Method for manufacturing semiconductor device

A method using a light-irradiated resin layer in semiconductor manufacturing addresses the challenges of wafer protection and base material removal, improving the efficiency and effectiveness of semiconductor device production.

CN119096332APending Publication Date: 2024-12-06RESONAC CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202380036437.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-10-11
Filing Date
2023-10-06
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing methods for manufacturing semiconductor devices face challenges in effectively protecting the semiconductor wafer during back grinding and efficiently removing the base material layer without damaging the wafer.

Method used

A method involving the use of a resin layer containing a resin reduced in molecular weight by light irradiation, which is used to form a stack with a semiconductor wafer and a substrate layer, followed by back grinding and light irradiation to remove the substrate layer to produce semiconductor chips, including steps of back grinding and resin layer irradiation to facilitate easy removal of the base material layer.

Benefits of technology

The method provides effective protection for the semiconductor wafer during grinding and enables easy removal of the base material layer, enhancing the manufacturing process efficiency and chip production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119096332A_ABST
    Figure CN119096332A_ABST
Patent Text Reader

Abstract

The invention discloses a manufacturing method of a semiconductor device. The method for manufacturing a semiconductor device includes: a first laminate manufacturing step of manufacturing a first laminate including a semiconductor wafer, a resin layer including a resin that is reduced in molecular weight by irradiation with light, and a base material layer in this order; a second laminate manufacturing step for manufacturing a second laminate by grinding the back surface of the semiconductor wafer of the first laminate; and a third laminate manufacturing step of removing the base material layer of the second laminate and manufacturing a third laminate including the semiconductor wafer and the resin layer, the back surface of which has been ground.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing a semiconductor device. Background Art

[0002] In the manufacture of semiconductor devices, the following steps are usually performed: a pattern is formed on one side (surface, circuit formation side) of a semiconductor wafer, and the other side (back side) of the semiconductor wafer is ground to a predetermined thickness using a back grinding machine or the like. In the back grinding step, the following steps are usually performed for the purpose of protecting the semiconductor wafer: a back grinding tape is attached to the semiconductor wafer and the back side is ground (for example, Patent Document 1).

[0003] Previous technical literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2010-034379 Summary of the invention

[0006] Technical issues to be solved by the invention

[0007] An object of the present invention is to provide a novel method for manufacturing a semiconductor device including a step of grinding the back surface of a semiconductor wafer.

[0008] Means for solving technical problems

[0009] The present invention provides a method for manufacturing a semiconductor device according to [1] to [3].

[0010] [1] A method for manufacturing a semiconductor device, comprising:

[0011] The first stack production step is to produce a first stack comprising, in sequence, a semiconductor wafer, a resin layer containing a resin that has been de-molecularized by irradiation with light, and a substrate layer; the second stack production step is to perform back grinding on the semiconductor wafer of the first stack to produce a second stack; and the third stack production step is to remove the substrate layer of the second stack and produce a third stack comprising the semiconductor wafer and the resin layer that have been back ground.

[0012] [2] The method for manufacturing a semiconductor device according to [1], wherein:

[0013] The third laminate production step is a step of irradiating the resin layer of the second laminate with light to remove the base material layer.

[0014] [3] The method for manufacturing a semiconductor device according to [1] or 2, further comprising:

[0015] A step of manufacturing individual semiconductor chips with resin layer sheets by dicing the third stacked body.

[0016] Effects of the Invention

[0017] According to the present invention, a novel method for manufacturing a semiconductor device including a step of grinding the back surface of a semiconductor wafer is provided. According to the method for manufacturing a semiconductor device of the present invention, the semiconductor wafer can be sufficiently protected and a base material layer can be easily removed. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 is a schematic cross-sectional view for explaining one embodiment of a method for manufacturing a semiconductor device. Figure 1 middle, Figure 1 (a) Figure 1 (b) Figure 1 (c) Figure 1 (d) and Figure 1 (e) is a diagram showing each process.

[0019] Figure 2 is a schematic cross-sectional view for explaining one embodiment of a method for manufacturing a semiconductor device. Figure 2 middle, Figure 2 (a) Figure 2 (b) Figure 2 (c) and Figure 2 (d) is a diagram showing each process.

[0020] Figure 3 is a schematic cross-sectional view for explaining one embodiment of a method for manufacturing a semiconductor device. Figure 3 middle, Figure 3 (a) Figure 3 (b) Figure 3 (c) and Figure 3 (d) is a diagram showing each process. DETAILED DESCRIPTION

[0021] Hereinafter, the present embodiment will be described in detail with reference to the accompanying drawings. However, the present invention is not limited to the following embodiments. In the following embodiments, the constituent elements (including steps, etc.) are not necessary except for the cases specifically indicated. The same symbols are marked on the same or equivalent parts, and repeated descriptions are omitted. In addition, regarding the positional relationship such as up, down, left, and right, unless otherwise specified, they are all based on the positional relationship shown in the accompanying drawings. The sizes of the constituent elements in each figure are conceptual, and the relative relationship between the sizes of the constituent elements is not limited to those shown in the figures.

[0022] The same is true for the numerical values ​​and their ranges in the present invention, and the present invention is not limited thereto. In this specification, the numerical range represented by "~" represents the range containing the numerical values ​​recorded before and after "~" as the minimum and maximum values, respectively. In the numerical ranges recorded in stages in this specification, the upper limit or lower limit recorded in a numerical range can be replaced by the upper limit or lower limit of the numerical range recorded in other stages. Moreover, in the numerical ranges recorded in this specification, the upper limit or lower limit of its numerical range can also be replaced by the value shown in the embodiments.

[0023] In this specification, the term "layer" includes not only a structure of a shape formed on the entire surface but also a structure of a shape formed on a part when viewed from a top view. In this specification, the term "process" includes not only an independent process but also a process that can achieve the desired effect of the process even if it cannot be clearly distinguished from other processes.

