Pigment dispersion liquid, photosensitive resin composition, cured product, black matrix, and image display device

A pigment dispersion with controlled water content and dispersant stabilizes the viscosity of photosensitive resin compositions, addressing foreign matter issues and improving the quality of color filter manufacturing.

CN119096172APending Publication Date: 2024-12-06MITSUBISHI CHEM CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380033283.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-22
Filing Date
2023-04-21
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The generation of foreign matter containing pigment aggregates during the repeated application of photosensitive resin compositions leads to defects and resolution issues in the manufacturing of color filters.

Method used

A pigment dispersion containing specific amounts of water, a dispersant, and an organic solvent, with carbon black as the pigment, to achieve viscosity stability and suppress foreign matter generation.

Benefits of technology

The solution provides a photosensitive resin composition with excellent viscosity stability, reducing foreign matter and enhancing the quality of the cured product and image display devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005076972510000271
    Figure BDA0005076972510000271
  • Figure BDA0005076972510000281
    Figure BDA0005076972510000281
  • Figure BDA0005076972510000282
    Figure BDA0005076972510000282
Patent Text Reader

Abstract

Provided is a pigment dispersion which is capable of obtaining a photosensitive resin composition having excellent viscosity stability and suppressed generation of foreign matter derived from a pigment. The pigment dispersion contains (A) a pigment, (B) a dispersant, an organic solvent, and water, the pigment (A) contains carbon black, and the water content of the pigment dispersion is 0.15-0.9 mass%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a pigment dispersion, a photosensitive resin composition, a cured product, a black matrix and an image display device.

[0002] This application claims priority based on Japanese Patent Application No. 2022-070967 filed with the Japan Patent Office on April 22, 2022, and the contents of which are incorporated herein by reference. Background Art

[0003] Color filters usually form a black matrix on the surface of a transparent substrate such as glass or plastic, and then form pixels of three or more different colors such as red, green, and blue in a grid, stripe, or mosaic pattern. The pattern size varies depending on the purpose of the color filter and the color of each color, but is usually around 5 to 700 μm.

[0004] As a representative method for manufacturing color filters, photolithography using a photosensitive resin composition is currently known. In the photolithography, for example, a photosensitive resin composition containing an alkali-soluble resin is coated on a transparent substrate, dried to form a photosensitive resin film, and the photosensitive resin film is exposed to light in a predetermined pattern, developed with an alkaline developer, and then cured by a high-temperature treatment of 200° C. or more to form a pattern.

[0005] The photosensitive resin composition contains a coloring material when used for forming pixels of a color filter, a black matrix, etc. As the coloring material, a pigment such as carbon black or a dye is used (Patent Document 1).

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2012-68613 Summary of the invention

[0009] Problem that the invention aims to solve

[0010] In the manufacture of color filters, the photosensitive resin composition is sometimes repeatedly applied using the same coating device. According to the research of the present inventors, in the case of a photosensitive resin composition containing a pigment, foreign matter containing aggregates of the pigment is sometimes generated on the nozzle surface of the coating device during the repeated application process. Such foreign matter may peel off from the nozzle and adhere to the photosensitive resin film or pattern, causing defects, and there is a concern that it may have an adverse effect on resolution, etc.

[0011] Therefore, an object of the present invention is to provide: a pigment dispersion liquid that can obtain a photosensitive resin composition that has excellent viscosity stability and suppresses the generation of foreign matter derived from the pigment; a photosensitive resin composition that has excellent viscosity stability and suppresses the generation of foreign matter derived from the pigment; and a cured product, a black matrix, and an image display device using the same.

[0012] Solutions for solving problems

[0013] The present inventors have conducted intensive studies to solve the above-mentioned problems, and as a result, have found that the above-mentioned problems can be solved by preparing the pigment into a pigment dispersion containing a specific amount of water in advance. That is, the gist of the present invention is as follows.

[0014] [1] A pigment dispersion comprising (A) a pigment, (B) a dispersant, an organic solvent and water,

[0015] The aforementioned (A) pigment contains carbon black,

[0016] The pigment dispersion has a water content of 0.15% by mass or more and 0.9% by mass or less.

[0017] [2] The pigment dispersion according to [1], wherein the water content is 0.2% by mass or more and 0.7% by mass or less.

[0018] [3] The pigment dispersion according to [1] or [2], wherein the content of the (A) pigment is 60% by mass or more based on the total solid content of the pigment dispersion.

[0019] [4] The pigment dispersion according to any one of [1] to [3], wherein the content ratio of the (A) pigment to the (B) dispersant ((A) pigment / (B) dispersant) based on mass is 4 or more.

[0020] [5] The pigment dispersion according to any one of [1] to [4], further comprising (C) a dispersing aid.

[0021] [6] The pigment dispersion according to [5], wherein the content ratio of the (A) pigment to the (C) dispersing aid ((A) pigment / (C) dispersing aid) based on mass is 10 or more.

[0022] [7] A photosensitive resin composition comprising: the pigment dispersion according to any one of [1] to [6], (D) an alkali-soluble resin, (E) a photopolymerizable compound, and (F) a photopolymerization initiator.

[0023] [8] The photosensitive resin composition according to [7], wherein the content of the pigment (A) is 30% by mass or more based on the total solid content of the photosensitive resin composition.

[0024] [9] A cured product obtained by curing the photosensitive resin composition according to [7] or [8].

[0025]

[10] A black matrix comprising the cured product described in [9].

[0026]

[11] An image display device comprising the cured product described in [9].

[0027] Effects of the Invention

[0028] According to the present invention, there can be provided: a pigment dispersion liquid that can obtain a photosensitive resin composition having excellent viscosity stability and in which generation of foreign matter originating from the pigment is suppressed; a photosensitive resin composition having excellent viscosity stability and in which generation of foreign matter originating from the pigment is suppressed; and a cured product, a black matrix, and an image display device using the same. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is a schematic cross-sectional view showing an example of the organic EL element of the present invention.

[0030] Figure 2 The photographs show the results of the peeling test on the photosensitive resin compositions of Examples 1 to 4 and Comparative Examples 1 and 2. DETAILED DESCRIPTION

[0031] Hereinafter, although embodiment of the present invention is described specifically, the present invention is not limited to the following embodiment, and various modifications can be implemented within the scope of the gist thereof.

[0032] In the present invention, "(meth)acrylic acid" means "acrylic acid and / or methacrylic acid", and the same applies to "(meth)acrylate" and "(meth)acryloyl".

[0033] In the present invention, "total solid content" refers to all components contained in the pigment dispersion or photosensitive resin composition except organic solvent and water. Even if the components except organic solvent and water are liquid at room temperature, such components are not included in the organic solvent and water but are included in the total solid content.

[0034] In the present invention, the "water content" is calculated by the Karl Fischer measurement method described in JIS K0113 (2005). Various moisture meters can be used for the measurement, and an example thereof is MKA-610 manufactured by Kyoto Electronics Industry Co., Ltd.

[0035] In the present invention, (A) the "average particle size" of the pigment is obtained by directly measuring the size of the primary particles based on electron microscope photographs. Specifically, the minor axis diameter and major axis diameter of each primary particle are measured, and the average is used as the particle size of the particle. Then, for more than 100 particles, the volume (mass) of each particle is approximated to a rectangular parallelepiped of the obtained particle size, and the volume average particle size is obtained, which is used as the average particle size. It should be noted that the same result can be obtained using any of a transmission electron microscope (TEM) and a scanning electron microscope (SEM).

[0036] In the present invention, the "weight average molecular weight" refers to a polystyrene-equivalent weight average molecular weight (Mw) based on GPC (gel permeation chromatography).

[0037] In the present invention, "amine value" means the amine value converted to effective solid content unless otherwise specified, and is a value represented by the mass of KOH equivalent to the amount of alkali per 1g of solid content of the dispersant. The measurement method will be described later.

[0038] [Pigment dispersion]

[0039] The pigment dispersion of the present invention contains (A) a pigment, (B) a dispersant, an organic solvent and water.

[0040] The water content of the pigment dispersion of the present invention is 0.15% by mass or more and 0.9% by mass or less relative to the total mass of the pigment dispersion. By setting the water content of the pigment dispersion to 0.9% by mass or less, the viscosity stability is excellent, and the thickening of the pigment dispersion and the associated decrease in filterability can be suppressed. By setting the water content to 0.15% by mass or more, the generation of foreign matter derived from the pigment when forming a pattern using a photosensitive resin composition containing the pigment dispersion can be suppressed.

[0041] The water content of the pigment dispersion is preferably 0.7% by mass or less, more preferably 0.5% by mass or less, and is preferably 0.2% by mass or more, more preferably 0.3% by mass or more.

[0042] The above upper and lower limits may be arbitrarily combined. For example, the content may be 0.2% by mass or more and 0.7% by mass or less, or 0.3% by mass or more and 0.5% by mass or less.

[0043] <(A) Pigments>

[0044] (A) The pigment contains carbon black.

[0045] By containing carbon black, there is a tendency to improve light-shielding properties. On the other hand, foreign matter containing carbon black has a high light-shielding rate, which can adversely affect the resolution of a pattern, for example. Therefore, when the pigment (A) contains carbon black, the usefulness of the present invention is high.

[0046] Examples of carbon black include the following.

[0047] Made by Mitsubishi Chemical Corporation: MA7, MA77, MA8, MA11, MA100, MA100R, MA220, MA230, MA600, #5, #10, #20, #25, #30, #32, #33, #40, #44, #45, #47, #50, #52, #55, #650, #750, #850, #950, #9 60, #970, #980, #990, #1000, #2200, #2300, #2350, #2400, #2600, #3050, #3150, # 3250, #3600, #3750, #3950, #4000, #4010, OIL7B, OIL9B, OIL11B, OIL30B, OIL31B.

[0048] Made by Degussa: Printex (registered trademark. Same as below) 3, Printex 3OP, Printex30, Printex 30OP, Printex 40, Printex 45, Printex 55, Printex 60, Printex 75, Printex80, Printex 85, Printex 90, Printex A, Printex L, Printex G, Printex P, Printex U, Printex V, Printex G, SpecialBlack550, SpecialBlack350, SpecialBlack250, SpecialBlack100, SpecialBlack6, SpecialBlack5, SpecialBlack4, Color Black FW1, Color Black FW2, Color Black FW2V, Color Black FW18, Color Black FW18, ColorBlack FW200, Color Black S160, Color Black S170.

[0049] Manufactured by Cabot Corporation: Monarch (registered trademark, the same below) 120, Monarch 280, Monarch 460, Monarch 800, Monarch 880, Monarch 900, Monarch 1000, Monarch 1100, Monarch 1300, Monarch 1400, Monarch 4630, REGAL (registered trademark, the same below) 99, REGAL 99R, REGAL 415, REGAL 415R, REGAL 250, REGAL 250R, REGAL 330, REGAL 400R, REGAL 550R, REGAL 660R, BLACK PEARLS 480, PEARLS 130, VULCAN (registered trademark) XC72R, ELFTEX (registered trademark) -8.

[0050] Birla Corporation: RAVEN11, RAVEN14, RAVEN15, RAVEN16, RAVEN22, RAVEN30, RAVEN35, RAVEN40, RAVEN410, RAVEN420, RAVEN450, RAVEN500, RAVEN780, RAVEN850, RAVEN890H, RAVEN1000, R AVEN1020, RAVEN1040, RAVEN1060U, RAVEN1080U, RAVEN1170, RAVEN1190U, RAVEN1250, RAVEN1500, RAVEN2000, RAVEN2500U, RAVEN3500, RAVEN5000, RAVEN5250, RAVEN5750, RAVEN7000.

[0051] Carbon black can be carbon black covered with resin. If carbon black covered with resin is used, the adhesion to the glass substrate and the volume resistance value are improved. As carbon black covered with resin, for example, carbon black described in Japanese Patent Publication No. 09-71733 can be suitably used. In terms of volume resistance and dielectric constant, it is preferred to use carbon black covered with resin.

[0052] As carbon black for resin-based coating treatment, the total content of Na and Ca is preferably 100 ppm or less. Carbon black usually contains ash composed of Na, Ca, K, Mg, Al, Fe, etc. mixed from raw material oil, combustion oil (or gas), reaction stop water, granulation water, and furnace materials of the reactor during manufacturing in the order of percentage. Among them, Na and Ca are usually contained in excess of several hundred ppm, and by reducing them, there is a tendency to suppress penetration into the transparent electrode (ITO) and other electrodes to prevent electrical short circuits.

[0053] As a method for reducing the content of ash containing Na and Ca, the raw material oil, fuel oil (or gas) and reaction stop water when manufacturing carbon black can be strictly selected as substances with very low content and the amount of alkaline substances added to adjust the structure can be reduced as much as possible. As another method, the method of washing the carbon black produced from the furnace with water, hydrochloric acid, etc. to dissolve and remove Na and Ca can be cited.

[0054] Specifically, after carbon black is mixed and dispersed in water, hydrochloric acid or hydrogen peroxide water, when a poorly soluble solvent is added to the water, the carbon black is transferred to the solvent side and completely separated from the water, and most of the Na and Ca present in the carbon black are dissolved in the water and acid and removed. In order to reduce the total amount of Na and Ca to less than 100 ppm, sometimes the carbon black manufacturing process of strictly selecting raw materials or the water or acid dissolution method can be carried out alone, but by combining these two methods, the total amount of Na and Ca can be more easily reduced to less than 100 ppm.

[0055] The resin-coated carbon black is preferably a so-called acidic carbon black with a pH of less than 6. Since the dispersion diameter (agglomerate diameter) in water becomes smaller, it can cover even fine units, which is suitable. Furthermore, the average particle size is preferably less than 40nm. In addition, the dibutyl phthalate (DBP) absorption is preferably less than 140mL / 100g. By making the average particle size and DBP absorption within the above range, there is a tendency to obtain a coating film with good light-shielding properties.

[0056] The method for preparing the resin-coated carbon black is not particularly limited. For example, the following method can be used: after appropriately adjusting the mixing amount of carbon black and resin,

[0057] 1. A method of mixing and stirring a resin solution obtained by mixing a resin with a solvent such as cyclohexanone, toluene, or xylene and heating and dissolving the resin, and a suspension obtained by mixing carbon black with water, separating the carbon black from the water, removing the water, and heating and kneading the mixture, forming the obtained composition into a sheet, crushing it, and then drying it;

[0058] 2. A method in which the resin solution prepared in the same manner as above is mixed and stirred with the suspension to granulate the carbon black and the resin, and then the obtained granules are separated and heated to remove the residual solvent and water;

[0059] 3. A method in which a carboxylic acid such as maleic acid or fumaric acid is dissolved in the solvent exemplified above, carbon black is added and mixed, and the mixture is dried, and after removing the solvent to obtain carboxylic acid-impregnated carbon black, a resin is added thereto for dry mixing;

[0060] 4. A method in which a monomer component containing reactive groups constituting a covering resin is stirred at high speed with water to prepare a suspension, and after polymerization, the suspension is cooled. After obtaining a resin containing reactive groups from the polymer suspension, carbon black is added thereto for mixing to react the carbon black with the reactive groups (to graft the carbon black), followed by cooling and pulverizing.

[0061] The type of resin to be coated is not particularly limited, but is generally a synthetic resin. In addition, resins having a benzene ring in their structure are preferred from the viewpoints of dispersibility and dispersion stability because they have a stronger amphoteric surfactant effect.

[0062] As synthetic resins, for example, thermosetting resins such as phenolic resins, melamine resins, xylene resins, diallyl phthalate resins, glyoxal resins, epoxy resins, and alkylbenzene resins can be used; thermoplastic resins such as polystyrene, polycarbonate, polyethylene terephthalate, polybutylene terephthalate, modified polyphenylene ether, polysulfone, poly-p-phenylene terephthalamide, polyamide-imide, polyimide, polyaminobismaleimide, polyphenylsulfone, polyarylate, and polyetheretherketone can be used. The amount of carbon black covered by the resin is preferably 1 to 30% by mass relative to the total amount of carbon black and resin. By setting it above the lower limit, there is a tendency to be able to cover sufficiently. On the other hand, by setting it below the upper limit, there is a tendency to be able to prevent the adhesion of the resins to each other and to make the dispersibility good.

[0063] The carbon black coated with resin can be used as a shading material for a coloring spacer according to a conventional method, and a color filter with the coloring spacer as a component can be made by a conventional method. When such carbon black is used, there is a tendency to realize a coloring spacer with high shading rate and low surface reflectivity at low cost. It can also be inferred that by covering the surface of the carbon black with resin, it also has the effect of enclosing Ca and Na in the carbon black.

[0064] As the (A) pigment other than carbon black, for example, pigments of various colors used as a coloring material for coloring a photosensitive resin composition can be used.

[0065] Examples of the pigment include blue pigments, green pigments, red pigments, yellow pigments, violet pigments, orange pigments, brown pigments, and black pigments. These pigments may be organic pigments or inorganic pigments.

[0066] The structure of the organic pigment is not particularly limited, and examples thereof include azo-based, phthalocyanine-based, quinacridone-based, benzimidazolone-based, isoindolinone-based, dioxazine-based, indanthrene-based, and perylene-based pigments.

[0067] Specific examples of the (A) pigment are shown below by pigment numbers. Terms such as "CI Pigment Red 2" listed below refer to the Color Index (CI).

[0068] Examples of the red pigment include CI Pigment Red 1, 2, 3, 4, 5, 6, 7, 8, 9, 12, 14, 15, 16, 17, 21, 22, 23, 31, 32, 37, 38, 41, 47, 48, 48:1, 48:2, 48:3, 48:4, 49, 49:1, 49:2, 50:1, 52:1, 52:2, 53, 53:1, 53:2, 53: 3, 57, 57:1, 57:2, 58:4, 60, 63, 63:1, 63:2, 64, 64:1, 68, 69, 81, 81:1, 81:2, 81:3, 81:4, 83, 88, 90:1, 101, 101:1, 104, 108, 108:1, 109, 112, 113, 114, 122, 123, 144, 146, 147, 1 49, 151, 166, 168, 169, 170, 172, 173, 174, 175, 176, 177, 178, 179, 181, 184, 185, 187, 188, 190, 193, 194, 200, 202, 206, 207, 208, 209, 210, 214, 216, 220, 221, 224, 230, 231, 232 2, 233, 235, 236, 237, 238, 239, 242, 243, 245, 247, 249, 250, 251, 253, 254, 255, 256, 257, 258, 259, 260, 262, 263, 264, 265, 266, 267, 268, 269, 270, 271, 272, 273, 274, 275, 276. Preferred examples include CI Pigment Red 48:1, 122, 168, 177, 202, 206, 207, 209, 224, 242, and 254, and more preferred examples include CI Pigment Red 177, 209, 224, and 254.

[0069] Examples of the blue pigment include CI Pigment Blue 1, 1:2, 9, 14, 15, 15:1, 15:2, 15:3, 15:4, 15:6, 16, 17, 19, 25, 27, 28, 29, 33, 35, 36, 56, 56:1, 60, 61, 61:1, 62, 63, 66, 67, 68, 71, 72, 73, 74, 75, 76, 78, and 79. Preferably, CI Pigment Blue 15, 15:1, 15:2, 15:3, 15:4, 15:6, and 60 are included, and more preferably, CI Pigment Blue 15:6 and 60 are included.

[0070] Examples of the green pigment include CI Pigment Green 1, 2, 4, 7, 8, 10, 13, 14, 15, 17, 18, 19, 26, 36, 45, 48, 50, 51, 54, 55, and 58. Preferably, CI Pigment Green 7, 36, and 58 are mentioned.

[0071] Examples of yellow pigments include CI Pigment Yellow 1, 1:1, 2, 3, 4, 5, 6, 9, 10, 12, 13, 14, 16, 17, 24, 31, 32, 34, 35, 35:1, 36, 36:1, 37, 37:1, 40, 41, 42, 43, 48, 53, 55, 61, 62, 62:1, 63, 65, 73, 74, 75, 81, 83, 87, 93, 94, 95, 97, 100, 101, 104, 105, 108, 109, 110, 111, 116, 117, 119, 120, 126, 127, 127:1, 128, 129, 133, 1 34, 136, 138, 139, 142, 147, 148, 150, 151, 153, 154, 155, 157, 158, 159, 160, 161, 162, 163, 164, 165, 166, 167, 168, 169, 170, 172, 173, 174, 175, 176, 180, 181, 182, 183, 184, 185, 188, 189, 190, 191, 191: 1, 192, 193, 194, 195, 196, 197, 198, 199, 200, 202, 203, 204, 205, 206, 207, 208. Preferred examples include CI Pigment Yellow 83, 117, 129, 138, 139, 150, 154, 155, 180, and 185, and more preferred examples include CI Pigment Yellow 83, 138, 139, 150, and 180.

[0072] Examples of the orange pigment include CI Pigment Orange 1, 2, 5, 13, 16, 17, 19, 20, 21, 22, 23, 24, 34, 36, 38, 39, 43, 46, 48, 49, 61, 62, 64, 65, 67, 68, 69, 70, 71, 72, 73, 74, 75, 77, 78, and 79. Preferably, CI Pigment Orange 38, 64, and 71 are used.

[0073] Examples of the violet pigment include CI Pigment Violet 1, 1:1, 2, 2:2, 3, 3:1, 3:3, 5, 5:1, 14, 15, 16, 19, 23, 25, 27, 29, 31, 32, 37, 39, 42, 44, 47, 49, and 50. Preferably, CI Pigment Violet 19, 23, and 29 are used, and more preferably, CI Pigment Violet 23 and 29 are used.

[0074] As the black pigment, a pigment that exhibits black by mixing a plurality of color pigments (for example, three colors of red, green, and blue) may be used, a pigment that exhibits black alone may be used alone, or a combination of these may be used.

[0075] Examples of pigments that can be used in combination to prepare black pigments include Victoria Pure Blue (42595), Auramine O (41000), Cation Brilliant Flavin (Basic 13), Rhodamine 6GCP (45160), Rhodamine B (45170), Safranine OK 70:100 (50240), Wool Red X (42080), No. 120 / Lionol Yellow (21090), Lionol Yellow GRO (21090), SYMULER Fast Yellow 8GF (21105), Benzidine Yellow 4T-564D (21095), SYMULER FastRed 4015 (12355), Lionol Red 7B4401 (15850), Fastogen Blue TGR-L (74160), Leonor Blue SM (26150), Leonor Blue ES (Pigment Blue 15:6), LIONOGEN RED GD (Pigment Red 168), Leonor Green 2YS (Pigment Green 36).

[0076] It should be noted that the numbers in () above refer to the color index (CI).

[0077] Other pigments that can be mixed and used are represented by CI numbers, for example, CI yellow pigments 20, 24, 86, 93, 109, 110, 117, 125, 137, 138, 147, 148, 153, 154, 166, CI orange pigments 36, 43, 51, 55, 59, 61, 64, CI red pigments 9, 97, 122, 123, 149, 168, 177, 180, 192, 215, 216, 217, 220, 223, 224, 226, 227, 228, 240, 254, CI violet pigments 19, 23, 29, 30, 37, 40, 50, CI blue pigments 15, 15:1, 15:4, 22, 60, 64, CI green pigment 7, and CI brown pigments 23, 25, 26.

[0078] Examples of the black pigment that can be used alone include lamp black, bone black, graphite, iron oxide-based black pigments (iron black and the like), aniline black, cyanine black, titanium black, perylene black, and lactam black.

[0079] As the (A) pigment, for example, barium sulfate, lead sulfate, titanium oxide, yellow lead, red iron, and chromium oxide can also be used.

