Adhesive film for semiconductor, dicing die bonding film, and method for manufacturing semiconductor device

By using a characteristic-optimized adhesive film during the thermal curing process, the thickness direction deformation of the adhesive film is suppressed, and the problem of semiconductor chip cracks caused by the deformation of the adhesive film in the prior art is solved, thereby achieving more stable chip connections.

CN119096359APending Publication Date: 2024-12-06RESONAC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380029855.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-03-24
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing adhesive film is prone to local deformation in the thickness direction during the thermal curing process, resulting in the possibility of cracks in the semiconductor chip.

Method used

A thermosetting semiconductor adhesive film containing epoxy resin, curing agent, imidazole compound, and inorganic was developed, which exhibited a maximum tanδ value of 1.0 or less and a minimum melt viscosity of 10,000 Pa·s, in the range of 90 to 180°C. The filler and the elastomer are composed of a dynamic viscoelastic characteristic measured at a temperature increase of 5°C/min and a frequency of 1 Hz to suppress deformation of the thickness direction of the adhesive film.

Benefits of technology

It effectively suppresses local deformation of the adhesive film in the thickness direction during the thermal curing process, improves the stability of the semiconductor chip and the effect of buried wires, and avoids the occurrence of cracks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119096359A_ABST
    Figure CN119096359A_ABST
Patent Text Reader

Abstract

An adhesive film for a semiconductor is used to adhere a semiconductor chip to an adherend while embedding a lead wire connected to another semiconductor chip. When the dynamic viscoelasticity of the adhesive film in the range of 90-180 DEG C is measured under the conditions of a temperature rise rate of 5 DEG C / min and a frequency of 1 Hz, the maximum value of tan [delta] is 1.0 or less, and the minimum melt viscosity is 10000 Pa.s or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an adhesive film for semiconductor, a dicing / die-bonding film and a method for manufacturing a semiconductor device. Background Art

[0002] Sometimes, it is necessary to embed wires connected to other semiconductor chips through a semiconductor adhesive film for bonding a semiconductor chip to an adherend (e.g., Patent Document 1). In order to properly embed the wires, such a wire embedding adhesive film is required to have a certain degree of high fluidity during its thermal curing process.

[0003] Previous technical literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent No. 6135202 Summary of the invention

[0006] Technical issues to be solved by the invention

[0007] However, conventional adhesive films having a certain degree of high fluidity deform in the thickness direction during the thermal curing process, resulting in a partially thinned portion of the adhesive film. The partially thinned portion of the adhesive film may cause cracks in the semiconductor chip, for example.

[0008] One aspect of the present invention relates to suppressing local deformation in the thickness direction of a thermosetting adhesive film for semiconductors used to bond a semiconductor chip to an adherend while embedding a wire connected to another semiconductor chip.

[0009] Means for solving technical problems

[0010] One aspect of the present invention relates to a thermosetting semiconductor adhesive film, which is used to bond a semiconductor chip to an adherend while embedding a wire connected to another semiconductor chip. The adhesive film shows a maximum tanδ value of 1.0 or less and a minimum melt viscosity of 10000 Pa·s or less in the range of 90 to 180°C. The maximum tanδ value and the minimum melt viscosity are values ​​obtained by measuring the dynamic viscoelasticity of the adhesive film under the conditions of a heating rate of 5°C / min and a frequency of 1 Hz.

[0011] Another aspect of the present invention relates to a dicing die bonding film including a dicing film and the above-mentioned adhesive film for a semiconductor provided on the dicing film.

[0012] Another aspect of the present invention relates to a method for manufacturing a semiconductor device, the method comprising the following steps: arranging a second semiconductor chip and an adhesive film on a structure having a substrate and a first semiconductor chip mounted on the substrate in such a manner that the adhesive film is interposed between the structure and the second semiconductor chip; and thermally curing the adhesive film to thereby adhere the second semiconductor chip to the structure. The adhesive film may be the above-mentioned adhesive film for semiconductors. A wire is connected to the first semiconductor chip, and a part or the entirety of the wire is buried through the adhesive film.

[0013] The present invention includes the following. [1]

[0015] A thermosetting semiconductor adhesive film is used to bond a semiconductor chip to an adherend while embedding a wire connected to another semiconductor chip.

[0016] The adhesive film has a maximum tanδ value of 1.0 or less and a minimum melt viscosity of 10000 Pa·s or less in the range of 90 to 180°C.

