Variable transmittance optical laminate, method for manufacturing same, and smart window including same

By directly forming a conductive layer on the polarizing plate and increasing the hardness of the functional coating, the traditional transmission fixed and light leakage problems are solved, and the process simplification and durability of the variable transmission optical laminate is achieved, ensuring that the difference Reliability in use under light conditions.

CN119096186AInactive Publication Date: 2024-12-06DONGWOO FINE CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380029387.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-24
Filing Date
2023-03-09
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The transmission rate of traditional mobile tools and home windows is fixed, which may cause it to be difficult for drivers or users to correctly view the surrounding situation under different light conditions, and there are light leakage or cracks, affecting the durability and reliability of the optical stack.

Method used

Using a transparent conductive layer that does not contain a separate substrate, the conductive layer is directly formed on the polarizing plate, and when the liquid crystal layer and the frame sealing glue are the same, the hardness of the functional coating is increased to reduce cracks and light leakage, ensuring the frame sealing. The glue height is between 2 and 20 μm.

Benefits of technology

The process simplification, durability and transmission of the optical laminate with variable transmission are achieved, light leakage and cracking are reduced, constant optical color is maintained in the plane, and bending characteristics and durability are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119096186A_ABST
    Figure CN119096186A_ABST
Patent Text Reader

Abstract

The invention relates to a transmittance-variable optical laminated body, a manufacturing method thereof and a smart window comprising the same. The transmittance-variable optical laminated body comprises a liquid crystal layer comprising frame sealing glue; a first polarizing plate including a first functional coating layer and positioned on one surface of the liquid crystal layer; a second polarizing plate including a second functional coating layer and positioned on the other surface of the liquid crystal layer; a first transparent conductive layer formed between the first polarizing plate and the liquid crystal layer; and a second transparent conductive layer formed between the second polarizing plate and the liquid crystal layer, in which at least one of the first transparent conductive layer and the second transparent conductive layer is formed so as to be in direct contact with either the first polarizing plate or the second polarizing plate. The surface pencil hardness of the first functional coating layer and the second functional coating layer is 3B-8H, and the sum of the thickness of the first functional coating layer and the thickness of the second functional coating layer is 2-50 [mu] m.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a variable transmittance optical stack, a method for manufacturing the same, and a smart window comprising the same. Background Art

[0002] Generally speaking, glass windows of mobile tools such as vehicles are often coated with external light blocking coatings. However, the transmittance of glass windows of conventional mobile tools is fixed, and the transmittance of the external light blocking coating is also fixed. Therefore, since the overall transmittance of the windows of such conventional mobile tools is fixed, accidents may occur. For example, if the overall transmittance is set low, there is no problem during the day when the surrounding light is sufficient. However, in situations such as the night when the surrounding light is insufficient, there is a problem that it is difficult for the driver and the like to correctly view the surrounding conditions of the mobile tool. In addition, if the overall transmittance is set high, there is a problem that it may cause glare to the driver and the like during the day when the surrounding light is sufficient. In addition, in the case of household windows, there are also cases where an external light blocking coating is provided, but in this case, as in the case of the windows of the above-mentioned mobile tools, the transmittance is fixed, so it is not easy to adjust the amount of light entering the room. For this reason, a variable transmittance optical laminate that can change the transmittance of light when a voltage is applied has been developed.

[0003] The above-mentioned variable transmittance optical stack is driven in a variable transmittance manner by applying voltage to drive the liquid crystal. The variable transmittance optical stack developed so far is made by forming a conductive layer for liquid crystal driving on a separate substrate and then combining it with other elements such as a polarizing plate, and sometimes further includes an insulating layer.

[0004] Korean Patent Gazette No. 10-2226630 discloses that in a dimming film such as an electronic blind that can be used to control the transmission of external light, the Vickers hardness value Xs of the spacer is 16.9 to 40.2, and the Vickers hardness value Xf of the second laminate is 11.8 to 35.9. However, the component corresponding to the sealant is not suitable for supporting the liquid crystal layer, and as a result, the problem that the optical laminate may produce defects cannot be solved, such as light leakage, cracks or scratches in the optical laminate and the smart window containing it.

[0005] Therefore, the actual situation is that it is necessary to develop a variable transmittance optical laminate that can minimize poor liquid crystal transmittance by simplifying the production process due to the lack of a separate substrate for forming a conductive layer, maintaining a constant optical color within the plane by ensuring that the height of the frame sealant is the same as the height of the liquid crystal. Summary of the invention

[0006] Technical issues

[0007] An object of the present invention is to provide a variable transmittance optical layered body which does not include a separate substrate for forming a conductive layer and thus has a simplified production process.

[0008] Another object of the present invention is to provide a variable transmittance optical layered body, wherein the surface hardness of the functional coating layer included in the polarizing plate is 3B to 8H, and the sum of the thicknesses of the functional coating layers is 2 to 50 μm.

[0009] In addition, an object of the present invention is to provide a variable transmittance optical stacked body, which comprises a frame sealant having a height of 2 to 20 μm after curing.

[0010] Another object of the present invention is to provide a variable transmittance optical stacked body, in which the height of the liquid crystal layer is substantially the same as the height of the frame sealant.

[0011] Another object of the present invention is to provide a variable transmittance optical layered body including a functional coating layer capable of increasing surface hardness, thereby minimizing cracks generated during the process.

[0012] Another object of the present invention is to provide a smart window including the variable transmittance optical laminate and a car or building window to which the smart window is applied.

[0013] However, the problems to be solved by the present invention are not limited to the problems mentioned above, and a person skilled in the art should be able to clearly understand other problems not mentioned based on the following description.

[0014] Solution to the problem

[0015] The present invention relates to a variable transmittance optical stack, which comprises: a liquid crystal layer comprising a sealing glue; a first polarizing plate comprising a first functional coating and located on one side of the liquid crystal layer; a second polarizing plate comprising a second functional coating and located on the other side of the liquid crystal layer; a first transparent conductive layer formed between the first polarizing plate and the liquid crystal layer; and a second transparent conductive layer formed between the second polarizing plate and the liquid crystal layer, wherein at least one of the first transparent conductive layer and the second transparent conductive layer is formed to directly contact one of the first polarizing plate and the second polarizing plate, the surface pencil hardness of the first functional coating and the second functional coating is respectively 3B to 8H, and the sum of the thickness of the first functional coating and the second functional coating is 2 to 50 μm.

[0016] In a first aspect of the present invention, the height of the frame sealant after curing may be 2 to 20 μm.

[0017] In a second aspect of the present invention, the thickness of the first functional coating layer and the second functional coating layer may each be 1 to 35 μm.

[0018] In a third aspect of the present invention, the first functional coating layer and the second functional coating layer may include at least one of a hard coating layer and a low refractive index layer.

[0019] In a fourth aspect of the present invention, the hard coat layer may contain an acrylate compound or an epoxy compound.

[0020] In a fifth aspect of the present invention, the low refractive index layer may include one or more selected from the group consisting of SiO 2 , Al 2 O 3 , MgF 2 , CaF 2 , and cryolite.

[0021] In a sixth aspect of the present invention, at least one of the first transparent conductive layer and the second transparent conductive layer may be formed to be in direct contact with one of the first polarizing plate and the second polarizing plate without including a separate substrate therebetween.

[0022] In a seventh aspect of the present invention, at least one of the first transparent conductive layer and the second transparent conductive layer may be formed to be in direct contact with one of the first polarizing plate and the second polarizing plate by including an easy-adhesion layer therebetween.

[0023] In an eighth aspect of the present invention, at least one of the first transparent conductive layer and the second transparent conductive layer may include one or more selected from the group consisting of transparent conductive oxides, metals, carbon-based materials, conductive polymers, conductive inks, and nanowires.

[0024] In a ninth aspect of the present invention, at least one of the first polarizing plate and the second polarizing plate may include one or more selected from the group consisting of a protective layer, a phase difference adjusting layer, and a refractive index adjusting layer.

[0025] In a tenth aspect of the present invention, at least one of the first polarizing plate and the second polarizing plate may have a thickness of 30 to 200 μm.

[0026] In an eleventh aspect of the present invention, the liquid crystal layer may include one or more spacers selected from the group consisting of ball spacers and column spacers.

[0027] In a twelfth aspect of the present invention, the height of the spacer may be 2 to 20 μm.

[0028] In a thirteenth aspect of the present invention, the area occupied by the spacer in the liquid crystal layer may be 0.01% to 10% of the area of ​​the liquid crystal layer.

[0029] In a fourteenth aspect of the present invention, the variable transmittance optical layered body may further include one or more selected from the group consisting of an adhesive / bonding layer, an ultraviolet absorbing layer, and an impact-resistant layer.

[0030] Furthermore, the present invention relates to a method for producing the variable transmittance optical layered body.