[0024] In the present specification, (meth)acrylate refers to acrylate or its corresponding methacrylate. The same applies to other similar expressions such as (meth)acrylic copolymers.

[0025] Each component and material exemplified in the present specification may be used alone or in combination of two or more unless otherwise specified.

[0026] [Method for manufacturing semiconductor device]

[0027] A method for manufacturing a semiconductor device according to one embodiment of the present invention relates to a method for manufacturing a semiconductor device including a step of back grinding a semiconductor wafer. The method for manufacturing a semiconductor device includes a first stacked body manufacturing step, a second stacked body manufacturing step, and a third stacked body manufacturing step. The method for manufacturing a semiconductor device may further include a step of manufacturing a semiconductor chip with a resin layer. Figure 1 , Figure 2 and Figure 3 This is a schematic cross-sectional view for explaining one embodiment of a method for manufacturing a semiconductor device.

[0028] <First laminate production step>

[0029] In this process, a first laminate 10A is prepared, which includes a semiconductor wafer 1, a resin layer 3A containing a resin that is reduced in molecular weight by irradiation with light (hereinafter, sometimes referred to as a "photofusible resin"), and a base material layer 5. The photofusible resin can be a resin having properties such as reduced in molecular weight by irradiation with light, thereby reducing the elastic modulus and increasing the loss tangent (tanδ). In addition, the photofusible resin is a water-insoluble resin, and can be a gel-like or liquid-like resin that is reduced in molecular weight by irradiation with light and thus imparts water solubility.

[0030] In one embodiment, the photofusible resin may be a reaction product of a compound A having a disulfide bond and having two or more thiol groups and a compound B having two or more functional groups capable of reacting with a thiol group. In addition to the photofusible resin, the resin layer 3A may further include a photoradical generator. With regard to the resin layer 3A, for example, it can be formed by: a curing composition comprising compound A, compound B, a photoradical generator, and a curing accelerator that promotes the reaction of compound A and compound B as needed is arranged at a predetermined position, and the curing composition is cured by heating or light irradiation (compound A and compound B react). At this time, the resin layer 3A may include the following cured product: a cured product of a curing composition comprising compound A, compound B, a photoradical generator, and a curing accelerator that promotes the reaction of compound A and compound B as needed. The cured product of the curing composition may include a reaction product of compound A and compound B and a photoradical generator. The curing composition may be a thermosetting composition cured by heating, or a photocurable composition cured by light irradiation, but in one embodiment, it may be a thermosetting composition.

[0031] In one embodiment, the curable composition may contain compound A, compound B, a photoradical generator, and a curing accelerator that accelerates the reaction of compound A and compound B as needed.

[0032] (Compound A)

[0033] Compound A is a compound having a disulfide bond (-SS-) and having two or more thiol groups (-SH). The upper limit of the number of thiol groups of compound A may be, for example, 10 or less, 8 or less, 6 or less, or 4 or less. Regarding component (A), for example, it may be a dithiol compound of a compound having two thiol groups (-SH). Component (A) may be a high molecular weight component of a polymer or oligomer. A compound having two thiol groups (-SH) may be considered to be a compound comprising two thiol groups and a disulfide bond, and formed by a group (the first linking group) linked to the two thiol groups.

[0034] The molecular weight or number average molecular weight of compound A may be, for example, 100 to 10,000,000, 200 to 3,000,000, 300 to 1,000,000, 400 to 10,000, or 500 to 5,000. The number average molecular weight is a polystyrene conversion value obtained by gel permeation chromatography (GPC) using a calibration curve based on standard polystyrene.

[0035] Compound A has one or more (two or more) disulfide bonds in the molecule. The number of disulfide bonds in Compound A may be, for example, 1 to 1000 or 4 to 50.

[0036] Compound A may be a compound (e.g., a polymer or oligomer) having a linear or branched molecular chain and an end group, and having a disulfide bond in the molecular chain. In this case, the end group in compound A may be a thiol group. By including such a compound as compound A in the curable composition, the optical meltability of the optical meltable resin (the reaction product of compound A and compound B) tends to be further improved. The molecular chain in compound A may include a disulfide bond and a polyether chain, or may be formed by a disulfide bond and a polyether chain.

[0037] Compound A may be, for example, a compound represented by formula (1): HS-(XSS) n1 -X-SH (compound (1)). In the formula, X represents a polyether chain. A plurality of Xs may be the same or different. n1 represents an integer greater than 1. For example, n1 may be 1 or more or 4 or more, and may be 1000 or less. When the component (A) is a compound represented by the formula (1), -(XSS) n1 The group represented by -X- is the first linking group. The compound for chain-extending the compound (1) may be, for example, a Michael adduct of the compound (1) or a thiocarbamate of the compound (1).

[0038] The polyether chain as X may be, for example, a polyoxyalkylene chain. The polyether chain as X may be, for example, a 1 -OX 2 -OX 3 - represents a group. 1 ~X 3 Each of them independently may be an alkylene group, or may be an alkylene group having 1 to 2 carbon atoms (for example, methylene group, ethylene group). As for the polyether chain as X, for example, -CH2CH2-O-CH2-O-CH2CH2- and the like can be mentioned.

[0039] As commercially available products of compound A, for example, polysulfide rubber LP series (dithiol with disulfide bond, manufactured by TORAY FINE CHEMICALS CO., LTD.) etc. can be cited. Compound A can be obtained by converting the reactive functional group of a compound having a reactive functional group (e.g., carboxyl group, hydroxyl group) and a disulfide bond at the terminal into a thiol group. As compounds having a reactive functional group and a disulfide bond at the terminal, 3,3'-dithiodipropionic acid (manufactured by Tokyo Chemical Industry Co., Ltd.), dithiodiethanol, cystamine etc. can be cited.