[0080] These various pigments may be used in combination of two or more. For example, in order to adjust the chromaticity, a green pigment and a yellow pigment may be used in combination, or a blue pigment and a violet pigment may be used in combination.

[0081] The average particle size of the pigment (A) is not particularly limited as long as the desired color development can be achieved in the case of a color filter color layer, and varies depending on the type of pigment used, but is preferably in the range of 10 to 100 nm, and more preferably in the range of 10 to 70 nm. By setting the average particle size of the pigment (A) to the above range, there is a tendency to make the color characteristics of a liquid crystal display device manufactured using a photosensitive resin composition containing the pigment dispersion of the present invention high quality.

[0082] The average particle size of carbon black is preferably 60 nm or less, more preferably 50 nm or less, and preferably 20 nm or more, for example, preferably 20 to 50 nm, and more preferably 20 to 60 nm. By setting the average particle size to be below the upper limit, there is a tendency that scattering becomes smaller and the color characteristics such as light shielding and contrast can be suppressed from being reduced. In addition, by setting the average particle size to be above the lower limit, the amount of dispersant (B) does not need to be too much, and there is a tendency that the dispersibility becomes good.

[0083] The content of the pigment (A) is preferably 60% by mass or more, more preferably 70% by mass or more, and further preferably 80% by mass or more relative to the total solid content in the pigment dispersion, and is preferably 99% by mass or less, more preferably 95% by mass or less, and further preferably 90% by mass or less. If the content of the pigment (A) is above the lower limit, the light shielding property of the obtained cured product tends to be more excellent, and if it is below the upper limit, the dispersibility tends to be more excellent.

[0084] The above upper and lower limits may be arbitrarily combined, for example, 60 to 99% by mass, 70 to 95% by mass, or 80 to 90% by mass.

[0085] The content of carbon black is preferably 90% by mass or more, more preferably 95% by mass or more, further preferably 99% by mass or more, and may be 100% by mass, relative to the total mass of the pigment (A).

[0086] <(B) Dispersant>

[0087] The (B) dispersant finely disperses the (A) pigment and stabilizes the dispersion state.

[0088] As the (B) dispersant, a polymer dispersant having a functional group is preferred. Furthermore, from the perspective of dispersion stability, a polymer dispersant having, for example, a carboxyl group; a phosphoric acid group; a sulfonic acid group; or a salt thereof; a primary, secondary or tertiary amino group; a quaternary ammonium salt group; or a group derived from a nitrogen-containing heterocyclic ring such as pyridine, pyrimidine, or pyrazine is preferred. In particular, a polymer dispersant having a basic functional group such as a primary, secondary or tertiary amino group; a quaternary ammonium salt group; or a group derived from a nitrogen-containing heterocyclic ring such as pyridine, pyrimidine, or pyrazine is preferred. By using these polymer dispersants having a basic functional group, there is a tendency to improve dispersibility.

[0089] Examples of the polymer dispersant include urethane dispersants, acrylic acid dispersants, polyethyleneimine dispersants, polyallylamine dispersants, dispersants containing monomers and macromonomers having an amino group, polyoxyethylene alkyl ether dispersants, polyoxyethylene diester dispersants, polyether phosphate dispersants, polyester phosphate dispersants, sorbitan aliphatic ester dispersants, and aliphatic modified polyester dispersants.

[0090] Examples of the dispersant include EFKA (registered trademark, manufactured by EFKA Chemicals (EFKA)), DISPERBYK (registered trademark, manufactured by BYK-Chemie), DISPARLON (registered trademark, manufactured by Kusumoto Chemicals Co., Ltd.), SOLSPERSE (registered trademark, manufactured by Lubrizol Corporation), KP (manufactured by Shin-Etsu Chemical Co., Ltd.), POLYFLOW or FLOWLEN (registered trademark, manufactured by Kyoeisha Chemical Co., Ltd.), and AJISPER (registered trademark, manufactured by Ajinomoto Fine-Techno Co., Inc.).

[0091] The polymer dispersants may be used alone or in combination of two or more.

[0092] In terms of adhesion and linearity, the dispersant preferably includes a carbamate polymer dispersant and / or an acrylic polymer dispersant having a basic functional group, and in terms of adhesion, a carbamate polymer dispersant is more preferably included. In addition, in terms of dispersibility and storage properties, a polymer dispersant having a basic functional group and a polyester and / or polyether bond is preferred.

[0093] The weight average molecular weight (Mw) of the polymer dispersant is preferably 700 or more, more preferably 1000 or more, and preferably 100000 or less, more preferably 50000 or less, and further preferably 30000 or less. By setting it to be below the above upper limit, there is a tendency that alkali developability becomes good even when the pigment concentration is high.

[0094] The above upper and lower limits may be arbitrarily combined, for example, 700 to 100,000, 700 to 50,000, or 1,000 to 30,000.

[0095] Examples of urethane or acrylic polymer dispersants include DISPERBYK 160 to 167, 182 series (all urethane series), DISPERBYK 2000, 2001, etc. (all acrylic series) (all manufactured by BYK-Chemie). Among urethane polymer dispersants having a basic functional group and polyester and / or polyether bonds, DISPERBYK 167 and 182 are particularly preferred polymer dispersants having a weight average molecular weight of 30,000 or less.

[0096] Examples of the urethane polymer dispersant include dispersion resins having a weight average molecular weight of 1,000 to 200,000 obtained by reacting a polyisocyanate compound with a compound having one or two hydroxyl groups in the molecule and having a number average molecular weight of 300 to 10,000 and a compound having active hydrogen and a tertiary amino group in the same molecule.

[0097] Examples of the polyisocyanate compound include aromatic diisocyanates such as p-phenylene diisocyanate, 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, 4,4'-diphenylmethane diisocyanate, naphthalene-1,5-diisocyanate, and dimethylbiphenyl diisocyanate; aliphatic diisocyanates such as hexamethylene diisocyanate, lysine methyl ester diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, and dimer acid diisocyanate; isophorone diisocyanate, 4,4'-methylenebis(cyclohexyl isocyanate), ω,ω'-diisocyanate, and the like. alicyclic diisocyanates such as ester dimethylcyclohexane, aliphatic diisocyanates having aromatic rings such as xylylene diisocyanate, α,α,α',α'-tetramethylxylylene diisocyanate, lysine ester triisocyanate, 1,6,11-undecane triisocyanate, 1,8-diisocyanate-4-isocyanate methyloctane, 1,3,6-hexamethylene triisocyanate, dicycloheptane triisocyanate, tris(isocyanate phenylmethane), tris(isocyanate phenyl)thiophosphate, and trimers thereof, water adducts thereof, and polyol adducts thereof. Trimers of organic diisocyanates are preferred, and trimers of toluene diisocyanate and trimers of isophorone diisocyanate are more preferred.

[0098] The polyisocyanate may be used alone or in combination of two or more.

[0099] As a method for producing a trimer of isocyanate, for example, the following method can be cited: a polyisocyanate is partially trimerized with an appropriate trimerization catalyst, such as tertiary amines, phosphines, alkoxides, metal oxides, carboxylates, etc., and after the trimerization is stopped by adding a catalyst poison, the unreacted polyisocyanate is removed by solvent extraction and thin film distillation to obtain the target isocyanurate group-containing polyisocyanate.

[0100] Examples of the compound having one or two hydroxyl groups in the same molecule and having a number average molecular weight of 300 to 10,000 include polyether diols, polyester diols, polycarbonate diols, polyolefin diols, and compounds in which one terminal hydroxyl group of these compounds is alkoxylated with an alkyl group having 1 to 25 carbon atoms.

[0101] The compound having one or two hydroxyl groups in the same molecule and having a number average molecular weight of 300 to 10,000 may be used alone or in combination of two or more.

[0102] Examples of the polyether diol include polyether diol and polyether ester diol.

[0103] Examples of the polyether diol include compounds obtained by using an alkylene oxide alone or in a copolymer, such as polyethylene glycol, polypropylene glycol, polyethylene-propylene glycol, polyoxytetramethylene glycol, polyoxyhexamethylene glycol, and polyoxyoctamethylene glycol.

[0104] Examples of the polyetherester diol include compounds obtained by reacting an ether group-containing diol or a mixture with other diols with dicarboxylic acids or anhydrides thereof, or reacting a polyester diol with an alkylene oxide, such as poly(polyoxytetramethylene) adipate.

[0105] As the polyether diol, polyethylene glycol, polypropylene glycol, polyoxytetramethylene glycol, or a compound in which one terminal hydroxyl group of these compounds is alkoxylated with an alkyl group having 1 to 25 carbon atoms.

[0106] Examples of the polyester diol include those obtained by reacting dicarboxylic acids (succinic acid, glutaric acid, adipic acid, sebacic acid, fumaric acid, maleic acid, phthalic acid, etc.) or anhydrides thereof with diols (ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, 3-methyl-1,5-pentanediol, neopentyl glycol, 2-methyl-1,3-propanediol, 2-methyl-2-propyl-1,3-propanediol, 2-butyl-2-ethyl-1,3-propanediol, 1,5-pentanediol, 1,6-hexanediol, 2-methyl-2,4-pentanediol, 2,2,4-trimethyl-1,3-pentanediol, 2-ethyl-1,3-propanediol, Compounds obtained by polycondensation of aliphatic diols such as 1,3-hexanediol, 2,5-dimethyl-2,5-hexanediol, 1,8-octamethylene glycol, 2-methyl-1,8-octamethylene glycol, 1,9-nonanediol, alicyclic diols such as bishydroxymethylcyclohexane, aromatic diols such as xylylene glycol and bishydroxyethoxybenzene, N-alkyldialkanolamines such as N-methyldiethanolamine, such as polyethylene adipate, polybutylene adipate, polyhexamethylene adipate, polyethylene / propylene adipate, or the like, or polylactone diols or polylactone monools obtained by using the above diols or monools having 1 to 25 carbon atoms as initiators, such as polycaprolactone diol and polymethylvalerolactone.

[0107] As the polyester diol, polycaprolactone diol or polycaprolactone produced by using an alcohol having 1 to 25 carbon atoms as an initiator is preferred.

[0108] Examples of the polycarbonate diol include poly(1,6-hexanediol) carbonate and poly(3-methyl-1,5-pentanediol) carbonate, and examples of the polyolefin diol include polybutadiene diol, hydrogenated polybutadiene diol, and hydrogenated polyisoprene diol.

[0109] The number average molecular weight of the compound having one or two hydroxyl groups in the same molecule is preferably 300 to 10,000, more preferably 500 to 6,000, and even more preferably 1,000 to 4,000.

[0110] Examples of active hydrogen in a compound having active hydrogen and a tertiary amino group in the same molecule, i.e., a hydrogen atom directly bonded to an oxygen atom, a nitrogen atom or a sulfur atom, include hydrogen atoms in functional groups such as a hydroxyl group, an amino group, and a thiol group. Preferably, there are hydrogen atoms in an amino group, and particularly preferably, hydrogen atoms in a primary amino group.

[0111] The tertiary amino group in the compound having active hydrogen and a tertiary amino group in the same molecule is not particularly limited, and examples thereof include an amino group having an alkyl group having 1 to 4 carbon atoms, and a heterocyclic structure such as an imidazole ring or a triazole ring.

[0112] Examples of the compound having active hydrogen and a tertiary amino group in the same molecule include N,N-dimethyl-1,3-propylenediamine, N,N-diethyl-1,3-propylenediamine, N,N-dipropyl-1,3-propylenediamine, N,N-dibutyl-1,3-propylenediamine, N,N-dimethylethylenediamine, N,N-diethylethylenediamine, N,N-dipropylethylenediamine, N,N-dibutylethylenediamine, N,N-dimethyl-1,4-butanediamine, N,N-diethyl-1,4-butanediamine, N,N-dipropyl-1,4-butanediamine, and N,N-dibutyl-1,4-butanediamine.

[0113] When the tertiary amino group is a nitrogen-containing heterocyclic structure, for example, a nitrogen-containing five-membered heterocyclic ring such as a pyrazole ring, an imidazole ring, a triazole ring, a tetrazole ring, an indole ring, a carbazole ring, an indazole ring, a benzimidazole ring, a benzotriazole ring, a benzoxazole ring, a benzothiazole ring, a benzothiadiazole ring, and a nitrogen-containing six-membered heterocyclic ring such as a pyridine ring, a pyridazine ring, a pyrimidine ring, a triazine ring, a quinoline ring, an acridine ring, and an isoquinoline ring can be cited. As the nitrogen-containing heterocyclic ring, an imidazole ring and a triazole ring are preferred.

[0114] Examples of the compound having an imidazole ring and an amino group include 1-(3-aminopropyl)imidazole, histidine, 2-aminoimidazole, and 1-(2-aminoethyl)imidazole.

[0115] Examples of the compound having a triazole ring and an amino group include 3-amino-1,2,4-triazole, 5-(2-amino-5-chlorophenyl)-3-phenyl-1H-1,2,4-triazole, 4-amino-4H-1,2,4-triazole-3,5-diol, 3-amino-5-phenyl-1H-1,3,4-triazole, 5-amino-1,4-diphenyl-1,2,3-triazole, and 3-amino-1-benzyl-1H-2,4-triazole.

[0116] As the compound having active hydrogen and a tertiary amino group in the same molecule, N,N-dimethyl-1,3-propylenediamine, N,N-diethyl-1,3-propylenediamine, 1-(3-aminopropyl)imidazole, and 3-amino-1,2,4-triazole are preferred.

[0117] The compound having active hydrogen and a tertiary amino group in the same molecule may be used alone or in combination of two or more.

[0118] The preferred blending ratio of the raw materials when manufacturing the carbamate polymer dispersant is: relative to 100 parts by mass of the polyisocyanate compound, the compound having a number average molecular weight of 300 to 10,000 and having one or two hydroxyl groups in the same molecule is 10 to 200 parts by mass, preferably 20 to 190 parts by mass, and more preferably 30 to 180 parts by mass, and the compound having active hydrogen and tertiary amino groups in the same molecule is 0.2 to 25 parts by mass, preferably 0.3 to 24 parts by mass. The above blending ratios can be combined arbitrarily. For example, the amount of the compound having a number average molecular weight of 300 to 10,000 and having one or two hydroxyl groups in the same molecule may be 10 to 200 parts by mass, and the amount of the compound having an active hydrogen and a tertiary amino group in the same molecule may be 0.2 to 25 parts by mass, relative to 100 parts by mass of the polyisocyanate compound. The amount of the compound having a number average molecular weight of 300 to 10,000 and having one or two hydroxyl groups in the same molecule may be 20 to 190 parts by mass, and the amount of the compound having an active hydrogen and a tertiary amino group in the same molecule may be 0.2 to 25 parts by mass. The amount of the compound having a number average molecular weight of 300 to 10,000 and having one or two hydroxyl groups in the same molecule may be 30 to 180 parts by mass, and the amount of the compound having an active hydrogen and a tertiary amino group in the same molecule may be 0.3 to 24 parts by mass, relative to 100 parts by mass of the polyisocyanate compound.

[0119] The manufacture of the carbamate polymer dispersant is carried out according to the known method in the manufacture of polyurethane resin. As the solvent used in the manufacture, for example, ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, cyclohexanone, isophorone, esters such as ethyl acetate, butyl acetate, and cellosolve acetate; hydrocarbons such as benzene, toluene, xylene, and hexane; some alcohols such as diacetone alcohol, isopropanol, sec-butyl alcohol, and tert-butyl alcohol; chlorides such as dichloromethane and chloroform; ethers such as tetrahydrofuran and diethyl ether; aprotic polar solvents such as dimethylformamide, N-methylpyrrolidone, and dimethyl sulfoxide. They can be used alone or in combination of two or more.

[0120] When the carbamate-based polymer dispersant is produced, a carbamate reaction catalyst can be used. Examples of the carbamate reaction catalyst include tin-based catalysts such as dibutyltin dilaurate, dioctyltin dilaurate, dibutyltin dioctoate, and stannous octoate, iron-based catalysts such as ferric acetylacetonate and ferric chloride, and tertiary amine-based catalysts such as triethylamine and triethylenediamine. These catalysts can be used alone or in combination of two or more.

[0121] It is preferred to control the amount of the compound having active hydrogen and tertiary amino groups in the same molecule so that the amine value after the reaction is preferably in the range of 1 to 100 mgKOH / g, more preferably 5 to 95 mgKOH / g. By setting the amine value to be above the aforementioned lower limit, dispersibility tends to be improved. In addition, by setting it to be below the aforementioned upper limit, developability tends to be improved.

[0122] The amine value is represented by the mass of KOH equivalent to the amount of alkali per 1 g of solid content in the sample excluding the solvent, and can be measured by the following method.

[0123] In a 100mL beaker, accurately weigh 0.5-1.5g of the sample and dissolve it in 50mL of acetic acid. Use an automatic titrator equipped with a pH electrode to neutralize and titrate the solution with 0.1mol / L HClO4 (perchloric acid) acetic acid solution. The inflection point of the titration pH curve is taken as the titration endpoint, and the amine value is calculated by the following formula.

[0124] Amine value [mgKOH / g] = (561×V) / (W×S)

[0125] [W: represents the amount of the dispersant sample weighed [g], V: represents the titration amount at the titration endpoint [mL], and S: represents the solid content concentration of the dispersant sample [mass %].]

[0126] In the above reaction, when isocyanate groups remain in the polymer dispersant, it is preferred to further use an alcohol or an amino compound to consume the isocyanate groups because the temporal stability of the product is improved.

[0127] The weight average molecular weight (Mw) of the carbamate polymer dispersant is preferably 1,000 to 200,000, more preferably 2,000 to 100,000, and further preferably 3,000 to 50,000. It is particularly preferably 30,000 or less. If Mw is above the lower limit, dispersibility and dispersion stability tend to be good, and if it is below the upper limit, solubility tends to be good.

[0128] The above upper and lower limits may be arbitrarily combined, for example, 1,000 to 30,000, 2,000 to 30,000, or 3,000 to 30,000.

[0129] In particular, when Mw is 30000 or less, and in particular when the pigment concentration is high, alkali developability tends to be good. Examples of commercially available urethane dispersants include DISPERBYK 167 and 182 (manufactured by BYK-Chemie).

[0130] The content ratio of (A) pigment to (B) dispersant on a mass basis ((A) pigment / (B) dispersant) is preferably 1 or more, more preferably 3 or more, and even more preferably 4 or more, and is preferably 50 or less, more preferably 30 or less, and even more preferably 15 or less. When the (A) pigment / (B) dispersant is at least the above lower limit, the developing solubility tends to be more excellent, and when it is at most the above upper limit, sufficient dispersibility of the (A) pigment tends to be easily ensured.

[0131] The above upper and lower limits may be arbitrarily combined, for example, 1 to 50, 3 to 30, or 4 to 15.

[0132] The content of the dispersant (B) is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more, relative to the total solid content in the pigment dispersion, and is preferably 30% by mass or less, more preferably 25% by mass or less, and even more preferably 20% by mass or less. If the content of the dispersant (B) is at least the lower limit, sufficient dispersibility of the pigment (A) tends to be easily ensured, and if it is at most the upper limit, film-forming properties tend to be more excellent without reducing the proportions of other components.

[0133] The above upper and lower limits may be arbitrarily combined, for example, 5 to 30% by mass, 10 to 25% by mass, or 15 to 20% by mass.

[0134] <Organic Solvents>

[0135] As the organic solvent, from the viewpoint of viscosity stability of the pigment dispersion, an organic solvent having a boiling point of 100 to 300° C. is preferred, and an organic solvent having a boiling point of 120 to 280° C. is more preferred. Here, the boiling point is a value at a pressure of 1013.25 hPa. Hereinafter, the boiling point is the same in all cases.

[0136] As an organic solvent which has a boiling point of 100-300 degreeC, the following are mentioned, for example.

[0137] Glycol monoalkyl ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol mono-n-butyl ether, propylene glycol-tert-butyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol mono-n-butyl ether, methoxymethylpentanol, dipropylene glycol monoethyl ether, dipropylene glycol monomethyl ether, 3-methyl-3-methoxybutanol, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, and tripropylene glycol methyl ether;

[0138] Glycol dialkyl ethers such as ethylene glycol dimethyl ether, ethylene glycol diethyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dipropyl ether, diethylene glycol dibutyl ether, and dipropylene glycol dimethyl ether;

[0139] Glycol alkyl ether acetates such as ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol mono-n-butyl ether acetate, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, propylene glycol monopropyl ether acetate, propylene glycol monobutyl ether acetate, methoxybutyl acetate, 3-methoxybutyl acetate, methoxypentyl acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol mono-n-butyl ether acetate, dipropylene glycol monomethyl ether acetate, triethylene glycol monomethyl ether acetate, triethylene glycol monoethyl ether acetate, and 3-methyl-3-methoxybutyl acetate;

[0140] Glycol diacetates such as ethylene glycol diacetate, 1,3-butylene glycol diacetate, and 1,6-hexanol diacetate;

[0141] Alkyl acetates such as cyclohexanol acetate;

[0142] Ethers such as amyl ether, diethyl ether, dipropyl ether, diisopropyl ether, dibutyl ether, diamyl ether, ethyl isobutyl ether, and dihexyl ether;

[0143] Ketones such as acetone, methyl ethyl ketone, methyl amyl ketone, methyl isopropyl ketone, methyl isoamyl ketone, diisopropyl ketone, diisobutyl ketone, methyl isobutyl ketone, cyclohexanone, ethyl amyl ketone, methyl butyl ketone, methyl hexyl ketone, methyl nonyl ketone, and methoxymethyl amyl ketone;

[0144] Monohydric or polyhydric alcohols such as ethanol, propanol, butanol, hexanol, cyclohexanol, ethylene glycol, propylene glycol, butylene glycol, diethylene glycol, dipropylene glycol, triethylene glycol, methoxymethylpentanol, glycerol, and benzyl alcohol;

[0145] Aliphatic hydrocarbons such as n-pentane, n-octane, diisobutylene, n-hexane, hexene, isoprene, dipentene, and dodecane;

[0146] Alicyclic hydrocarbons such as cyclohexane, methylcyclohexane, methylcyclohexene, and bicyclohexane;

[0147] Aromatic hydrocarbons such as benzene, toluene, xylene, and cumene;

[0148] Chain or cyclic esters such as amyl formate, ethyl formate, ethyl acetate, butyl acetate, propyl acetate, amyl acetate, methyl isobutyrate, ethylene glycol acetate, ethyl propionate, propyl propionate, butyl butyrate, isobutyl butyrate, methyl isobutyrate, ethyl octanoate, butyl stearate, ethyl benzoate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, propyl 3-methoxypropionate, butyl 3-methoxypropionate, and γ-butyrolactone;

[0149] Alkoxycarboxylic acids such as 3-methoxypropionic acid and 3-ethoxypropionic acid;

[0150] Halogenated hydrocarbons such as butyl chloride and amyl chloride;

[0151] Ether ketones such as methoxymethylpentyl ketone;

[0152] Nitriles such as acetonitrile and benzonitrile.

[0153] Examples of commercially available organic solvents include mineral spirit, Varsol #2, Apco #18 Solvent, Apco thinner, Sorcal solvent No. 1 and No. 2, Solvesso #150, Shell TS28 Solvent, carbitol, ethyl carbitol, butyl carbitol, methyl cellosolve (“Cellosolve” is a registered trademark. The same shall apply hereinafter), ethyl cellosolve, ethyl cellosolve acetate, methyl cellosolve acetate, and Diglyme (all trade names).

[0154] The organic solvent may be used alone or in combination of two or more.

