to any one of <1> to <3>, which is disposed in the housing; and

[0186] A working fluid is sealed in the housing in a state where the working fluid can come into contact with the core.

[0187] The present invention claims priority based on Japanese Patent Application No. 2022-079566, which is a Japanese patent application. Japanese Patent Application No. 2022-079566 is incorporated into this specification by reference.

[0188] Description of Reference Numerals

[0189] 1: Shell

[0190] 3: Core

[0191] 11: Evaporator

[0192] 13: Condenser

[0193] 15: Gas flow path

[0194] 17: Liquid flow path

[0195] 20: Heat transfer device

Claims

1. A core for heat transfer, the core comprising a material comprising nanofibers and / or a two-dimensional material, wherein the nanofibers and / or the two-dimensional material are represented by the following formula: MQ a O b express, MQ a O b wherein M is at least one element selected from Groups 3, 4, 5, 6 and 7, Q is at least one element selected from Groups 12, 13, 14, 15 and 16, wherein Excluding O, a is greater than or equal to 0 and less than or equal to 2, b is greater than 0 and less than or equal to 2.

2. The core according to claim 1, wherein: The material including the nanofibers and / or the two-dimensional material has a peak in a range of a diffraction angle 2θ of 2° to 10° in an X-ray diffraction spectrum.

3. The core according to claim 1 or 2, wherein: The material including the nanofibers and / or the two-dimensional material has a Raman shift of 140 to 160 cm in a Raman spectrum using a laser with a wavelength of 514 nm. -1 、275~295cm -1 、435~455cm -1 and 665~745cm -1 The position has a peak.

4. The core according to any one of claims 1 to 3, wherein The material including the nanofibers and / or the two-dimensional material has an anatase type or a lepidocrocite type crystal structure, or a mixture of the two types.

5. The core according to any one of claims 1 to 4, wherein: The material including the nanofibers and / or the two-dimensional substance has a lepidocrocite type crystal structure.

6. The core according to any one of claims 1 to 5, wherein: The material containing the nanofibers and / or the two-dimensional material has a Raman shift of at least 180 to 200 cm in a Raman spectrum using a laser with a wavelength of 514 nm. -1 、275~295cm -1 、375~395cm -1 、435~455cm -1 and 665~745cm -1 There is a peak at the position of , and when the intensity of each peak is defined as V, X, Y, Z, and W, X is the largest.

7. The core according to any one of claims 1 to 6, wherein: The nanofiber has a cross-sectional dimension of not less than 1 nm and not more than 15 nm.

8. A heat transport device utilizing a phase change of a working fluid, the heat transport device comprising: a housing having a space therein; The core according to any one of claims 1 to 7, which is arranged in the shell; as well as A working fluid is sealed in the housing in a state where the working fluid can come into contact with the core.

Citation Information

Patent Citations

  • Wick for heat radiation

    JP2020112326A

  • Heat conductive member

    JP2022027310A