[0017] The maximum value of tan δ and the minimum melt viscosity are values ​​obtained by measuring the dynamic viscoelasticity of the adhesive film in a temperature range including 90 to 180° C. under the conditions of a temperature increase rate of 5° C. / min and a frequency of 1 Hz. [2]

[0019] The adhesive film for a semiconductor according to [1], wherein

[0020] The adhesive film comprises a thermosetting resin containing epoxy resin, a curing agent and an imidazole compound. [3]

[0022] The adhesive film for a semiconductor according to [2], wherein

[0023] The content of the imidazole compound is 0.30 to 5.0 parts by mass based on 100 parts by mass of the epoxy resin. [4]

[0025] The adhesive film for a semiconductor according to any one of [1] to [3], wherein

[0026] The adhesive film contains an inorganic filler, and the content of the inorganic filler is 35 to 50% by mass based on the mass of the adhesive film. [5]

[0028] The adhesive film for a semiconductor according to any one of [1] to [4], wherein

[0029] The adhesive film contains an elastomer, and the content of the elastomer is 15 to 30% by mass based on the mass of the adhesive film. [6]

[0031] The adhesive film for a semiconductor according to [5], wherein

[0032] The elastomer contains acrylic resin. [7]

[0034] The adhesive film for a semiconductor according to any one of [1] to [6], wherein

[0035] The adhesive film has a thickness of 25 to 80 μm. [8]

[0037] The adhesive film for a semiconductor according to any one of [1] to [7], wherein

[0038] The adhesive film exhibits the minimum melt viscosity of 2500 Pa·s or more in the range of 90 to 180° C. [9]

[0040] The adhesive film for a semiconductor according to [1], wherein

[0041] The adhesive film exhibits the minimum melt viscosity of 2500 Pa·s or more in the range of 90 to 180° C.

[0042] The adhesive film contains inorganic fillers and elastomers.

[0043] Based on the mass of the adhesive film, the content of the inorganic filler is 35-50% by mass.

[0044] The content of the elastomer is 15 to 30% by mass based on the mass of the adhesive film.

[10]

[0046] The adhesive film for a semiconductor according to [9], wherein

[0047] The elastomer contains acrylic resin.

[11]

[0049] A dicing die bonding film, comprising:

[0050] Cutting film; and

[0051] The adhesive film for a semiconductor according to any one of [1] to

[10] provided on the dicing film.

[12]

[0053] A method for manufacturing a semiconductor device comprises the following steps:

[0054] On a structure having a substrate and a first semiconductor chip mounted on the substrate, a second semiconductor chip and an adhesive film are arranged in such a manner that the adhesive film is interposed between the structure and the second semiconductor chip; and

[0055] thermally curing the adhesive film to bond the second semiconductor chip to the structure,

[0056] The adhesive film is the adhesive film for a semiconductor according to any one of [1] to

[10] ,

[0057] A wire is connected to the first semiconductor chip,

[0058] A part or the whole of the lead wire is buried through the adhesive film.

[13]

[0060] The method according to

[12] , wherein:

[0061] The structure further includes a spacer disposed on the substrate and around the first semiconductor chip.

[0062] The second semiconductor chip and the adhesive film are arranged on the structure such that the adhesive film is interposed between the spacer and the second semiconductor chip.

[14]

[0064] The method according to

[13] , wherein:

[0065] The adhesive film is thermally cured in such a manner that the adhesive film is in contact with the first semiconductor chip.

[15]

[0067] The method according to any one of

[12] to

[14] , wherein

[0068] The method further includes the step of forming a sealing layer, wherein the sealing layer seals the first semiconductor chip and the second semiconductor chip.

[0069] Effects of the Invention

[0070] In a thermosetting adhesive film for a semiconductor for bonding a semiconductor chip to an adherend while embedding a wire connected to another semiconductor chip, local deformation in the thickness direction of the adhesive film due to thermal curing can be suppressed. BRIEF DESCRIPTION OF THE DRAWINGS

[0071] Figure 1 It is a cross-sectional view showing an example of a laminated film having an adhesive film.

[0072] Figure 2 It is a cross-sectional view showing an example of a method for manufacturing a semiconductor device.

[0073] Figure 3 It is a cross-sectional view showing an example of a method for manufacturing a semiconductor device.

[0074] Figure 4 It is a cross-sectional view showing an example of a method for manufacturing a semiconductor device.

[0075] Figure 5 It is a cross-sectional view showing an example of a method for manufacturing a semiconductor device.

[0076] Figure 6 It is a cross-sectional view showing an example of a method for manufacturing a semiconductor device.

[0077] Figure 7 It is a graph showing the relationship between the shear viscosity of the adhesive film and the temperature.

[0078] Figure 8 It is a graph showing the relationship between tanδ of the adhesive film and temperature.

[0079] Fig. 9 This is a schematic cross-sectional view showing an adhesive body for evaluation for evaluating deformation of an adhesive film accompanying curing. DETAILED DESCRIPTION

[0080] The present invention is not limited to the following examples. In the following examples, except for the cases specifically indicated, the constituent elements (including steps, etc.) are not essential. The sizes of the constituent elements in each figure are conceptual sizes, and the relative relationship between the sizes of the constituent elements is not limited to the relationship shown in each figure. The numerical values ​​and their ranges exemplified below do not limit the present invention.