[0155] When forming color filter pixels or a black matrix by photolithography using a photosensitive resin composition containing a pigment dispersion, an organic solvent having a boiling point of 100 to 250°C is preferred, and an organic solvent having a boiling point of 120 to 230°C is more preferred.

[0156] As the organic solvent, glycol alkyl ether acetates are preferred from the viewpoints of good balance of coating properties, surface tension, etc., relatively high solubility of the constituent components in the photosensitive resin composition, and viscosity stability of the pigment dispersion. The glycol alkyl ether acetates may be used alone or in combination of two or more.

[0157] Glycol alkyl ether acetates may also be used in combination with other organic solvents.

[0158] As other organic solvents, glycol monoalkyl ethers are preferred. Propylene glycol monomethyl ether is preferred from the viewpoint of solubility of the constituent components in the photosensitive resin composition.

[0159] Since glycol monoalkyl ethers have high polarity, from the viewpoint of the aggregation of the pigment (A) and the storage stability related to the viscosity of the photosensitive resin composition obtained later, when the organic solvent contains glycol monoalkyl ethers, the content ratio of glycol monoalkyl ethers is preferably 5 to 30% by mass, more preferably 5 to 20% by mass, relative to the total mass of the organic solvent.

[0160] Glycol alkyl ether acetates and organic solvents having a boiling point of 200°C or more (hereinafter sometimes referred to as "high boiling point solvents") may also be used in combination. By using a high boiling point solvent in combination, the photosensitive resin composition containing the pigment dispersion is not easy to dry, and the uniform dispersion state of the pigment (A) in the composition is prevented from being destroyed by rapid drying. That is, for example, there is an effect of preventing the generation of foreign matter defects caused by precipitation or solidification of the pigment at the front end of the slit nozzle. The upper limit of the boiling point of the high boiling point solvent is not particularly limited, for example, it is 300°C or less.

[0161] Since the above-mentioned effect is high, examples of the high boiling point solvent include dipropylene glycol methyl ether acetate, diethylene glycol mono-n-butyl ether acetate, diethylene glycol monoethyl ether acetate, 1,4-butanediol diacetate, 1,3-butylene glycol diacetate, triacetin, and 1,6-hexanediol diacetate.

[0162] The high boiling point solvent may be used alone or in combination of two or more.

[0163] The content of the high boiling point solvent is preferably 0 to 50% by mass, more preferably 0.5 to 40% by mass, and further preferably 1 to 30% by mass relative to the total mass of the organic solvent. If the content of the high boiling point solvent is below the upper limit, there is a tendency to suppress the problem of poor rhythm of the reduced pressure drying process in the color filter manufacturing process or pre-baking pin marks due to the lowering of the drying temperature of the composition. If the content of the high boiling point solvent is 0.5% by mass or more, there is a tendency to suppress, for example, the precipitation or solidification of the pigment at the front end of the slit nozzle and the resulting foreign matter defects.

[0164] The content of the organic solvent in the pigment dispersion of the present invention can be appropriately selected in consideration of the content of the total solid content and the water content in the pigment dispersion.

[0165] From the viewpoint of light-shielding properties, the content ratio of the total solid content in the pigment dispersion is preferably 10% by mass or more, more preferably 20% by mass or more, and further preferably 30% by mass or more, relative to the total mass of the pigment dispersion. From the viewpoint of viscosity stability and temporal viscosity stability, it is preferably 60% by mass or less, more preferably 50% by mass or less, and further preferably 40% by mass or less.

[0166] The above upper and lower limits may be arbitrarily combined, and may be, for example, 10 to 60% by mass, 20 to 50% by mass, or 30 to 40% by mass.

[0167] From the viewpoint of viscosity stability and temporal viscosity stability, the pigment dispersion of the present invention preferably contains a glycol alkyl ether acetate as an organic solvent and the content ratio of the total solid content in the pigment dispersion is 40% by mass or less.

[0168] When the pigment dispersion of the present invention contains glycol alkyl ether acetate as an organic solvent, the content of glycol alkyl ether acetate in the total organic solvent is preferably 60% by mass or more, more preferably 70% by mass or more, and even more preferably 80% by mass or more from the viewpoint of viscosity stability. In addition, from the viewpoint of reducing unevenness during drying of the coating film, it is preferably 100% by mass or less, more preferably 95% by mass or less, and even more preferably 90% by mass or less.

[0169] The above upper and lower limits may be arbitrarily combined, and may be, for example, 60 to 100% by mass, 70 to 100% by mass, or 80 to 100% by mass.

[0170] <(C) Dispersing aid>

[0171] The pigment dispersion of the present invention preferably contains (C) a dispersing aid in order to improve the dispersion stability of the (A) pigment.

[0172] As the (C) dispersing aid, for example, pigment derivatives can be cited. As the pigment derivatives, for example, azo derivatives, phthalocyanine derivatives, quinacridone derivatives, benzimidazolone derivatives, quinophthalone derivatives, isoindolinone derivatives, dioxazine derivatives, anthraquinone derivatives, indanthrene derivatives, perylene derivatives, perinone derivatives, diketopyrrolopyrrole derivatives, and dioxazine derivatives are cited, and phthalocyanine derivatives and quinophthalone derivatives are preferred.

[0173] Examples of substituents of the pigment derivative include sulfonic acid groups, sulfonamide groups and quaternary salts thereof, phthalimidomethyl groups, dialkylaminoalkyl groups, hydroxyl groups, carboxyl groups, and amide groups directly bonded to the pigment skeleton or bonded to the pigment skeleton via, for example, alkyl groups, aryl groups, and heterocyclic groups, preferably sulfonic acid groups. Multiple substituents may be substituted in one pigment skeleton.

[0174] Examples of the pigment derivative include sulfonic acid derivatives of phthalocyanine, sulfonic acid derivatives of quinophthalone, sulfonic acid derivatives of anthraquinone, sulfonic acid derivatives of quinacridone, sulfonic acid derivatives of diketopyrrolopyrrole, and sulfonic acid derivatives of dioxazine.

[0175] The dispersing aid may be used alone or in combination of two or more.

[0176] When the pigment dispersion of the present invention contains (C) a dispersing aid, the content ratio of the (A) pigment to the (C) dispersing aid on a mass basis ((A) pigment / (C) dispersing aid) is preferably 10 or more, more preferably 30 or more, and even more preferably 50 or more, and is preferably 200 or less, more preferably 150 or less, and even more preferably 100 or less. When the (A) pigment / (C) dispersing aid is at least the above lower limit, the developability tends to be stable and the substrate adhesion tends to be more excellent, and when it is at most the above upper limit, the dispersion stability tends to be more excellent.

[0177] The above upper and lower limits may be arbitrarily combined, for example, 10 to 200, 30 to 150, or 50 to 100.

[0178] When the pigment dispersion of the present invention contains a dispersing aid (C), the content of the dispersing aid (C) is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and further preferably 1% by mass or more, relative to the total solid content of the pigment dispersion, and is preferably 10% by mass or less, more preferably 5% by mass or less, and further preferably 3% by mass or less. If the content of the dispersing aid (C) is above the lower limit, there is a tendency for the dispersion stability to be more excellent, and if it is below the upper limit, there is a tendency for the developability to be stable and the substrate adhesion to be more excellent.

[0179] The above upper and lower limits may be arbitrarily combined, and may be, for example, 0.1 to 10% by mass, 0.5 to 5% by mass, or 1 to 3% by mass.

[0180] The pigment dispersion of the present invention may further contain other components in addition to (A) the pigment, (B) the dispersant, (C) the dispersing aid, the organic solvent and water as necessary. Examples of other components include other compounding components in the photosensitive resin composition described below.

[0181] The content of other components is preferably 5% by mass or less, more preferably 1% by mass or less, and may be 0% by mass, relative to the total solid content of the pigment dispersion.

[0182] The absolute value of the Zeta potential of the pigment dispersion of the present invention is preferably 50 mV or less, more preferably 48 mV or less, further preferably 45 mV or less, and particularly preferably 40 mV or less. The lower limit is not particularly limited, and is usually 0 mV or more. If the absolute value of the Zeta potential is below the above upper limit, the stability of the pigment dispersion is high, and the aggregation of the pigment is small, so there is a tendency to suppress the generation of foreign matter and improve the linearity of the pattern.

[0183] The absolute value of the zeta potential of the pigment dispersion can be measured, for example, using a laser zeta potentiometer ELSZ-2000ZS manufactured by Otsuka Electronics Co., Ltd. using a cell for a low dielectric constant solvent.

[0184] <Method for producing pigment dispersion>

[0185] The pigment dispersion of the present invention is produced, for example, by mixing (A) a pigment, (B) a dispersant, an organic solvent, and water, and optionally (C) an optional component such as a dispersing aid, and subjecting the resulting mixed solution to a dispersion treatment.

[0186] The amount of water to be mixed is set so that the final water content falls within the above range.

[0187] The (A) pigment is micronized by the dispersion treatment, so the coating properties of the pigment dispersion and the photosensitive resin composition containing the pigment dispersion are improved. When the (A) pigment contains a black pigment, the light shielding ability is also improved by the dispersion treatment. In particular, when a polymer dispersant is used as the (B) dispersant, the thickening of the obtained pigment dispersion and the photosensitive resin composition containing the same over time is suppressed (excellent dispersion stability).

[0188] The dispersion treatment can be carried out using a known dispersion treatment device such as a paint conditioner, sand mill, ball mill, roll mill, stone mill, jet mill, homogenizer, etc. When the dispersion treatment is carried out using a sand mill, glass beads or zirconia beads having a diameter of about 0.1 to 8 mm are preferably used.

[0189] The dispersion treatment conditions are not particularly limited, and the temperature is, for example, in the range of 0°C to 100°C, preferably in the range of room temperature to 80°C. As for the dispersion time, since the appropriate time varies depending on the composition of the liquid and the size of the dispersion treatment device, it is appropriately adjusted. The dispersion standard is: the dispersion state of the (A) pigment is controlled so that the 20 degree specular gloss (JIS Z8741) of the coating film of the photosensitive resin composition becomes in the range of 100 to 200. In the case where the gloss of the photosensitive resin composition is low, most of the dispersion treatment is insufficient, and coarse pigment particles remain, and there is a possibility of insufficient developability, adhesion, resolution, etc. In addition, if the dispersion treatment is carried out until the gloss value exceeds the above range, the pigment is broken and a large number of ultrafine particles are generated, so there is a tendency for the dispersion stability to be impaired.

[0190] After the dispersion treatment, the obtained dispersion treatment product may be subjected to filtration treatment using a filter or the like, if necessary, for example, to separate the beads used in the dispersion treatment from the pigment dispersion liquid.

[0191] [Photosensitive resin composition]

[0192] The photosensitive resin composition of the present invention contains the pigment dispersion of the present invention, (D) an alkali-soluble resin, (E) a photopolymerizable compound, and (F) a photopolymerization initiator.

[0193] The content ratio of the pigment dispersion of the present invention, when converted into the content ratio of the (A) pigment relative to the total solid content of the photosensitive resin composition of the present invention, is preferably 30% by mass or more, more preferably 40% by mass or more, and further preferably 50% by mass or more, and is preferably 75% by mass or less, more preferably 70% by mass or less, and further preferably 65% ​​by mass or less. If the content ratio of the (A) pigment is above the lower limit, the light shielding property of the obtained cured product tends to be more excellent, and if it is below the upper limit, the formability of the cured product tends to be more excellent.

[0194] The above upper and lower limits may be arbitrarily combined, and may be, for example, 30 to 75% by mass, 40 to 70% by mass, or 50 to 65% by mass.

[0195] The solid content of the pigment dispersion of the present invention is preferably 40% by mass or more, more preferably 50% by mass or more, and further preferably 60% by mass or more relative to the total solid content of the photosensitive resin composition of the present invention, and is preferably 90% by mass or less, more preferably 80% by mass or less, and further preferably 70% by mass or less. If the solid content of the pigment dispersion is above the lower limit, the light-shielding property tends to be more excellent, and if it is below the upper limit, the developing solubility tends to be more excellent.

[0196] The above upper and lower limits may be arbitrarily combined, and may be, for example, 40 to 90% by mass, 50 to 80% by mass, or 60 to 70% by mass.

[0197] <(D) Alkali-soluble resin>

[0198] (D) alkali-soluble resin is not particularly limited as long as it is a resin showing alkali solubility, and examples thereof include resins containing carboxyl groups or hydroxyl groups. More specifically, examples thereof include epoxy (meth) acrylate resins, acrylic resins, carboxyl-containing epoxy resins, carboxyl-containing polyurethane resins, novolac resins, and polyvinylphenol resins. In particular, from the viewpoint of excellent platemaking properties, the following may be suitably used:

[0199] (D1) Epoxy (meth)acrylate resin

[0200] (D2) Acrylic copolymer resin

[0201] The alkali-soluble resin may be used alone or in combination of two or more.

[0202] <(D1) Epoxy (meth)acrylate resin>

[0203] (D1) Epoxy (meth)acrylate resin is a resin obtained by further reacting a hydroxyl group generated by the reaction of an epoxy compound (epoxy resin) with an α,β-unsaturated monocarboxylic acid and / or an α,β-unsaturated monocarboxylic acid ester having a carboxyl group in the ester portion with a compound having two or more substituents capable of reacting with the hydroxyl group, such as a polybasic acid and / or its anhydride.

[0204] The (D1) epoxy (meth)acrylate resin includes a resin obtained by reacting a compound having two or more substituents reactive with a hydroxyl group before reacting the polybasic acid and / or its anhydride with the hydroxyl group and then reacting the polybasic acid and / or its anhydride.

[0205] A resin obtained by reacting the carboxyl group of the resin obtained by the above reaction with a compound having a further reactive functional group is also included in the (D1) epoxy (meth)acrylate resin.

[0206] Epoxy (meth)acrylate resins do not substantially have epoxy groups in their chemical structures and are not limited to "(meth)acrylates". However, since epoxy compounds (epoxy resins) are raw materials and "(meth)acrylates" are representative examples, they are conventionally named as such.

[0207] As the epoxy (meth)acrylate resin (D1), from the viewpoint of developability and reliability, epoxy (meth)acrylate resin (D1-1) and / or epoxy (meth)acrylate resin (D1-2) (hereinafter sometimes referred to as “carboxyl group-containing epoxy (meth)acrylate resin”) are preferably used.

[0208] As the epoxy (meth)acrylate resin (D1), a resin having an aromatic ring in the main chain can be more preferably used from the viewpoint of outgassing.

[0209] <Epoxy (meth)acrylate resin (D1-1)>

[0210] An alkali-soluble resin obtained by adding an α,β-unsaturated monocarboxylic acid or an α,β-unsaturated monocarboxylic acid ester having a carboxyl group to an epoxy resin and further reacting the epoxy resin with a polybasic acid and / or an anhydride thereof.

[0211] <Epoxy (meth)acrylate resin (D1-2)>

[0212] An alkali-soluble resin obtained by adding an α,β-unsaturated monocarboxylic acid or an α,β-unsaturated monocarboxylic acid ester having a carboxyl group to an epoxy resin and further reacting the epoxy resin with a polyol and a polybasic acid and / or an anhydride thereof.

[0213] Here, epoxy resin refers to also forming the raw material compound before the resin by thermosetting, and as this epoxy resin, can suitably select to use from known epoxy resin.In addition, epoxy resin can use the compound that makes phenolic compound and epihalohydrin react and obtain.As phenolic compound, preferably have the compound of binary or more than binary phenolic hydroxyl group, can be monomer and can also be polymer.

[0214] As the type of epoxy resin that becomes the raw material, for example, cresol novolac type epoxy resin, phenol novolac type epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, trisphenol methane type epoxy resin, biphenyl novolac type epoxy resin, naphthol novolac type epoxy resin, epoxy resin that is a reaction product of a polyaddition reaction product of dicyclopentadiene and phenol or cresol and an epihalohydrin, epoxy resin containing an adamantyl group, and fluorene type epoxy resin can be suitably used, and epoxy resins having an aromatic ring in the main chain can be more suitably used.

[0215] As the epoxy resin, for example, bisphenol A type epoxy resin (for example, "jER (registered trademark, hereinafter the same) 828", "jER1001", "jER1002", "jER1004", etc. manufactured by Mitsubishi Chemical Corporation), epoxy resin obtained by reaction of alcoholic hydroxyl group of bisphenol A type epoxy resin with epichlorohydrin (for example, "NER-1302" manufactured by Nippon Kayaku Co., Ltd. (epoxy equivalent 323, softening point 76° C.)), bisphenol F type resin (for example, "jER 807", "EP-4001", "EP-4002", "EP-4004", etc.), epoxy resins obtained by the reaction of alcoholic hydroxyl groups of bisphenol F type epoxy resins with epichlorohydrin (for example, "NER-7406" manufactured by Nippon Kayaku Co., Ltd. (epoxy equivalent 350, softening point 66°C)), bisphenol S type epoxy resins, biphenyl glycidyl ether (for example, "YX-4000" manufactured by Mitsubishi Chemical Corporation), phenol novolac type epoxy resins (for example, "EPPN-201" manufactured by Nippon Kayaku Co., Ltd., "EP-152", "EP-154" manufactured by Mitsubishi Chemical Corporation, "DEN-438" manufactured by Dow Chemical Company), (o, m, p -) cresol novolac type epoxy resin (for example, "EOCN (registered trademark, hereinafter the same)-102S", "EOCN-1020", "EOCN-104S" manufactured by Nippon Kayaku Co., Ltd.), triglycidyl isocyanurate (for example, "TEPIC (registered trademark)" manufactured by Nissan Chemical Co., Ltd.), trisphenol methane type epoxy resin (for example, "EPPN (registered trademark, hereinafter the same)-501", "EPPN-502", "EPPN-503" manufactured by Nippon Kayaku Co., Ltd.), alicyclic epoxy resin ("CELLOXIDE (registered trademark, hereinafter the same) 2021P", "CELLOXIDE EHPE" manufactured by Daicel Corporation), epoxy resin obtained by glycidylating a phenol resin obtained by reaction of dicyclopentadiene and phenol (for example, "EXA-7200" manufactured by DIC Corporation, "NC-7300" manufactured by Nippon Kayaku Co., Ltd.), epoxy resins represented by the following general formulas (B1) to (B4). Specifically, for example, as the epoxy resin represented by the following general formula (B1), "XD-1000" manufactured by Nippon Kayaku Co., Ltd. can be listed, as the epoxy resin represented by the following general formula (B2), "NC-3000" manufactured by Nippon Kayaku Co., Ltd. can be listed, as the epoxy resin represented by the following general formula (B3), "E-201" manufactured by Osaka Organic Chemical Industry Co., Ltd. can be listed, and as the epoxy resin represented by the following general formula (B4), "ESF-300" manufactured by Nippon Steel & Sumigin Chemical Corporation can be listed.

[0216]

[0217] In formula (B1), a is an average value, representing a number from 0 to 10, and R111 Each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 8 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a phenyl group, a naphthyl group or a biphenyl group. 111 Each are optionally the same as or different from each other.

[0218]

[0219] In formula (B2), b1 and b2 are each independently an average value and represent a number from 0 to 10, and R 121 Each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 8 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a phenyl group, a naphthyl group or a biphenyl group. 121 Each are optionally the same as or different from each other.

[0220]

[0221] In formula (a3), X represents a linking group represented by the following general formula (B3-1) or (B3-2), wherein the molecular structure contains one or more adamantane structures, and c represents 2 or 3.

[0222]

[0223] In formula (B3-1) and (B3-2), R 131 ~R 134 and R 135 ~R 137 Each independently represents an adamantyl group which may have a substituent, a hydrogen atom, an alkyl group having 1 to 12 carbon atoms which may have a substituent, or a phenyl group which may have a substituent, and * represents a bond.

[0224]

[0225] In formula (B4), p and q each independently represent an integer of 0 to 4, and R 141 and R 142 Each independently represents an alkyl group having 1 to 4 carbon atoms or a halogen atom, and R 143 and R 144 Each independently represents an alkylene group having 1 to 4 carbon atoms, and x and y each independently represent an integer greater than or equal to 0.

[0226] As the epoxy resin, an epoxy resin represented by any of formulas (B1) to (B4) is preferably used.

[0227] Examples of the α,β-unsaturated monocarboxylic acid or α,β-unsaturated monocarboxylic acid ester having a carboxyl group include: (meth)acrylic acid, crotonic acid, o-vinylbenzoic acid, m-vinylbenzoic acid or p-vinylbenzoic acid, monocarboxylic acids such as (meth)acrylic acid substituted with halogenated alkyl, alkoxy, halogen, nitro or cyano groups at the α-position; 2-(meth)acryloyloxyethylsuccinic acid, 2-(meth)acryloyloxyethyladipic acid, 2-(meth)acryloyloxyethylphthalic acid, 2-(meth)acryloyloxyethylhexahydrophthalic acid, 2-(meth)acryloyloxyethylmaleic acid, 2-(meth)acryloyloxypropylsuccinic acid, 2-(meth)acryloyloxypropyladipic acid, 2-(meth)acryloyloxypropyltetrahydrophthalic acid Acid, 2-(meth)acryloxypropylphthalic acid, 2-(meth)acryloxypropylmaleic acid, 2-(meth)acryloxybutylsuccinic acid, 2-(meth)acryloxybutyladipic acid, 2-(meth)acryloxybutylhydrophthalic acid, 2-(meth)acryloxybutylphthalic acid, 2-(meth)acryloxybutylmaleic acid; a monomer of a product obtained by adding lactones such as ε-caprolactone, β-propiolactone, γ-butyrolactone, and δ-valerolactone to (meth)acrylic acid; or a monomer obtained by adding acids (anhydrides) such as succinic acid (anhydride), phthalic acid (anhydride), and maleic acid (anhydride) to hydroxyalkyl (meth)acrylates and pentaerythritol tri(meth)acrylates; (meth)acrylic acid dimers.

[0228] Among these, (meth)acrylic acid is preferred from the viewpoint of sensitivity.

[0229] As a method for adding an α,β-unsaturated monocarboxylic acid or an α,β-unsaturated monocarboxylic acid ester having a carboxyl group to an epoxy resin, a known method can be used. For example, an α,β-unsaturated monocarboxylic acid or an α,β-unsaturated monocarboxylic acid ester having a carboxyl group can be reacted with an epoxy resin in the presence of an esterification catalyst at a temperature of 50 to 150°C. As the esterification catalyst used here, for example, a tertiary amine such as triethylamine, trimethylamine, benzyldimethylamine, benzyldiethylamine, etc.; a quaternary ammonium salt such as tetramethylammonium chloride, tetraethylammonium chloride, dodecyltrimethylammonium chloride, etc. can be used.

[0230] Each component of the epoxy resin, the α,β-unsaturated monocarboxylic acid or the α,β-unsaturated monocarboxylic acid ester having a carboxyl group, and the esterification catalyst may be used alone or in combination of two or more.

[0231] The amount of α,β-unsaturated monocarboxylic acid or α,β-unsaturated monocarboxylic acid ester having a carboxyl group is preferably 0.5 to 1.2 equivalents, and more preferably 0.7 to 1.1 equivalents relative to 1 equivalent of epoxy group of the epoxy resin. By setting the amount of α,β-unsaturated monocarboxylic acid or α,β-unsaturated monocarboxylic acid ester having a carboxyl group to be above the aforementioned lower limit, it is possible to suppress the insufficient amount of unsaturated group introduction, and there is a tendency to facilitate the subsequent reaction with polyacids and / or their anhydrides to be sufficient. By setting it below the aforementioned upper limit, it is possible to suppress the unreacted product of α,β-unsaturated monocarboxylic acid or α,β-unsaturated monocarboxylic acid ester having a carboxyl group from remaining, and it is confirmed that it is easy to make the curing characteristics good.