[0031] Furthermore, the present invention relates to a smart window including the variable transmittance optical laminate.

[0032] In addition, the present invention relates to a vehicle comprising the above-mentioned smart window.

[0033] In addition, the present invention relates to a car in which the above-mentioned smart window is applied to more than one of a front window, a rear window, a side window, a sunroof and an interior partition.

[0034] In addition, the present invention relates to a wearable device comprising the above-mentioned smart window.

[0035] In addition, the present invention relates to a building window including the above-mentioned smart window.

[0036] Effects of the Invention

[0037] According to the variable transmittance optical stack of the present invention, the hardness of the polarizer hard coating, that is, the functional coating, meets the range of 3B to 8H, and the sum of the thicknesses of the first polarizer and the second polarizer is 2 to 50 μm, thereby ensuring a frame sealant height of 2 to 20 μm, so that the frame sealant height is the same as the liquid crystal thickness, thereby improving the extrusion phenomenon and diffusion of the frame sealant, and preventing light leakage between the liquid crystal layer and other substrates to maintain a constant optical color within the plane.

[0038] In addition, according to the variable transmittance optical layered body of the present invention, since cracks are not generated and the durability is excellent, it is possible to minimize defects in the optical layered body and the smart window.

[0039] Furthermore, according to the variable transmittance optical layered body of the present invention, the conventional steps of forming a conductive layer on a substrate and bonding it to other members for forming an optical layered body can be omitted, and thus the production process can be simplified compared with conventional optical layered bodies.

[0040] Furthermore, according to the variable transmittance optical layered body of the present invention, since the conductive layer is directly formed on one surface of the polarizing plate without including a separate substrate for forming the conductive layer, the thickness can be significantly reduced compared to conventional optical layered bodies.

[0041] Furthermore, according to the variable transmittance optical layered body of the present invention, since the conductive layer is directly formed on one surface of the polarizing plate without including a separate substrate for forming the conductive layer, the transmittance in the light transmission mode can be improved compared to conventional optical layered bodies.

[0042] Furthermore, since the variable transmittance optical layered body of the present invention includes a functional coating layer capable of increasing the surface hardness, cracks generated during the process can be minimized compared to conventional optical layered bodies. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 This is a diagram showing a stacked structure of a variable transmittance optical stack according to an embodiment of the present invention.

[0044] Figure 2 This is a diagram showing a stacked structure of a variable transmittance optical stack according to another embodiment of the present invention.

[0045] Figure 3 1 is a diagram showing a stacked structure of a smart window for a vehicle according to an embodiment of the present invention.

[0046] Figure 4 It is a diagram showing the stacked structure of a smart window for building according to one embodiment of the present invention.

[0047] Figure 5 It is a diagram showing a stacked structure of a smart window for building according to another embodiment of the present invention.

[0048] The reference numerals in the drawings are as follows.

[0049] 100-1 and 100-2: Polarizing plate

[0050] 110-1 and 110-2: Polarizer

[0051] 120-1 and 120-2: Functional coating

[0052] 200-1 and 200-2: Transparent conductive layer

[0053] 300: Transmittance adjustment layer

[0054] 400-1 and 400-2: Oriented film

[0055] 500: Frame Sealing Adhesive

[0056] 600: Adhesive / adhesive layer

[0057] 700: Glass for vehicles

[0058] 800: Glass for windows DETAILED DESCRIPTION

[0059] The present invention relates to a variable transmittance optical laminate, which can not only minimize cracks generated during the process, but also form a sealant height of less than 20 μm, thereby making the height of the liquid crystal layer and the height of the sealant substantially the same.

[0060] In more detail, it relates to a variable transmittance optical stack, which includes: a liquid crystal layer including a sealing glue; a first polarizing plate including a first functional coating and located on one side of the liquid crystal layer; a second polarizing plate including a second functional coating and located on the other side of the liquid crystal layer; a first transparent conductive layer formed between the first polarizing plate and the liquid crystal layer; and a second transparent conductive layer formed between the second polarizing plate and the liquid crystal layer, wherein at least one of the first transparent conductive layer and the second transparent conductive layer is formed to directly contact one of the first polarizing plate and the second polarizing plate, the surface pencil hardness of the first functional coating and the second functional coating is respectively 3B to 8H, and the sum of the thickness of the first functional coating and the second functional coating is 2 to 50 μm.

[0061] The variable transmittance optical laminate of the present invention is particularly suitable for the technical field of being able to change the transmittance of light according to the application of voltage, for example, it can be used for smart windows, etc. The so-called smart window refers to an optical structure that changes the transmittance of light according to the application of an electrical signal to control the amount of light or heat passed. That is, the smart window can change into a transparent, opaque or translucent state according to the voltage, and is also called a transmittance variable glass, dimming glass, smart glass, etc. The smart window can be used as a partition or privacy protection partition for dividing the internal space of a vehicle and a building, or as a daylighting window configured in the opening of a building. In addition, it can also be used as a highway sign, a bulletin board, a scoreboard, a clock or an advertising screen, and can be used instead of the glass of a transportation tool such as windows or skylights of a vehicle such as a car, bus, airplane, ship or train. The variable transmittance optical laminate of the present invention can also be used as a smart window in the above-mentioned technical fields, but because the conductive layer is directly formed on the polarizing plate and does not include a separate substrate for forming the conductive layer, the thickness is thin, which is beneficial to the bending characteristics, and can be particularly suitable for use in smart windows for vehicles or buildings. In one or more embodiments, the smart window using the variable transmittance optical laminate of the present invention can be used in transportation tools, such as the front window, rear window, side window and / or skylight of a car, windows for buildings, etc. In addition to the use of blocking external light, it can also be used for the internal space division of cars or buildings, etc. or privacy protection purposes, such as internal partitions, etc., and can also be used in wearable devices such as helmets, glasses, and watches.

[0062] Hereinafter, the embodiments of the present invention will be described in more detail with reference to the accompanying drawings. However, the following drawings attached to this specification are only examples of preferred embodiments of the present invention, which serve to further understand the above-mentioned invention content together with the technical ideas of the present invention, so the present invention should not be interpreted only in terms of the matters recorded in these drawings. The terms used in this specification are intended to illustrate the embodiments and are not intended to limit the present invention.

[0063] In this specification, unless otherwise specified in the context, the singular form also includes the plural form. For example, the "polarizing plate" used in this specification may refer to at least one of the first polarizing plate and the second polarizing plate, the "transparent conductive layer" may refer to at least one of the first transparent conductive layer and the second transparent conductive layer, and the "functional coating" may refer to at least one of the first functional coating and the second functional coating.

[0064] The terms "comprises" and / or "comprising" used in this specification are used to mean that they do not exclude the existence or addition of one or more other constituent elements, steps, actions and / or elements other than the mentioned constituent elements, steps, actions and / or elements. Throughout the specification, the same reference numerals refer to the same constituent elements.

[0065] As illustrated in the accompanying drawings, spatially relative terms such as "below", "bottom", "lower", "above", "upper surface", "upper part", etc. can be used to easily describe the relationship between one element or constituent element and other elements or constituent elements. Spatially relative terms should be understood as terms that include different directions of the elements when in use or in operation in addition to the directions illustrated in the drawings. For example, when the elements illustrated in the drawings are turned over, the elements described as "below" or "lower" of other elements can be placed "above" other elements. Therefore, the exemplary term "below" can include the two directions of below and above. The elements can also be oriented in other directions, so the spatially relative terms can be interpreted according to the orientation. The "top-down direction" used in this specification can be interpreted as a direction orthogonal to the polarizing plate and / or the transparent conductive layer, that is, the direction observed from the visible side of the user.

[0066] The term “substantially” as used in this specification may be interpreted not only as physically identical or identical but also as including the situation within the error range in the measurement or manufacturing process. For example, it may be interpreted as being within the error range of 0.1% or less.

[0067] <Transmittance variable optical laminate and method for producing the same>

[0068] Reference Figure 1 The variable transmittance optical stack of one embodiment of the present invention may include a first polarizing plate 100-1, a second polarizing plate 100-2, a first transparent conductive layer 200-1, a second transparent conductive layer 200-2 and a liquid crystal layer, and the liquid crystal layer may include a transmittance adjustment layer 300, an alignment film 400 and a sealant 500. In addition, referring to Figure 2 For another embodiment of the variable transmittance optical stack of the present invention, a sticking / adhesive layer 600 may be further included on the outermost surface of the stack. More specifically, referring to Figures 3 to 5 The first polarizing plate 100 - 1 and the second polarizing plate 100 - 2 may each include a polarizer 110 and at least one functional coating 120 for improving the surface hardness of the polarizing plate, and in one or more embodiments, may include an adhesive / bonding layer 600 and glasses 700 and 800 .