[0081] In this specification, the numerical range represented by "~" indicates a range including the numerical values ​​recorded before and after "~" as the minimum value and the maximum value, respectively. In the numerical range recorded in stages in this specification, the upper limit value or lower limit value recorded in one numerical range can also be replaced by the upper limit value or lower limit value of the numerical range recorded in other stages. In the numerical range recorded in this specification, the upper limit value or lower limit value of the numerical range can be replaced by the value shown in the embodiment.

[0082] In this specification, (meth)acrylate refers to acrylate or its corresponding methacrylate. This also applies to other similar expressions such as (meth)acryloyl, (meth)acrylic copolymer, etc.

[0083] Figure 1 It is a cross-sectional view showing an example of a laminated film having an adhesive film. Figure 1The laminated film 50 shown in the figure includes a substrate 20, an adhesive film 12, and a protective film 30 in this order. The adhesive film 12 may be a thermosetting semiconductor adhesive film for bonding a semiconductor chip to an adherend while embedding a wire connected to another semiconductor chip. The substrate 20 may be a dicing film, in which case the laminated film 50 can be used as a dicing die bonding film.

[0084] The adhesive film 12 can show a maximum tan δ value of 1.0 or less and a minimum melt viscosity of 10000 Pa·s or less in the range of 90 to 180° C. The maximum tan δ value and the minimum melt viscosity are values ​​obtained by measuring the dynamic viscoelasticity of the adhesive film 12 under the conditions of a heating rate of 5° C. / min and a frequency of 1 Hz.

[0085] When the tan δ of the adhesive film 12 is 1.0 or less in the range of 90 to 180° C., deformation of the adhesive film 12 during heat curing is suppressed. From the same viewpoint, the maximum value of the tan δ of the adhesive film 12 in the range of 90 to 180° C. may be 0.95 or less, 0.90 or less, 0.85 or less, 0.80 or less, 0.75 or less, or 0.70 or less, and may be 0.50 or more.

[0086] The minimum melt viscosity of the adhesive film refers to the shear viscosity (or complex viscosity η) measured by measuring the dynamic viscoelasticity of the adhesive film 12. * ). The shear viscosity of the adhesive film 12 usually decreases with the increase in temperature and then increases with the progress of the curing reaction. When the minimum melt viscosity of the adhesive film 12 is 10000 Pa·s or less, the adhesive film 12 can properly bury the wires and the like. From the same point of view, the minimum melt viscosity of the adhesive film 12 can be 9000 Pa·s or less, 8500 Pa·s or less, 8000 Pa·s or less, 7500 Pa·s or less, 7000 Pa·s or less, 6500 Pa·s or less, 6000 Pa·s or less, or 5500 Pa·s or less.

[0087] Maintaining a relatively high shear viscosity of the adhesive film 12 within the range of 90 to 180°C can also help suppress deformation of the adhesive film 12 during the curing process. From this point of view, the minimum melt viscosity of the adhesive film 12 within the range of 90 to 180°C can be 2500 Pa·s or more, 3000 Pa·s or more, or 3500 Pa·s or more. An adhesive film that exhibits a relatively high minimum melt viscosity within the range of 90 to 180°C tends to easily exhibit a maximum value of tanδ of less than 1.0 within the range of 90 to 180°C.

[0088] The thickness of the adhesive film 12 may be, for example, 1 μm or more, 3 μm or more, 20 μm or more, 30 μm or more, 35 μm or more, 40 μm or more, or 50 μm or more, and may be 200 μm or less, 150 μm or less, 120 μm or less, 80 μm or less, or 60 μm or less. From the perspective of bonding the semiconductor chip to the adherend while embedding a wire connected to another semiconductor chip, the thickness of the adhesive film 12 may be 25 to 80 μm.

[0089] The adhesive film 12 contains, for example, a thermosetting resin and a curing agent that reacts with the thermosetting resin. The thermosetting resin is a compound that forms a crosslinked structure through a curing reaction including a reaction with a curing agent and / or self-polymerization, and an example thereof is an epoxy resin that is a compound having an epoxy group. As examples of epoxy resins, bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, phenol novolac type epoxy resins, cresol novolac type epoxy resins, bisphenol A novolac type epoxy resins, bisphenol F novolac type epoxy resins, stilbene type epoxy resins, epoxy resins containing triazine skeletons, epoxy resins containing fluorene skeletons, trisphenol methane type epoxy resins, biphenyl type epoxy resins, xylylene type epoxy resins, biphenyl aralkyl type epoxy resins, naphthalene type epoxy resins and diglycidyl ether compounds derived from polyfunctional phenol compounds or polycyclic aromatic compounds (anthracene, etc.) can be cited. These can also be used alone or in combination of two or more. The epoxy resin can also contain a combination of o-cresol novolac type epoxy resin and bisphenol F type epoxy resin and / or bisphenol A type epoxy resin.

