Separator for electrochemical device and electrochemical device including same

By using a porous coating on a porous polymer substrate in a lithium secondary battery, the transition metal ions are adsorbed using the coordination bonds of the first polymer binder and inorganic particles, the migration of transition metal ions in the manganese positive electrode active material is solved. The electrochemical device deterioration problem achieves more stable battery performance and longer life.

CN119096408APending Publication Date: 2024-12-06LG ENERGY SOLUTION LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202480002096.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-04-04
Filing Date
2024-01-19
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

When using a transition metal positive electrode active material containing manganese in lithium secondary batteries, transition metal ions may dissolve from the positive electrode and migrate to the negative electrode during charging and discharging, resulting in impurity precipitation and uneven film formation, causing capacity deterioration of the electrochemical device. .

Method used

Using a porous coating on the porous polymer substrate, coordination bonds are formed through the first polymer binder and inorganic particles to adsorb transition metal ions to prevent them from migrating to the negative electrode. The porous coating consists of a porous polymer substrate, a first polymer binder, an inorganic particles and a second polymer binder, each of which introduces different ligands to form in the porous polymerization The surface of the substrate contains 40% to 80% of inorganic particles to ensure metal ions adsorption and adhesion.

Benefits of technology

It effectively prevents metal ions precipitation, avoids deterioration of electrochemical device performance, improves the cycle stability and output characteristics of lithium secondary batteries, and extends the battery life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005072520860000191
    Figure BDA0005072520860000191
Patent Text Reader

Abstract

The present invention provides a separator for an electrochemical device, the separator comprising a porous polymer substrate and a porous coating layer comprising a first polymer binder and inorganic particles and formed on at least one surface of the porous polymer substrate, wherein the first polymeric binder and the inorganic particles are each introduced with different ligands.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application is based on and claims the benefit of priority from Korean Patent Application No. 10-2023-0044174 filed on April 4, 2023, in the Korean Intellectual Property Office, the disclosure of which is incorporated herein in its entirety by reference.

[0002] The present disclosure relates to a separator for an electrochemical device and an electrochemical device including the same. Background Art

[0003] Electrochemical devices convert chemical energy into electrical energy using electrochemical reactions, and lithium secondary (rechargeable) batteries have been widely used in recent years due to their high energy density and voltage, long cycle life, and wide use in various applications.

[0004] A lithium secondary battery may include an electrode assembly made of a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode, and the electrode assembly is housed in a housing together with an electrolyte. The positive electrode is capable of providing lithium ions, and the lithium ions can pass through a separator made of a porous material and move to the negative electrode. The negative electrode may be a carbon-based active material that has an electrochemical reaction potential close to that of lithium metal and is capable of inserting and removing lithium ions. Summary of the invention

[0005] Technical issues

[0006] The present disclosure provides a separator for an electrochemical device that uses a positive electrode active material containing a transition metal such as manganese and is capable of adsorbing transition metal ions eluted from a positive electrode.

[0007] Technical Solution

[0008] According to one aspect, the present disclosure provides a separator for an electrochemical device, the separator for an electrochemical device comprising a porous polymer substrate and a porous coating layer comprising a first polymer binder and inorganic particles and formed on at least one surface of the porous polymer substrate. The first polymer binder and the inorganic particles are each introduced with different ligands. The first polymer binder and the inorganic particles form a coordination bond to a single metal ion.

[0009] The first polymer binder and the inorganic particles may each independently be chemically bonded to one or more ligands selected from a first ligand having a single degree of toothing and a second ligand having two or more degrees of toothing.

[0010] The first ligand may be at least one selected from the group consisting of imidazole, pyrazole, triazole, tetrazole, indazole, benzimidazole, azaindole, purine, and derivatives thereof.

[0011] The second ligand may be at least one selected from the group consisting of nitrilotriacetic acid, iminodiacetic acid, ethylenediaminetetraacetic acid, 1,2-cyclohexanediaminetetraacetic acid, and derivatives thereof.

[0012] The inorganic particle may have a second ligand chemically bonded to its surface.

[0013] The inorganic particles may be included in an amount of 40 wt % to 80 wt % based on the total weight of the porous coating layer.

[0014] The porous coating layer further includes a second polymer binder, and the content of the first polymer binder is greater than or equal to the content of the second polymer binder.

[0015] According to another aspect of the present disclosure, an electrochemical device is provided, which includes a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode, wherein the separator is the separator for an electrochemical device according to one aspect above.

[0016] The electrochemical device may be a lithium secondary battery.

[0017] Metal ions can be generated during charging and discharging of electrochemical devices.

[0018] The metal ions may be transition metal ions derived from the positive electrode.

[0019] According to another aspect, the present disclosure provides an electric device including the electrochemical device.

[0020] According to yet another aspect, the present disclosure provides a method for manufacturing a separator for an electrochemical device, the method comprising forming a porous coating layer comprising a first polymer binder and inorganic particles on at least one surface of a porous polymer substrate, wherein the first polymer binder and the inorganic particles are each introduced with different ligands.

[0021] The step of forming the porous coating layer may include preparing a coating slurry including a first polymer binder, inorganic particles, and a dispersion medium, and applying the coating slurry to at least one surface of the porous polymer substrate.

[0022] The coating slurry may also include a second polymeric binder.