[0040] The content of compound A may be 15 mass % or more, 25 mass % or more, or 35 mass % or more, and may be 80 mass % or less, 70 mass % or less, or 60 mass % or less, based on the total amount of the curable composition (solid content excluding the solvent).

[0041] (Compound B)

[0042] Compound B is a compound having two or more functional groups capable of reacting with a thiol group. As a functional group capable of reacting with a thiol group, for example, a cyclic ether group (oxirane group (oxiranyl group, epoxy group), oxetane group (oxetanyl group), tetrahydrofuranyl group, tetrahydropyranyl group, etc.), an isocyanate group; an ethylenically unsaturated group (C=C), etc. Regarding the upper limit of the number of functional groups of compound B, for example, it can be 10 or less, 8 or less, 6 or less, or 4 or less.

[0043] In one embodiment, compound B may be compound B1 having a polyether chain and having two or more cyclic ether groups. Since the curable composition includes compound B1 as compound B, the low molecular weight component generated by irradiating the photo-fusible resin with light has a large number of polyether chains or hydroxyl groups and tends to be water-soluble, and the low molecular weight component can be removed in an aqueous solvent.

[0044] From the viewpoint of reactivity and easy availability, cyclic ether group can be oxirane group. That is, compound B1 is an oxirane compound (epoxy compound) with a polyether chain and with more than 2 oxirane groups (oxiranyl, epoxy group). In addition, in this specification, in the cyclic ether group, a group with a cyclic ether structure (structure comprising a cyclic ether group) is included. For example, in the oxirane group, a group with an oxirane structure (structure comprising an oxirane group (oxiranyl, epoxy group)) such as a glycidyl group, a glycidyl ether group, an epoxycyclohexyl group is included.

[0045] The molecular weight or number average molecular weight of compound B1 may be, for example, 100 to 1,000,000, 100 to 500,000, 100 to 10,000, 150 to 5,000, or 200 to 2,000. The number average molecular weight is a polystyrene conversion value obtained by gel permeation chromatography (GPC) using a calibration curve based on standard polystyrene.

[0046] When the cyclic ether group of compound B1 is an oxirane group (oxiranyl group, epoxy group), the epoxy equivalent of component (B) may be 50 to 2000 g / eq, 80 to 1500 g / eq, or 100 to 1000 g / eq.

[0047] Compound B1 may be a compound B1a having two cyclic ether groups, or a compound B1b having three or more cyclic ether groups. Compound B1a may be a compound (e.g., a polymer or oligomer) having a linear molecular chain and an end group, and having a polyether chain in the molecular chain. At this time, the end group in compound B1a may be a cyclic ether group. Compound B1a can be regarded as a compound comprising two cyclic ether groups and a polyether chain, and formed by a group (the second linking group) linked to the two cyclic ether groups. Compound B1b may be a compound having one or more cyclic ether groups as a side chain or substituent of the second linking group in compound B1a. From the viewpoint of being able to further shorten the curing time and being able to further improve the optical solubility and water solubility, compound B1 may include both compound B1a and compound B1b.

[0048] Compound B1a can be a compound (e.g., a polymer or oligomer) having a linear molecular chain and an end group, and having a polyether chain in the molecular chain. At this time, the end group in compound B1a can be a cyclic ether group. When compound B is compound B1a, it has a tendency to become easy to remove low molecular components produced by irradiating light to the photofusible resin in an aqueous solvent. The polyether chain as a molecular chain can have a hydroxyl group and a substituent such as an alkyl group that can have a hydroxyl group. The molecular chain in compound B1a can include a polyether chain or can be composed of a polyether chain.

[0049] Compound B1a may be, for example, a compound represented by the formula (2): Z-(Y) n2 -Z represents a compound (compound (2)). In the formula, Y represents a polyether chain, and Z represents a cyclic ether group. Multiple Zs may be the same or different. n2 represents an integer greater than 1. For example, n2 may be greater than 1 or greater than 2, and may be less than 1000. When compound B1a is compound (2), -(Y) n2 The group represented by - is the second linking group.

[0050] The polyether chain as Y may be, for example, a polyoxyalkylene chain. 1 -OY 2 -OY 3 -represented by a group. 1 ~Y 3 Each of them independently may be an alkylene group, or may be an alkylene group having 1 to 3 carbon atoms (for example, methylene, ethylene, propylene). As for the polyether chain as Y, for example, -CH2CH2-O-CH2-CH2-O-CH2CH2- and the like can be mentioned.

[0051] Examples of commercially available products of compound B1a include DENACOL EX series (EX-850, EX-851, EX-821, EX-830, EX-832, EX-841, EX-861, and EX-920, manufactured by Nagase ChemteX Corporation).

[0052] Compound B1b may be a compound having one or more cyclic ether groups as side chains of the second linking group (polyether chain as Y) in compound B1a.

[0053] Examples of commercially available products of compound B1b include DENACOL EX series (EX-614B, EX-313, EX-512, and EX-521, manufactured by Nagase ChemteX Corporation).

[0054] The mass ratio of the content of compound B1b to the total content of compound B1a and compound B1b (content (mass) of compound B1b / total content (mass) of compound B1a and compound B1b) may be 0.01 to 0.40. If the mass ratio is 0.01 or more, there is a tendency that the curing time of the curable composition can be further shortened, and if the mass ratio is 0.40 or less, there is a tendency that the optical melting property and water solubility can be further improved. The mass ratio may be 0.02 or more or 0.03 or more, and may be 0.35 or less, 0.30 or less, 0.25 or less, 0.20 or less, 0.15 or less, or 0.10 or less.

[0055] The content of compound B may be 10 mass % or more, 20 mass % or more, or 30 mass % or more, and 60 mass % or less, 50 mass % or less, or 40 mass % or less, based on the total amount of the curable composition (solid content excluding the solvent).