[0090] The curing agent that can be combined with the epoxy resin as a thermosetting resin can contain a phenolic resin, for example. As an example of a phenolic resin used as a curing agent, there can be cited a novolac type phenolic resin, allylated bisphenol A, allylated bisphenol F, allylated naphthalene diol, phenol aralkyl resin and naphthol aralkyl resin. These can also be used alone or in combination of two or more. Novolac type phenolic resin is obtained by condensing or co-condensing a compound having an aldehyde group such as phenols (for example, phenol, cresol, resorcinol, catechol, bisphenol A, bisphenol F, phenylphenol, aminophenol) and / or naphthols (for example, α-naphthol, β-naphthol, dihydroxynaphthalene) with formaldehyde under an acidic catalyst. Phenol aralkyl resin and naphthol aralkyl resin are synthesized from phenols (for example, phenol novolac, phenol) and / or naphthols and dimethoxy-p-xylene or bis(methoxymethyl)biphenyl.

[0091] The total content of the thermosetting resin and the curing agent can be, for example, more than 10 mass % or more than 15 mass %, and can be less than 80 mass %, less than 75 mass %, less than 70 mass %, less than 65 mass %, less than 60 mass %, less than 55 mass %, less than 50 mass %, less than 45 mass %, less than 35 mass %, or less than 30 mass %.

[0092] The adhesive film 12 may contain an imidazole compound. An imidazole compound is a compound having an imidazole ring, and can, for example, act as a curing accelerator that promotes the curing reaction between an epoxy resin and its curing agent (phenolic resin, etc.). The type and content of the imidazole compound can be associated with the maximum value of tanδ and the minimum melt viscosity of the adhesive film 12. Imidazole compounds with a low softening point or melting point tend to increase the maximum value and the minimum melt viscosity of tanδ. For example, at least one imidazole compound selected from the group consisting of 1-cyanoethyl-2-phenylimidazole, 2-phenylimidazole and 1-benzyl-2-methylimidazole has a tendency to easily provide an adhesive film having a maximum value of tanδ of less than 1.0 and / or a minimum melt viscosity of less than 10,000 Pa·s (or more than 2,500 Pa·s and less than 10,000 Pa·s).

[0093] When the content of the imidazole compound is large, the maximum value of tan δ and the minimum melt viscosity tend to increase. For example, based on the mass of the adhesive film 12, the content of the imidazole compound can be 0.06 mass% or more, 0.07 mass% or more, 0.08 mass% or more, 0.09 mass% or more, 0.10 mass% or more, or 0.11 mass% or more, and can be 1.0 mass% or less, 0.90 mass% or less, 0.80 mass% or less, 0.70 mass% or less, 0.60 mass% or less, 0.5 mass% or less, 0.40 mass% or less, 0.30 mass% or less, or 0.20 mass% or less.

[0094] When the thermosetting resin contains an epoxy resin, from the same viewpoint as above, the content of imidazole may be 0.30 mass part or more, 0.35 mass part or more, 0.40 mass part or more, 0.45 mass part or more, or 0.50 mass part or more, and may be 5.0 mass parts or less, 4.5 mass parts or less, 4.0 mass parts or less, 3.5 mass parts or less, 3.0 mass parts or less, 2.5 mass parts or less, 2.0 mass parts or less, 1.5 mass parts or less, 1.0 mass parts or less, 0.95 mass parts or less, 0.90 mass parts or less, 0.85 mass parts or less, 0.80 mass parts or less, 0.75 mass parts or less, 0.70 mass parts or less, 0.65 mass parts or less, or 0.60 mass parts or less, based on 100 mass parts of the epoxy resin content.

[0095] When using a curing accelerator other than an imidazole compound, by appropriately adjusting its reactivity and content, an adhesive film having a maximum tan δ of 1.0 or less and / or a minimum melt viscosity of 10,000 Pa·s or less (or 2,500 Pa·s or more and 10,000 Pa·s or less) can be obtained.

[0096] The adhesive film 12 may further contain an inorganic filler. When an inorganic filler is introduced, the maximum value of tan δ and the minimum melt viscosity of the adhesive film 12 tend to increase. Based on the mass of the adhesive film 12, the content of the inorganic filler may be 10% by mass or more, 15% by mass or more, 20% by mass or more, 25% by mass or more, 30% by mass or more, or 35% by mass or more, and may be 60% by mass or less, 55% by mass or less, 50% by mass or less, or 45% by mass or less.

[0097] The inorganic filler may be, for example, particles containing at least one inorganic material selected from aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, calcium silicate, magnesium silicate, calcium oxide, magnesium oxide, aluminum oxide, aluminum nitride, aluminum borate whisker, boron nitride and silicon dioxide. From the viewpoint of adjusting the melt viscosity, the inorganic filler may contain silicon dioxide.

[0098] From the viewpoint of fluidity, the average particle size of the inorganic filler can be 0.01 μm or more, or 0.03 μm or more, and can be 1.5 μm or less, 1.0 μm or less, 0.8 μm or less, 0.08 μm or less, or 0.06 μm or less. Two or more inorganic fillers with different average particle sizes can also be combined. The average particle size refers to the value calculated by converting the BET specific surface area.