[0069] polarizing plate

[0070] The first polarizing plate 100-1 and the second polarizing plate 100-2 may be referred to as polarizing plate 100 in this specification. The polarizing plate 100 may include a polarizer 110 and a functional coating 120, and in one or more embodiments, may further include a protective layer, a phase difference adjustment layer, and a refractive index adjustment layer.

[0071] polarizer

[0072] The polarizer 110 may be a conventional polarizer or a polarizer developed in the future. For example, a stretched polarizer or a coating polarizer may be used.

[0073] In one embodiment, the stretched polarizer may include, for example, a stretched polyvinyl alcohol (PVA) resin. The polyvinyl alcohol resin may preferably be a polyvinyl alcohol resin obtained by saponifying a polyvinyl acetate resin. As the polyvinyl acetate resin, in addition to polyvinyl acetate, which is a homopolymer of vinyl acetate, copolymers of vinyl acetate and other monomers copolymerizable therewith may also be cited. As the other monomers, unsaturated carboxylic acid series, unsaturated sulfonic acid series, olefin series, vinyl ether series, acrylamide series monomers having an ammonium group, etc. may be mentioned. In addition, the polyvinyl alcohol resin may also be a modified substance, for example, polyvinyl formal or polyvinyl acetal modified by aldehydes.

[0074] In some embodiments, the liquid crystal layer can be formed by coating a liquid crystal coating composition on one side of the protective film. The liquid crystal coating composition can include a reactive liquid crystal compound and a dichroic dye.

[0075] The reactive liquid crystal compound may include a monomer molecule having a reactive mesogen (RM) capable of exhibiting liquid crystal properties and a polymerizable terminal functional group and having a liquid crystal phase after a cross-linking reaction by heat or light. If the reactive liquid crystal compound is polymerized by light or heat, a polymer network can be formed while maintaining the liquid crystal arrangement. By utilizing the reactive liquid crystal compound, a polarizer in the form of a thin film can be formed in which the optical anisotropy or dielectric constant characteristics of the liquid crystal are maintained and the mechanical stability and thermal stability are improved.

[0076] The above-mentioned dichroic dye is a component added to the liquid crystal coating composition to impart polarization characteristics, and has a property that the absorbance in the long axis direction of the molecule is different from the absorbance in the short axis direction. As non-limiting examples of the above-mentioned dichroic dye, acridine pigments, oxazine pigments, cyanine pigments, naphthalene pigments, azo pigments, anthraquinone pigments, etc. can be included. They can be used alone or in combination of two or more.

[0077] The liquid crystal coating composition may further include a solvent capable of dissolving the reactive liquid crystal compound and the dichroic dye, for example, propylene glycol monomethyl ether acetate (PGMEA), methyl ethyl ketone (MEK), xylene, chloroform, etc. The liquid crystal coating composition may further include a leveling agent, a polymerization initiator, etc. within a range that does not hinder the polarization characteristics of the coating film.

[0078] Functional coating

[0079] Reference Figures 3 to 5 The functional coating 120 is provided to improve the hardness of the polarizing plate 100 .

[0080] Generally speaking, as the height of the liquid crystal layer decreases, the optical laminate contained in the smart window has a tendency to increase transmittance or decrease driving voltage. Therefore, from the perspective of suppressing light leakage and improving reliability, it is advantageous to reduce the thickness of the liquid crystal layer, preferably to make it less than 20 μm. However, in the production process of the optical laminate, after applying the sealant, during the bonding process of the upper laminate and the lower laminate, due to the surface extrusion of the above-mentioned laminate substrates caused by the sealant, the height of the sealant will not be reduced to less than 20 μm, and the height of the liquid crystal layer adjacent to the sealant will exceed 20 μm, so there is a problem of light leakage or reduced reliability of the spacer. In addition, in order to solve the above-mentioned problem, in the case of reducing the thickness of the sealant by reducing the viscosity of the sealant material, there is not only difficulty in keeping the uniformity of the sealant line constant, but also a decrease in adhesion, and liquid crystal contamination of the inside of the sealant.

[0081] Therefore, in order to solve the above-mentioned technical problems of the prior art, the technical feature of the present invention is that it includes the above-mentioned functional coating, so as to suppress the surface extrusion of the substrate during the coating and bonding process of the sealant by giving a predetermined hardness to the polarizing plate, thereby making the thickness of the sealant less than 20 μm. In this way, by making the thickness of the sealant less than 20 μm, the thickness of the sealant and the liquid crystal layer are made substantially the same, thereby further effectively suppressing the light leakage phenomenon in the liquid crystal area adjacent to the sealant, and not only that, but also further improving the reliability of the spacer.

[0082] The functional coating is not particularly limited as long as it can impart a predetermined hardness to the polarizing plate to solve the above-mentioned technical problems, and may include, for example, a hard coating layer and / or a low refractive index layer.

[0083] The hard coating layer may be a hard coating layer developed in the past or in the future. In one or more embodiments, the hard coating layer may include an acrylate compound or an epoxy compound, and may further include inorganic particles, a photoinitiator, and the like.

[0084] The above-mentioned acrylate compounds may include monomers or oligomers containing (meth)acrylate groups. The term "(meth)acryloyl-" used in this specification may be used to refer to "methacryloyl-", "acryloyl-" or both. Non-limiting examples of the above-mentioned acrylate compounds include neopentyl glycol acrylate, 1,6-hexanediol (meth)acrylate, propylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, trimethylolethane tri(meth)acrylate, 1,2,4-cyclohexane tetra(meth)acrylate, pentaglycerol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol tri(meth)acrylate, and the like. (Meth) acrylate, dipentaerythritol penta (meth) acrylate, dipentaerythritol tetra (meth) acrylate, dipentaerythritol hexa (meth) acrylate, tripentaerythritol tri (meth) acrylate, tripentaerythritol hexa (meth) acrylate, bis (2-hydroxyethyl) isocyanurate di (meth) acrylate, hydroxyethyl (meth) acrylate, hydroxypropyl (meth) acrylate, hydroxybutyl (meth) acrylate, isooctyl (meth) acrylate, isodecyl (meth) acrylate, stearyl (meth) acrylate, tetrahydrofurfuryl (meth) acrylate, phenoxyethyl (meth) acrylate, isobornyl (meth) acrylate, etc. They can be used alone or in combination of two or more. The above-mentioned acrylate compound can include epoxy (meth) acrylate compound and / or urethane (meth) acrylate compound.

[0085] In addition, the epoxy compound may include a monomer or oligomer having at least one epoxy group in the molecule. The epoxy group may be an alicyclic epoxy group. The carbon number of the alicyclic ring contained in the epoxy group may be 3 to 7, for example, it may be an alicyclic epoxy group (cyclohexyl epoxy group) containing a cyclohexane ring. The alicyclic ring may also have a substituent. For example, the alicyclic ring may include an alkyl substituent having a carbon number of 1 to 20. When the carbon number of the alkyl substituent is greater than 20, it may be disadvantageous in terms of curing speed. The alkyl substituent includes a straight chain type or a branched type, and when it is a branched type, the carbon number may be 3 or more.

[0086] According to one embodiment of the present invention, in terms of the method for manufacturing a hard coating film, the hard coating composition may include inorganic particles. According to one embodiment of the present invention, as the inorganic particles, inorganic particles with a particle size of nanometers can be used, for example, nanoparticles with a particle size of less than 100nm, preferably 10 to 100nm, and more preferably 10 to 50nm. In addition, as the inorganic particles, for example, silica particles, aluminum oxide particles, titanium oxide particles, zinc oxide particles, etc. can be used. By including the inorganic particles, the hardness of the hard coating can be further improved. According to one embodiment of the present invention, the content of the inorganic particles can be 10 to 60% by weight, preferably 20 to 50% by weight, relative to the total weight of the hard coating composition. By including the inorganic particles in the above range, the hardness improvement effect of the hard coating film brought about by the addition of inorganic particles can be achieved within the range that the physical properties of the hard coating composition are not reduced.

[0087] According to one embodiment of the present invention, in terms of the method for manufacturing a hard coating film, the hard coating composition may include a photoinitiator. According to one embodiment of the present invention, as the photoinitiator, 1-hydroxy-cyclohexyl-phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, 2-hydroxy-1-[4-(2-hydroxyethoxy)phenyl]-2-methyl-1-propanone, methyl benzoylformate, α,α-dimethoxy-α-phenylacetophenone, 2-benzoyl-2-(dimethylamino)-1-[4-(4-morpholinyl)phenyl]-1-butanone, 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholinyl)-1-propanone, diphenyl(2,4,6-trimethylbenzoyl)-phosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, etc. can be cited, but are not limited thereto. In addition, currently commercially available products include Irgacure 184, Irgacure 500, Irgacure 651, Irgacure 369, Irgacure 907, Darocur 1173, Darocur MBF, Irgacure 819, Darocur TPO, Irgacure 907, Esacure KIP 100F, etc. These photoinitiators may be used alone or in combination of two or more different ones.