[0232] Examples of the polybasic acid and / or its anhydride include maleic acid, succinic acid, itaconic acid, phthalic acid, tetrahydrophthalic acid, hexahydrophthalic acid, pyromellitic acid, trimellitic acid, benzophenonetetracarboxylic acid, methylhexahydrophthalic acid, endomethylenetetrahydrophthalic acid, chlorendic acid, methyltetrahydrophthalic acid, biphenyltetracarboxylic acid, and anhydrides thereof.

[0233] Preferred are maleic acid, succinic acid, itaconic acid, phthalic acid, tetrahydrophthalic acid, hexahydrophthalic acid, pyromellitic acid, trimellitic acid, biphenyltetracarboxylic acid, or anhydrides thereof. Particularly preferred are tetrahydrophthalic acid, biphenyltetracarboxylic acid, tetrahydrophthalic anhydride, or biphenyltetracarboxylic dianhydride.

[0234] The addition reaction of the polyacid and / or its anhydride can be carried out using a known method, and the target product can be obtained by continuing the reaction under the same conditions as the addition reaction of α,β-unsaturated monocarboxylic acid or α,β-unsaturated monocarboxylic acid ester having a carboxyl group to the epoxy resin. It is preferred to control the addition amount of the polyacid and / or its anhydride component so that the acid value of the generated carboxyl-containing epoxy (meth) acrylate resin is preferably 10 to 150 mgKOH / g, more preferably 20 to 140 mgKOH / g. By setting it to above the aforementioned lower limit, there is a tendency for alkali developability to become good. By setting it to below the aforementioned upper limit, there is a tendency for curing performance to become good.

[0235] In the addition reaction of the polyacid and / or its anhydride, a polyfunctional alcohol (polyol) such as trimethylolpropane, ditrimethylolpropane, pentaerythritol, dipentaerythritol, trimethylolethane, 1,2,3-propanetriol, etc. can be added to introduce a multi-branched structure. In this case, there is no particular restriction on the mixing order of the polyacid and / or its anhydride and the polyfunctional alcohol. By heating, the polyacid and / or its anhydride react with any hydroxyl group present in the mixture of the reactant of the epoxy resin and the α,β-unsaturated monocarboxylic acid or the α,β-unsaturated monocarboxylic acid ester having a carboxyl group and the polyfunctional alcohol.

[0236] By using a polyol, the molecular weight of the epoxy (meth)acrylate resin (D1) can be increased, branches can be introduced into the molecule, and a balance between molecular weight and viscosity can be achieved. In addition, there is a tendency to increase the introduction rate of acid groups into the molecule, making it easier to achieve a balance between sensitivity and adhesion.

[0237] Examples of the carboxyl group-containing epoxy (meth)acrylate resin include, in addition to the above-described resins, resins described in Korean Patent Publication No. 10-2013-0022955.

[0238] The weight average molecular weight (Mw) of the carboxyl-containing epoxy (meth) acrylate resin measured by gel permeation chromatography (GPC) in terms of polystyrene is preferably 1000 or more, more preferably 1500 or more, further preferably 2000 or more, further preferably 3000 or more, further preferably 4000 or more, and particularly preferably 5000 or more. In addition, it is preferably 30000 or less, more preferably 20000 or less, and further preferably 15000 or less. By setting it to be above the aforementioned lower limit, there is a tendency that the solubility in the developer becomes too high. By setting it to be below the aforementioned upper limit, there is a tendency that the solubility in the developer is easily improved. The above upper and lower limits can be combined arbitrarily. For example, it can be 1000 to 30000, can be 1500 to 20000, can be 1500 to 15000, or can be 2000 to 15000.

[0239] The acid value of the carboxyl-containing epoxy (meth) acrylate resin is not particularly limited, but is preferably 20 mgKOH / g or more, more preferably 40 mgKOH / g or more, further preferably 60 mgKOH / g or more, further preferably 80 mgKOH / g or more, and particularly preferably 100 mgKOH / g or more. In addition, it is preferably 200 mgKOH / g or less, more preferably 150 mgKOH / g or less, further preferably 130 mgKOH / g or less, and particularly preferably 120 mgKOH / g or less. By setting it to the above lower limit value or more, there is a tendency that the developing solubility is improved and the resolution becomes good. By setting it to the above upper limit value or less, there is a tendency that the residual film rate of the photosensitive coloring composition becomes good. The above upper and lower limits can be combined arbitrarily. For example, it may be 20 mgKOH / g to 200 mgKOH / g, 60 mgKOH / g to 150 mgKOH / g, 80 mgKOH / g to 130 mgKOH / g, or 100 mgKOH / g to 130 mgKOH / g.

[0240] The chemical structure of the epoxy (meth)acrylate resin is not particularly limited. From the viewpoint of developability and reliability, it is preferred to contain an epoxy (meth)acrylate resin having a partial structure represented by the following general formula (d1-I) (hereinafter, sometimes referred to as "(d1-I) epoxy (meth)acrylate resin") and / or an epoxy (meth)acrylate resin having a partial structure represented by the following general formula (d1-II) (hereinafter, sometimes referred to as "(d1-II) epoxy (meth)acrylate resin").

[0241]

[0242] In formula (d1-I), R 11 represents a hydrogen atom or a methyl group, R 12 represents a divalent hydrocarbon group which may have a substituent, k represents 1 or 2, and * represents a connecting bond.

[0243] The benzene ring in formula (d1-I) may be further substituted by any substituent.

[0244]

[0245] In formula (d1-II), R 13 Each independently represents a hydrogen atom or a methyl group, R 14 represents a divalent hydrocarbon group having a cyclic hydrocarbon group as a side chain, R 15 and R 16 Each independently represents a divalent aliphatic group which may have a substituent, m and n each independently represent an integer of 0 to 2, and * represents a connecting bond.

[0246] <(d1-I) Epoxy (meth)acrylate resin>

[0247]

[0248] In formula (d1-I), R 11 represents a hydrogen atom or a methyl group, R 12 represents a divalent hydrocarbon group which may have a substituent, k represents 1 or 2, and * represents a connecting bond.

[0249] The benzene ring in formula (d1-I) may be further substituted by any substituent.

[0250] (R 12 )

[0251] In formula (d1-I), R 12 It represents a divalent hydrocarbon group which may have a substituent.

[0252] Examples of the divalent hydrocarbon group include a divalent aliphatic group, a divalent aromatic ring group, and a group in which one or more divalent aliphatic groups and one or more divalent aromatic ring groups are linked.

[0253] The divalent aliphatic group may be a straight-chain, branched, or cyclic aliphatic group. From the viewpoint of development solubility, a straight-chain aliphatic group is preferred. On the other hand, from the viewpoint of reducing the penetration of the developer into the exposed portion, a cyclic aliphatic group is preferred. The number of carbon atoms is preferably 1 or more, more preferably 3 or more, and further preferably 6 or more. In addition, it is preferably 20 or less, more preferably 15 or less, and further preferably 10 or less. By setting it to above the aforementioned lower limit, it is easy to obtain a firm film, and there is a tendency that the surface roughness generated during development is not easily generated, and the adhesion to the substrate becomes good. By setting it to below the aforementioned upper limit, it is easy to suppress the deterioration of sensitivity or the reduction of the film during development, and there is a tendency to improve the resolution. The above upper and lower limits may be arbitrarily combined. For example, it may be 1 to 20, 1 to 15, or 1 to 10.

[0254] Examples of the divalent straight-chain aliphatic group include a methylene group, an ethylene group, an n-propylene group, an n-butylene group, an n-pentylene group, an n-hexylene group, and an n-heptylene group. From the viewpoint of rigidity of the skeleton, a methylene group is preferred.

[0255] Examples of the divalent branched aliphatic group include a structure in which the divalent linear aliphatic group has, for example, a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, or a tert-butyl group as a side chain.

[0256] The number of rings of the divalent cyclic aliphatic group is not particularly limited, but is preferably 1 or more, more preferably 2 or more. In addition, it is preferably 12 or less, more preferably 10 or less. By setting it to be above the aforementioned lower limit, a strong film is formed, and there is a tendency that the substrate adhesion becomes good. By setting it to be below the aforementioned upper limit, it is easy to suppress the deterioration of sensitivity or the reduction of the film during development, and there is a tendency that the resolution is improved. The above upper and lower limits can be combined arbitrarily. For example, it can be 1 to 12, 1 to 10, or 2 to 10.

[0257] Examples of the divalent cyclic aliphatic group include groups obtained by removing two hydrogen atoms from a cyclohexane ring, a cycloheptane ring, a cyclodecane ring, a cyclododecane ring, a norbornane ring, an isobornane ring, an adamantane ring, a cyclododecane ring, a dicyclopentadiene ring, a dicyclopentane ring, etc. From the viewpoint of rigidity of the skeleton, groups obtained by removing two hydrogen atoms from a dicyclopentadiene ring, a dicyclopentane ring, or an adamantane ring are preferred.

[0258] Examples of the substituent that the divalent aliphatic group may have include alkoxy groups having 1 to 5 carbon atoms, such as methoxy and ethoxy groups; hydroxyl groups; nitro groups; cyano groups; and carboxyl groups. From the viewpoint of ease of synthesis, unsubstituted groups are preferred.

[0259] As the divalent aromatic ring group, a divalent aromatic hydrocarbon ring group and a divalent aromatic heterocyclic group can be listed. The carbon number is not particularly limited, but is preferably 4 or more, more preferably 5 or more, and further preferably 6 or more. In addition, it is preferably 20 or less, more preferably 15 or less, and further preferably 10 or less. By setting it to above the aforementioned lower limit, it is easy to obtain a firm film, and there is a tendency that the surface roughness generated during development is not easy to occur, and the adhesion to the substrate becomes good. By setting it to below the aforementioned upper limit, it is easy to suppress the deterioration of sensitivity or the reduction of the film during development, and there is a tendency to improve the resolution. The above upper and lower limits can be arbitrarily combined. For example, it can be 4 to 20, 5 to 15, or 6 to 10.

[0260] The aromatic hydrocarbon ring in the divalent aromatic hydrocarbon ring group may be a monocyclic ring or a condensed ring. Examples of the divalent aromatic hydrocarbon ring group include a benzene ring, a naphthalene ring, an anthracene ring, a phenanthrene ring, a perylene ring, a tetracene ring, a pyrene ring, a benzopyrene ring, Ring, triphenylene ring, acenaphthene ring, fluoranthene ring, fluorene ring.

[0261] The aromatic heterocyclic ring in the divalent aromatic heterocyclic group may be a monocyclic ring or a condensed ring. Examples of the divalent aromatic heterocyclic group include a furan ring, a benzofuran ring, a thiophene ring, a benzothiophene ring, a pyrrole ring, a pyrazole ring, an imidazole ring, an oxadiazole ring, an indole ring, a carbazole ring, a pyrroloimidazole ring, a pyrrolopyrazole ring, a pyrrolopyrrole ring, a thienopyrrole ring, a thienothiophene ring, a furanopyrrole ring, a furanofuran ring, a thienofuran ring, a benzisoxazole ring, a benzisothiazole ring, a benzimidazole ring, a pyridine ring, a pyrazine ring, a pyridazine ring, a pyrimidine ring, a triazine ring, a quinoline ring, an isoquinoline ring, a cinnoline ring, a quinoxaline ring, a phenanthridine ring, a phenanthridine ring, a quinazoline ring, a quinazolinone ring, and an azulene ring.

[0262] From the viewpoint of patterning characteristics, a benzene ring or a naphthalene ring having two free valences is preferred, and a benzene ring having two free valences is more preferred.

[0263] Examples of the substituent that the divalent aromatic ring group may have include a hydroxyl group, a methyl group, a methoxy group, an ethyl group, an ethoxy group, a propyl group, and a propoxy group. From the viewpoint of development solubility, it is preferably unsubstituted.

[0264] Examples of the group in which one or more divalent aliphatic groups are linked to one or more divalent aromatic ring groups include groups in which one or more of the aforementioned divalent aliphatic groups are linked to one or more of the aforementioned divalent aromatic ring groups.

[0265] The number of divalent aliphatic groups is not particularly limited, but is preferably 1 or more, more preferably 2 or more, preferably 10 or less, more preferably 5 or less, and further preferably 3 or less. By setting the number to be above the aforementioned lower limit, a strong film can be easily obtained, and the surface roughness generated during development is not easily generated, and the adhesion to the substrate tends to be good. By setting the number to be below the aforementioned upper limit, the deterioration of sensitivity or the reduction of the film during development can be easily suppressed, and the resolution tends to be improved. The above upper and lower limits can be arbitrarily combined. For example, it can be 1 to 10, 1 to 5, 1 to 3, or 2 to 3.

[0266] The number of the divalent aromatic ring groups is not particularly limited, but is preferably 1 or more, more preferably 2 or more, preferably 10 or less, more preferably 5 or less, and further preferably 3 or less. By setting it to be above the aforementioned lower limit, a strong film is easily obtained, and it is not easy to produce surface roughness during development, and the adhesion to the substrate tends to be good. By setting it to be below the aforementioned upper limit, it is easy to suppress the deterioration of sensitivity or the reduction of the film during development, and there is a tendency to improve the resolution. The above upper and lower limits can be combined arbitrarily. For example, it can be 1 to 10, 1 to 5, 1 to 3, or 2 to 3.

[0267] As a group obtained by connecting one or more divalent aliphatic groups to one or more divalent aromatic ring groups, for example, groups represented by the following formulae (d1-IA) to (d1-IF) can be cited. From the viewpoint of rigidity of the skeleton and hydrophobization of the membrane, a group represented by the following formula (d1-IA) is preferred.

[0268]

[0269] In formula (d1-I), k represents 1 or 2. From the viewpoint of adhesion and patterning properties, k is preferably 1. From the viewpoint of NMP resistance, k is preferably 2. In addition, the epoxy (meth)acrylate (d1-I) may contain both a partial structure in which k is 1 and a partial structure in which k is 2.

[0270] The benzene ring in formula (d1-I) may be further substituted by any substituent.

[0271] As a substituent, for example, a hydroxyl group, a methyl group, a methoxy group, an ethyl group, an ethoxy group, a propyl group, and a propoxy group can be listed. The number of substituents is not particularly limited, and can be 1 or 2 or more. From the viewpoint of patterning characteristics, it is preferably unsubstituted.

[0272] From the viewpoint of ease of synthesis, the partial structure represented by formula (d1-I) is preferably a partial structure represented by the following general formula (d1-I-1).

[0273]

[0274] In formula (d1-I-1), R 11 , R 12 and k have the same meanings as in formula (d1-I), R X represents a hydrogen atom or a polyacid residue, and * represents a connecting bond.

[0275] The benzene ring in the formula (d1-I-1) may be further substituted by any substituent.

[0276] The polyacid residue refers to a monovalent group obtained by removing one OH group from a polyacid. Examples of the polyacid include maleic acid, succinic acid, itaconic acid, phthalic acid, tetrahydrophthalic acid, hexahydrophthalic acid, pyromellitic acid, trimellitic acid, benzophenonetetracarboxylic acid, methylhexahydrophthalic acid, endomethylenetetrahydrophthalic acid, chlorendic acid, methyltetrahydrophthalic acid, and biphenyltetracarboxylic acid.

[0277] From the viewpoint of patterning properties, preferred are maleic acid, succinic acid, itaconic acid, phthalic acid, tetrahydrophthalic acid, hexahydrophthalic acid, pyromellitic acid, trimellitic acid, and biphenyltetracarboxylic acid, and more preferred are tetrahydrophthalic acid, biphenyltetracarboxylic acid, and biphenyltetracarboxylic acid.

[0278] The benzene ring in the formula (d1-I-1) may be further substituted by any substituent. As the substituent, the groups listed for the benzene ring in the formula (d1-I) can be preferably used.

[0279] The partial structure represented by formula (d1-I-1) contained in one molecule of the epoxy (meth)acrylate resin may be one or more, for example, R X is the partial structure of the hydrogen atom and R X Partial structures of polyacid residues are mixed.

[0280] (d1-I) The number of partial structures represented by formula (d1-I) contained in one molecule of epoxy (meth) acrylate resin is not particularly limited, and is preferably 1 or more, and more preferably 3 or more. In addition, it is preferably 20 or less, and further preferably 15 or less. By setting it to be above the aforementioned lower limit, it is easy to obtain a firm film, and there is a tendency that surface roughness generated during development is not easily generated. By setting it to be below the aforementioned upper limit, it is easy to suppress the deterioration of sensitivity or the reduction of film during development, and there is a tendency that the resolution is improved. The above upper and lower limits can be arbitrarily combined. For example, it can be 1 to 20, it can be 1 to 15, or it can be 3 to 15.

[0281] (d1-I) The weight average molecular weight (Mw) of the epoxy (meth) acrylate resin measured by gel permeation chromatography (GPC) in terms of polystyrene is not particularly limited, but is preferably 1000 or more, more preferably 1500 or more, further preferably 2000 or more, further preferably 3000 or more, particularly preferably 4000 or more, most preferably 5000 or more, preferably 30000 or less, more preferably 20000 or less, and further preferably 15000 or less. By setting it to be above the aforementioned lower limit, there is a tendency that the residual film rate of the photosensitive coloring composition becomes good. By setting it to be below the aforementioned upper limit, there is a tendency that the developability becomes good. The above upper and lower limits may be arbitrarily combined. For example, it may be 1000 to 30000, it may be 1500 to 2000, it may be 1500 to 15000, or it may be 2000 to 1500.

[0282] (d1-I) The acid value of the epoxy (meth) acrylate resin is not particularly limited, but is preferably 20 mgKOH / g or more, more preferably 40 mgKOH / g or more, further preferably 60 mgKOH / g or more, further preferably 80 mgKOH / g or more, and particularly preferably 100 mgKOH / g or more. In addition, it is preferably 200 mgKOH / g or less, more preferably 150 mgKOH / g or less, further preferably 130 mgKOH / g or less, and particularly preferably 120 mgKOH / g or less. By setting it to above the aforementioned lower limit, there is a tendency that the developing solubility is improved and the resolution becomes good. By setting it to below the aforementioned upper limit, there is a tendency that the residual film rate of the photosensitive coloring composition becomes good. The above upper and lower limits can be combined arbitrarily. For example, it may be 20 mgKOH / g to 200 mgKOH / g, 60 mgKOH / g to 150 mgKOH / g, 80 mgKOH / g to 130 mgKOH / g, or 100 mgKOH / g to 130 mgKOH / g.

[0283] Specific examples of (d1-I) epoxy (meth)acrylate resins are listed below. In addition, * in the examples represents a connecting bond.

[0284]

[0285]

[0286] <(d1-II) Epoxy (meth)acrylate resin>

[0287]

[0288] In formula (d1-II), R13 Each independently represents a hydrogen atom or a methyl group, R 14 represents a divalent hydrocarbon group having a cyclic hydrocarbon group as a side chain, R 15 and R 16 Each independently represents a divalent aliphatic group which may have a substituent, m and n each independently represent an integer of 0 to 2, and * represents a connecting bond.

[0289] (R 14 )

[0290] In formula (d1-II), R 14 It represents a divalent hydrocarbon group having a cyclic hydrocarbon group as a side chain.

[0291] Examples of the cyclic hydrocarbon group include an aliphatic ring group and an aromatic ring group.

[0292] The number of rings of the aliphatic cyclic group is not particularly limited, but is preferably 1 or more, more preferably 2 or more. In addition, it is preferably 10 or less, more preferably 5 or less, and further preferably 3 or less. By setting it to be above the aforementioned lower limit, a strong film is easily obtained, and there is a tendency that surface roughness generated during development is not easily generated. By setting it to be below the aforementioned upper limit, it is easy to suppress the deterioration of sensitivity or the reduction of the film during development, and there is a tendency to improve the resolution. The above upper and lower limits can be arbitrarily combined. For example, it can be 1 to 10, 1 to 5, 1 to 3, or 2 to 3.

[0293] The carbon number of the aliphatic ring group is not particularly limited, but is preferably 4 or more, more preferably 6 or more, and further preferably 8 or more. In addition, it is preferably 40 or less, more preferably 30 or less, further preferably 20 or less, and particularly preferably 15 or less. By setting it to be above the aforementioned lower limit, a strong film is easily obtained, and there is a tendency that surface roughness generated during development is not easily generated. By setting it to be below the aforementioned upper limit, it is easy to suppress the deterioration of sensitivity or the reduction of the film during development, and there is a tendency to improve the resolution. The above upper and lower limits can be arbitrarily combined. For example, it can be 4 to 40, 4 to 30, 6 to 20, or 8 to 15.

[0294] Examples of the aliphatic ring in the aliphatic cyclic group include a cyclohexane ring, a cycloheptane ring, a cyclodecane ring, a cyclododecane ring, a norbornane ring, an isobornane ring, an adamantane ring, and a cyclododecane ring. From the viewpoint of the residual film rate and resolution of the photosensitive coloring composition, an adamantane ring is preferred.

[0295] The number of rings of the aromatic ring group is not particularly limited, but is preferably 1 or more, more preferably 2 or more, and further preferably 3 or more. In addition, it is preferably 10 or less, more preferably 5 or less, and further preferably 4 or less. The above upper and lower limits may be combined arbitrarily. For example, it is preferably 1 to 10, more preferably 1 to 5, further preferably 1 to 4, further preferably 2 to 4, and particularly preferably 3 to 4. By setting it to be above the above lower limit, it is easy to obtain a strong film, and there is a tendency that the surface roughness generated during development is not easy to occur. By setting it to be below the above upper limit, it is easy to suppress the deterioration of sensitivity or the reduction of the film during development, and there is a tendency to improve the resolution.

[0296] As the aromatic ring group, an aromatic hydrocarbon ring group and an aromatic heterocyclic group can be cited. The number of carbon atoms in the aromatic ring group is not particularly limited, but is preferably 4 or more, more preferably 6 or more, further preferably 8 or more, further preferably 10 or more, and particularly preferably 12 or more. In addition, it is preferably 40 or less, more preferably 30 or less, further preferably 20 or less, and particularly preferably 15 or less. By setting it to above the aforementioned lower limit, a firm film is easily obtained, and there is a tendency that the surface roughness generated during development is not easily generated. By setting it to below the aforementioned upper limit, there is a tendency that the patterning characteristics become good. The above upper and lower limits can be arbitrarily combined. For example, it can be 4 to 40, 6 to 40, 8 to 30, 10 to 20, or 12 to 15.

[0297] Examples of the aromatic ring in the aromatic ring group include a benzene ring, a naphthalene ring, an anthracene ring, a phenanthrene ring, a perylene ring, a tetracene ring, a pyrene ring, a benzopyrene ring, A fluorene ring is preferably a fluorene ring.

[0298] The divalent hydrocarbon group in the divalent hydrocarbon group having a cyclic hydrocarbon group as a side chain is not particularly limited, and examples thereof include a divalent aliphatic group, a divalent aromatic ring group, and a group in which one or more divalent aliphatic groups and one or more divalent aromatic ring groups are linked.