[0099] The adhesive film 12 may contain an elastomer. When the elastomer is introduced, the maximum value of tan δ and the minimum melt viscosity of the adhesive film 12 tend to increase. Based on the mass of the adhesive film 12, the content of the elastomer may be 5 mass % or more, 10 mass % or more, or 15 mass % or more, and may be 50 mass % or less, 45 mass % or less, 40 mass % or less, 35 mass % or less, or 30 mass % or less.

[0100] The elastomer may contain an acrylic resin. Here, an acrylic resin refers to a polymer containing monomer units derived from (meth)acrylate. Based on the total amount of the acrylic resin, the content of the constituent units derived from (meth)acrylate in the acrylic resin may be, for example, 70% by mass or more, 80% by mass or more, or 90% by mass or more. The acrylic resin may contain monomer units derived from (meth)acrylate having crosslinking functional groups such as epoxy groups, alcoholic or phenolic hydroxyl groups, and carboxyl groups. The acrylic resin may be an acrylic rubber, which is a copolymer containing (meth)acrylate and acrylonitrile as monomer units.

[0101] The glass transition temperature (Tg) of an elastomer (e.g., acrylic resin) may be -50°C or higher, -30°C or higher, 0°C or higher, or 3°C or higher, and may be 50°C or lower, 45°C or lower, 40°C or lower, 35°C or lower, 30°C or lower, or 25°C or lower. The glass transition temperature (Tg) refers to a value measured using a DSC (differential scanning calorimeter) (e.g., "Thermo Plus 2" manufactured by Rigaku Corporation). By adjusting the type and content of the constituent units constituting the elastomer (in the case of an acrylic resin, constituent units derived from (meth)acrylate), the Tg of the elastomer can be adjusted to a desired range.

[0102] The weight average molecular weight (Mw) of the elastomer (e.g., acrylic resin) may be 100,000 or more, 200,000 or more, or 300,000 or more, and may be 3,000,000 or less, 2,000,000 or less, or 1,000,000 or less. When the Mw of the elastomer is within such a range, it tends to be easy to appropriately control the viscoelasticity of the adhesive film 12. Mw refers to a value measured by gel permeation chromatography (GPC) and converted using a calibration curve based on standard polystyrene.

[0103] Examples of commercially available products of acrylic resins include SG-70L, SG-708-6, WS-023EK30, SG-280EK23, and SG-P3 (all manufactured by Nagase ChemteX Corporation), and H-CT-865 (manufactured by Resonac Corporation).

[0104] The adhesive film 12 may also contain a coupling agent. The coupling agent may also be a silane coupling agent. Examples of silane coupling agents include γ-ureidopropyltriethoxysilane, γ-mercaptopropyltrimethoxysilane, 3-phenylaminopropyltrimethoxysilane, and 3-(2-aminoethyl)aminopropyltrimethoxysilane. These may also be used alone or in combination of two or more.

[0105] The adhesive film 12 may further contain other components such as a pigment, an ion scavenger, and an antioxidant.

[0106] The substrate 20 constituting the laminated film 50 may be a resin film, and examples thereof include films of polytetrafluoroethylene, polyethylene, polypropylene, polymethylpentene, polyethylene terephthalate, or polyimide. The thickness of the resin film as the substrate 20 may be, for example, 60 to 200 μm or 70 to 170 μm.

[0107] The substrate 20 may be a dicing film, and the laminated film 50 may be a dicing die bonding film. The dicing die bonding film may be in a tape shape.

[0108] As examples of cutting films, resin films such as polytetrafluoroethylene film, polyethylene terephthalate film, polyethylene film, polypropylene film, polymethylpentene film and polyimide film can be cited. As needed, the cutting film can also be a resin film that has been surface-treated by primer coating, UV treatment, corona discharge treatment, grinding treatment, and etching treatment. The cutting film can have adhesiveness. The cutting film with adhesiveness can be, for example, a resin film endowed with adhesiveness, or a laminate having a resin film and a pressure-sensitive adhesive layer disposed on one side thereof. The pressure-sensitive adhesive layer can be formed by a pressure-sensitive adhesive of a pressure-sensitive adhesive type or a UV-curable type. A pressure-sensitive adhesive is a pressure-sensitive adhesive that shows constant adhesiveness under a short period of pressure. A radiation-curable pressure-sensitive adhesive is a pressure-sensitive adhesive that has a property of reduced adhesiveness by irradiation with radiation (e.g., ultraviolet rays). The thickness of the pressure-sensitive adhesive layer can be appropriately set according to the shape and size of the semiconductor device, for example, 1 to 100 μm, 5 to 70 μm, or 10 to 40 μm. From the perspective of economic efficiency and film handling, the thickness of the substrate 20 as a dicing film can be 60 to 150 μm or 70 to 130 μm.

[0109] The protective film 30 may be the same resin film as the base material 20. The thickness of the protective film 30 may be, for example, 15 to 200 μm or 70 to 170 μm.