[0088] According to one embodiment of the present invention, the content of the photoinitiator may be 0.5 to 10 wt %, preferably 1 to 5 wt %, relative to the total weight of the hard coating composition. When the photoinitiator is within the above range, sufficient cross-linking photopolymerization can be achieved without reducing the physical properties of the hard coating film.

[0089] On the other hand, in the method for producing a hard coating film of the present invention, in addition to the above-mentioned components, the hard coating composition may further contain additives commonly used in the technical field to which the present invention belongs, such as surfactants, anti-yellowing agents, leveling agents, and antifouling agents. In addition, the content thereof can be variously adjusted within the range that does not reduce the physical properties of the hard coating composition of the present invention, and therefore is not particularly limited.

[0090] The low refractive index layer is also provided to improve the hardness of the polarizing plate within the scope of not impairing the purpose of the present invention. The low refractive index layer may include one or more low refractive index agents selected from the group consisting of, for example, SiO2, Al2O3, MgF2, CaF, cryloite, etc., and in some embodiments, may include the compounds and / or resins used in the hard coating layer.

[0091] The hard coating layer and the low refractive index layer can be used alone or in a multilayer structure in some embodiments. Figures 3 to 5 As shown, the functional coating 120 can be formed by direct contact on one side of the polarizer 110, but is not limited to this. For example, in the case where the polarizing plate includes a phase difference adjustment layer and / or a refractive index adjustment layer, the functional coating can be formed on one side of the phase difference adjustment layer and / or the refractive index adjustment layer described later, whereby the functional coating, the phase difference adjustment layer, the refractive index adjustment layer and the polarizer are stacked in sequence. The functional coating 120 is preferably formed on the liquid crystal layer side of the polarizer 110, that is, on the inner side of the polarizer, for example, the first functional coating 120-1 and the second functional coating 120-2 can each be present on the inner sides of the first polarizer 110-1 and the second polarizer 110-2 and arranged in a manner opposite to each other. In this case, the functional coating will impart a hardness to the polarizing plate at a level suitable for forming components such as a transparent conductive layer, thereby not only minimizing cracks or scratches generated during the manufacturing or processing steps of the optical laminate, but also more effectively suppressing the extrusion of the substrate surface caused by the frame sealant, thereby also being beneficial in reducing the thickness of the frame sealant.

[0092] In one embodiment, the surface pencil hardness of the functional coating 120 is preferably 3B to 8H. Regarding the surface pencil hardness, the pencil hardness of the functional coating can be measured by using a pencil hardness tester (Pencil Hardness Tester, Sukbo Science Co., Ltd., South Korea), placing a pencil at a 45° angle on the surface of the functional coating, applying a load of 750g, and scratching the pencil at a speed of 300mm / min. The pencil uses Mitsubishi products, and each pencil hardness is implemented 5 times, heat treated at 100°C for 10 minutes, and evaluated based on whether scratches can be confirmed with the naked eye. When the surface pencil hardness of the functional coating meets the above range, it can not only have excellent wear resistance, but also further improve the bending resistance or durability of the optical laminate.

[0093] In one or more embodiments, the thickness of the first functional coating 120-1 and the second functional coating 120-2 may be 1 to 35 μm, more preferably 5 to 25 μm, and the sum of the thickness of the first functional coating 120-1 and the second functional coating 120-2 may be 2 to 50 μm. The above thickness may refer to the thickness after drying. When the sum of the thickness of the first functional coating 120-1 and the second functional coating 120-2 satisfies the above range, a hard coating film with excellent hardness, thinness, and almost no curling can be manufactured. Furthermore, since the extrusion phenomenon of the substrate surface caused by the frame sealant is more effectively suppressed, it is also advantageous in reducing the thickness of the frame sealant.

[0094] The functional coating can be coated by a suitable method such as a die coater, an air knife, a reverse roller, a spray coater, a doctor blade, casting, gravure printing, micro gravure printing, spin coating, etc.

[0095] Protective layer

[0096] The protective layer is intended to protect the polarization characteristics of the polarizer from the influence of the subsequent process and the external environment, and can be implemented in the form of a protective film or the like. The protective layer can be formed by directly contacting one or both sides of the polarizer, but is not limited thereto. For example, the protective layer can also be used in a multilayer structure in which more than one protective layer is continuously stacked, and can be formed by directly contacting other components such as a phase difference adjustment layer. In one or more embodiments, the protective layer may include one or more selected from the group consisting of polyethylene terephthalate (PET), polyethylene isophthalate (PEI), polyethylene naphthalate (PEN), polybutylene terephthalate (PBT), diacetyl cellulose, triacetyl cellulose (TAC), polycarbonate (PC), polyethylene (PE), polypropylene (PP), polymethyl acrylate (PMA), polymethyl methacrylate (PMMA), polyethyl acrylate (PEA), polyethyl methacrylate (PEMA), and cyclic olefin polymer (COP). The thickness of the protective layer may be 10 to 100 μm, more preferably 20 to 80 μm.

[0097] In addition, the protective layer may further contain an ultraviolet absorber on the outermost surface to prevent the function of the optical laminate from being reduced. The ultraviolet absorbing layer is not particularly limited as long as it is used to prevent the degradation of the optical laminate caused by ultraviolet rays. For example, salicylic acid ultraviolet absorbers (phenyl salicylate, p-tert-butyl salicylate, etc.), benzophenone ultraviolet absorbers (2,4-dihydroxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, etc.), benzotriazole ultraviolet absorbers (2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)benzotriazole, 2-(2'-hydroxy- 3'-tert-butyl-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3'-(3",4",5",6"-tetrahydrophthalimidomethyl)-5'-methylphenyl)benzotriazole, 2,2-methylenebis(4-(1,1,3,3-tetramethylbutyl)-6-(2H-benzotriazol-2-yl)phenol), 2-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, -3'-tert-butyl-5'-(2-octyloxycarbonylethyl)-phenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3'-(1-methyl-1-phenylethyl)-5'-(1,1,3,3-tetramethylbutyl)-phenyl)benzotriazole, 2-(2H-benzotriazol-2-yl)-6-(straight chain and side chain dodecyl)-4-methylphenol, octyl-3-[3-tert-butyl-4-hydroxy-5-(chloro-2H-benzotriazol-2-yl)phenyl]propionate and 2-ethylhexyl-3-[3-tert-butyl-4-hydroxy-5-( The invention also includes a mixture of cyanoacrylate-based UV absorbers (2'-ethylhexyl-2-cyano-3,3-diphenylacrylate, ethyl-2-cyano-3-(3',4'-methylenedioxyphenyl)-acrylate, etc.), triazine-based UV absorbers, etc., preferably a benzotriazole-based UV absorber or a triazine-based UV absorber which has high transparency and an excellent effect of preventing degradation of the polarizing plate or the transmittance variable layer, and particularly preferably a benzotriazole-based UV absorber having a more suitable spectral absorption spectrum. The above-mentioned benzotriazole-based ultraviolet absorber can also be a bis (Bis) substance, for example, it can be 6,6'-methylenebis (2-(2H-benzo [d] [1,2,3] triazol-2-yl) -4- (2,4,4-trimethylpentane-2-yl) phenol), 6,6'-methylenebis (2-(2H-benzo [d] [1,2,3] triazol-2-yl) -4- (2-hydroxyethyl) phenol), etc.

[0098] Phase difference adjustment layer

[0099] The above-mentioned phase difference adjustment layer is intended to supplement the optical properties of the optical laminate, and can be implemented in the form of a phase difference film, etc., and a phase difference film developed in the past or in the future can be used. For example, a quarter wave plate (1 / 4 wave plate), a half wave plate (1 / 2 wave plate), etc. for delaying the phase of light can be used, and they can be used alone or in combination. The above-mentioned phase difference adjustment layer can be formed by direct contact on one side of the polarizer, but is not limited to this. For example, the above-mentioned phase difference adjustment layer can be formed by direct contact on one side of the protective layer, and can also be formed by direct contact on one side of the refractive index adjustment layer.