[0299] The divalent aliphatic group may be a straight-chain, branched, or cyclic aliphatic group. From the viewpoint of development solubility, a straight-chain aliphatic group is preferred. On the other hand, from the viewpoint of reducing the penetration of the developer into the exposed portion, a cyclic aliphatic group is preferred. The number of carbon atoms is not particularly limited, but is preferably 1 or more, more preferably 3 or more, and further preferably 6 or more. In addition, it is preferably 25 or less, more preferably 20 or less, and further preferably 15 or less. By setting it to above the aforementioned lower limit, a firm film is easily obtained, and there is a tendency that the surface roughness generated during development is not easily generated, and the adhesion to the substrate becomes good. By setting it to below the aforementioned upper limit, it is easy to suppress the deterioration of sensitivity or the reduction of the film during development, and there is a tendency that the resolution is improved. The above upper and lower limits may be arbitrarily combined. For example, it may be 1 to 25, 3 to 20, or 6 to 15.

[0300] Examples of the divalent straight-chain aliphatic group include a methylene group, an ethylene group, an n-propylene group, an n-butylene group, an n-pentylene group, an n-hexylene group, and an n-heptylene group. From the viewpoint of rigidity of the skeleton, a methylene group is preferred.

[0301] Examples of the divalent branched aliphatic group include a structure in which the divalent straight-chain aliphatic group has a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group or a tert-butyl group as a side chain.

[0302] The number of rings of the divalent cyclic aliphatic group is not particularly limited, but is preferably 1 or more, more preferably 2 or more. In addition, it is preferably 10 or less, more preferably 5 or less, and further preferably 3 or less. By setting it to be above the aforementioned lower limit, a strong film is formed, and there is a tendency that the substrate adhesion becomes good. In addition, by setting it to be below the aforementioned upper limit, it is easy to suppress the deterioration of sensitivity and the reduction of the film during development, and there is a tendency that the resolution is improved. The above upper and lower limits can be combined arbitrarily. For example, it can be 1 to 10, 1 to 5, 1 to 3, or 2 to 3.

[0303] Examples of the divalent cyclic aliphatic group include groups obtained by removing two hydrogen atoms from a cyclohexane ring, a cycloheptane ring, a cyclodecane ring, a cyclododecane ring, a norbornane ring, an isobornane ring, an adamantane ring, and a cyclododecane ring. From the viewpoint of rigidity of the skeleton, a group obtained by removing two hydrogen atoms from an adamantane ring is preferred.

[0304] Examples of the substituent that the divalent aliphatic group may have include alkoxy groups having 1 to 5 carbon atoms, such as methoxy and ethoxy groups; hydroxyl groups; nitro groups; cyano groups; and carboxyl groups. From the viewpoint of ease of synthesis, unsubstituted groups are preferred.

[0305] As the divalent aromatic ring group, a divalent aromatic hydrocarbon ring group and a divalent aromatic heterocyclic group can be listed. The carbon number is not particularly limited, but is preferably 4 or more, more preferably 5 or more, and further preferably 6 or more. In addition, it is preferably 30 or less, more preferably 20 or less, and further preferably 15 or less. By setting it to above the aforementioned lower limit, it is easy to obtain a firm film, and there is a tendency that the surface roughness generated during development is not easy to occur, and the adhesion to the substrate becomes good. By setting it to below the aforementioned upper limit, it is easy to suppress the deterioration of sensitivity or the reduction of the film during development, and there is a tendency to improve the resolution. The above upper and lower limits can be arbitrarily combined. For example, it can be 4 to 30, 5 to 20, or 6 to 15.

[0306] The aromatic hydrocarbon ring in the divalent aromatic hydrocarbon ring group may be a monocyclic ring or a condensed ring. Examples of the divalent aromatic hydrocarbon ring group include a benzene ring, a naphthalene ring, an anthracene ring, a phenanthrene ring, a perylene ring, a tetracene ring, a pyrene ring, a benzopyrene ring, Ring, triphenylene ring, acenaphthene ring, fluoranthene ring, fluorene ring.

[0307] The aromatic heterocyclic ring in the divalent aromatic heterocyclic group may be a monocyclic ring or a condensed ring. Examples of the divalent aromatic heterocyclic group include a furan ring, a benzofuran ring, a thiophene ring, a benzothiophene ring, a pyrrole ring, a pyrazole ring, an imidazole ring, an oxadiazole ring, an indole ring, a carbazole ring, a pyrroloimidazole ring, a pyrrolopyrazole ring, a pyrrolopyrrole ring, a thienopyrrole ring, a thienothiophene ring, a furanopyrrole ring, a furanofuran ring, a thienofuran ring, a benzisoxazole ring, a benzisothiazole ring, a benzimidazole ring, a pyridine ring, a pyrazine ring, a pyridazine ring, a pyrimidine ring, a triazine ring, a quinoline ring, an isoquinoline ring, a cinnoline ring, a quinoxaline ring, a phenanthridine ring, a benzimidazole ring, a phenanthridine ring, a quinazoline ring, a quinazolinone ring, and an azulene ring. Among these, from the viewpoint of patterning properties, a benzene ring or a naphthalene ring having two free valences is preferred, and a benzene ring having two free valences is more preferred.

[0308] Examples of the substituent that the divalent aromatic ring group may have include a hydroxyl group, a methyl group, a methoxy group, an ethyl group, an ethoxy group, a propyl group, and a propoxy group. From the viewpoint of development solubility, it is preferably unsubstituted.

[0309] Examples of the group in which one or more divalent aliphatic groups are linked to one or more divalent aromatic ring groups include groups in which one or more of the aforementioned divalent aliphatic groups are linked to one or more of the aforementioned divalent aromatic ring groups.

[0310] The number of divalent aliphatic groups is not particularly limited, but is preferably 1 or more, more preferably 2 or more, preferably 10 or less, more preferably 5 or less, and further preferably 3 or less. By setting the number to be above the aforementioned lower limit, a strong film can be easily obtained, and the surface roughness generated during development is not easily generated, and the adhesion to the substrate tends to be good. By setting the number to be below the aforementioned upper limit, the deterioration of sensitivity or the reduction of the film during development can be easily suppressed, and the resolution tends to be improved. The above upper and lower limits can be arbitrarily combined. For example, it can be 1 to 10, 1 to 5, 1 to 3, or 2 to 3.

[0311] The number of the divalent aromatic ring groups is not particularly limited, but is preferably 1 or more, more preferably 2 or more, preferably 10 or less, more preferably 5 or less, and further preferably 3 or less. By setting it to be above the aforementioned lower limit, a strong film is easily obtained, and it is not easy to produce surface roughness during development, and the adhesion to the substrate tends to be good. By setting it to be below the aforementioned upper limit, it is easy to suppress the deterioration of sensitivity or the reduction of the film during development, and there is a tendency to improve the resolution. The above upper and lower limits can be combined arbitrarily. For example, it can be 1 to 10, 1 to 5, 1 to 3, or 2 to 3.

[0312] As a group obtained by connecting one or more divalent aliphatic groups to one or more divalent aromatic ring groups, for example, groups represented by the above formulae (d1-IA) to (d1-IF) can be cited. From the viewpoint of rigidity of the skeleton and hydrophobization of the membrane, a group represented by formula (d1-IC) is preferred.

[0313] The bonding method of the cyclic hydrocarbon group as a side chain to these divalent hydrocarbon groups is not particularly limited, and examples thereof include a method in which one hydrogen atom of an aliphatic group or an aromatic ring group is substituted by the cyclic hydrocarbon group as a side chain, and a method in which the cyclic hydrocarbon group as a side chain is composed of one carbon atom of an aliphatic group.

[0314] (R 15 , R 16 )

[0315] In formula (d1-II), R 15 and R 16 Each independently represents a divalent aliphatic group which may have a substituent.

[0316] The divalent aliphatic group may be a straight-chain, branched, or cyclic aliphatic group. From the viewpoint of development solubility, a straight-chain aliphatic group is preferred. On the other hand, from the viewpoint of reducing the penetration of the developer into the exposed portion, a cyclic aliphatic group is preferred. The number of carbon atoms is not particularly limited, but is preferably 1 or more, more preferably 3 or more, and further preferably 6 or more. In addition, it is preferably 20 or less, more preferably 15 or less, and further preferably 10 or less. By setting it to above the aforementioned lower limit, a firm film is easily obtained, and there is a tendency that the surface roughness generated during development is not easily generated, and the adhesion to the substrate becomes good. By setting it to below the aforementioned upper limit, it is easy to suppress the deterioration of sensitivity or the reduction of the film during development, and there is a tendency to improve the resolution. The above upper and lower limits may be arbitrarily combined. For example, it may be 1 to 20, 3 to 15, or 6 to 10.

[0317] Examples of the divalent straight-chain aliphatic group include a methylene group, an ethylene group, an n-propylene group, an n-butylene group, an n-pentylene group, an n-hexylene group, and an n-heptylene group. From the viewpoint of rigidity of the skeleton, a methylene group is preferred.

[0318] Examples of the divalent branched aliphatic group include a structure in which the divalent linear aliphatic group has, for example, a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, or a tert-butyl group as a side chain.

[0319] The number of rings of the divalent cyclic aliphatic group is not particularly limited, but is preferably 1 or more, more preferably 2 or more. In addition, it is preferably 12 or less, more preferably 10 or less. By setting it to above the aforementioned lower limit, a firm film is formed, and there is a tendency that substrate adhesion becomes good. By setting it to below the aforementioned upper limit, it is easy to suppress the deterioration of sensitivity or the film reduction during development, and there is a tendency that resolution is improved.

[0320] The upper and lower limits mentioned above may be arbitrarily combined. For example, they may be 1 to 12, or 2 to 10.

[0321] Examples of the divalent cyclic aliphatic group include groups obtained by removing two hydrogen atoms from a cyclohexane ring, a cycloheptane ring, a cyclodecane ring, a cyclododecane ring, a norbornane ring, an isobornane ring, an adamantane ring, a cyclododecane ring, or a dicyclopentadiene ring. From the viewpoint of rigidity of the skeleton, groups obtained by removing two hydrogen atoms from a dicyclopentadiene ring or an adamantane ring are preferred.

[0322] Examples of the substituent that the divalent aliphatic group may have include alkoxy groups having 1 to 5 carbon atoms, such as methoxy and ethoxy groups; hydroxyl groups; nitro groups; cyano groups; and carboxyl groups. From the viewpoint of ease of synthesis, unsubstituted groups are preferred.

[0323] (m, n)

[0324] In formula (d1-II), m and n each independently represent an integer of 0 to 2. By setting it to be above the aforementioned lower limit, there is a tendency that patterning adaptability is good and surface roughness generated during development is not easily generated. In addition, by setting it to be below the aforementioned upper limit, there is a tendency that developability becomes good. From the viewpoint of developability, m and n are preferably 0. From the viewpoint of patterning adaptability and suppression of surface roughness generated during development, m and n are preferably 1 or more.

[0325] From the viewpoint of adhesion to the substrate, the partial structure represented by formula (d1-II) is preferably a partial structure represented by the following general formula (d1-II-1).

[0326]

[0327] In formula (d1-II-1), R 13 , R 15 , R 16 , m and n have the same meanings as in formula (d1-II), R α represents a monovalent cyclic hydrocarbon group which may have a substituent, p represents an integer greater than 1, and * represents a connecting bond. The benzene ring in formula (d1-II-1) may be further substituted by any substituent.

[0328] (R α )

[0329] In formula (d1-II-1), R α It represents a monovalent cyclic hydrocarbon group which may have a substituent.

[0330] Examples of the cyclic hydrocarbon group include an aliphatic ring group and an aromatic ring group.

[0331] The number of rings of the aliphatic cyclic group is not particularly limited, but is preferably 1 or more, more preferably 2 or more. In addition, it is preferably 6 or less, more preferably 4 or less, and further preferably 3 or less. By setting it to be above the aforementioned lower limit, a strong film is easily obtained, and there is a tendency that the surface roughness generated during development is not easily generated. By setting it to be below the aforementioned upper limit, there is a tendency that the patterning characteristics become good. The above upper and lower limits can be arbitrarily combined. For example, it can be 1 to 6, it can be 1 to 4, it can be 1 to 3, or it can be 2 to 3.

[0332] The carbon number of the aliphatic ring group is not particularly limited, but is preferably 4 or more, more preferably 6 or more, and further preferably 8 or more. In addition, it is preferably 40 or less, more preferably 30 or less, further preferably 20 or less, and particularly preferably 15 or less. By setting it to be above the aforementioned lower limit, a strong film is easily obtained, and there is a tendency that the surface roughness generated during development is not easily generated. By setting it to be below the aforementioned upper limit, there is a tendency that the patterning characteristics become good. The above upper and lower limits can be arbitrarily combined. For example, it can be 4 to 40, 4 to 30, 6 to 20, or 8 to 15.

[0333] Examples of the aliphatic ring in the aliphatic cyclic group include a cyclohexane ring, a cycloheptane ring, a cyclodecane ring, a cyclododecane ring, a norbornane ring, an isobornane ring, an adamantane ring, and a cyclododecane ring. From the viewpoint of strong film properties, an adamantane ring is preferred.

[0334] The number of rings of the aromatic ring group is not particularly limited, but is preferably 1 or more, preferably 2 or more, and more preferably 3 or more. In addition, it is preferably 10 or less, and more preferably 5 or less. By setting it to be above the aforementioned lower limit, a strong film is easily obtained, and there is a tendency that the surface roughness generated during development is not easily generated. By setting it to be below the aforementioned upper limit, there is a tendency that the patterning characteristics become good. The above upper and lower limits can be combined arbitrarily. For example, it can be 1 to 10, 1 to 5, 2 to 5, or 3 to 5.

[0335] As the aromatic ring group, an aromatic hydrocarbon ring group and an aromatic heterocyclic group can be cited. In addition, the carbon number of the aromatic ring group is not particularly limited, and is preferably 4 or more, more preferably 5 or more, and further preferably 6 or more. In addition, it is preferably 30 or less, more preferably 20 or less, and further preferably 15 or less. By setting it to above the aforementioned lower limit, it is easy to obtain a firm film, and there is a tendency that the surface roughness generated during development is not easy to occur. By setting it to below the aforementioned upper limit, there is a tendency that the patterning characteristics become good. The above upper and lower limits can be arbitrarily combined. For example, it can be 4 to 30, can be 5 to 20, and can be 6 to 15.

[0336] Examples of the aromatic ring in the aromatic ring group include a benzene ring, a naphthalene ring, an anthracene ring, a phenanthrene ring, and a fluorene ring. From the viewpoint of development solubility, a fluorene ring is preferred.

[0337] Examples of the substituents that the cyclic hydrocarbon group may have include alkyl groups having 1 to 5 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, pentyl, and isopentyl; alkoxy groups having 1 to 5 carbon atoms, such as methoxy and ethoxy; hydroxyl groups; nitro groups; cyano groups; and carboxyl groups. From the viewpoint of ease of synthesis, unsubstituted groups are preferred.

[0338] p represents an integer greater than or equal to 1, and is preferably greater than or equal to 2. In addition, it is preferably less than or equal to 3. For example, it is preferably 1 to 3, and more preferably 2 to 3. By setting it to be greater than or equal to the above lower limit, there is a tendency that the film curing degree and the residual film rate become good. By setting it to be less than or equal to the above upper limit, there is a tendency that the developability becomes good.

[0339] From the perspective of firm film curing, R α It is preferably a monovalent aliphatic ring group, and more preferably an adamantyl group.

[0340] The benzene ring in formula (d1-II-1) may be further substituted by any substituent. As a substituent, for example, hydroxyl, methyl, methoxy, ethyl, ethoxy, propyl, propoxy can be listed. The number of substituents is not particularly limited, and can be 1 or more than 2.

[0341] From the viewpoint of patterning properties, unsubstituted is preferred.

[0342] Specific examples of the partial structure represented by formula (d1-II-1) are listed below.

[0343]

[0344]

[0345] From the viewpoint of rigidity of the skeleton and hydrophobization of the membrane, the partial structure represented by the formula (d1-II) is preferably a partial structure represented by the following general formula (d1-II-2).

[0346]

[0347] In formula (d1-II-2), R 13 , R 15 , R 16 , m and n have the same meanings as in formula (d1-II), R β represents a divalent cyclic hydrocarbon group which may have a substituent, and * represents a connecting bond.

[0348] The benzene ring in the formula (d1-II-2) may be further substituted by any substituent.

[0349] (R β )

[0350] In formula (d1-II-2), R β It represents a divalent cyclic hydrocarbon group which may have a substituent.

[0351] Examples of the cyclic hydrocarbon group include an aliphatic ring group and an aromatic ring group.

[0352] The number of rings of the aliphatic cyclic group is not particularly limited, but is preferably 1 or more, more preferably 2 or more. In addition, it is preferably 10 or less, more preferably 5 or less. By setting it to be above the aforementioned lower limit, a strong film is easily obtained, and there is a tendency that the surface roughness generated during development is not easily generated. By setting it to be below the aforementioned upper limit, it is easy to suppress the deterioration of sensitivity or the reduction of the film during development, and there is a tendency to improve the resolution. The above upper and lower limits can be combined arbitrarily. For example, it can be 1 to 10, or it can be 2 to 5.

[0353] The carbon number of the aliphatic ring group is preferably 4 or more, more preferably 6 or more, and further preferably 8 or more. In addition, it is preferably 40 or less, more preferably 35 or less, and further preferably 30 or less. By setting it to be above the aforementioned lower limit, there is a tendency to suppress the roughness of the film surface during development. By setting it to be below the aforementioned upper limit, it is easy to suppress the deterioration of sensitivity or the reduction of the film during development, and there is a tendency to improve the resolution. The above upper and lower limits can be combined arbitrarily. For example, it can be 4 to 40, 6 to 35, or 8 to 30.

[0354] Examples of the aliphatic ring in the aliphatic cyclic group include cyclohexane ring, cycloheptane ring, cyclodecane ring, cyclododecane ring, norbornane ring, isobornane ring, adamantane ring, and cyclododecane ring. From the viewpoint of film reduction and resolution during development, adamantane ring is preferred.

[0355] The number of rings of the aromatic ring group is not particularly limited, but is preferably 1 or more, more preferably 2 or more, and further preferably 3 or more. In addition, it is preferably 10 or less, and more preferably 5 or less. By setting it to be above the aforementioned lower limit, a strong film is easily obtained, and there is a tendency that surface roughness generated during development is not easily generated. By setting it to be below the aforementioned upper limit, it is easy to suppress the deterioration of sensitivity or film reduction, and there is a tendency that the resolution is improved. The above upper and lower limits can be combined arbitrarily. For example, it can be 1 to 10, 1 to 5, 2 to 5, or 3 to 5.

[0356] Examples of the aromatic ring group include an aromatic hydrocarbon ring group and an aromatic heterocyclic group.

[0357] The number of carbon atoms in the aromatic ring group is preferably 4 or more, more preferably 6 or more, further preferably 8 or more, and further preferably 10 or more. In addition, it is preferably 40 or less, more preferably 30 or less, further preferably 20 or less, and particularly preferably 15 or less. By setting it to be above the aforementioned lower limit, it is easy to obtain a strong film, and there is a tendency that the surface roughness generated during development is not easy to occur. By setting it to be below the aforementioned upper limit, it is easy to suppress the deterioration of sensitivity or the reduction of the film, and there is a tendency to improve the resolution. The above upper and lower limits can be combined arbitrarily. For example, it can be 4 to 40, 6 to 30, 8 to 20, or 10 to 15.

[0358] Examples of the aromatic ring in the aromatic ring group include a benzene ring, a naphthalene ring, an anthracene ring, a phenanthrene ring, and a fluorene ring. From the viewpoint of developability, a fluorene ring is preferred.

[0359] Examples of the substituents that the cyclic hydrocarbon group may have include alkyl groups having 1 to 5 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, pentyl, and isopentyl; alkoxy groups having 1 to 5 carbon atoms, such as methoxy and ethoxy; hydroxyl groups; nitro groups; cyano groups; and carboxyl groups. From the viewpoint of ease of synthesis, unsubstituted groups are preferred.

[0360] From the viewpoint of suppressing film reduction and resolution, R β Preferably, it is a divalent aliphatic ring group, and more preferably a divalent adamantane ring group. On the other hand, from the viewpoint of patterning properties, R β It is preferably a divalent aromatic ring group, and more preferably a divalent fluorene ring group.

[0361] The benzene ring in formula (d1-II-2) may be further substituted by any substituent. As a substituent, for example, hydroxyl, methyl, methoxy, ethyl, ethoxy, propyl, propoxy can be listed. The number of substituents is not particularly limited, and can be 1 or more than 2.

[0362] In addition, the two benzene rings in formula (d1-II-2) are connected by R β When connected, they can be further connected via substituents to form a tricyclic structure. As substituents in this case, divalent groups such as -O-, -S-, -NH-, and -CH2- can be listed. For example, forming a tricyclic structure via -O- means that each benzene ring is connected to R β Carbon atoms adjacent to the bonded carbon atoms are linked to each other via -O- to form a xanthene skeleton.

[0363] From the viewpoint of patterning properties, unsubstituted is preferred, while methyl substitution is preferred from the viewpoint of less likely to cause film reduction.

[0364] Specific examples of the partial structure represented by formula (d1-II-2) are listed below. It should be noted that * in the examples represents a connecting bond.

[0365]

[0366]

[0367] From the viewpoint of the coating film residual rate and patterning characteristics, the partial structure represented by formula (d1-II) is preferably a partial structure represented by the following general formula (d1-II-3).

[0368]

[0369] In formula (d1-II-3), R 13 , R 14 , R 15 , R 16 , m and n have the same meanings as in formula (d1-II), R Z represents a hydrogen atom or a polyacid residue.

[0370] The polyacid residue is a monovalent group obtained by removing one OH group from a polyacid. It should be noted that another OH group may be further removed to form a monovalent group with R Z That is, multiple formulas (d1-II-3) can be shared by R Z And connect.

[0371] Examples of the polybasic acid include maleic acid, succinic acid, itaconic acid, phthalic acid, tetrahydrophthalic acid, hexahydrophthalic acid, pyromellitic acid, trimellitic acid, benzophenonetetracarboxylic acid, methylhexahydrophthalic acid, endomethylenetetrahydrophthalic acid, chlorendic acid, methyltetrahydrophthalic acid, and biphenyltetracarboxylic acid.

[0372] From the viewpoint of patterning properties, preferred are maleic acid, succinic acid, itaconic acid, phthalic acid, tetrahydrophthalic acid, hexahydrophthalic acid, pyromellitic acid, trimellitic acid, and biphenyltetracarboxylic acid, and more preferred are tetrahydrophthalic acid, biphenyltetracarboxylic acid, and biphenyltetracarboxylic acid.

[0373] The partial structure represented by formula (d1-II-3) contained in one molecule of the epoxy (meth)acrylate resin (d1-II) may be one or more, for example, R Z is the structure of hydrogen atom and R Z The structures of polyacid residues are mixed.

[0374] (d1-II) The number of partial structures represented by formula (d1-II) contained in one molecule of epoxy (meth) acrylate resin is not particularly limited, and is preferably 1 or more, more preferably 3 or more. In addition, it is preferably 20 or less, more preferably 15 or less, and further preferably 10 or less. By setting it to be above the aforementioned lower limit, it is easy to obtain a firm film, and there is a tendency that surface roughness generated during development is not easily generated. By setting it to be below the aforementioned upper limit, it is easy to suppress the deterioration of sensitivity and the reduction of film, and there is a tendency that the resolution is improved. The above upper and lower limits can be arbitrarily combined. For example, it can be 1 to 20, it can be 1 to 15, or it can be 3 to 10.