[0110] Figure 2 , Figure 3 , Figure 4 , Figure 5 and Figure 6 1 is a cross-sectional view showing an example of a method for manufacturing a semiconductor device using the adhesive film 12 .

[0111] like Figure 2As shown, an example of a method for manufacturing a semiconductor device includes the following steps: preparing a structure 15 having a substrate 1 and a first semiconductor chip T1 mounted on the substrate 1; and preparing an adhesive chip TA having a second semiconductor chip T2 and an adhesive film 12 attached thereto. The structure 15 also has a plurality of spacers 3 arranged on the substrate 1 and around the first semiconductor chip.

[0112] The first semiconductor chip T1 is bonded to the substrate 1 by the first adhesive film 11. The first semiconductor chip T1 is connected to the wire w on the surface of the first semiconductor chip T1 opposite to the substrate 1. The first semiconductor chip T1 can be a controller chip. The substrate 1 can be an organic substrate or a metal substrate such as a lead frame. The thickness of the substrate 1 can be, for example, 90 to 300 μm. The spacer 3 can be a spacer commonly used in a semiconductor device having a dolmen structure. The height of the spacer 3 from the substrate 1 can be greater than the height of the first semiconductor chip T1 from the substrate 1.

[0113] The chip TA with adhesive formed of the second semiconductor chip T2 and the adhesive film 12 can be made of, for example, Figure 1 The laminate film 50 (cutting die bonding film) is prepared by a cutting die bonding film having the same structure as the laminate film 50 illustrated in the figure. In this case, for example, the laminate film 50 (cutting die bonding film) is attached to a single surface of the semiconductor wafer in a direction in which its adhesive film 12 contacts the semiconductor wafer. The surface to which the adhesive film 12 is attached can be the circuit surface of the semiconductor wafer or the back surface on the opposite side thereof. The semiconductor wafer to which the laminate film 50 (cutting die bonding film) is attached is divided by cutting to form a single-piece second semiconductor chip T2. As examples of cutting, there can be cited a method of cutting using a rotary blade and a method of cutting the adhesive film 12 together with the semiconductor wafer by laser. It is also possible to reduce the adhesive force of the cutting film by irradiating ultraviolet rays after cutting. The second semiconductor chip T2 is picked up together with the divided adhesive film 12.

[0114] The thickness of the second semiconductor chip T2 may be, for example, 1 to 100 μm. The width of the second semiconductor chip T2 may be, for example, 20 mm or less. The width (or length of one side) of the second semiconductor chip T2 may be 3 to 15 mm, or 5 to 10 mm.

[0115] like Figure 3 As shown, the second semiconductor chip T2 and the adhesive film 12 are arranged on the structure 15 in such a manner that the adhesive film 12 is interposed between the structure 15 and the second semiconductor chip T2. Figure 3 In the example of FIG. 1 , an adhesive film 12 is disposed on the spacer 3 of the structure 15, and the adhesive film 12 is separated from the first semiconductor chip T1. By thermally curing the adhesive film 12 in this state, as shown in FIG. Figure 4 As shown, the second semiconductor chip T2 is bonded to the structure 15 (adherend). The heat-cured adhesive film 12 is in contact with the first semiconductor chip T1 and buries a portion of the wire w connected to the first semiconductor chip T1. The heating temperature for heat curing the adhesive film 12 can be constant or can be changed in stages. The maximum heating temperature can be 90 to 180°C. The adhesive film 12 is heat cured under pressure, atmospheric pressure, or reduced pressure. The adhesive film 12 designed according to the maximum value of tanδ and / or the minimum melt viscosity can properly bury the wire w through moderate flow during the heat curing process, and can form a cured product that suppresses local deformation in its thickness direction.

[0116] Then, if Figure 5 As shown, a wire w is provided to connect the second semiconductor chip T2 and the substrate 1. Furthermore, a third semiconductor chip T3 and a fourth semiconductor chip T4 may be sequentially stacked via an adhesive film 13 on the surface of the second semiconductor chip T2 opposite to the substrate 1. A wire w is provided to connect the third semiconductor chip T3 or the fourth semiconductor chip T4 and the substrate 1. Figure 5 In the example of , the number of semiconductor chips stacked on the spacer 3 is 3, but the number may be 4 or more.

[0117] like Figure 6 As shown, a semiconductor device 100 having a dolmen structure is obtained by forming a sealing layer 60, which seals a structure having a plurality of semiconductor chips including a first semiconductor chip T1 and a second semiconductor chip T2. The sealing layer 60 also fills the vicinity of the end of the first semiconductor chip. If there is local deformation in the thickness direction on the adhesive film 12, the sealing layer 60 enters therein, which may cause defects such as cracks on the second semiconductor chip T2. By suppressing the deformation of the adhesive film 12, such defects can be avoided.

[0118] Example

[0119] The present invention is not limited to the following examples.