[0100] The phase difference adjustment layer may be a polymer stretched film or a liquid crystal polymer film obtained by stretching a polymer film capable of imparting optical anisotropy in an appropriate manner. In one embodiment, the polymer stretched film may be a polymer layer containing the following substances: polyolefins such as polyethylene (PE) or polypropylene (PP), cycloolefin polymers (COP: cyclo olefin polymer) such as polynorbornene, polyvinyl chloride (PVC), polyacrylonitrile (PAN), polysulfone (PSU), acrylic resin (acryl resin), polycarbonate (PC), polyesters such as polyethylene terephthalate (PET), polyacrylate (polyacrylate), polyvinyl alcohol (PVA), cellulose ester polymers such as triacetylcellulose (TAC), or copolymers of two or more monomers of the monomers forming the above polymers. The method for obtaining the above-mentioned polymer stretch film is not particularly limited, for example, it can be obtained by stretching the above-mentioned polymer material after being molded into a film shape. The above-mentioned method of being molded into a film shape is not particularly limited, and can be molded into a film by known methods such as injection molding, sheet molding, blow molding, injection blow molding, inflation molding, extrusion molding, foam molding, and tape casting, or by secondary processing molding methods such as compression molding and vacuum molding. Among them, extrusion molding and tape casting are preferably used. At this time, for example, an extruder equipped with a T-shaped mold, a circular mold, etc. can be used to extrusion mold the unstretched film. In the case of obtaining a molded product by extrusion molding, a material that has been melt-mixed in advance with various resin components, additives, etc. can be used, and it is also possible to mold via melt mixing during extrusion molding. In addition, a solvent shared by various resin components can also be used, such as chloroform, dichloromethane, etc. After the various resin components are dissolved, tape casting, drying and solidification are performed, thereby the unstretched film is tape cast. The polymer stretched film may be uniaxially stretched along the mechanical flow direction (MD; Mechanical Direction, longitudinal or length direction) and uniaxially stretched along the direction perpendicular to the mechanical flow direction (TD; Transverse Direction, transverse or width direction). In addition, a biaxially stretched film may be produced by stretching by a sequential biaxial stretching method of roll stretching and tenter stretching, a simultaneous biaxial stretching method based on tenter stretching, a biaxial stretching method based on tubular stretching, or the like.The liquid crystal polymer film may contain a reactive liquid crystal compound in a polymerized state. The reactive liquid crystal compound may be similarly applicable to the reactive liquid crystal compound of the coated polarizer. In one or more embodiments, the thickness of the phase difference adjustment layer may be 10 μm to 100 μm in the case of a polymer stretched film, and more preferably may be 20 to 80 μm.

[0101] Refractive index adjustment layer

[0102] The refractive index adjustment layer is provided to compensate for the refractive index difference of the optical laminate caused by the transparent conductive layer 200, and can play a role in improving visible characteristics by reducing the refractive index difference. In addition, the refractive index adjustment layer can also be provided to correct the color caused by the transparent conductive layer 200. On the other hand, in the case where the transparent conductive layer has a pattern, the refractive index adjustment layer can compensate for the transmittance difference between the pattern area with the pattern and the non-pattern area without the pattern. Specifically, the transparent conductive layer 200 is stacked adjacent to other components (such as polarizers, etc.) with different refractive indices, and due to the refractive index difference with other adjacent layers, the difference in light transmittance can be induced. Especially in the case where the transparent conductive layer is formed with a pattern, the problem that the pattern area and the non-pattern area look different may occur. Therefore, by including the refractive index adjustment layer, the refractive index can be compensated to reduce the difference in light transmittance of the optical laminate, especially in the case where the transparent conductive layer is formed with a pattern, the pattern area and the non-pattern area will not look different. In one embodiment, the refractive index of the refractive index adjustment layer can be appropriately selected according to the materials of other adjacent components, preferably 1.4 to 2.6, and more preferably 1.4 to 2.4. In this case, light loss caused by a significant refractive index difference between the other components such as the polarizer and the transparent conductive layer 200 can be prevented. The refractive index adjustment layer is not particularly limited as long as it can prevent a significant refractive index difference between other components such as the polarizer and the transparent conductive layer 200. A compound for forming a refractive index adjustment layer developed in the past or in the future can be used, for example, it can be formed by a refractive index adjustment layer forming composition containing a polymerizable isocyanurate compound.

[0103] In one embodiment, in addition to the above-mentioned components, the polarizing plate 100 may further include other components to assist or enhance the characteristics of the polarizer, for example, to further improve the mechanical durability, an outer coating may be further included. In one or more embodiments, the polarizing plate 100 may have a thickness of 30 to 200 μm, preferably 30 to 170 μm, and more preferably 50 to 150 μm. In this case, a thin optical laminate can be manufactured while maintaining the optical characteristics of the polarizing plate 100.

[0104] Transparent conductive layer

[0105] The transparent conductive layer 200 is provided for driving the liquid crystal layer and can be formed by directly contacting the polarizing plate 100. Figure 1 As shown, the first transparent conductive layer 200-1 and the second transparent conductive layer 200-2 can each be formed by directly contacting the first polarizing plate 100-1 and the second polarizing plate 100-2. In the past, optical laminates used to manufacture smart windows and the like were manufactured by forming a conductive layer for liquid crystal driving on one side of a substrate and bonding the other side of the substrate to a polarizing plate. However, the variable transmittance optical laminate of the present invention is characterized in that a conductive layer is directly formed on one side of a polarizing plate without including a separate substrate for forming a conductive layer, thereby reducing the thickness of the laminate and improving the transmittance and bending characteristics in a light transmission mode. In one embodiment, the transparent conductive layer 200 can be formed by direct vapor deposition on one side of the polarizing plate 100. At this time, for the transparent conductive layer 200, in order to improve the adhesion to the polarizing plate 100, it can be formed by directly contacting the pre-treated surface of the polarizing plate 100 after pre-treatment such as corona treatment and plasma treatment is performed on one side of the polarizing plate 100. The above-mentioned pretreatment is not limited to corona treatment or plasma treatment, and a pretreatment process developed in the past or in the future can be used within the scope that does not impair the purpose of the present invention. In another embodiment, in order to improve the adhesion between the above-mentioned transparent conductive layer 200 and the polarizing plate 100, an easy-adhesion layer (not shown) provided on one side of the polarizing plate 100 can be formed by being located between them and directly contacting the polarizing plate 100. The transmittance of the above-mentioned transparent conductive layer 200 relative to visible light is preferably 50% or more. For example, it can include one or more selected from the group consisting of transparent conductive oxides, metals, carbon-based substances, conductive polymers, conductive inks and nanowires, but is not limited thereto, and materials for transparent conductive layers developed in the past or in the future can be used. In addition, the above-mentioned conductive layer can be composed of a combination of the above-mentioned substances to form a structure of more than two layers. For example, the above-mentioned conductive layer can reduce the reflectivity of the incident light and improve the transmittance by having a two-layer structure including a metal layer and a transparent conductive oxide layer. The metal layer has a high reflectivity and reduces the visibility of the screen when used alone. However, by laminating the transparent conductive oxide layer, the reflectivity can be reduced and the transmittance can be improved.

[0106] More specifically, in one or more embodiments, the transparent conductive oxide may include one or more selected from the group consisting of indium tin oxide (ITO), indium zinc oxide (IZO), indium tin zinc oxide (IZTO), aluminum zinc oxide (AZO), gallium zinc oxide (GZO), fluorine tin oxide (FTO), zinc oxide (ZnO), etc. In addition, the metal may include one or more selected from the group consisting of gold (Au), silver (Ag), copper (Cu), molybdenum (Mo), aluminum (Al), platinum (Pt), palladium (Pd), chromium (Cr), titanium (Ti), tungsten (W), niobium (Nb), tantalum (Ta), vanadium (V), iron (Fe), manganese (Mn), cobalt (Co), nickel (Ni), zinc (Zn), neodymium (Nd), alloys containing at least one of them, etc., for example, may include silver-palladium-copper (APC) alloy or copper-calcium (CuCa) alloy. The carbon-based material may include one or more selected from the group consisting of carbon nanotubes (CNT), graphene, etc., and the conductive polymer may include one or more selected from the group consisting of polypyrrole, polythiophene, polyacetylene, poly(3,4-ethylenedioxythiophene) (PEDOT), polyaniline, etc. The conductive ink may be an ink mixed with metal powder and a curable polymer binder, and the nanowire may be, for example, silver nanowire (AgNW).

[0107] In addition, the transparent conductive layer 200 can be formed by combining the above-mentioned substances and having a structure of more than two layers. For example, in order to reduce the reflectivity of the incident light and improve the transmittance, it can be formed by a two-layer structure including a metal layer and a transparent conductive oxide layer. The transparent conductive layer 200 can be formed by a method commonly used in the art, for example, it can be formed by a coating process such as spin coating, roller coating, rod coating, dip coating, gravure coating, curtain coating, die coating, spray coating, blade coating, kneader coating, etc.; a printing process such as screen printing, spray printing, inkjet printing, letterpress printing, gravure printing, lithography, etc.; an in-mold labeling (IML) injection method and a vapor deposition process such as chemical vapor deposition (CVD), physical vapor deposition (PVD), plasma enhanced chemical vapor deposition (PECVD), a dry or wet plating process, etc., by selecting an appropriate process to form.