[0375] (d1-II) The weight average molecular weight (Mw) of the epoxy (meth) acrylate resin measured by gel permeation chromatography (GPC) in terms of polystyrene is not particularly limited, but is preferably 1000 or more, more preferably 1500 or more, further preferably 2000 or more, further preferably 3000 or more, further preferably 4000 or more, and particularly preferably 5000 or more. In addition, it is preferably 10000 or less, more preferably 8000 or less, and further preferably 7000 or less. By setting it to be above the aforementioned lower limit, there is a tendency for the residual film rate of the photosensitive coloring composition to become good. By setting it to be below the aforementioned upper limit, there is a tendency for the developability to become good. The above upper and lower limits may be arbitrarily combined. For example, it may be 1000 to 10000, may be 1500 to 10000, may be 1500 to 8000, may be 2000 to 8000, may be 2000 to 7000.

[0376] (d1-II) The acid value of the epoxy (meth) acrylate resin is not particularly limited, but is preferably 20 mgKOH / g or more, more preferably 40 mgKOH / g or more, further preferably 60 mgKOH / g or more, further preferably 80 mgKOH / g or more, and particularly preferably 100 mgKOH / g or more. In addition, it is preferably 200 mgKOH / g or less, more preferably 150 mgKOH / g or less, further preferably 130 mgKOH / g or less, and particularly preferably 120 mgKOH / g or less. By setting it to above the aforementioned lower limit, there is a tendency for the developing solubility to be improved and the resolution to be improved. By setting it to below the aforementioned upper limit, there is a tendency for the residual film rate of the photosensitive coloring composition to be improved. The above upper and lower limits may be combined arbitrarily. For example, it may be 20 mgKOH / g to 200 mgKOH / g, 60 mgKOH / g to 150 mgKOH / g, 80 mgKOH / g to 130 mgKOH / g, or 100 mgKOH / g to 130 mgKOH / g.

[0377] The carboxyl group-containing epoxy (meth)acrylate resin may be used alone or in combination of two or more.

[0378] In addition, a part of the aforementioned carboxyl-containing epoxy (meth) acrylate resin can also be replaced with other binder resins for use. That is, carboxyl-containing epoxy (meth) acrylate resin and other binder resins can be used in combination. In this case, the ratio of the carboxyl-containing epoxy (meth) acrylate resin in (b) the alkali-soluble resin is preferably set to 50% by mass or more, more preferably set to 60% by mass or more, further preferably set to 70% by mass or more, particularly preferably set to 80% by mass or more, and can also be 100% by mass or less.

[0379] <(D2) Acrylic Copolymer Resin>

[0380] As the (D) alkali-soluble resin, from the viewpoint of compatibility with a pigment, a dispersant, etc., it is preferred to use an acrylic copolymer resin (D2), and the resins described in JP-A-2014-137466 can be preferably used.

[0381] Examples of the (D2) acrylic copolymer resin include copolymers of an ethylenically unsaturated monomer having one or more carboxyl groups (hereinafter referred to as “unsaturated monomer (d2-1)”) and other copolymerizable ethylenically unsaturated monomers (hereinafter referred to as “unsaturated monomer (d2-2)”).

[0382] Examples of the unsaturated monomer (d2-1) include unsaturated monocarboxylic acids such as (meth)acrylic acid, crotonic acid, α-chloroacrylic acid, and cinnamic acid; unsaturated dicarboxylic acids or their anhydrides such as maleic acid, maleic anhydride, fumaric acid, citraconic acid, citraconic anhydride, and mesaconic acid; mono(meth)acryloxyalkyl) esters of polycarboxylic acids having a valence of 2 or more such as mono(2-(meth)acryloxyethyl) succinate and mono(2-(meth)acryloxyethyl) phthalate; mono(meth)acrylates of polymers having carboxyl groups and hydroxyl groups at both ends such as ω-carboxy polycaprolactone mono(meth)acrylate; and p-vinylbenzoic acid.

[0383] These unsaturated monomers (d2-1) can be used alone or in combination of two or more.

[0384] Examples of the unsaturated monomer (d2-2) include:

[0385] N-substituted maleimides such as N-phenylmaleimide and N-cyclohexylmaleimide;

[0386] Aromatic vinyl compounds such as styrene, α-methylstyrene, p-hydroxystyrene, p-hydroxy-α-methylstyrene, p-vinylbenzyl glycidyl ether, and acenaphthylene;

[0387] Methyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, allyl (meth)acrylate, benzyl (meth)acrylate, polyethylene glycol (degree of polymerization 2-10) methyl ether (meth)acrylate, polypropylene glycol (degree of polymerization 2-10) methyl ether (meth)acrylate, polyethylene glycol (degree of polymerization 2-10) mono(meth)acrylate, polypropylene glycol (degree of polymerization 2-10) mono(meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, tricyclo[5.2.1.0](meth)acrylate 2,6] decane-8-acrylate, dicyclopentenyl (meth)acrylate, glycerol mono(meth)acrylate, 4-hydroxyphenyl (meth)acrylate, ethylene oxide-modified (meth)acrylate of p-cumylphenol, glycidyl (meth)acrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, 3-〔(meth)acryloyloxymethyl〕oxetane, 3-〔(meth)acryloyloxymethyl〕-3-ethyloxetane and the like (meth)acrylates;

[0388] Cyclohexyl vinyl ether, isobornyl vinyl ether, tricyclic [5.2.1.0 2,6 ] vinyl ethers such as decane-8-yl vinyl ether, pentacyclopentadecyl vinyl ether, 3-(vinyloxymethyl)-3-ethyloxetane;

[0389] A macromonomer having a mono(meth)acryloyl group at the end of a polymer molecular chain such as polystyrene, poly(methyl)acrylate, poly(n-butyl)(meth)acrylate, and polysiloxane.

[0390] These unsaturated monomers (d2-2) can be used alone or in combination of two or more.

[0391] In the copolymer of the unsaturated monomer (d2-1) and the unsaturated monomer (d2-2), the copolymerization ratio of the unsaturated monomer (d2-1) is preferably 5 to 50% by mass, and more preferably 10 to 40% by mass. By copolymerizing the unsaturated monomer (d2-1) in such a range, there is a tendency to obtain a photosensitive coloring composition having excellent alkali developability and storage stability.

[0392] Examples of copolymers of an unsaturated monomer (d2-1) and an unsaturated monomer (d2-2) include copolymers disclosed in JP-A-7-140654, JP-A-8-259876, JP-A-10-31308, JP-A-10-300922, JP-A-11-174224, JP-A-11-258415, JP-A-2000-56118, and JP-A-2004-101728.

[0393] The copolymer of the unsaturated monomer (d2-1) and the unsaturated monomer (d2-2) can be produced by a known method, for example, its structure, Mw, and Mw / Mn (Mn is the number average molecular weight) can also be controlled by the method disclosed in Japanese Patent Publication No. 2003-222717, Japanese Patent Publication No. 2006-259680, and International Publication No. 2007 / 029871.

[0394] Resins described in International Publication No. 2016 / 194619 and International Publication No. 2017 / 154439 may also be used.

[0395] <(E) Photopolymerizable Compound>

[0396] The photosensitive resin composition of the present invention contains (E) a photopolymerizable compound for reasons of sensitivity and the like.

[0397] (E) The photopolymerizable compound includes compounds having at least one ethylenically unsaturated group in the molecule (hereinafter sometimes referred to as "ethylenic monomers"), and specifically, for example, (meth)acrylic acid, (meth)acrylic acid alkyl esters, acrylonitrile, styrene, and esters of carboxylic acids having one ethylenically unsaturated bond and polyols or monools.

[0398] As the (E) photopolymerizable compound, it is particularly preferred to use a multifunctional ethylenic monomer having two or more ethylenically unsaturated groups in one molecule. The number of ethylenically unsaturated groups in the multifunctional ethylenic monomer is preferably three or more, more preferably four or more, further preferably five or more, particularly preferably six or more, and preferably ten or less, more preferably eight or less. By setting the number to be above the lower limit, the photosensitive resin composition tends to have a high sensitivity, and by setting the number to be below the upper limit, the curing shrinkage during polymerization tends to be reduced.

[0399] The above upper and lower limits may be arbitrarily combined, for example, 2 to 10, 3 to 10, 4 to 10, 5 to 8, or 6 to 8.

[0400] Examples of the polyfunctional ethylenic monomer include esters of aliphatic polyhydroxy compounds and unsaturated carboxylic acids; esters of aromatic polyhydroxy compounds and unsaturated carboxylic acids; and esters obtained by esterification of polyhydroxy compounds such as aliphatic polyhydroxy compounds and aromatic polyhydroxy compounds with unsaturated carboxylic acids and polycarboxylic acids.

[0401] Examples of the esters of aliphatic polyhydroxy compounds and unsaturated carboxylic acids include acrylates of aliphatic polyhydroxy compounds such as ethylene glycol diacrylate, triethylene glycol diacrylate, trimethylolpropane triacrylate, trimethylolethane triacrylate, pentaerythritol diacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, dipentaerythritol tetraacrylate, dipentaerythritol pentaacrylate, dipentaerythritol hexaacrylate, and glycerol acrylate; methacrylates obtained by replacing the acrylates of these exemplified compounds with methacrylates, itaconates obtained by similarly replacing the acrylates with itaconates, crotonates obtained by replacing the acrylates with crotonates, or maleates obtained by replacing the acrylates with maleates.

[0402] Examples of the esters of an aromatic polyhydroxy compound and an unsaturated carboxylic acid include acrylates and methacrylates of aromatic polyhydroxy compounds such as hydroquinone diacrylate, hydroquinone dimethacrylate, resorcinol diacrylate, resorcinol dimethacrylate, and pyrogallol triacrylate.

[0403] The esters obtained by the esterification reaction of polycarboxylic acids and unsaturated carboxylic acids with polyhydroxy compounds are not necessarily single substances. Representative specific examples include condensates of acrylic acid, phthalic acid, and ethylene glycol; condensates of acrylic acid, maleic acid, and diethylene glycol; condensates of methacrylic acid, terephthalic acid, and pentaerythritol; and condensates of acrylic acid, adipic acid, butanediol, and glycerol.

[0404] In addition, examples of the multifunctional olefinic monomers used in the present invention include: urethane (meth)acrylates obtained by reacting a polyisocyanate compound with a hydroxyl group-containing (meth)acrylate or a polyisocyanate compound with a polyol and a hydroxyl group-containing (meth)acrylate; epoxy acrylates such as addition reaction products of a polyvalent epoxy compound with a hydroxyl (meth)acrylate or (meth)acrylic acid; acrylamides such as ethylenebisacrylamide; allyl esters such as diallyl phthalate; and vinyl-containing compounds such as divinyl phthalate.

[0405] These may be used alone or in combination of two or more.

[0406] The content ratio of the (E) photopolymerizable compound is not particularly limited, but is preferably 90% by mass or less, more preferably 70% by mass or less, further preferably 50% by mass or less, further preferably 30% by mass or less, particularly preferably 20% by mass or less, and most preferably 10% by mass or less. In addition, it is preferably 1% by mass or more, and more preferably 5% by mass or more. By making the content ratio of the (E) photopolymerizable compound less than the above upper limit, there is a tendency that the permeability of the developer to the exposed part becomes moderate, and a good image can be obtained. By being more than the above lower limit, there is a tendency that the photocuring based on ultraviolet irradiation is improved, and the alkali developability also becomes good.

[0407] The above upper and lower limits may be arbitrarily combined, for example, 1 to 90% by mass, 1 to 70% by mass, 1 to 50% by mass, 5 to 30% by mass, 5 to 20% by mass, or 5 to 10% by mass.

[0408] <(F) Photopolymerization Initiator>

[0409] The photosensitive resin composition of the present invention contains (F) a photopolymerization initiator. (F) The photopolymerization initiator is a component that directly absorbs light and undergoes a decomposition reaction or a hydrogen abstraction reaction to generate polymerization-active free radicals. An additive such as a sensitizing dye may be added as needed.

[0410] (F) Photopolymerization initiator, for example, metallocene compounds including titanocene compounds described in Japanese Patent Application Laid-Open No. 59-152396 and Japanese Patent Application Laid-Open No. 61-151197; hexaarylbiimidazole derivatives described in Japanese Patent Application Laid-Open No. 2000-56118; halogenated methylated oxadiazole derivatives, halogenated methyl s-triazine derivatives, N-aryl-α-amino acids such as N-phenylglycine, N-aryl-α-amino acid salts, free radical activators such as N-aryl-α-amino acid esters, α-aminoalkylphenone derivatives described in Japanese Patent Application Laid-Open No. 10-39503; oxime ester derivatives described in Japanese Patent Application Laid-Open No. 2000-80068 and Japanese Patent Application Laid-Open No. 2006-36750.

[0411] Examples of the titanocene derivatives include dicyclopentadienyl titanium dichloride, dicyclopentadienyl bisphenyl titanium, dicyclopentadienyl bis(2,3,4,5,6-pentafluorophenyl)titanium, dicyclopentadienyl bis(2,3,5,6-tetrafluorophenyl)titanium, dicyclopentadienyl bis(2,4,6-trifluorophenyl)titanium, dicyclopentadienyl bis(2,6-difluorophenyl)titanium, dicyclopentadienyl bis(2,4-difluorophenyl)titanium, di(methylcyclopentadienyl)bis(2,3,4,5,6-pentafluorophenyl)titanium, di(methylcyclopentadienyl)bis(2,6-difluorophenyl)titanium, and dicyclopentadienyl [2,6-difluoro-3-(pyrrol-1-yl)-phenyl]titanium.

[0412] Examples of biimidazole derivatives include 2-(2'-chlorophenyl)-4,5-diphenylimidazole dimer, 2-(2'-chlorophenyl)-4,5-bis(3'-methoxyphenyl)imidazole dimer, 2-(2'-fluorophenyl)-4,5-diphenylimidazole dimer, 2-(2'-methoxyphenyl)-4,5-diphenylimidazole dimer, and (4'-methoxyphenyl)-4,5-diphenylimidazole dimer.

[0413] Examples of the halogenated methylated oxadiazole derivatives include 2-trichloromethyl-5-(2'-benzofuranyl)-1,3,4-oxadiazole, 2-trichloromethyl-5-[β-(2'-benzofuranyl)vinyl]-1,3,4-oxadiazole, 2-trichloromethyl-5-[β-(2'-(6"-benzofuranyl)vinyl)]-1,3,4-oxadiazole, and 2-trichloromethyl-5-furanyl-1,3,4-oxadiazole.

[0414] Examples of the halomethyl-s-triazine derivatives include 2-(4-methoxyphenyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(4-methoxynaphthyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(4-ethoxynaphthyl)-4,6-bis(trichloromethyl)-s-triazine, and 2-(4-ethoxycarbonylnaphthyl)-4,6-bis(trichloromethyl)-s-triazine.

[0415] Examples of the α-aminoalkylphenone derivatives include 2-methyl-1〔4-(methylthio)phenyl〕-2-morpholinopropane-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butane-1-one, 4-dimethylaminoethyl benzoate, 4-dimethylaminoisoamyl benzoate, 4-dimethylaminoacetophenone, 4-dimethylaminopropiophenone, 1,4-dimethylaminobenzoic acid 2-ethylhexyl ester, 2,5-bis(4-diethylaminobenzylidene)cyclohexanone, 7-diethylamino-3-(4-diethylaminobenzoyl)coumarin, and 4-(diethylamino)chalcone.

[0416] As (F) photopolymerization initiator, oxime derivatives (oxime ester compounds and ketoxime ester compounds) are preferred from the aspect of sensitivity. Among oxime derivatives, oxime ester compounds are preferred from the viewpoint of adhesion to the substrate. When an alkali-soluble resin containing a phenolic hydroxyl group is used, it may sometimes become disadvantageous in terms of sensitivity.

[0417] The photopolymerization initiator of the oxime ester compound has a structure for absorbing ultraviolet rays, a structure for transmitting light energy, and a structure for generating free radicals in its structure, so a small amount of high sensitivity can be obtained, and the thermal reaction is stable, and a small amount of high-sensitivity photosensitive resin composition can be designed. In particular, from the viewpoint of light absorption of the i-ray (365nm) of the exposure light source, in the case of an oxime ester compound containing an optionally substituted carbazole group (a group having an optionally substituted carbazole ring), the structural characteristics can be well expressed, which is more preferred. Now, in the market, a black matrix with high light-shielding degree and thin film is required, and the pigment concentration is also increasing. It is particularly effective under such conditions.

[0418] Examples of the oxime ester compound include compounds containing a structural portion represented by the following general formula (22), and preferably include oxime ester compounds represented by the following general formula (23).

[0419]

[0420] In formula (22), R 22Each represents an optionally substituted alkanoyl group having 2 to 12 carbon atoms, a heteroarylalkanoyl group having 1 to 20 carbon atoms, an alkenoyl group having 3 to 25 carbon atoms, a cycloalkanoyl group having 3 to 8 carbon atoms, an alkoxycarbonylalkanoyl group having 3 to 20 carbon atoms, a phenoxycarbonylalkanoyl group having 8 to 20 carbon atoms, a heteroaryloxycarbonylalkanoyl group having 3 to 20 carbon atoms, an aminoalkylcarbonyl group having 2 to 10 carbon atoms, an aroyl group having 7 to 20 carbon atoms, a heteroaroyl group having 1 to 20 carbon atoms, an alkoxycarbonyl group having 2 to 10 carbon atoms, or an aryloxycarbonyl group having 7 to 20 carbon atoms.

[0421]

[0422] In formula (23), R 21a represents hydrogen, or optionally substituted, alkyl having 1 to 20 carbon atoms, alkenyl having 2 to 25 carbon atoms, heteroarylalkyl having 1 to 20 carbon atoms, alkoxycarbonylalkyl having 3 to 20 carbon atoms, phenoxycarbonylalkyl having 8 to 20 carbon atoms, heteroaryloxycarbonylalkyl or heteroarylsulfanyl having 1 to 20 carbon atoms, aminoalkyl having 1 to 20 carbon atoms, alkanoyl having 2 to 12 carbon atoms, alkenoyl having 3 to 25 carbon atoms, cycloalkanoyl having 3 to 8 carbon atoms, aroyl having 7 to 20 carbon atoms, heteroaroyl having 1 to 20 carbon atoms, alkoxycarbonyl having 2 to 10 carbon atoms, aryloxycarbonyl having 7 to 20 carbon atoms, or cycloalkylalkyl having 1 to 10 carbon atoms;

[0423] R 21b It represents an arbitrary substituent containing an aromatic ring or a heteroaromatic ring.

[0424] It should be noted that R 21a Can be used with R 21b Together they form a ring, and examples of the linking group include an alkylene group having 1 to 10 carbon atoms, a polyvinyl group (-(CH=CH) r -), polyethynyl (-(C≡C) r -) or a group formed by combining them (it should be noted that r is an integer of 0 to 3).

[0425] R 22a It is expressed as R in formula (22) 22 Same group.

[0426] As R in formula (22) 22 And R in formula (23) 22a Preferred examples include an alkanoyl group having 2 to 12 carbon atoms, a heteroarylalkanoyl group having 1 to 20 carbon atoms, and a cycloalkanoyl group having 3 to 8 carbon atoms.

[0427] As R in formula (23) 21a Preferred examples include unsubstituted straight-chain alkyl or cycloalkylalkyl groups such as methyl, ethyl and propyl groups, and propyl groups substituted with N-acetyl-N-acetoxyamino groups.

[0428] As R in formula (23) 21b Preferred examples include an optionally substituted carbazolyl group, an optionally substituted thioxanthone group, and an optionally substituted phenyl sulfide group.

[0429] As the photopolymerization initiator of the oxime ester compound, R in the formula (23) 21b Compounds that are optionally substituted carbazolyl groups are more preferred for the reasons described above. Furthermore, it is preferred that the carbazolyl group has at least one group selected from the group consisting of an optionally substituted aryl group having 6 to 25 carbon atoms, an optionally substituted arylcarbonyl group having 7 to 25 carbon atoms, an optionally substituted heteroaryl group having 5 to 25 carbon atoms, an optionally substituted heteroarylcarbonyl group having 6 to 25 carbon atoms, and a nitro group. It is particularly preferred that the carbazolyl group has at least one group selected from the group consisting of a benzoyl group, a toluoyl group, a naphthoyl group, a thienylcarbonyl group, and a nitro group. In addition, it is desirable that these groups are bonded to the 3-position of the carbazolyl group.

[0430] Examples of commercially available products of the photopolymerization initiator of the oxime ester compound include OXE-02 manufactured by BASF Corporation and TR-PBG-304 and TR-PBG-314 manufactured by Changzhou Qiangli Electronics Corporation.

[0431] Examples of the photopolymerization initiator of the oxime ester compound include the following.

[0432]

[0433]

[0434]

[0435] Examples of the ketoxime ester compound include compounds containing a structural portion represented by the following general formula (24), and preferably include ketoxime ester compounds represented by the following general formula (25).

[0436]

[0437] In formula (24), R 24 With R in formula (22) 22 Same meaning.

[0438]

[0439] In formula (25), R 23arepresents an optionally substituted phenyl group, an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 25 carbon atoms, a heteroarylalkyl group having 1 to 20 carbon atoms, an alkoxycarbonylalkyl group having 3 to 20 carbon atoms, a phenoxycarbonylalkyl group having 8 to 20 carbon atoms, an alkylsulfanyl group having 2 to 20 carbon atoms, a heteroaryloxycarbonylalkyl group or a heteroarylsulfanyl group having 1 to 20 carbon atoms, an aminoalkyl group having 1 to 20 carbon atoms, an alkanoyl group having 2 to 12 carbon atoms, an alkenoyl group having 3 to 25 carbon atoms, a cycloalkanoyl group having 3 to 8 carbon atoms, an aroyl group having 7 to 20 carbon atoms, a heteroaroyl group having 1 to 20 carbon atoms, an alkoxycarbonyl group having 2 to 10 carbon atoms, an aryloxycarbonyl group having 7 to 20 carbon atoms, or a cycloalkylalkyl group having 1 to 10 carbon atoms.

[0440] R 23b It represents an arbitrary substituent containing an aromatic ring or a heteroaromatic ring.

[0441] R 23a Can be used with R 23b Together they form a ring, and examples of the linking group include an alkylene group having 1 to 10 carbon atoms, a polyvinyl group (-(CH=CH) r -), polyethynyl (-(C≡C) r -) or a group formed by combining them (r is an integer of 0 to 3).

[0442] R 24a represents an alkanoyl group having 2 to 12 carbon atoms, an alkenoyl group having 3 to 25 carbon atoms, a cycloalkanoyl group having 4 to 8 carbon atoms, a benzoyl group having 7 to 20 carbon atoms, a heteroaroyl group having 3 to 20 carbon atoms, an alkoxycarbonyl group having 2 to 10 carbon atoms, an aryloxycarbonyl group having 7 to 20 carbon atoms, a heteroaryl group having 2 to 20 carbon atoms, or an alkylaminocarbonyl group having 2 to 20 carbon atoms, each of which is optionally substituted.

[0443] As R in formula (24) 24 and R in the general formula (25) 24a Preferred examples include an alkanoyl group having 2 to 12 carbon atoms, a heteroarylalkanoyl group having 1 to 20 carbon atoms, a cycloalkanoyl group having 3 to 8 carbon atoms, and an aroyl group having 7 to 20 carbon atoms.

[0444] As R in formula (25) 23a Preferred examples include unsubstituted ethyl, propyl, butyl, and ethyl or propyl substituted with methoxycarbonyl.

[0445] As R in formula (25) 23b Preferably, an optionally substituted carbazolyl group and an optionally substituted phenyl sulfide group are mentioned.

[0446] Examples of the ketoxime ester compounds include the following.