[0056] The ratio of the total number of moles of thiol groups in compound A to the total number of moles of functional groups in compound B may be, for example, 0.90 or more or 0.95 or more and 1.10 or less or 1.05 or less.

[0057] (Photoradical Generator)

[0058] The photoradical generator is a component that generates free radicals by light irradiation. As the photoradical generator, for example, a component used as a photopolymerization initiator can be used. As the photoradical generator, there can be mentioned an intramolecular cleavage type photoradical polymerization initiator in which the substance itself is photo-cleaved by light irradiation to generate two free radicals.

[0059] Examples of the intramolecular cleavage type photoradical generator include benzyl ketal photoradical generators, α-aminoalkylphenone photoradical generators, α-hydroxyalkylphenone photoradical generators, α-hydroxyacetophenone photoradical generators, and acylphosphine oxide photoradical generators.

[0060] Examples of the benzyl ketal-based photoradical generator include 2,2-dimethoxy-1,2-diphenylethane-1-one (Omnirad 651) and the like.

[0061] Examples of α-aminoalkylphenone-based photoradical generators include 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1 (Omnirad369), 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropane-1-one (Omnirad907), and 2-dimethylamino-2-(4-methyl-benzyl)-1-(4-morpholino-4-yl-phenyl)-butane-1-one (Omnirad379EG).

[0062] Examples of the α-hydroxyalkylphenone-based photoradical generator include 1-hydroxy-cyclohexyl-phenyl-ketone (Omnirad 184) and the like.

[0063] Examples of the α-hydroxyacetophenone-based photoradical generator include 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]-phenyl}-2-methyl-propane-1-one (Omnirad127) and 2-hydroxy-2-methyl-1-phenyl-propane-1-one (Omnirad1173).

[0064] Examples of the acylphosphine oxide-based photoradical generator include 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide (Omnirad TPO H) and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (Omnirad 819).

[0065] The content of the photoradical generator may be 1 mass % or more, 3 mass % or more, or 5 mass % or more, and may be 30 mass % or less, 20 mass % or less, or 15 mass % or less, based on the total amount of the curable composition (solid content excluding the solvent).

[0066] From the viewpoint of further improving the photosensitivity, the ratio of the mole number of the photoradical generator to the mole number of the compound A (mole number of the photoradical generator / mole number of the compound A) may be 0.1 or more, 0.2 or more, or 0.3 or more.

[0067] (Curing accelerator)

[0068] The curing accelerator is a component for accelerating the reaction between compound A and compound B, and includes a component that functions as a catalyst for the curing reaction (catalyst-type curing agent). Examples of the curing accelerator include amine compounds, imidazole derivatives, quaternary ammonium salts, organic metal salts, phosphorus compounds, and the like.

[0069] Examples of the amine compound include dicyandiamide, trimethylamine, triethylamine, tripropylamine, tributylamine, tri-n-octylamine, dimethylethylamine, dimethylpropylamine, dimethylbutylamine, dimethyl-n-octylamine, 1,4-diazabicyclo[2.2.2]octane, 1,8-diazabicyclo[5.4.0]undec-7-ene, benzyldimethylamine, 4-methyl-N,N-dimethylbenzylamine, 2,4,6-tris(dimethylaminomethyl)phenol, and 4-dimethylaminopyridine.

[0070] Examples of the imidazole derivatives include 1-(1-cyanomethyl)-2-ethyl-4-methyl-1H-imidazole, 2-ethyl-4-methylimidazole, 2-methylimidazole, 2-phenylimidazole, 1-cyanoethyl-2-phenylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2,4,5-triphenylimidazole, 1-benzyl-2-imidazole, 1,2-dimethylimidazole, and 1-benzyl-2-phenylimidazole.

[0071] Examples of the quaternary ammonium salt include tetramethylammonium chloride, tetraethylammonium chloride, tetrabutylammonium chloride, benzyltrimethylammonium chloride, benzyltriethylammonium chloride, benzyltributylammonium chloride, tetramethylammonium bromide, tetraethylammonium bromide, tetrabutylammonium bromide, benzyltrimethylammonium bromide, benzyltriethylammonium bromide, tetramethylammonium iodide, tetraethylammonium iodide, tetrabutylammonium iodide, and benzyltributylammonium iodide.

[0072] Examples of the organic metal salt include organic metal salts such as bis(2,4-pentanedione)zinc(II), zinc octylate, zinc naphthenate, cobalt naphthenate, copper naphthenate, iron acetylacetonate, nickel octylate, and manganese octylate.

[0073] Examples of the phosphorus compound include sodium tetraphenylphosphonium tetra-p-tolylborate, tetraphenylphosphonium tetraphenylborate, triphenylphosphine, tri-p-tolylphosphine, tri(4-chlorophenyl)phosphine, tri(4-methoxyphenyl)phosphine, tri(2,6-dimethoxyphenyl)phosphine, triphenylphosphine triphenylborane, tetraphenylphosphonium dicyanimide, and tetraphenylphosphonium tetra(4-methylphenyl)borate.

[0074] The content of the curing accelerator may be 0.01 mass % or more, 0.1 mass % or more, or 0.5 mass % or more, and may be 10 mass % or less, 5 mass % or less, or 2 mass % or less, based on the total amount of the curable composition (solid content excluding the solvent).

[0075] The curable composition may further include compound A, compound B, a photoradical generator, and components (other components) that do not conform to the curing accelerator. As other components, for example, plasticizers, adhesiveness imparting agents such as tackifiers, antioxidants, leuco dyes, sensitizers, adhesion improvers such as coupling agents, polymerization inhibitors, light stabilizers, defoamers, fillers, chain transfer agents, thixotropy imparting agents, flame retardants, release agents, surfactants, lubricants, antistatic agents and other additives can be used for these additives. Known additives can be used. When the curable composition includes other components, the total amount of the content of the other components is based on the total amount of the curable composition, and can be 0 to 95% by mass, 0.01 to 50% by mass, or 0.1 to 10% by mass.