[0108] Liquid crystal layer

[0109] The above-mentioned liquid crystal layer can adjust the transmittance of light incident from one or more directions according to the electric field, thereby changing the driving mode of the above-mentioned optical laminate. The above-mentioned liquid crystal layer may include a liquid crystal compound in the transmittance adjustment layer 300, and may include an alignment film 400. For example, it may be located in the space provided by the sealant 500 and the spacer (not shown) present between the first polarizer 100-1 and the second polarizer 100-2 in the light control area. As long as the above-mentioned liquid crystal compound can be driven and control the transmittance of light by an electric field, there is no special restriction, and liquid crystal compounds developed in the past or in the future can be used. For example, the content of the reactive liquid crystal compound of the above-mentioned coating type polarizer can be applied in the same way. There is no special restriction on the liquid crystal behavior of the above-mentioned liquid crystal layer. For example, it can be driven by a twisted nematic (TN) mode, a super twisted nematic (STN) mode, a vertical alignment (VA) mode, etc.

[0110] Frame Sealing Adhesive

[0111] The sealant 500 may be located between the first polarizing plate 100-1 and the second polarizing plate 100-2 in the inactive region. The sealant may combine the first polarizing plate and the second polarizing plate, and together with the spacer, may ensure a space for providing liquid crystal compounds between the first polarizing plate and the second polarizing plate.

[0112] The above-mentioned frame sealant 500 may include a curable resin as a base resin. As the above-mentioned base resin, a UV curable resin or a thermosetting resin known in the art as being usable for frame sealants may be used. The above-mentioned UV curable resin may be a polymer of a UV curable monomer. The above-mentioned thermosetting resin may be a polymer of a thermosetting monomer. As the base resin of the above-mentioned frame sealant 500, for example, an acrylate resin, an epoxy resin, a urethane resin, a phenol resin or a mixture of the above-mentioned resins may be used. In one embodiment, the above-mentioned base resin may be an acrylate resin, and the above-mentioned acrylate resin may be a polymer of an acrylic monomer. The above-mentioned acrylic monomer may be, for example, a multifunctional acrylate. In another embodiment, the above-mentioned frame sealant may further include a monomer component in the base resin. The above-mentioned monomer component may be, for example, a monofunctional acrylate. In this specification, a monofunctional acrylate may refer to a compound having one acryloyl group, and a multifunctional acrylate may refer to a compound having two or more acryloyl groups. The above-mentioned curable resin may be cured by irradiating ultraviolet rays and / or heating. The above-mentioned ultraviolet irradiation conditions or heating conditions can be appropriately implemented within the scope that does not harm the purpose of the present application. The above-mentioned frame sealant may further include an initiator, such as a photoinitiator or a thermal initiator, as needed. The above-mentioned frame sealant 500 can be formed by a method commonly used in the art, for example, the frame sealant can be applied to the periphery of the above-mentioned liquid crystal layer (i.e., the inactive area) using a glue dispenser with a nozzle.

[0113] The height of the sealant after curing is preferably substantially the same as that of the liquid crystal layer, for example, 2 to 20 μm. In this case, as described above, light leakage in the liquid crystal layer region adjacent to the sealant will not occur, and the reliability of the spacer can be further improved.

[0114] Spacer

[0115] The above-mentioned spacer (not shown) plays a role in keeping the liquid crystal gap of the liquid crystal layer constant, and may include at least one of a spherical spacer and a columnar spacer. In particular, a spherical spacer is preferably used from the perspective of processability. The above-mentioned spacer may be one or more, and the height of the above-mentioned spacer is 2 to 20 μm, which is preferred in terms of supporting the liquid crystal layer. In addition, when viewed from a top view, the area occupied by the above-mentioned spacer in the liquid crystal layer is preferably 0.01 to 10% relative to the area of ​​the liquid crystal layer in terms of improving the visibility of the user and the transmittance in the light-transmitting mode.

[0116] Other functional layers

[0117] The variable transmittance optical laminate of the present invention may further include other components within the range not impairing the purpose of the present invention. For example, it may further include an adhesive / bonding layer 600 (see Figures 2 to 5 ), and may further include an ultraviolet absorbing layer (not shown) and an impact-resistant layer (not shown).

[0118] The above-mentioned adhesive / adhesive layer 600 can be formed using an adhesive or an adhesive, preferably with appropriate adhesive force to prevent peeling, bubbles, etc. when operating the optical laminate, while also having transparency and thermal stability, and can have viscoelastic properties that can be applied to smart windows. The above-mentioned adhesive can use an adhesive developed in the past or in the future, for example, a photocurable adhesive can be used. The above-mentioned photocurable adhesive will be cross-linked and cured due to irradiation with active energy rays such as ultraviolet (UV) and electron beam (EB), thereby showing strong adhesive force, and can be composed of reactive oligomers, reactive monomers, photopolymerization initiators, etc. The above-mentioned reactive oligomer is an important component that determines the characteristics of the adhesive, and forms a cured film by forming a polymer bond through a photopolymerization reaction. The reactive oligomers that can be used can include polyester resins, polyether resins, polyurethane resins, epoxy resins, polyacrylic resins, silicone resins, etc. The above-mentioned reactive monomer plays the role of a cross-linking agent and a diluent of the above-mentioned reactive oligomer, and affects the bonding characteristics. The reactive monomers that can be used include monofunctional monomers, multifunctional monomers, epoxy monomers, vinyl ethers, cyclic ethers, etc. The above-mentioned photopolymerization initiator absorbs light energy and generates free radicals or cations to initiate photopolymerization. A suitable photopolymerization initiator can be selected and used according to the photopolymer resin. The above-mentioned adhesive can use an adhesive developed in the past or in the future. In one or more embodiments, acrylic adhesives, rubber adhesives, silicone adhesives, urethane adhesives, polyvinyl alcohol adhesives, polyvinyl pyrrolidone adhesives, polyacrylamide adhesives, cellulose adhesives, vinyl alkyl ether adhesives, etc. can be used.

[0119] As long as the adhesive has adhesion and viscoelasticity, there is no particular restriction, but from the perspective of ease of acquisition, it is preferably an acrylic adhesive, for example, it may include a (meth) acrylate copolymer, a crosslinking agent, and a solvent. The crosslinking agent may use a crosslinking agent developed in the past or in the future, for example, it may include a polyisocyanate compound, an epoxy resin, a melamine resin, a urea resin, a dialdehyde, a hydroxymethyl polymer, etc., and preferably may include a polyisocyanate compound. The solvent may include a common solvent used in the field of resin compositions, for example, alcohol compounds such as methanol, ethanol, isopropanol, butanol, and propylene glycol methoxy alcohol may be used; ketone compounds such as methyl ethyl ketone, methyl butyl ketone, methyl isobutyl ketone, diethyl ketone, and dipropyl ketone; acetate compounds such as methyl acetate, ethyl acetate, butyl acetate, and propylene glycol methoxy acetate; cellosolve compounds such as methyl cellosolve, ethyl cellosolve, and propyl cellosolve; solvents such as hydrocarbon compounds such as hexane, heptane, benzene, toluene, and xylene. They may be used alone or in combination of two or more.

[0120] The thickness of the above-mentioned adhesive / bonding layer 600 can be appropriately determined according to the type of resin that acts as an adhesive / adhesive, the adhesive / bonding strength, the environment in which the adhesive / adhesive is used, etc. In one embodiment, regarding the above-mentioned adhesive / bonding layer, in order to ensure sufficient adhesive / bonding force and minimize the thickness of the optical laminate, in the case of an adhesive layer, it can be 0.1 to 500 μm, preferably 0.5 to 450 μm, and more preferably 1 to 400 μm thick. In the case of an adhesive layer, it can be 2 to 30 μm, preferably 3 to 20 μm, and more preferably 5 to 10 μm thick. In one embodiment, the above-mentioned adhesive / bonding layer 600 can be formed on one or both sides of the polarizing plate by lamination or vacuum bonding.

[0121] The ultraviolet absorbing layer (not shown) is not particularly limited as long as it is used to prevent degradation of the optical laminate due to ultraviolet rays, and the contents regarding the ultraviolet absorber described in the protective layer can be applied as is, so description thereof is omitted.

[0122] The impact-resistant layer (not shown) is not particularly limited as long as it is located in the inner direction and has the function of buffering the impact and preventing the damage of the inner substrate when the impact is applied to the front of the window. It is preferably a material with a large tolerance to strain energy, for example, a thermoplastic resin with high toughness. As such resins, for example, polycarbonate resins, polyimide resins, polyamide resins, polyamide-imide resins, polyester resins, etc. can be cited. In addition, since the purpose of the present invention is to be used for a display device, it is preferred to use a resin with excellent light transmittance, preferably optically transparent.