[0120] 1. Preparation of adhesive film

[0121] An adhesive varnish was prepared containing the following materials in the contents (unit: parts by mass) shown in Table 1. The contents of SG-P3 (elastomer) and SC2050-HLG shown in Table 1 are the amounts of solid components (acrylic rubber or silica filler) excluding the solvent.

[0122] (A) Epoxy resin

[0123] N-500P-10 (trade name, manufactured by DIC Corporation, o-cresol novolac type epoxy resin, epoxy equivalent: 203 g / eq)

[0124] EXA-830CRP (trade name, manufactured by DIC Corporation, bisphenol F type epoxy resin, epoxy equivalent: 158 to 168 g / eq)

[0125] (B) Curing agent (phenolic resin)

[0126] MEH-7800M (trade name, manufactured by Meiwa Chemical Industry Co., Ltd., phenol novolac type phenolic resin, hydroxyl equivalent: 175 g / eq, softening point: 61 to 90°C)

[0127] (C) Inorganic fillers

[0128] SC2050-HLG (trade name, manufactured by Admatechs Co., Ltd., silica filler dispersion, average particle size: 0.50 μm)

[0129] (D) Elastomer

[0130] SG-P3 (trade name, acrylic rubber, weight average molecular weight: 800,000, Tg: 12°C, cyclohexanone solution)

[0131] (E) Coupling agent

[0132] · Z-6119 (trade name, manufactured by Dow Toray Co., Ltd., 3-ureidopropyltriethoxysilane)

[0133] ·A-189 (trade name, manufactured by Nippon Unicar Company Limited, γ-mercaptopropyltrimethoxysilane)

[0134] (F) Curing accelerator

[0135] ·2PZ-CN (trade name, manufactured by SHIKOKU CHEMICALS CORPORATION, 1-cyanoethyl-2-phenylimidazole)

[0136] Each of the prepared adhesive varnishes was filtered through a 500-mesh filter and vacuum defoamed. The vacuum defoamed adhesive varnish was applied to a polyethylene terephthalate (PET) film (support film) that had been subjected to a demolding treatment. The coating film was heated at 90°C for 5 minutes and then heated at 130°C for 5 minutes, and dried in these two stages to form an adhesive film (thickness: 50 μm) in a B-stage state on the support film.

[0137] 2. Evaluation

[0138] (1) Viscoelasticity of adhesive film

[0139] Eight adhesive films having a predetermined size were cut out from the adhesive film and prepared. These were laminated on a hot plate at 70° C. using a rubber roller to prepare a laminate having a thickness of 400 μm. The laminate was punched out with a punch to produce a sample. The sample was mounted on the measuring fixture of a rotary viscoelasticity measuring device (manufactured by TA Instruments Japan Inc., trade name: ARES-RDA). The gap of the measuring fixture was adjusted so that the load applied to the sample at this moment was 10 to 15 g. Next, the viscoelasticity of the sample was measured under the following conditions. Figure 7 This is a graph showing the relationship between the shear viscosity (complex viscosity) and the temperature of the adhesive films of Examples 1 to 3 and Comparative Example. Figure 8 This is a graph showing the relationship between tanδ and temperature of the adhesive films of Examples 1 to 3 and Comparative Example. The minimum melt viscosity and the maximum value of tanδ in the range of 90 to 180°C were read from the measurement results. The minimum melt viscosity is the minimum value of the shear viscosity (complex viscosity) in the range of 90 to 180°C.

[0140] Determination conditions:

[0141] Plate: Aluminum, round

[0142] Measuring frequency: 1Hz

[0143] Heating rate: 5℃ / min

[0144] Strain: 5%

[0145] Measuring temperature: 35~180℃

[0146] Initial load: 100g

[0147] (2) Deformation of adhesive film

[0148] Fig. 9Schematic cross-sectional view showing an adhesive body for evaluation for evaluating deformation of an adhesive film accompanying curing. A first semiconductor chip T1 (thickness: 60 μm) having a size of 3 mm × 2 mm and four spacers 3 (thickness: 100 μm) surrounding the first semiconductor chip T1 are arranged on a substrate 1. The first semiconductor chip T1 and the spacers 3 are bonded to the substrate 1 via a first adhesive film 11 (thickness: 20 μm). The height difference between the spacers 3 on the substrate 1 and the first semiconductor chip T1 is 40 μm. The interval between the first semiconductor chip T1 and each spacer 3 is 1.5 mm on the short side of the first semiconductor chip T1 and 1.0 mm on the long side of the first semiconductor chip T1.

[0149] A chip with adhesive having a second semiconductor chip T2 having a size of 12 mm×6 mm and a second adhesive film 12 attached thereto was prepared. As the second adhesive film 12, each adhesive film prepared in "1. Preparation of adhesive film" was used. The prepared chip with adhesive was pressed onto the spacer 3 to cover the first semiconductor chip T1. The formed structure was heated in an oven at a maximum temperature of 140°C, thereby curing the second adhesive film 12. Thereafter, an ultrasonic digital image diagnostic system (manufactured by Insight CO., LTD., IS-350 or IS-450) was used to observe the first semiconductor chip T1 of the structure and the cured adhesive film 12 through an ultrasonic microscope (SAM), and the case where a part of the black shadow was not observed was evaluated as "OK", and the case where a part of the black shadow was observed was evaluated as "NG". The part of the black shadow is caused by the deformation of the adhesive film 12. When the part of the black shadow is not observed, it is considered that the adhesive film has good embedding properties. The conditions of SAM are as follows.