[0076] The curable composition can be used as a varnish of the curable composition diluted with a solvent. As the solvent, for example, aromatic hydrocarbons such as toluene, xylene, mesitylene, cumene, and p-cymene; aliphatic hydrocarbons such as hexane and heptane; cycloalkanes such as methylcyclohexane; cyclic ethers such as tetrahydrofuran and 1,4-dioxane; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, and 4-hydroxy-4-methyl-2-pentanone; esters such as methyl acetate, ethyl acetate, butyl acetate, methyl lactate, ethyl lactate, and γ-butyrolactone; carbonates such as ethylene carbonate and propylene carbonate; amides (NMP) such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone. The content of the solid content in the varnish, that is, the content other than the solvent in the varnish, can be 10 to 95% by mass, 15 to 70% by mass, or 20 to 50% by mass based on the total amount of the varnish.

[0077] The first stacked body manufacturing step is not particularly limited as long as the first stacked body having the semiconductor wafer 1, the resin layer 3A and the base material layer 5 in sequence can be obtained. In one embodiment, the first stacked body manufacturing step may include: a step of preparing the semiconductor wafer 1; a step of disposing a curable composition comprising compound A, compound B, a photoradical generator and a curing accelerator for accelerating the reaction of compound A and compound B on the semiconductor wafer 1 to form a curable composition layer 3 comprising the curable composition (see Figure 1 (a)); a step of configuring a substrate layer 5 on the curable composition layer 3 to prepare a laminate 10 (reference Figure 1and the laminate 10 is heated to cure the curable composition layer 3 to form a resin layer 3A comprising a cured product of the curable composition (reference Figure 1 (c)) The resin layer 3A may also contain a reaction product of the compound A and the compound B (photofusible resin) and a photoradical generator.

[0078] In other embodiments, the first stack production process may include: a process of preparing a substrate layer 5; a process of configuring a curing composition comprising compound A, compound B, a photoradical generator, and a curing accelerator that promotes the reaction of compound A and compound B as needed on the substrate layer 5 to form a curing composition layer 3; a process of bonding the curing composition layer 3 disposed on the substrate layer 5 and the semiconductor wafer 1 to produce a stack 10; and a process of heating the stack 10 to cure the curing composition layer 3 to form a resin layer 3A comprising a cured product of the curing composition.

[0079] Examples of the semiconductor wafer 1 include single crystal silicon, polycrystalline silicon, various ceramics, and compound semiconductors such as gallium arsenide. The semiconductor wafer 1 may have a circuit formation surface.

[0080] The thickness d1 of the semiconductor wafer 1 may be, for example, 50 to 3000 μm, 100 to 2000 μm, or 200 to 1500 μm.

[0081] The curable composition can be prepared, for example, by a method including the step of mixing or kneading the above-mentioned components. The mixing and kneading can be performed by appropriately combining a common disperser such as a stirrer, a pestle, a three-roll mill, a ball mill, or a bead mill.

[0082] There is no particular limitation on the method of configuring the curable composition on the semiconductor wafer, but for example, there can be cited a method of applying the curable composition on the semiconductor wafer 1 using a spin coater, a rod coater, etc., a method of forming the curable composition into a film and attaching the formed curable composition film to the semiconductor wafer 1 (transfer), etc. The curable composition film can be in a semi-cured state (B stage state) before the curable composition film is bonded to the semiconductor wafer 1. Regarding the curable composition, for example, it can be configured on the circuit formation surface of the semiconductor wafer 1.

[0083] The thickness of the curable composition layer 3 may be, for example, 10 to 1000 μm, 30 to 750 μm, or 50 to 500 μm.

[0084] As the substrate layer 5, for example, there can be cited polyolefin films such as polyethylene (PE) and polypropylene (PP); polyester films such as polyethylene terephthalate (PET), polybutylene terephthalate (PBT), and polyethylene naphthalate; polyvinyl chloride (PVC) films; polyimide (PI) films; polyphenylene sulfide (PPS) films; ethylene vinyl acetate (EVA) films; polytetrafluoroethylene (PTFE) films, etc.

[0085] The thickness of the base material layer 5 may be, for example, 10 to 1000 μm, 30 to 500 μm, or 50 to 200 μm.

[0086] About curable composition, for example, can form the solidified material of curable composition by heating.By heating curable composition, compound A and compound B are reacted.At this time, curing accelerator can promote reaction.About the reaction product (light-melting resin) of compound A and compound B, for example, can be the compound (polymer) of the structure represented by the following formula.On the other hand, the participation of light free radical generator in the reaction is small, and the solidified material of curable composition can include the reaction product (light-melting resin) of compound A and compound B and light free radical generator.

[0087]

[0088] In the formula, X represents the first linking group, and Y represents the second linking group. m represents an integer greater than 1. For example, m may be greater than 50, greater than 100, greater than 500, or greater than 1000. * represents an atomic bonding.

[0089] The heating temperature of the laminate 10 (curable composition layer 3) may be, for example, 0 to 200° C., 30 to 150° C., or 60 to 100° C. The heating time of the curable composition may be, for example, 0.1 to 168 hours, or 72 hours or less, 48 ​​hours or less, or 24 hours or less.

[0090] The resin layer 3A may be in a (completely) cured state (C-stage state). The thickness of the resin layer 3A may be, for example, 10 to 1000 μm, 30 to 500 μm, or 50 to 200 μm.

[0091] In this manner, the first laminate 10A including the semiconductor wafer 1 , the resin layer 3A containing the photofusible resin, and the base material layer 5 in this order can be manufactured.