[0123] <Smart Window>

[0124] In addition to the above-mentioned variable transmittance optical laminate, the present invention also includes a smart window including the above-mentioned variable transmittance optical laminate, and the above-mentioned smart window is applied to at least one of the front window, rear window, side window, skylight and interior partition of an automobile and a building window including the above-mentioned smart window. For example, a car including the smart window of the present invention can be joined to the vehicle glass 700 on both sides of the optical laminate including the polarizing plate 100, the transparent conductive layer 200, the liquid crystal layer and the adhesive / adhesive layer 600 (see Figure 3 ), for example, after placing adhesive films and vehicle glass on both sides of the optical laminate, a press machine is used to heat the adhesive films at 90°C and under a vacuum of about 1 bar for 10 to 20 minutes. The adhesive films may include EVA films, PVB films, etc. In addition, the optical laminate may be formed on both sides (see Figure 4 ) or one side (refer to Figure 5 ) is joined to a building window (window glass 800), and a UV adhesive can be applied to both sides of the optical laminate to join the window glass, and then UV curing is performed to produce a Figure 4 or Figure 5 The smart window product for windows of the same structure can also be manufactured by laminating window glass on one side of the optical laminate. Figure 4 or Figure 5 Smart window products for windows of the same structure.

[0125] In addition, in addition to this, the above-mentioned smart window can also be applied to transportation tools and wearable devices generally used in the field.

[0126] Implementation

[0127] The following are specific examples of the present invention. However, the present invention is not limited to the examples disclosed below, and can be implemented in a variety of different ways. These examples are only provided to make the disclosure of the present invention complete and to fully inform the general technicians of the technical field to which the present invention belongs of the scope of the invention. The present invention is only defined by the scope of the claims.

[0128] Manufacturing Example 1: Polarizing Plate Manufacturing

[0129] (1) Swelling treatment process

[0130] A polyvinyl alcohol film (stock film) with a thickness of 60 μm (manufactured by Kuraray Co., Ltd., trade name "Kuraraypoval film VF-PE#6000", average degree of polymerization 2400, saponification degree 99.9 mol%) was continuously unwound from a stock roll while being conveyed and immersed in a swelling bath filled with pure water at 20°C for 30 seconds. In this swelling treatment step, inter-roll stretching (uniaxial longitudinal stretching) was performed by generating a difference in peripheral speed between the nip rolls. The stretching ratio was set to 2.5 times based on the stock film.

[0131] (2) Dyeing process

[0132] Next, the film passed through the nip rollers was immersed in a dyeing bath at 30°C with a mass ratio of pure water / potassium iodide / iodine / boric acid of 100 / 2 / 0.01 / 0.3 for 120 seconds. In this dyeing treatment, inter-roll stretching (longitudinal uniaxial stretching) was also performed by generating a difference in peripheral speed between the nip rollers. The stretching ratio was set to 1.1 times based on the film after the swelling treatment step.

[0133] (3) Cross-linking treatment process

[0134] Next, the film passed through the nip rollers was immersed in a first crosslinking bath at 56°C with a mass ratio of pure water / potassium iodide / boric acid of 100 / 12 / 4 for 70 seconds. Inter-roll stretching (longitudinal uniaxial stretching) was performed by causing a difference in peripheral speed between the nip rollers and the nip rollers provided between the first crosslinking bath and the second crosslinking bath. The stretching ratio was set to 1.9 times based on the film after the dyeing treatment step.

[0135] (4) Color correction process

[0136] Next, the cross-linked film was immersed in a second cross-linking bath having a mass ratio of potassium iodide / boric acid / pure water of 9 / 2.9 / 100 at 40° C. for 10 seconds.

[0137] (5) Cleaning process

[0138] Next, the membrane after the second crosslinking treatment was immersed in a cleaning bath filled with pure water at 14° C. for 5 seconds and rinsed with 5 ml 3 / h and elution temperature of 14°C for cleaning.

[0139] (6) Drying process

[0140] Next, the film after the washing treatment step was passed through a drying furnace to be heated and dried at 80° C. for 190 seconds to produce a polarizer film. The moisture content after drying was 13.6%, and the thickness of the obtained polarizer film was about 21 μm.

[0141] (7) Joining process

[0142] Next, as an adhesive, a water-based adhesive containing 5 parts by mass of polyvinyl alcohol relative to 100 parts by mass of water was prepared. Then, protective films were laminated on both sides of the polarizer film using the prepared UV adhesive. The obtained laminate was exposed to UV light to cure the adhesive, thereby producing a polarizing plate.

[0143] The thickness of the adhesive layer in the obtained polarizing plate was about 2 μm.

[0144] Production Example 2: Production of Composition HC1 for Forming Hard Coat Layer

[0145] A hard coating composition HC1 was prepared by mixing 16.2 g of a dendrimer compound (SP-1106, Miyoshi Specialty Chemicals Co., Ltd.), 14.4 g of inorganic nanoparticles (MEK-AC-2140, Nissan Chemical Co., Ltd., solid content 40 wt%), 1.8 g of a polyfunctional (meth)acrylate containing an ethylene glycol group (DPEA126, Nippon Kayaku Co., Ltd.), 0.7 g of a photoinitiator (1-hydroxycyclohexyl phenyl ketone), and 2.9 g of methyl ethyl ketone.

[0146] Production Example 3: Production of hard coat layer forming composition HC2

[0147] A hard coating composition HC2 was prepared by mixing 18 wt% of a multifunctional acrylate DPEA-12 (Nippon Kayaku Co., Ltd.) having an ethylene glycol group, 12 wt% of a multifunctional urethane acrylate SOU-1700B (SHIN-A T&C Co., Ltd.) having a cyclohexyl group, 20 wt% of silica inorganic nanoparticles Nanopol-784 (50% dilution of n-butyl acetate, 20 nm, Evonik Co., Ltd.), 1.8 wt% of Irgacure 184 (BASF Co., Ltd.), 0.2 wt% of BYK-333 (BYK Chemie Co., Ltd.), 38 wt% of methyl ethyl ketone and 10 wt% of n-butyl acetate.

[0148] Production Example 4: Hard Coating Formation

[0149] The hard coating composition prepared in the above-mentioned Preparation Example 2 or Preparation Example 3 was applied to one side of the polarizing plate prepared in Preparation Example 1 by using a Mayer Bar to adjust the thickness after drying, and dried at 80°C for 5 minutes. 2 The upper polarizing plate and the lower polarizing plate each having a hard coating layer formed on one surface are cured by applying light of an amount of light.

[0150] Manufacturing Example 5: Transparent Conductive Layer Manufacturing

[0151] The upper polarizing plate and the lower polarizing plate produced by the above-mentioned manufacturing examples 1 to 4 were placed, a 450W DC power supply was applied to start the sputtering gun, and then plasma was induced to the ITO (10wt% Sn doped In2O3) target, thereby forming a transparent conductive film (90nm). The ion gun was started with a 50W DC power to perform ion treatment on the transparent conductive film formed above. At this time, the pressure was maintained at 3mTorr at room temperature and argon and oxygen were supplied at 30sccm and 1sccm respectively. At this time, the thickness of the transparent conductive layer was measured by FT-SEM.

[0152] Manufacturing Example 6: Orientation Film Preparation

[0153] An alignment liquid was applied and dried (80° C. / 2 minutes) on the transparent conductive layers of the upper polarizing plate and the lower polarizing plate manufactured in Manufacturing Example 5. Then, UV was irradiated on the dried alignment liquid to produce an alignment film.

[0154] Manufacturing Example 7: Spacer Dispersion Manufacturing

[0155] The mixed solvent was prepared by mixing spherical spacers (SEKISUI Co., Ltd., SP series) of the heights of the liquid crystal gaps (Gap) of the following examples with 100 ml of IPA as the reference. Then, the conductive layer laminate of the lower polarizing plate of Manufacturing Example 6 was placed in a spacer dispenser (SDSS-KHU02, Shinto Giken Co., Ltd.), the mixed solvent prepared above was spread at 110° C. and then dried for 20 minutes, thereby forming spherical spacers on the alignment film of the lower polarizing plate.

[0156] Manufacturing Example 8: Manufacturing of Frame Sealing Adhesive Layer

[0157] On the orientation film of the lower polarizing plate manufactured in the above-mentioned manufacturing example 6, a frame sealant (UVF-006, 70,000 mPa·s, Sekisui Co., Ltd.) is applied according to the product size using a frame sealant applicator (SHOTmini200Ωx, MUSASHI Co., Ltd.). Then, in a state where the polarization axes of the upper polarizing plate and the lower polarizing plate are arranged parallel to each other at 0° or 90°, liquid crystal is injected into the orientation film of the upper polarizing plate by the ODF process, and the upper polarizing plate and the lower polarizing plate are bonded at the same time. Then, UV curing (500mJ / cm 2 ).