[0150] Reflection method

[0151] Frequency: 75MHz

[0152] Focus distance: 9mm

[0153] Then, the structure was cut into half, and the adhesive film 12 in the cross section was observed with an optical microscope, and the minimum value t of the thickness of the second adhesive film 12 was measured.

[0154] The evaluation results are shown in Table 1. It was confirmed that the adhesive films of Examples 1 to 5 were able to suppress local shrinkage in the thickness direction accompanying curing. The adhesive film of the comparative example was greatly deformed in the thickness direction near the end of the first semiconductor chip T1 due to curing, and as a result, a portion with a thickness of 0 μm was observed, that is, a portion where the adhesive film 12 substantially disappeared. The adhesive films of Examples 1 to 5 were also excellent in embedding properties.

[0155] [Table 1]

[0156]

[0157] Explanation of symbols

[0158] 1-substrate, 3-spacer, 11, 12, 13-adhesive film, 15-structure, 20-base material (dicing film), 30-protective film, 50-laminated film (dicing die bonding film), 60-sealing layer, 100-semiconductor device, T1-first semiconductor chip, T2-second semiconductor chip, w-wire.

Claims

1. A thermosetting semiconductor adhesive film for bonding a semiconductor chip to an adherend while embedding a wire connected to another semiconductor chip, The adhesive film has a maximum tanδ value of 1.0 or less and a minimum melt viscosity of 10000 Pa·s or less in the range of 90 to 180°C. The maximum value of tan δ and the minimum melt viscosity are values ​​obtained by measuring the dynamic viscoelasticity of the adhesive film in a temperature range including 90 to 180° C. under the conditions of a temperature increase rate of 5° C. / min and a frequency of 1 Hz.

2. The adhesive film for semiconductor according to claim 1, wherein The adhesive film comprises a thermosetting resin containing epoxy resin, a curing agent and an imidazole compound.

3. The adhesive film for semiconductor according to claim 2, wherein: The content of the imidazole compound is 0.30 to 5.0 parts by mass based on 100 parts by mass of the epoxy resin.

4. The adhesive film for semiconductor according to claim 1, wherein The adhesive film contains an inorganic filler, and the content of the inorganic filler is 35 to 50% by mass based on the mass of the adhesive film.

5. The adhesive film for semiconductor according to claim 1, wherein The adhesive film contains an elastomer, and the content of the elastomer is 15 to 30% by mass based on the mass of the adhesive film.

6. The adhesive film for semiconductor according to claim 5, wherein The elastomer contains acrylic resin.

7. The adhesive film for a semiconductor according to claim 1, wherein The adhesive film has a thickness of 25 to 80 μm.

8. The adhesive film for a semiconductor according to claim 1, wherein The adhesive film exhibits the minimum melt viscosity of 2500 Pa·s or more in the range of 90 to 180° C.

9. The adhesive film for a semiconductor according to claim 1, wherein The adhesive film exhibits the minimum melt viscosity of 2500 Pa·s or more in the range of 90 to 180° C. The adhesive film contains inorganic fillers and elastomers. Based on the mass of the adhesive film, the content of the inorganic filler is 35-50% by mass. The content of the elastomer is 15 to 30% by mass based on the mass of the adhesive film.

10. The adhesive film for a semiconductor according to claim 9, wherein The elastomer contains acrylic resin.

11. A dicing die bonding film comprising: Cutting film; and The adhesive film for a semiconductor according to claim 1 is provided on the dicing film.

12. A method for manufacturing a semiconductor device, comprising the steps of: On a structure having a substrate and a first semiconductor chip mounted on the substrate, a second semiconductor chip and an adhesive film are arranged in such a manner that the adhesive film is interposed between the structure and the second semiconductor chip; and thermally curing the adhesive film to bond the second semiconductor chip to the structure, The adhesive film is the adhesive film for semiconductor according to claim 1, A wire is connected to the first semiconductor chip, A part or the whole of the lead wire is buried through the adhesive film.

13. The method according to claim 12, wherein: The structure further includes a spacer disposed on the substrate and around the first semiconductor chip. The second semiconductor chip and the adhesive film are arranged on the structure such that the adhesive film is interposed between the spacer and the second semiconductor chip.

14. The method according to claim 13, wherein: The adhesive film is thermally cured in such a manner that the adhesive film is in contact with the first semiconductor chip.

15. The method according to claim 12, wherein: The method further includes the step of forming a sealing layer, wherein the sealing layer seals the first semiconductor chip and the second semiconductor chip.