[0092] <Second laminate production step>

[0093] In this step, the semiconductor wafer 1 of the first stack 10A is back-ground to produce the second stack 20 (see Figure 1 (d)). The base layer 5 and the resin layer 3A of the first stack 10A can be regarded as a back grinding tape 7 having the base layer 5 and the resin layer 3A provided on the base layer 5. The first stack 10A can be attached with the back grinding tape 7 on the semiconductor wafer 1, and the first stack 10A can be directly used in the back grinding (back grinding) process.

[0094] The back grinding of the semiconductor wafer 1 can be performed using a conventional back grinding machine. Figure 1 As shown in (d), the semiconductor wafer 1 is thinned using, for example, a grinder 9 on the surface of the semiconductor wafer 1 opposite to the surface to which the back grinding tape 7 is attached.

[0095] The thickness d1A of the semiconductor wafer (semiconductor wafer 1A) subjected to back grinding is thinner than the thickness d1 of the semiconductor wafer 1 , and may be, for example, 10 to 1000 μm, 20 to 900 μm, or 30 to 800 μm.

[0096] In this manner, the second laminated body 20 including the semiconductor wafer 1A, the resin layer 3A containing the photofusible resin, and the base material layer 5 in this order can be manufactured.

[0097] <Third laminate production step>

[0098] In this step, the base layer 5 of the second stack 20 is removed to produce a third stack 30 including the semiconductor wafer 1A and the resin layer 3A. This step may be a step of irradiating the resin layer 3A of the second stack 20 with light A to remove the base layer 5 (see Figure 2 (a)) The photofusible resin contained in the resin layer 3A can easily remove the base material layer 5 from the second laminate 20 from the viewpoint of reducing the molecular weight by irradiation with the light A and thereby providing a gel-like or liquid-like substance.

[0099] The mechanism of low molecular weight (melting) of photofusible resin is not always obvious, but for example, the following mechanism can be considered. However, it is not limited to these mechanisms. The photofusible resin contains a compound having a disulfide bond (the reaction product of compound A and compound B). The disulfide bonds in the photofusible resin are decomposed (cracked) by light irradiation of the photofusible resin contained in the resin layer, and sulfur radicals are generated. At this time, if there is a photoradical generator (intramolecular cleavage type photoradical generator), the sulfur radical reacts with the photoradical generator, and the sulfur radical is capped by the photoradical generator. Thus, it can be considered that the compound with a disulfide bond is low molecular weight and the cured product is photo-softened (photo-melted). As another mechanism, it can also be considered that the photoinduced radical caused by the photoradical generator (intramolecular cleavage type photoradical generator) directly reacts with the disulfide bond, causing the formation of a photoinduced radical-thioether bond and the generation of a sulfur radical, and the sulfur radical reacts with another photoinduced radical, and the compound with a disulfide bond itself is low molecular weight and softens the photocured material. The disulfide bond cleavage reaction can be said to be an irreversible reaction.

[0100] The light A irradiated to the resin layer 3A may be, for example, ultraviolet light or visible light. The wavelength of the light A may be appropriately selected, for example, according to the type of the photo-radical generator used. The wavelength of the light A may be, for example, 150 to 830 nm. The light A may include, for example, light having a wavelength of 405 nm or a wavelength of 365 nm.

[0101] Regarding the irradiation of light A, for example, a light irradiation device can be used and the irradiation amount can be set to 1000 mJ / cm 2 The above conditions are performed. The irradiation amount can be appropriately set according to, for example, the wavelength of light A. For example, the irradiation amount can be 3000 mJ / cm 2 Above, 5000mJ / cm 2 Above or 10000mJ / cm 2 Above, and can be 100000mJ / cm 2 Below, 80000mJ / cm 2 Below, or 60000mJ / cm 2 the following.

[0102] The irradiation amount is the product of the illuminance and the irradiation time (seconds). Examples of the light source for irradiation with ultraviolet light or visible light include low-pressure mercury lamps, medium-pressure mercury lamps, high-pressure mercury lamps, metal halide lamps, and LED lamps.

[0103] The irradiation with light A can be performed under the condition that the resin layer 3A near the interface between the resin layer 3A and the substrate layer 5 is optically melted from the substrate layer 5 side (via the substrate layer 5), and the entire resin layer 3A is not optically melted. Thus, the substrate layer 5 can be easily removed, and the remaining resin layer 3A can be used as a protective layer for the semiconductor wafer 1A after the next process.

[0104] This step may be a step of removing the base layer 5 without irradiating the resin layer 3A of the second laminate 20 with light A. As such a method, for example, a method of attaching a support tape to the base layer 5 and stretching the support tape to peel the base layer 5 from the resin layer 3A can be cited.

[0105] In this manner, the third stacked body 30 including the semiconductor wafer 1A and the resin layer 3A containing the photofusible resin can be manufactured.

[0106] <Process for manufacturing semiconductor chips with resin layers>

[0107] In this step, the third stacked body 30 is diced to produce individual semiconductor chips 15 with resin layers.

[0108] The process of manufacturing a semiconductor chip with a resin layer sheet may include, for example, a step of preparing a stacked body 40 having a dicing tape 11, a semiconductor wafer 1A, and a resin layer 3A in sequence (see Figure 2 and in the laminate 40, at least by cutting the semiconductor wafer 1A and the resin layer 3A, and obtaining a single-piece semiconductor chip 15 with a resin layer (reference Figure 2 (d)).

[0109] As the dicing tape 11, for example, plastic films such as polytetrafluoroethylene film, polyethylene terephthalate film, polyethylene film, polypropylene film, polymethylpentene film, polyimide film, etc. can be cited. In addition, the dicing tape can also be subjected to surface treatments such as primer coating, UV treatment, corona discharge treatment, grinding treatment, etching treatment, etc. as needed. The dicing tape can have adhesiveness. This dicing tape can impart adhesiveness to the above-mentioned plastic film, or it can be a dicing tape with a pressure-sensitive adhesive layer provided on one side of the above-mentioned plastic film. The pressure-sensitive adhesive layer can be formed by a UV-curable or UV-non-curable pressure-sensitive pressure-sensitive adhesive. As long as it has sufficient adhesive force to prevent the semiconductor elements from flying apart during dicing, there is no particular limitation, and a previously known pressure-sensitive adhesive layer can be used.