[0158] Examples 1 to 8 and Comparative Examples 1 to 7: Production of Optical Laminated Body

[0159] According to the compositions shown in Tables 1 to 2 below, variable transmittance optical laminates for smart windows of Examples 1 to 8 and Comparative Examples 1 to 7 were produced.

[0160] [Table 1]

[0161]

[0162] [Table 2]

[0163]

[0164] Experimental example

[0165] (1) Pencil hardness

[0166] The pencil hardness of the hard-coated surface of the polarizing plate was measured using a pencil hardness tester (Sukbo Science, South Korea). The polarizing plate was bonded to an 80mm x 60mm glass using an adhesive. Then, a pencil (Mitsubishi Corporation) was placed at an angle of 45° on the hard-coated surface, a load was applied using a 750g weight, and the pencil was scratched at a speed of 300mm / min. Each pencil hardness was implemented 5 times, and heat treated at 100°C for 10 minutes. For each pencil hardness, the hardness was measured based on whether scratches were generated. The results are recorded in the following Tables 3 and 4.

[0167] (2) Thickness measurement

[0168] The thickness was measured using a thickness meter (MH-15M, SENDAI NIKON). The thickness, height or width of the hard coating layer of the polarizing plate, the gap of the liquid crystal and the sealant at the same position before and after production were measured and calculated. The results are recorded in the following Tables 3 and 4.

[0169] (3) Reliability mandrel evaluation

[0170] In order to evaluate the bending characteristics and crack resistance by a cylindrical bending tester (Lab-Q D605, CKSI), the optical laminate sample after the upper / lower plate bonding was placed in a size of 100mm x 100mm in such a way that the lower plate surface of the polarizing plate was in contact with an iron rod with a diameter of 4mm. In the folded state, a load of 1kg was applied to the outside of the folded part, and the sample was placed in a 90°C oven for 2 hours, and then the sample was placed at room temperature, and the folded area was observed to confirm whether cracks occurred. The results are recorded in the following Tables 3 and 4.

[0171] <Evaluation Criteria>

[0172] -0 cracks: Good

[0173] -One or more cracks: Defective

[0174] [Table 3]

[0175]

[0176] [Table 4]

[0177]

[0178] Referring to the experimental data in Tables 3 and 4 above, in the case of Examples 1 to 8 of the variable transmittance optical stack of the embodiments of the present invention, the pencil hardness of the hard coating surface of the first polarizing plate and the second polarizing plate was measured to be 3B to 8H, the sum of the thickness of the first functional coating and the second functional coating was 2 to 50 μm, and the thickness of the liquid crystal layer and the height of the frame sealant were observed to be 2 to 20 μm. On the other hand, in the case of Comparative Examples 1 to 7 that are separated from the present invention, the pencil hardness or the sum of the thickness of the first functional coating and the second functional coating is less than or greater than the range disclosed in the present invention. In particular, in the case of Comparative Examples 1, 2, 4 and 5, in which both polarizing plates do not include a hard coating, it is observed that the height of the frame sealant is higher than the thickness of the liquid crystal layer. In addition, it is observed that the pencil hardness of the hard coating surface of the polarizing plate is less than the range disclosed in the present application in Comparative Example 6, and the sum of the thickness of the first functional coating and the second functional coating is greater than 50 μm in Comparative Example 7, in which the thickness of the liquid crystal layer is different from the height of the frame sealant. In this case, the reliability of the optical laminate may be reduced, such as light leakage between the liquid crystal layer and other substrates. In the reliability core rod evaluation, cracks were generated in Comparative Examples 1 to 7, while no cracks were observed in Examples 1 to 8 of the present invention. In particular, in the case of Comparative Example 3 where the sum of the pencil hardness and the thickness of the first functional coating and the second functional coating was greater than the range disclosed in the present invention, cracks were generated even though there was no difference in the thickness of the liquid crystal layer and the height of the frame sealant.

[0179] Therefore, it can be confirmed that the variable transmittance optical stack of the present invention and the smart window containing the same have a hardness of the first functional coating and the second functional coating that satisfies the range of 3B to 8H, and the sum of the thickness of the first functional coating and the second functional coating is 2 to 50 μm. Therefore, the height of the frame sealant after curing is 2 to 20 μm, which can ensure the same height of the frame sealant as the thickness of the liquid crystal layer below 20 μm, so no cracks are generated and the durability is excellent.

[0180] Industrial Applicability

[0181] According to the variable transmittance optical stack of the present invention, the hardness of the polarizer hard coating, that is, the functional coating, meets the range of 3B to 8H, and the sum of the thicknesses of the first polarizer and the second polarizer is 2 to 50 μm, thereby ensuring a frame sealant height of 2 to 20 μm, so that the frame sealant height is the same as the liquid crystal thickness, thereby improving the extrusion phenomenon and diffusion of the frame sealant, and preventing light leakage between the liquid crystal layer and other substrates to maintain a constant optical color within the plane.

Claims

1. A variable transmittance optical stack, comprising: A liquid crystal layer including a sealing adhesive; A first polarizing plate comprising a first functional coating and located on one side of the liquid crystal layer; a second polarizing plate including a second functional coating and located on the other side of the liquid crystal layer; a first transparent conductive layer formed between the first polarizing plate and the liquid crystal layer; as well as a second transparent conductive layer formed between the second polarizing plate and the liquid crystal layer, At least one of the first transparent conductive layer and the second transparent conductive layer is formed to be in direct contact with one of the first polarizing plate and the second polarizing plate. The surface pencil hardness of the first functional coating and the second functional coating is respectively 3B to 8H, The sum of the thicknesses of the first functional coating and the second functional coating is 2 to 50 μm. 2 . The variable transmittance optical stack according to claim 1 , wherein the height of the frame sealant after curing is 2 to 20 μm. 3 . The variable transmittance optical stack according to claim 1 , wherein the thickness of each of the first functional coating layer and the second functional coating layer is 1 to 35 μm. 4 . The variable transmittance optical layered body according to claim 1 , wherein each of the first functional coating layer and the second functional coating layer comprises at least one of a hard coating layer and a low refractive index layer. 5 . The variable transmittance optical laminate according to claim 4 , wherein the hard coat layer comprises an acrylate compound or an epoxy compound.

6. The variable transmittance optical laminate according to claim 4, wherein the low refractive index layer comprises a material selected from the group consisting of SiO 2 、Al 2 O 3 MgF 2 , CaF 2 One or more of the group consisting of and cryolite. 7 . The variable transmittance optical laminate according to claim 1 , wherein at least one of the first transparent conductive layer and the second transparent conductive layer is formed to be in direct contact with one of the first polarizing plate and the second polarizing plate without including a separate substrate therebetween. 8 . The variable transmittance optical laminate according to claim 1 , wherein at least one of the first transparent conductive layer and the second transparent conductive layer is formed to be in direct contact with one of the first polarizing plate and the second polarizing plate by including an easy-adhesion layer therebetween.

9. The variable transmittance optical stack according to claim 1, wherein at least one of the first transparent conductive layer and the second transparent conductive layer comprises one or more selected from the group consisting of transparent conductive oxides, metals, carbon-based materials, conductive polymers, conductive inks, and nanowires. 10 . The variable transmittance optical laminate according to claim 1 , wherein at least one of the first polarizing plate and the second polarizing plate comprises one or more selected from the group consisting of a protective layer, a phase difference adjusting layer, and a refractive index adjusting layer. 11 . The variable transmittance optical stack according to claim 1 , wherein at least one of the first polarizing plate and the second polarizing plate has a thickness of 30 to 200 μm. 12 . The variable transmittance optical stack according to claim 1 , wherein the liquid crystal layer includes one or more spacers selected from the group consisting of spherical spacers and columnar spacers. 13 . The variable transmittance optical stack according to claim 12 , wherein the height of the spacer is 2 to 20 μm. 14 . The variable transmittance optical stack according to claim 12 , wherein an area of ​​the spacer in the liquid crystal layer is 0.01% to 10% of an area of ​​the liquid crystal layer. 15 . The variable transmittance optical stack according to claim 1 , further comprising at least one selected from the group consisting of a sticking / adhesive layer, a UV absorbing layer, and an impact-resistant layer. 16 . A method for producing the variable transmittance optical layered body according to claim 1 . 17 . A smart window comprising the variable transmittance optical laminate according to claim 1 .

18. A vehicle comprising the smart window according to claim 17.

19. An automobile, wherein the smart window according to claim 17 is applied to at least one of a front window, a rear window, a side window, a skylight, and an interior partition.

20. A wearable device comprising the smart window according to claim 17.

21. A building window, comprising the smart window according to claim 17.