[0447]

[0448]

[0449] Examples of commercially available products of the photopolymerization initiator of the ketoxime ester compound include OXE-01 manufactured by BASF and TR-PBG-305 manufactured by Changzhou Qiangli Electronics Co., Ltd.

[0450] Oxime ester compounds and ketoxime ester compounds are known compounds per se, and are described in, for example, JP-A-2000-80068 and JP-A-2006-36750.

[0451] The photopolymerization initiator may be used alone or in combination of two or more.

[0452] In addition, for example, benzoin alkyl ethers such as benzoin methyl ether, benzoin phenyl ether, benzoin isobutyl ether, and benzoin isopropyl ether; anthraquinone derivatives such as 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert-butylanthraquinone, and 1-chloroanthraquinone; benzophenone derivatives such as benzophenone, Michler's ketone, 2-methylbenzophenone, 3-methylbenzophenone, 4-methylbenzophenone, 2-chlorobenzophenone, 4-bromobenzophenone, and 2-carboxybenzophenone; 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxyacetophenone, 1-hydroxycyclohexyl phenyl ketone, α-hydroxy-2-methylphenylacetone, 1-hydroxy-1-methylethyl-(p-isopropylphenyl)ketone, 1-hydroxy 1-(p-dodecylphenyl)ketone, 2-methyl-(4'-methylthiophenyl)-2-morpholinyl-1-propanone, 1,1,1-trichloromethyl-(p-butylphenyl)ketone and other acetophenone derivatives; thioxanthone derivatives such as 2-ethylthioxanthone, 2-isopropylthioxanthone, 2-chlorothioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2,4-diisopropylthioxanthone and other thioxanthone derivatives; benzoate derivatives such as ethyl p-dimethylaminobenzoate and ethyl p-diethylaminobenzoate; acridine derivatives such as 9-phenylacridine and 9-(p-methoxyphenyl)acridine; phenazine derivatives such as 9,10-dimethylbenzophenazine; anthrone derivatives such as benzanthrone.

[0453] As the photopolymerization initiator, oxime ester derivatives are particularly preferred for the reasons described above.

[0454] The content ratio of the (F) photopolymerization initiator is not particularly limited, but is preferably 1% by mass or more, more preferably 2% by mass or more, further preferably 3% by mass or more, particularly preferably 4% by mass or more, and preferably 30% by mass or less, more preferably 20% by mass or less, further preferably 15% by mass or less, particularly preferably 10% by mass or less, and most preferably 8% by mass or less, relative to the total solid content of the photosensitive resin composition. If the content ratio of the (F) photopolymerization initiator is above the lower limit, the sensitivity tends to be improved, and if it is below the upper limit, the solubility of the unexposed portion in the developer tends to be improved.

[0455] The above upper and lower limits may be arbitrarily combined, and may be, for example, 1 to 30% by mass, 1 to 20% by mass, 2 to 15% by mass, 3 to 10% by mass, or 4 to 8% by mass.

[0456] <Sensitizing pigment>

[0457] (F) The photopolymerization initiator may be used in combination with a sensitizing dye corresponding to the wavelength of the image exposure light source for the purpose of improving the sensitivity as needed. Examples of the sensitizing dye include xanthene dyes described in Japanese Patent Laid-Open Nos. 4-221958 and 4-219756; coumarin dyes having a heterocyclic ring described in Japanese Patent Laid-Open Nos. 3-239703 and 5-289335; 3-coumarin keto compounds described in Japanese Patent Laid-Open Nos. 3-239703 and 5-289335; pyrromethene dyes described in Japanese Patent Laid-Open Nos. 6-19240; and pyrromethene dyes described in Japanese Patent Laid-Open Nos. 47-2528 and 54-546. -155292, Japanese Patent Publication No. 45-37377, Japanese Patent Application Laid-Open No. 48-84183, Japanese Patent Application Laid-Open No. 52-112681, Japanese Patent Application Laid-Open No. 58-15503, Japanese Patent Application Laid-Open No. 60-88005, Japanese Patent Application Laid-Open No. 59-56403, Japanese Patent Application Laid-Open No. 2-69, Japanese Patent Application Laid-Open No. 57-168088, Japanese Patent Application Laid-Open No. 5-107761, Japanese Patent Application Laid-Open No. 5-210240, and Japanese Patent Application Laid-Open No. 4-288818.

[0458] Among these sensitizing dyes, a sensitizing dye containing an amino group is preferred, and a compound having an amino group and a phenyl group in the same molecule is more preferred. Further preferred are benzophenone compounds such as 4,4'-dimethylaminobenzophenone, 4,4'-diethylaminobenzophenone, 2-aminobenzophenone, 4-aminobenzophenone, 4,4'-diaminobenzophenone, 3,3'-diaminobenzophenone, 3,4-diaminobenzophenone; 2-(p-dimethylaminophenyl)benzoxazole, 2-(p-diethylaminophenyl)benzoxazole, 2-(p-dimethylaminophenyl)benzo[4,5]benzoxazole, 2-(p-dimethylaminophenyl)benzo[6,7]benzoxazole, 2,5-bis(p-diethylaminophenyl)1,3,4-oxadiazole; Preferably, the compound contains p-dialkylaminophenyl group, such as oxazole, 2-(p-dimethylaminophenyl)benzothiazole, 2-(p-diethylaminophenyl)benzothiazole, 2-(p-dimethylaminophenyl)benzimidazole, 2-(p-diethylaminophenyl)benzimidazole, 2,5-bis(p-diethylaminophenyl)1,3,4-thiadiazole, (p-dimethylaminophenyl)pyridine, (p-diethylaminophenyl)pyridine, (p-dimethylaminophenyl)quinoline, (p-diethylaminophenyl)quinoline, (p-dimethylaminophenyl)pyrimidine, (p-diethylaminophenyl)pyrimidine, and the like, and 4,4'-dialkylaminobenzophenone is particularly preferred.

[0459] The sensitizing dye may be used alone or in combination of two or more.

[0460] The content of the sensitizing dye is not particularly limited, but is preferably 0 to 20% by mass, more preferably 0 to 15% by mass, and even more preferably 0 to 10% by mass, relative to the total solid content of the photosensitive resin composition.

[0461] <Organic Solvents>

[0462] The photosensitive resin composition of the present invention may contain an organic solvent not derived from the pigment dispersion of the present invention in order to adjust the solid content ratio and coatability. Examples of the organic solvent not derived from the pigment dispersion of the present invention include the same organic solvents as those in the pigment dispersion.

[0463] In the photosensitive resin composition of the present invention, the content of other organic solvents can be appropriately selected in consideration of the content of the total solid content in the photosensitive resin composition.

[0464] From the viewpoint of light-shielding properties, the content ratio of all solid components in the photosensitive resin composition is preferably 5% by mass or more, more preferably 8% by mass or more, and further preferably 10% by mass or more, relative to the total mass of the photosensitive resin composition. From the viewpoint of development solubility and patterning characteristics, it is preferably 40% by mass or less, more preferably 30% by mass or less, and further preferably 25% by mass or less.

[0465] The above upper and lower limits may be arbitrarily combined, and may be, for example, 5 to 40% by mass, 8 to 30% by mass, or 10 to 25% by mass.

[0466] <Other Compounding Components in the Photosensitive Resin Composition>

[0467] The photosensitive resin composition of the present invention may contain, in addition to the above components, other coloring materials other than the (A) pigment, thiols, adhesion improvers, coating improvers, development improvers, ultraviolet absorbers, antioxidants, and the like as appropriate.

[0468] (Other coloring materials)

[0469] (A) As a coloring material other than a pigment, a dye is mentioned, for example.

[0470] Examples of the dye include azo dyes, anthraquinone dyes, phthalocyanine dyes, quinoneimine dyes, quinoline dyes, nitro dyes, carbonyl dyes, and methylene dyes.

[0471] Examples of the azo dye include CI Acid Yellow 11, CI Acid Orange 7, CI Acid Red 37, CI Acid Red 180, CI Acid Blue 29, CI Direct Red 28, CI Direct Red 83, CI Direct Yellow 12, CI Direct Orange 26, CI Direct Green 28, CI Direct Green 59, CI Reactive Yellow 2, CI Reactive Red 17, CI Reactive Red 120, CI Reactive Black 5, CI Disperse Orange 5, CI Disperse Red 58, CI Disperse Blue 165, CI Basic Blue 41, CI Basic Red 18, CI Mordant Red 7, CI Mordant Yellow 5, and CI Mordant Black 7.

[0472] Examples of the anthraquinone dye include CI Vat Blue 4, CI Acid Blue 40, CI Acid Green 25, CI Reactive Blue 19, CI Reactive Blue 49, CI Disperse Red 60, CI Disperse Blue 56, and CI Disperse Blue 60.

[0473] Examples of phthalocyanine dyes include CI Vat Blue 5. Examples of quinoneimine dyes include CI Basic Blue 3 and CI Basic Blue 9. Examples of quinoline dyes include CI Solvent Yellow 33, CI Acid Yellow 3, and CI Disperse Yellow 64. Examples of nitro dyes include CI Acid Yellow 1, CI Acid Orange 3, and CI Disperse Yellow 42.

[0474] When the photosensitive resin composition of the present invention contains other coloring materials, the content ratio of the other coloring materials is preferably 0 to 10% by mass, more preferably 0 to 5% by mass, based on the total solid content of the photosensitive resin composition of the present invention.

[0475] (Thiols)

[0476] The photosensitive resin composition of the present invention may contain thiols for the purpose of increasing sensitivity and improving adhesion to a substrate.

[0477] Examples of the thiols include hexanedithiol, decanedithiol, 1,4-dimethylmercaptobenzene, butanediol bisthiopropionate, butanediol bisthioglycolate, ethylene glycol bisthioglycolate, trimethylolpropane trimerthioglycolate, butanediol bisthiopropionate, trimethylolpropane trithiopropionate, trimethylolpropane trimerthioglycolate, pentaerythritol tetrathiopropionate, pentaerythritol tetrathioglycolate, trihydroxyethyl trithiopropionate, ethylene glycol bis(3-mercaptobutyrate), propylene glycol bis(3-mercaptobutyrate) (PGMB), butanediol bis(3-mercaptobutyrate), 1,4-bis(3-mercaptobutyryloxy)butane (trade name: Karenz MTBD1, manufactured by Showa Denko K.K.), butanediol trimethylolpropane tris(3-mercaptobutyrate), pentaerythritol tetrakis(3-mercaptobutyrate) (trade name: Karenz MTPE1, manufactured by Showa Denko K.K.), pentaerythritol tris(3-mercaptobutyrate), ethylene glycol bis(3-mercaptoisobutyrate), butanediol bis(3-mercaptoisobutyrate), trimethylolpropane tris(3-mercaptoisobutyrate), trimethylolpropane tris(3-mercaptoisobutyrate) (TPMB), trimethylolpropane tris(2-mercaptoisobutyrate) (TPMIB), 1,3,5-tris(3-mercaptobutyloxyethyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione (trade name: Karenz MTNR1, manufactured by Showa Denko K.K.). These may be used alone or in combination of two or more.

[0478] As the thiols, polyfunctional thiol compounds such as PGMB, TPMB, TPMIB, Karenz MT BD1, Karenz MT PE1 and Karenz MTNR1 are preferred, among which Karenz MT BD1, Karenz MT PE1 and Karenz MTNR1 are more preferred, and Karenz MT PE1 is particularly preferred.

[0479] The thiols may be used alone or in combination of two or more.

[0480] When the photosensitive resin composition of the present invention contains thiols, the content of thiols is preferably 0.1% by mass or more, more preferably 0.3% by mass or more, and further preferably 0.5% by mass or more, relative to the total solid content of the photosensitive resin composition, and is preferably 10% by mass or less, and more preferably 5% by mass or less. If the content of thiols is more than the lower limit, there is a tendency to suppress the decrease in sensitivity, and if it is less than the upper limit, there is a tendency to easily improve the storage stability.

[0481] The above upper and lower limits may be arbitrarily combined, and may be, for example, 0.1 to 10% by mass, 0.3 to 10% by mass, or 0.5 to 5% by mass.

[0482] <Adhesion Improver>

[0483] The photosensitive resin composition of the present invention may contain an adhesion enhancer in order to improve adhesion with a substrate.

[0484] Examples of the adhesion-improving agent include a silane coupling agent and a titanium coupling agent, and a silane coupling agent is particularly preferred.

[0485] Examples of the silane coupling agent include KBM-402, KBM-403, KBM-502, KBM-5103, KBE-9007, X-12-1048, and X-12-1050 (manufactured by Shin-Etsu Silicones Co., Ltd.), and Z-6040, Z-6043, and Z-6062 (manufactured by Dow Corning Toray Co., Ltd.).

[0486] The silane coupling agents may be used alone or in combination of two or more.

[0487] The photosensitive resin composition of the present invention may contain an adhesion improver other than the silane coupling agent and the titanium coupling agent. Examples of the adhesion improver other than the silane coupling agent and the titanium coupling agent include a phosphoric acid-based adhesion improver and other adhesion improvers.

[0488] As the phosphoric acid-based adhesion improver, a (meth)acryloyloxy group-containing phosphoric acid ester is preferred, and phosphoric acid-based adhesion improvers represented by the following general formulas (g1), (g2), and (g3) are more preferred.

[0489]

[0490] In formula (g1), (g2), and (g3), R 51 Each independently represents a hydrogen atom or a methyl group, l and l' each independently represent an integer of 1 to 10, and m each independently represents 1, 2 or 3.

[0491] As another adhesion improver, TEGO*Add Bond LTH (produced by Evonik) can be mentioned, for example.

[0492] The adhesion improver may be used alone or in combination of two or more.

[0493] When the photosensitive resin composition of the present invention contains a close contact enhancer, the content ratio of the close contact enhancer in the photosensitive resin composition is not particularly limited, and is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, and further preferably 0.5% by mass or more, relative to the total solid content of the photosensitive resin composition, and preferably 5% by mass or less, more preferably 3% by mass or less, further preferably 2% by mass or less, and particularly preferably 1.5% by mass or less. If the content ratio of the close contact enhancer is above the lower limit, there is a tendency for the close contact strength to be improved, and if it is below the upper limit, there is a tendency for the developability to be improved.

[0494] The above upper and lower limits may be arbitrarily combined, for example, 0.01 to 5% by mass, 0.01 to 3% by mass, 0.1 to 2% by mass, or 0.5 to 1.5% by mass.

[0495] (Applicability Enhancer)

[0496] The photosensitive resin composition of the present invention may contain a coating property enhancer in order to improve coating properties.

[0497] As the coating property improving agent, for example, surfactants can be cited. As surfactants, for example, anionic, cationic, nonionic and amphoteric surfactants can be used. Among them, nonionic surfactants are preferred, and fluorine-based surfactants and silicone-based surfactants are more preferred, from the perspective of low possibility of adverse effects on various properties.

[0498] Examples of surfactants that can be used as coating improvers include TSF4460 (manufactured by Momentive Performance Materials), DFX-18 (manufactured by Neos), BYK-300, BYK-325, BYK-330 (manufactured by BYK-Chemie), KP340 (manufactured by Shin-Etsu Silicones), F-470, F-475, F-478, F-554, F-559 (manufactured by DIC Corporation), SH7PA (manufactured by Dow Corning Toray Co., Ltd.), DS-401 (manufactured by Daikin Corporation), L-77 (manufactured by Unicar Japan Co., Ltd.), and FC4430 (manufactured by 3M Japan Co., Ltd.).

[0499] The coating property-improving agent may be used alone or in combination of two or more.

[0500] When the photosensitive resin composition of the present invention contains a coating improver, the content ratio of the coating improver in the photosensitive resin composition is not particularly limited, and is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, relative to the total solid content of the photosensitive resin composition, and preferably 1.0% by mass or less, more preferably 0.7% by mass or less, further preferably 0.5% by mass or less, and particularly preferably 0.3% by mass or less. If the content ratio of the coating improver is above the lower limit, there is a tendency for coating uniformity to be improved, and if it is below the upper limit, there is a tendency that the sensitivity of the resist does not decrease.

[0501] The above upper and lower limits may be arbitrarily combined, and may be, for example, 0.01 to 1.0% by mass, 0.01 to 0.7% by mass, 0.05 to 0.5% by mass, or 0.05 to 0.3% by mass.

[0502] <Physical Properties of Photosensitive Resin Composition>

[0503] The photosensitive resin composition of the present invention can be suitably used for black matrix formation, and from this viewpoint, it is preferably black. In addition, the optical density (OD) of each 1 μm film thickness of the coating is preferably 1.0 or more, more preferably 2.0 or more, further preferably 2.5 or more, further preferably 3.0 or more, particularly preferably 4.0 or more, and most preferably 4.5 or more. If OD is above the aforementioned lower limit, there is a tendency to ensure sufficient light-shielding properties. The upper limit of OD is not particularly limited, for example, 6.0. OD can be, for example, 1.0 to 6.0, 2.0 to 6.0, 2.5 to 6.0, 3.0 to 6.0, 4.0 to 6.0, or 4.5 to 6.0.

[0504] <Method for producing photosensitive resin composition>

[0505] The photosensitive resin composition of the present invention can be produced by, for example, mixing the pigment dispersion of the present invention, (D) an alkali-soluble resin, (E) a photopolymerizable compound, (F) a photopolymerization initiator, and, if necessary, an organic solvent and other blending components.

[0506] The temperature during mixing is, for example, 20 to 30°C.

[0507] After mixing, the obtained photosensitive resin composition may be filtered using a filter or the like as necessary.

[0508] The photosensitive resin composition of the present invention can be used as a resist for members constituting a color filter such as pixels and a black matrix. When the photosensitive resin composition of the present invention is for a black matrix, it contains a black coloring material such as a black pigment.

[0509] The photosensitive resin composition of the present invention can also be used as a resist for coloring spacers.

[0510] The photosensitive resin composition of the present invention can also be used to form partition walls, especially partition walls for partitioning the organic layer of an organic electroluminescent element. As the organic layer of the organic electroluminescent element, for example, an organic layer used in a hole injection layer, a hole transport layer, or a hole transport layer on a hole injection layer described in Japanese Patent Application Laid-Open No. 2016-165396 can be cited.

[0511] [cured material]

[0512] The cured product of the present invention is obtained by curing the photosensitive resin composition of the present invention.

[0513] The cured product of the present invention can be suitably used as a member constituting a color filter such as a pixel or a black matrix.

[0514] The cured product of the present invention can also be used as a coloring spacer.

[0515] The photosensitive resin composition of the present invention can also be used as a partition wall, particularly a partition wall for partitioning an organic layer of an organic electroluminescent element.

[0516] [Black Matrix]

[0517] The black matrix including the cured product of the present invention will be described in accordance with the production method thereof.

[0518] The black matrix including the cured product of the present invention can be formed, for example, by applying the photosensitive resin composition of the present invention on a support on which the black matrix is ​​to be provided and drying it, placing a photomask on the dried coating film, exposing it through the photomask (image exposure) and developing it, and performing a curing treatment as needed.

[0519] (1) Support

[0520] As a support for forming a black matrix, as long as there is appropriate strength, its material is not particularly limited, and a transparent substrate is mainly used. As the material of the transparent substrate, for example, polyester resins such as polyethylene terephthalate, polyolefin resins such as polypropylene and polyethylene, polycarbonate, polymethyl methacrylate, polysulfone and other thermoplastic resin films, epoxy resins, unsaturated polyester resins, poly (methyl) acrylic resins and other thermosetting resin sheets, various glasses can be listed. Among them, from the viewpoint of heat resistance, glass and heat-resistant resins are preferred. In addition, transparent electrodes such as ITO and IZO can also be formed on the surface of the transparent substrate. It can also be formed on a support other than the transparent substrate, such as a TFT array.

[0521] To improve surface properties such as adhesiveness, the support may be subjected to corona discharge treatment, ozone treatment, atmospheric pressure plasma treatment, or thin film formation treatment using a silane coupling agent, urethane resin, or other resin, as necessary.

[0522] The thickness of the transparent substrate is preferably 0.05 to 10 mm, more preferably 0.1 to 7 mm. When thin film formation of various resins is performed, the film thickness is preferably 0.01 to 10 μm, more preferably 0.05 to 5 μm.

[0523] (2) Formation of black matrix

[0524] (2-1) Application of photosensitive resin composition

[0525] The photosensitive resin composition for black matrix can be applied to the support by, for example, spin coating, wire bar coating, flow coating, die coating, roll coating, or spray coating. Die coating is preferred from the comprehensive viewpoints of greatly reducing the amount of coating liquid, completely eliminating the influence of mist attached in the case of spin coating, and suppressing the generation of foreign matter.

[0526] The thickness of the coating film is preferably 0.2 to 10 μm, more preferably 0.5 to 6 μm, and further preferably 1 to 4 μm in terms of the film thickness after drying. By setting it below the upper limit, there is a tendency that pattern development becomes easier and gap adjustment in the liquid crystal cell formation process becomes easier. By setting it above the lower limit, there is a tendency that the desired color expression becomes easier.

[0527] (2-2) Drying of coating film

[0528] The drying of the coating film after applying the photosensitive resin composition on the support is preferably based on a drying method using a hot plate, an IR oven or a convection oven. The drying conditions can be appropriately selected according to the type of liquid medium (organic solvent, water) contained in the photosensitive resin composition, the performance of the dryer used, etc. For example, it is selected at a temperature of 40 to 200° C. and within a range of 15 seconds to 5 minutes, preferably at a temperature of 50 to 130° C. and within a range of 30 seconds to 3 minutes.

[0529] The higher the drying temperature, the better the adhesion of the coating to the transparent substrate. However, if the drying temperature is too high, the alkali-soluble resin may decompose and initiate thermal polymerization, resulting in poor development. It should be noted that the drying process of the coating may also be a reduced pressure drying method in which the drying is performed in a reduced pressure chamber without increasing the temperature.

[0530] (2-3) Exposure

[0531] Image exposure is performed by overlapping a photomask on the coating of the photosensitive resin composition and irradiating light of a wavelength from the ultraviolet region to the visible region through the photomask. As a photomask, a negative mask pattern is typically used. At this time, as required, in order to prevent the sensitivity of the coating caused by oxygen from being reduced, an oxygen barrier layer such as a polyvinyl alcohol layer can be formed on the coating before exposure. The light source used in image exposure is not particularly limited. As a light source, for example, a xenon lamp, a halogen lamp, a tungsten lamp, a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a metal halide lamp, a medium-pressure mercury lamp, a low-pressure mercury lamp, a carbon arc, and the like can be cited. When used by irradiating light of a specific wavelength, a filter can also be used.

[0532] (2-4) Development

[0533] The development is carried out using an organic solvent or an aqueous solution containing an alkaline compound and a surfactant. The aqueous solution may further contain an organic solvent, a buffer, a complexing agent, a dye or a pigment.

[0534] Examples of the alkaline compound include inorganic alkaline compounds such as sodium hydroxide, potassium hydroxide, lithium hydroxide, sodium carbonate, potassium carbonate, sodium bicarbonate, potassium bicarbonate, sodium silicate, potassium silicate, sodium metasilicate, sodium phosphate, potassium phosphate, sodium hydrogen phosphate, potassium hydrogen phosphate, sodium dihydrogen phosphate, potassium dihydrogen phosphate, and ammonium hydroxide; and organic alkaline compounds such as monoethanolamine, diethanolamine, or triethanolamine, monomethylamine, dimethylamine, or trimethylamine, monoethylamine, diethylamine, or triethylamine, monoisopropylamine, or diisopropylamine, n-butylamine, monoisopropanolamine, diisopropanolamine, or triisopropanolamine, ethyleneimine, ethylenediamine, tetramethylammonium hydroxide (TMAH), and choline.