[0110] The thickness of the dicing tape 11 may be, for example, 10 to 1000 μm, 30 to 500 μm, or 50 to 300 μm.

[0111] The stacked body 40 can be obtained by attaching the dicing tape 11 to the semiconductor wafer 1A of the third stacked body 30 .

[0112] Next, in the stacked body 40, at least the semiconductor wafer 1A and the resin layer 3A (and a portion of the dicing tape 11) are cut and singulated. The cutting may be, for example, cutting by a dicing blade 13. The cutting by the dicing blade 13 may be performed using a commercially available device. The cutting by the dicing blade 13 may be performed, for example, in a grid-shaped cutting pattern when viewed from above with respect to the semiconductor wafer 1A and the resin layer 3A.

[0113] From the viewpoint of suppressing the temperature rise of the contact portion between the semiconductor wafer 1A or the resin layer 3A and the dicing blade 13, the dicing by the dicing blade 13 is usually performed while spraying cooling water (cutting water) on these contact portions. From the viewpoint that the optically fusible resin is a water-insoluble resin, the resin layer 3A can fully suppress the dissolution of the resin layer caused by the cooling water (cutting water), and can function as a protective layer to prevent the cuttings (chips) from adhering to the circuit formation surface of the semiconductor wafer.

[0114] As for the cutting instead of the blade cutting, for example, it may be plasma cutting, stealth cutting, or laser cutting.

[0115] In this manner, the semiconductor wafer 1A and the resin layer 3A can be singulated separately to obtain the semiconductor chip 15 with the resin layer sheet including the semiconductor chip 1Aa and the resin layer sheet 3Aa.

[0116] The shape of the semiconductor chip 1Aa in plan view may be, for example, a square or a rectangle. The area of ​​the semiconductor chip 1Aa may be, for example, 1 to 250 mm. 2 , 4~200mm 2 , or 9~150mm 2 The length of one side of the semiconductor chip 1Aa may be greater than 1 mm, greater than 2 mm, or greater than 3 mm, and may be less than 20 mm, less than 18 mm, or less than 15 mm. The thickness of the semiconductor chip 1Aa may be the same as the thickness of the semiconductor wafer 1A.

[0117] The manufacturing method of the semiconductor device of the present embodiment may further include: a resin layer removal step of irradiating the resin layer 3Aa of the semiconductor chip 15 with the resin layer with light B to remove the resin layer 3Aa from the semiconductor chip 15 with the resin layer; an ultraviolet irradiation step of irradiating the pressure-sensitive adhesive layer of the dicing tape 11 with ultraviolet rays; a picking up step of picking up the semiconductor chip 1Aa; a semiconductor chip bonding step of bonding the picked up semiconductor chip 1Aa and the supporting component 19 by thermal compression bonding via an adhesive layer 21 (grain bonding film, etc.); and a thermal curing step of thermally curing the adhesive layer 21, etc.

[0118] <Resin layer removal process>

[0119] In this step, the resin layer sheet 3Aa of the semiconductor chip 15 with the resin layer sheet is irradiated with light B, and the resin layer sheet 3Aa is removed from the semiconductor chip 15 with the resin layer sheet (see Figure 3 (a)) Since the light-melting resin contained in the resin layer 3Aa is reduced in molecular weight by irradiation with light B and thus becomes a gel or liquid, the resin layer 3Aa can be easily removed from the semiconductor chip 15 with the resin layer.

[0120] The light B irradiated to the resin layer sheet 3Aa may be the same as the light A irradiated to the resin layer 3A, and may be, for example, ultraviolet light or visible light. The wavelength of the light B may be appropriately selected, for example, according to the type of the photo-radical generator used. The wavelength of the light B may be, for example, 150 to 830 nm. The light B may include, for example, light having a wavelength of 405 nm or a wavelength of 365 nm.

[0121] Regarding the irradiation of light B, for example, a light irradiation device can be used to set the irradiation amount to 1000 mJ / cm 2 The irradiation dose can be appropriately set, for example, according to the wavelength of the light B. For example, the irradiation dose can be 3000 mJ / cm 2 Above, 5000mJ / cm 2 Above or 10000mJ / cm 2 Above, and can be 100000mJ / cm 2 Below, 80000mJ / cm 2 Below, or 60000mJ / cm 2 the following.

[0122] In one embodiment, the resin layer sheet removal step may be a step of removing the resin layer sheet 3Aa from the semiconductor chip 15 with the resin layer sheet using an aqueous solvent. From the viewpoint of reducing the molecular weight by irradiating light and thereby providing a gel or liquid substance, the photofusible resin contained in the resin layer sheet 3Aa can be fully removed by washing with an aqueous solvent.

[0123] Examples of the aqueous solvent include water, a mixed solvent of water and a hydrophilic organic solvent, etc. In the mixed solvent of water and a hydrophilic organic solvent, the proportion of water can be, for example, 80% by mass or more. For example, a pH adjuster can be added to the aqueous solvent.

[0124] The aqueous solvent can be water. As water, for example, tap water, natural water, purified water, distilled water, ion exchanged water, pure water, ultrapure water (Milli-Q water, etc.) can be cited. In addition, Milli-Q water refers to ultrapure water obtained by the Milli-Q water manufacturing device of Merck Millipore (Merck KGaA). From the viewpoint of impurity reduction, water can be purified water, distilled water, ion exchanged water, pure water, or ultrapure water.