[0535] The basic compound may be used alone or as a mixture of two or more.

[0536] Examples of the surfactant include nonionic surfactants such as polyoxyethylene alkyl ethers, polyoxyethylene alkyl aryl ethers, polyoxyethylene alkyl esters, sorbitan alkyl esters, and monoglyceride alkyl esters; anionic surfactants such as alkylbenzene sulfonates, alkylnaphthalene sulfonates, alkyl sulfates, alkyl sulfonates, and sulfosuccinate salts; and amphoteric surfactants such as alkyl betaines and amino acids.

[0537] Examples of the organic solvent include isopropyl alcohol, benzyl alcohol, ethyl cellosolve, butyl cellosolve, phenyl cellosolve, propylene glycol, and diacetone alcohol.

[0538] The organic solvent may be used alone or in combination with an aqueous solution.

[0539] The conditions for the development treatment are not particularly limited. The development temperature is preferably 10 to 50° C., more preferably 15 to 45° C., and further preferably 20 to 40° C. The development method may be any method such as immersion development, spray development, brush development, and ultrasonic development.

[0540] (2-5) Curing treatment

[0541] Examples of the curing treatment include thermal curing treatment and photocuring treatment, and thermal curing treatment is preferred.

[0542] Regarding the heat curing treatment conditions, the temperature is selected within the range of 100 to 280° C., preferably within the range of 150 to 250° C., and the time is selected within the range of 5 to 60 minutes.

[0543] The height of the black matrix formed as described above is preferably 0.5 to 5 μm, more preferably 0.8 to 4 μm, and the optical density (OD) per 1 μm thickness is preferably 2.0 or more, more preferably 2.5 or more, further preferably 3.0 or more, and particularly preferably 3.2 or more.

[0544] [Color Filter]

[0545] On a transparent substrate provided with a black matrix, a photosensitive resin composition containing a coloring material of one color among red (R), green (G), and blue (B) is applied and dried by the same process as above (2-1) to (2-5), and a photomask is overlapped on the coating film. Through the photomask, a pixel image is formed by image exposure, development, and thermal curing or photocuring as required to prepare a coloring layer. The photosensitive resin compositions of the three colors of R, G, and B are respectively subjected to this operation, thereby forming a color filter. Their order is not limited to the above.

[0546] (2-6) Formation of transparent electrode

[0547] The color filter can be used as a part of a color display, a liquid crystal display device, or the like by forming a transparent electrode such as ITO on an image as it is.

[0548] To improve surface smoothness and durability, a top coat layer of polyamide, polyimide or the like may be provided on the image as needed. In some applications, such as applications in a planar alignment type drive system (IPS mode), a transparent electrode may not be formed.

[0549] [Coloring spacer]

[0550] When spacers are used in TFT-type LCDs, TFTs as switching elements may malfunction due to light incident on the TFTs, and colored spacers are used to prevent this. For example, Japanese Patent Application Laid-Open No. 8-234212 describes making spacers light-shielding.

[0551] The coloring spacers formed of the cured product of the present invention can be formed by the same method as the above-mentioned black matrix except that a mask for the coloring spacers is used.

[0552] [Partition wall]

[0553] The partition wall formed of the cured product of the present invention will be described below based on its production method.

[0554] The partition wall composed of the cured product of the present invention can be formed, for example, by applying the photosensitive resin composition of the present invention on a support body on which the partition wall is to be provided and drying it, placing a photomask on the dried coating film, exposing it through the photomask (image exposure) and developing it, and performing a curing treatment as needed.

[0555] (3-1) Support

[0556] As the support for forming the partition wall, the same support as the support for forming the black matrix described above can be used.

[0557] (3-2) Formation of partition wall

[0558] The specific methods of coating the photosensitive resin composition on the support, drying, exposure, development, and curing in the method for forming the partition walls can be the same as those for forming the black matrix.

[0559] The size and shape of the partition wall are appropriately adjusted according to the specifications of the organic electroluminescent element to which the partition wall is applied, and the height of the partition wall formed from the photosensitive resin composition is preferably about 0.5 to 10 μm.

[0560] [Organic electroluminescent element]

[0561] Various organic electroluminescent elements are produced using a support having partition walls produced by the above method.

[0562] For example, the method for forming the organic electroluminescent element is not particularly limited, but it is preferred to form an organic layer such as pixels after forming partition walls on a support by the above-mentioned method, thereby manufacturing the organic electroluminescent element.

[0563] Examples of the method for forming the organic layer include a wet process such as a vapor deposition method, a casting method, a spin coating method, and an inkjet printing method, in which a functional material is sublimated in a vacuum state and adhered to the region surrounded by the partition wall on the substrate to form a film.

[0564] Examples of the types of organic electroluminescent elements include bottom emission type and top emission type.

[0565] In the bottom emission type, a partition wall is formed on a glass substrate laminated with a transparent electrode, and a hole transport layer, a light-emitting layer, an electron transport layer, and a metal electrode layer are laminated in the opening surrounded by the partition wall. On the other hand, in the top emission type, a partition wall is formed on a glass substrate laminated with a metal electrode layer, and an electron transport layer, a light-emitting layer, a hole transport layer, and a transparent electrode layer are laminated in the opening surrounded by the partition wall.

[0566] Examples of the light-emitting layer include organic electroluminescent layers described in Japanese Patent Application Publication No. 2009-146691 and Japanese Patent No. 5734681. In addition, quantum dots described in Japanese Patent No. 5653387 and Japanese Patent No. 5653101 may also be used.

[0567] The layer structure is not limited thereto, for example, from the viewpoint of luminous efficiency, each of the hole transport layer and the electron transport layer may be a stacked structure including two or more layers. The thickness of each layer is not particularly limited, but is preferably 1 to 500 nm from the viewpoint of luminous efficiency and brightness.

[0568] The organic electroluminescent element can be formed into RGB colors separately in each opening, or two or more colors can be stacked in one opening. From the viewpoint of improving reliability, the organic electroluminescent element can have a sealing layer. The sealing layer has the function of preventing moisture in the air from being adsorbed on the organic electroluminescent element and reducing the luminous efficiency. From the viewpoint of improving light extraction efficiency, the organic electroluminescent element can have a low-reflection film at the interface with the air. By configuring the low-reflection film at the interface between the air and the element, the difference in refractive index can be reduced and the reflection at the interface can be suppressed. Such a low-reflection film can, for example, apply the technology of moth-eye structure and super multilayer film.

[0569] When an organic electroluminescent element is used as a pixel of an image display device, in order to prevent light from a light-emitting layer of a certain pixel from leaking to other pixels and further to prevent degradation of image quality due to reflection of external light when the electrodes are made of metal, it is preferred to give light-shielding properties to the partition walls constituting the organic electroluminescent element.

[0570] In an organic electroluminescent element, since electrodes are provided on the upper and lower surfaces of the partition wall, the partition wall is preferably high-resistance and low-dielectric constant from the viewpoint of insulation. Therefore, when a colorant is used to provide light-shielding properties to the partition wall, it is preferred to use the aforementioned organic pigment having high resistance and low dielectric constant.

[0571] [Image display device]

[0572] The image display device of the present invention includes the cured product of the present invention.

[0573] Examples of the image display device of the present invention include an image display device including the above-described black matrix and a partition wall.

[0574] The image display device is not particularly limited as long as it is a device that displays images or videos, and examples thereof include a liquid crystal display device and an organic EL display described below.

[0575] [Liquid crystal display device]

[0576] The liquid crystal display device in the present invention can be produced, for example, using a color filter having the above-mentioned black matrix. It should be noted that the formation order and formation position of the color pixels and the black matrix are not particularly limited.

[0577] Liquid crystal display devices are usually completed as follows: an alignment film is formed on a color filter, spacers are spread on the alignment film, and then a liquid crystal cell is formed by bonding with an opposing substrate, and liquid crystal is injected into the formed liquid crystal cell, and the alignment film is completed by wiring with an opposing electrode. As an alignment film, a resin film such as polyimide is suitable. Gravure printing and / or flexographic printing are usually used in the formation of the alignment film, and the thickness of the alignment film is set to several 10nm. After the alignment film is cured by thermal sintering, the surface is treated by irradiation of ultraviolet rays and treatment based on a brushing cloth to be processed into a surface state that can adjust the tilt of the liquid crystal.

[0578] As a spacer, an object of a size corresponding to the gap between the opposing substrate and the substrate is used, and a spacer of 2 to 8 μm is suitable. A photolithography spacer (PS) of a transparent resin film can also be formed on the color filter substrate by photolithography and used as a substitute for the spacer. As an opposing substrate, an array substrate is usually used, and a TFT (thin film transistor) substrate is particularly suitable.

[0579] The gap between the substrate and the opposing substrate varies depending on the purpose of the liquid crystal display device, and is preferably in the range of 2 to 8 μm. After bonding to the opposing substrate, the portion other than the liquid crystal injection port is sealed with a sealing material such as epoxy resin. The sealing material is cured by UV irradiation and / or heating to seal the periphery of the liquid crystal unit.

[0580] After the sealed liquid crystal cell is cut into unit panels, the vacuum chamber is set to a reduced pressure, the liquid crystal injection port is immersed in liquid crystal, and the cavity is leaked to inject liquid crystal into the liquid crystal cell. The reduced pressure in the liquid crystal cell is preferably 1×10 -7 ~1×10 -2 Pa, more preferably 1×10 -6 ~1×10 -3 Pa. In addition, the liquid crystal cell is preferably heated during decompression, and the heating temperature is preferably 30 to 100° C., more preferably 50 to 90° C. The heating during decompression is preferably maintained for 10 to 60 minutes. Then, it is immersed in liquid crystal. The liquid crystal cell injected with liquid crystal is sealed by curing the UV curable resin to complete the liquid crystal display device (panel).

[0581] The type of liquid crystal is not particularly limited, and may be any known liquid crystal such as aromatic, aliphatic, or polycyclic compounds, lyotropic liquid crystal, thermotropic liquid crystal, etc. Among thermotropic liquid crystals, nematic liquid crystal, smectic liquid crystal, and cholesteric liquid crystal are known, and any of them may be used.

[0582] [Organic EL display]

[0583] The organic EL display of the present invention can be produced, for example, using a color filter having the above-mentioned black matrix and an organic electroluminescent element having the above-mentioned partition wall.

[0584] When an organic EL display is produced using the color filter of the present invention, for example Figure 1As shown, first, a color filter is formed on a transparent supporting substrate 10 with a pattern formed by a photosensitive resin composition (i.e., a pixel 20 and a black matrix (not shown) disposed between adjacent pixels 20), and an organic light-emitting body 500 is stacked on the color filter via an organic protective layer 30 and an inorganic oxide film 40, thereby an organic EL element 100 can be manufactured. It should be noted that at least one of the pixel 20 and the black matrix is ​​made using the photosensitive resin composition of the present invention. As a stacking method of the organic light-emitting body 500, there can be listed: a method of successively forming a transparent anode 50, a hole injection layer 51, a hole transport layer 52, a light-emitting layer 53, an electron injection layer 54 and a cathode 55 on the upper surface of the color filter; a method of bonding an organic light-emitting body 500 formed on another substrate to an inorganic oxide film 40, etc. Using the organic EL element 100 thus produced, an organic EL display can be produced by, for example, the method described in “Organic EL Display” (Ohmsha, Ltd., published on August 20, 2004, written by Shizuo Tokito, Chihaya Adachi, and Hideyuki Murata).

[0585] It should be noted that the color filter of the present invention can be applied to both passively driven organic EL displays and actively driven organic EL displays.

[0586] Example

[0587] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples unless the gist of the invention is exceeded.

[0588] The constituent components of the pigment dispersion and the photosensitive resin composition used in the following Examples and Comparative Examples are as follows.

[0589] <Pigment-1>

[0590] "RAVEN1060" (carbon black) manufactured by Birla Carbon.

[0591] <Dispersant-1>

[0592] “DISPERBYK-167” manufactured by BYK-Chemie (urethane-based polymer dispersant).

[0593] <Dispersing Aid-1>

[0594] "S12000-S" manufactured by Lubrizol Corporation (copper phthalocyanine sulfonate derivative).

[0595] <Organic Solvents>

[0596] Propylene glycol monomethyl ether acetate (PGMEA).

[0597] <Alkali soluble resin-1>

[0598] The resin obtained in the synthesis example described later was used.

[0599] <Photopolymerizable compound-1>

[0600] “KAYARAD DPHA” (multifunctional acrylate) manufactured by Nippon Kayaku Co., Ltd.

[0601] <Photopolymerization Initiator-1>

[0602] “TR-PBG-304” (oxime ester compound having a carbazole skeleton) manufactured by Changzhou Qiangli Electronic New Materials Co., Ltd.

[0603] <Surfactant-1>

[0604] “MEGAFAC F554” manufactured by DIC Corporation (fluorine-based surfactant).

[0605] <Additive-1>

[0606] “X-12-1048” (polyfunctional acrylic silane) manufactured by Shin-Etsu Chemical Co., Ltd.

[0607] <Synthesis Example: Synthesis of Alkali-Soluble Resin>

[0608]

[0609] 240 parts by mass of the epoxy compound (epoxy equivalent 264) of the above structure, 81.6 parts by mass of methacrylic acid, 263.1 parts by mass of methoxybutyl acetate, 6.4 parts by mass of triphenylphosphine and 0.16 parts by mass of p-methoxyphenol were placed in a flask equipped with a thermometer, a stirrer and a condenser, and reacted at 90° C. for 12 hours while stirring until the acid value was 5 mgKOH / g or less.

[0610] Next, in a flask equipped with a thermometer, a stirrer and a condenser, 8.3 parts by mass of trimethylolpropane (TMP), 80.7 parts by mass of biphenyltetracarboxylic dianhydride (BPDA) and 51.6 parts by mass of tetrahydrophthalic anhydride (THPA) were added to the reaction solution obtained by the above reaction, and the temperature was slowly raised to 105°C while stirring to carry out a reaction, thereby obtaining an alkali-soluble resin having a solid acid value of 112 mgKOH / g and a weight average molecular weight (Mw) of 2500 in terms of polystyrene measured by GPC.

[0611] <Preparation of Pigment Dispersion>

[0612] Pigment-1, dispersant-1, dispersing aid-1, PGMEA and water described in Table 1 were mixed to obtain a mixed solution at the mass ratio and water content described in Table 1. The blending ratio of the solvent in Table 1 also includes the amount of the solvent derived from the dispersant and the solvent derived from the dispersing aid.

[0613] Beads were added to the mixed solution, and a dispersion treatment was performed at 25 to 45° C. for 6 hours using a paint shaker. Zirconia beads of 0.5 mm φ were used as beads, and 2.5 times the mass of the dispersion was added. After the dispersion was completed, the beads and the dispersion were separated using a filter to obtain dispersions 1 to 8.

[0614] <Evaluation of Pigment Dispersion>

[0615] The obtained dispersions 1 to 8 were evaluated as follows.

[0616] [Viscosity]

[0617] The viscosity of each of the dispersions 1 to 8 at 23° C. was measured using an E-type viscometer (RE-80L manufactured by Toki Sangyo Co., Ltd.).

[0618] [Filterability]

[0619] 5 mL of each dispersion 1 to 8 was filtered at room temperature using a Teflon tube equipped with a filter (Millipore 1.2 μm, manufactured by Merck) under a pressure of 0.004 MPa to 0.006 MPa, and the time (seconds) from the start of filtration to completion was measured. This value was taken as filterability. The results are shown in Table 1.

[0620] Dispersion liquid 7 had a high viscosity and could not be measured for filterability, so subsequent evaluation was not performed.

[0621] [Viscosity stability]

[0622] The obtained dispersions 1 to 8 were stored at 35° C. for 30 days, and then the viscosity of each dispersion at 23° C. was measured using an E-type viscometer (RE-80L manufactured by Toki Sangyo Co., Ltd.).

[0623] [Zeta potential measurement]

[0624] The dispersion 1 was diluted 1500 times with PGMEA and then injected into a cell for a low dielectric constant solvent using a laser zeta potentiometer ELSZ-2000ZS manufactured by Otsuka Electronics Co., Ltd., and the zeta potential was measured by applying a voltage of 300 V.

[0625] The absolute value of the zeta potential of the dispersion 1 was 37 mV.

[0626] [Table 1]

[0627]

[0628] <Preparation of Photosensitive Resin Composition>

[0629] In the dispersions 1 to 6 and 8 prepared above, the components shown in Table 2 were added so that the solid content ratio of each component in the total solid content of the photosensitive resin composition became the blending ratio of Table 2, and propylene glycol monomethyl ether acetate (PGMEA), 3-methoxybutyl acetate (MBA) and diethylene glycol monoethyl ether acetate (EDGAC) were further added so that the content ratio of the total solid content of the photosensitive resin composition became 14% by mass, and the mass ratio of PGMEA / MBA / EDGAC in the solvent became 68 / 30 / 2, and the dispersions were stirred to dissolve, thereby obtaining the photosensitive resin compositions of Examples 1 to 5 and Comparative Examples 1 to 2.

[0630] <Evaluation of Photosensitive Resin Composition>

[0631] The following evaluations were performed on each of the obtained photosensitive resin compositions.

[0632] [Peel test]

[0633] At an ambient temperature of 23°C and a humidity of 50%, a 20 mm front end portion in the longitudinal direction of a glass test piece having a length of 100 mm, a width of 5 mm, and a thickness of 0.7 mm was immersed in the photosensitive resin composition at a speed of 12.5 mm / second, maintained at that position for 4 seconds, and taken out of the photosensitive resin composition at a speed of 12.5 mm / second. The glass test piece was dried at an ambient temperature of 23°C, a humidity of 55%, and a wind speed of 0.5±0.2 seconds while being held vertically with the front end of the glass test piece facing downward. This process was repeated 250 times.

[0634] Then, the front end portion (the portion immersed in the photosensitive resin composition) of the glass test piece was observed using an optical microscope at both ends (ridgeline portions) in the width direction of the front and back surfaces at a total of 4 locations, and evaluation was performed according to the number of ridgeline portions where deposits were observed, based on the following criteria. The results are shown in Table 2.

[0635] A: No attachment was observed on the ridge line.

[0636] B: Adhesion was observed at one ridge line.

[0637] C: Adhesions were observed at two or more ridgeline locations.

[0638] In addition, the ridgeline of the glass test piece of each example is shown in Figure 2 .exist Figure 2In the figure, optical microscope images of two edge positions are arranged side by side for Examples 1 to 5 and Comparative Examples 1 to 2. The line extending in the vertical direction near the center of each of the two arranged optical microscope images is the edge position, and the part inside each edge position (center side in the figure) is the front end of the glass test piece.

[0639] [Dissolution time]

[0640] The photosensitive resin composition was applied on a glass substrate by a spin coater so that the film thickness after heat curing was 1.2 μm, and dried under reduced pressure at 100 Pa for 60 seconds, and then dried on a hot plate at 100° C. for 120 seconds. For the obtained coating film, a photomask having openings with a line width of 1 μm to 30 μm per 1 μm was used as a photomask, and an intensity of 60 mW / cm at a wavelength of 365 nm was used. 2 The exposure amount is 40mJ / cm 2 The exposure process is implemented in this way.

[0641] Then, using a developer formed of a 0.04 mass % KOH (potassium hydroxide) aqueous solution, spray development was performed at a water pressure of 0.05 MPa at 23° C., and then development was stopped with pure water and washed with a water washing spray. The time when the patterning can be visually observed during the spray development was measured as the dissolution time. The results are shown in Table 2.

[0642] [Minimum fit]

[0643] The glass substrate after the shower development in the evaluation of the dissolution time was observed with an optical microscope, and the line width (μm) of the photomask opening corresponding to the pattern with the smallest width among the patterns (line patterns) that remained on the glass substrate without a gap and with good linearity was taken as the minimum adhesion. It can be said that the smaller this value is, the better the substrate adhesion is. The results are shown in Table 2.

[0644] [Line Width]

[0645] The glass substrate after shower development in the evaluation of the dissolution time was observed with an optical microscope, and the width of the pattern corresponding to the opening of the photomask with a line width of 30 μm was measured.

[0646] [Table 2]

[0647]

[0648] The results in Table 1 show that when the water content of the pigment dispersion is less than 1.2% by mass, the viscosity and filterability of the pigment dispersion immediately after preparation are good. On the other hand, when the water content is 1.2% by mass or more, a sharp thickening is observed, indicating that the viscosity stability deteriorates. The reasons for this are believed to be: oil separation from the organic solvent occurs due to the increase in water content; and the solubility of the dispersant in the organic solvent decreases, making it impossible to uniformly adsorb the pigment.

[0649] In addition, when the water content of the pigment dispersion is less than 0.95% by mass, the viscosity stability after storage for 30 days is also good. The reasons for this are considered to be: as the water content increases, the oil separation from the organic solvent gradually advances during the storage period; and the solubility of the dispersant in the organic solvent decreases, making it impossible to uniformly adsorb the pigment.

[0650] The results in Table 2 show that when the water content of the pigment dispersion is 0.14% by mass or less, the result of the peel test deteriorates. In addition, it can be seen that when the water content exceeds 0.14% by mass, the result of the peel test is good, and there is no effect on solubility, minimum adhesion, and line width. As the reason for this, it can be considered that: if it is the optimal water content, the dispersion stability of the pigment over time becomes good, and no aggregates are generated. In addition, the moisture inhibits the rapid drying of the photosensitive resin composition, thereby inhibiting the aggregation of the pigment.

[0651] Description of Reference Numerals

[0652] 10 Transparent support substrate

[0653] 20 pixels

[0654] 30 Organic protective layer

[0655] 40 Inorganic oxide film

[0656] 50 Transparent Anode

[0657] 51 Hole injection layer

[0658] 52 Hole transport layer

[0659] 53 Luminous layer

[0660] 54 Electron injection layer

[0661] 55 cathode

[0662] 100 organic EL components

[0663] 500 organic light emitting bodies

Claims

1. A pigment dispersion comprising (A) a pigment, (B) a dispersant, an organic solvent and water, The pigment (A) contains carbon black, The pigment dispersion has a water content of 0.15% by mass or more and 0.9% by mass or less. 2 . The pigment dispersion according to claim 1 , wherein the water content is 0.2% by mass or more and 0.7% by mass or less.

3. The pigment dispersion according to claim 1, wherein The content ratio of the (A) pigment is 60% by mass or more based on the total solid content of the pigment dispersion.

4. The pigment dispersion according to claim 1, wherein The content ratio of the (A) pigment to the (B) dispersant based on mass ((A) pigment / (B) dispersant) is 4 or more. The pigment dispersion according to claim 1 , further comprising (C) a dispersing aid.

6. The pigment dispersion according to claim 5, wherein The content ratio of the (A) pigment to the (C) dispersing aid based on mass ((A) pigment / (C) dispersing aid) is 10 or more. 7 . A photosensitive resin composition comprising: the pigment dispersion according to claim 1 , (D) an alkali-soluble resin, (E) a photopolymerizable compound, and (F) a photopolymerization initiator.

8. The photosensitive resin composition according to claim 7, wherein The content of the pigment (A) is 30% by mass or more relative to the total solid content of the photosensitive resin composition. 9 . A cured product obtained by curing the photosensitive resin composition according to claim 7 . 10 . A black matrix comprising the cured product according to claim 9 .

11. An image display device comprising the cured product according to claim 9.