[0125] Examples of the hydrophilic organic solvent include alcohols such as methanol, ethanol, 2-propanol, and 1,2-propylene glycol; and glycol ethers such as ethylene glycol monomethyl ether, propylene glycol monomethyl ether, ethyl cellosolve, propylene glycol monopropyl ether, propylene glycol monoisopropyl ether, butyl cellosolve, ethylene glycol monoisobutyl ether, propylene glycol monobutyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, and dipropylene glycol monomethyl ether.

[0126] As the pH adjusting agent, inorganic acids, inorganic bases, organic acids, organic bases, etc. can be mentioned. As inorganic acids, nitric acid, sulfuric acid, hydrochloric acid, phosphoric acid, boric acid, etc. can be mentioned. As inorganic bases, sodium hydroxide, potassium hydroxide, calcium hydroxide, etc. can be mentioned. As organic acids, formic acid, acetic acid, propionic acid, butyric acid, acrylic acid, benzoic acid, picolinic acid, etc. can be mentioned. As organic bases, primary amines, secondary amines, tertiary amines, tetramethylammonium hydroxide, tetraethylammonium hydroxide, imidazole compounds, etc. can be mentioned.

[0127] In one embodiment, the resin layer removal step may be a step of irradiating the resin layer 3Aa with light B from the semiconductor chip 15 with the resin layer in the aqueous solvent 17 (see Figure 3 (b)). The photofusible resin contained in the resin layer 3Aa is reduced in molecular weight by irradiation with light, thereby providing a gel or liquid substance. Therefore, by irradiating the resin layer 3Aa with light B in the aqueous solvent 17, the gel or liquid substance flows out in the aqueous solvent 17, and the resin layer 3Aa can be removed efficiently.

[0128] In this manner, a plurality of semiconductor chips 1Aa (see FIG. 1A ) in which adhesion of cut materials (chips) is sufficiently suppressed can be obtained from the semiconductor wafer 1A. Figure 3 (c)).

[0129] <Ultraviolet irradiation process>

[0130] When the pressure-sensitive adhesive layer of the dicing tape 11 is composed of a UV-curable pressure-sensitive adhesive, the method for manufacturing a semiconductor device may include an ultraviolet irradiation step. In this step, the pressure-sensitive adhesive layer is irradiated with ultraviolet rays. In the ultraviolet irradiation, the wavelength of the ultraviolet rays may be 200 to 400 nm. In the ultraviolet irradiation conditions, the illumination and the irradiation amount may be 30 to 240 mW / cm 2 The range is 50~500mJ / cm 2 range.

[0131] <Pick-up process>

[0132] In this step, the individualized semiconductor chips 1Aa are separated from each other, and the semiconductor chips 1Aa pushed up from the dicing tape 11 side by the needles are sucked by a suction chuck and picked up from the dicing tape 11 .

[0133] The ultraviolet irradiation step and the pickup step may be performed after the resin layer sheet removal step or may be performed before the resin layer sheet removal step.

[0134] <Semiconductor chip bonding process>

[0135] In this step, the picked-up semiconductor chip 1Aa and the support member 19 are bonded by thermocompression via an adhesive layer 21 (die bonding film, etc.). The die bonding film can be a die bonding film used in this field. A plurality of semiconductor chips 1Aa can be bonded to the support member 19.

[0136] The heating temperature during the thermocompression bonding may be, for example, 80 to 160° C. The load during the thermocompression bonding may be, for example, 5 to 15 N. The heating time during the thermocompression bonding may be, for example, 0.5 to 20 seconds.

[0137] <Thermosetting process>

[0138] In this step, the adhesive layer 21 is thermally cured. The heating temperature can be appropriately changed according to the constituent components of the die bonding film. The heating temperature can be, for example, 60 to 200° C., 90 to 190° C., or 120 to 180° C. The heating time can be 30 minutes to 5 hours, 1 to 3 hours, or 2 to 3 hours. In addition, the temperature or pressure can be changed in stages.

[0139] In this manner, a semiconductor device 50 including a semiconductor chip 1Aa, a support member 19 on which the semiconductor chip 1Aa is mounted, and an adhesive layer 21 provided between the semiconductor chip 1Aa and the support member 19 to bond the semiconductor chip 1Aa and the support member 19 can be manufactured (see Figure 3 (d)).

[0140] According to the method for manufacturing a semiconductor device of the present invention, the semiconductor wafer can be sufficiently protected and the base layer can be easily removed.

[0141] Explanation of symbols

[0142] 1. 1A-semiconductor wafer, 1Aa-semiconductor chip, 3-curable composition layer, 3A-resin layer, 3Aa-resin layer sheet, 5-base layer, 7-back grinding tape, 9-grinder, 10-laminated body, 10A-first laminated body, 11-dicing tape, 13-dicing blade, 15-semiconductor chip with resin layer sheet, 17-aqueous solvent, 19-support member, 20-second laminated body, 21-adhesive layer, 30-third laminated body, 40-laminated body, 50-semiconductor device.

Claims

1. A method for manufacturing a semiconductor device, comprising: a first laminate manufacturing step of manufacturing a first laminate including, in order, a semiconductor wafer, a resin layer including a resin reduced in molecular weight by irradiation with light, and a base material layer; a second stacked body manufacturing step of performing back grinding on the semiconductor wafer of the first stacked body to manufacture a second stacked body; and The third stacked body manufacturing step is to remove the base layer of the second stacked body and manufacture a third stacked body including the semiconductor wafer and the resin layer that have been back-ground.

2. The method for manufacturing a semiconductor device according to claim 1, wherein: The third laminate production step is a step of irradiating the resin layer of the second laminate with light to remove the base material layer.

3. The method for manufacturing a semiconductor device according to claim 1 or 2, further comprising: The step of manufacturing a semiconductor chip with a resin layer is to manufacture individual semiconductor chips with a resin layer by dicing the third stacked body.

Citation Information

Patent Citations

  • Back grinding tape

    JP2010034379A