[0023] The step of forming a porous coating layer may further include subjecting the at least one surface of the porous polymer substrate to a corona discharge treatment before applying the coating slurry to the at least one surface of the porous polymer substrate.

[0024] The step of forming the porous coating layer may include drying the coating slurry applied to at least one surface of the porous polymer substrate and evaporating the dispersion medium.

[0025] Beneficial Effects

[0026] The separator for an electrochemical device according to the present disclosure prevents performance degradation caused by precipitation of impurities in an electrochemical device by adsorbing metal ions generated during charge and discharge. DETAILED DESCRIPTION

[0027] Hereinafter, with reference to the accompanying drawings, embodiments of the present disclosure will be described in detail to facilitate practice by those skilled in the art to which the present disclosure belongs. The present disclosure can be implemented in various different forms and is not limited or constrained by the embodiments described below.

[0028] As used herein, the term "including" is used to list materials, compositions, devices and methods that can be used in the present disclosure and is not limited to the listed examples.

[0029] As used herein, the words "about," "approximately," and "substantially" are used to mean a range or approximation of a value or degree, taking into account inherent manufacturing and material tolerances, and are used to prevent an infringer from taking unfair advantage of the present disclosure where precise or absolute numbers are provided to aid in the understanding of the present disclosure.

[0030] As used herein, the term "electrochemical device" may refer to a primary battery, a secondary battery, or a supercapacitor.

[0031] The positive electrode active material of the lithium secondary battery may contain lithium and various metal or transition metal elements. For example, nickel can improve the capacity of the electrochemical device, cobalt can improve the capacity and cycle stability of the electrochemical device, manganese can improve the stability of the electrochemical device, and aluminum can improve the output characteristics of the electrochemical device. That is, electrochemical devices with higher energy density and stability use transition metals to improve various characteristics of the device. For example, lithium-manganese-based positive electrode active materials containing manganese have attracted attention due to their superior thermal stability compared to nickel-based active materials and their cost competitiveness compared to nickel-based or cobalt-based active materials.

[0032] In an electrochemical device using a positive electrode active material containing a transition metal such as manganese, transition metal ions may be dissolved from the positive electrode during the charge and discharge process. The dissolved transition metal ions may migrate to the negative electrode and precipitate as impurities or form an uneven film on the surface of the negative electrode, thereby causing capacity degradation of the electrochemical device.

[0033] Therefore, as a separator for an electrochemical device including a cathode active material containing a transition metal such as manganese, a separator capable of capturing transition metal ions eluted from the cathode and preventing them from migrating to the anode is provided, thereby preventing deterioration of the anode and the electrochemical device.

[0034] According to one embodiment, the present disclosure provides a separator for an electrochemical device, the separator for an electrochemical device comprising a porous polymer substrate and a porous coating layer comprising a first polymer binder and inorganic particles and formed on at least one surface of the porous polymer substrate. The first polymer binder and the inorganic particles are each introduced with different ligands. The first polymer binder and the inorganic particles form a coordination bond to a single metal ion.

[0035] The porous polymer substrate can be a porous film having a plurality of pores that electrically insulates the positive electrode and the negative electrode to prevent short circuits. For example, when the electrochemical device is a lithium secondary battery, the porous polymer substrate can be an ion-conducting barrier that allows lithium ions to pass while blocking electrical contact between the positive electrode and the negative electrode. At least a portion of the pores can form a three-dimensional network that communicates with the surface and interior of the porous polymer substrate, and a fluid can pass through the porous polymer substrate via the pores.

[0036] The porous polymer substrate can be a material that is physically and chemically stable to an electrolyte that is an organic solvent. Examples of porous polymer substrates include resins, such as polyolefins (e.g., polyethylene, polypropylene, and polybutylene), polyvinyl chloride, polyethylene terephthalate, polycycloolefins, polyethersulfones, polyamides, polyimides, polyimide amides, nylons, polytetrafluoroethylene, and copolymers or mixtures thereof, but are not limited thereto. Preferably, polyolefin-based resins can be used. Polyolefin-based resins are suitable for manufacturing electrochemical devices with higher energy density because they can be processed into relatively small thicknesses and are easily coated with slurries.

[0037] The porous polymer substrate may have a monolayer or multilayer structure. The porous polymer substrate may include two or more polymer resin layers with different melting points (Tm) to provide a shutdown capability during high temperature runaway of the battery. For example, the porous polymer substrate may include a polypropylene layer with a relatively high melting point and a polyethylene layer with a relatively low melting point. For example, the porous polymer substrate may be a three-layer structure in which polypropylene, polyethylene, and polypropylene are laminated in this order. When the temperature of the battery rises above a predetermined temperature, the polyethylene layer melts and closes the pores, thereby preventing thermal runaway of the battery.

[0038] The thickness of the porous polymer substrate may be about 1 μm or more and 100 μm or less. For example, the thickness of the porous polymer substrate may be about 10 μm or more and 90 μm or less, 20 μm or more and 80 μm or less, 30 μm or more and 70 μm or less, or 40 μm or more and 60 μm or less. For example, the thickness of the polymer substrate may be about 1 μm or more and 30 μm or less. As another example, the thickness of the polymer substrate may be about 5 μm or more and 15 μm or less, or 8 μm or more and 13 μm or less. When the thickness of the porous polymer substrate is adjusted within the above range, the amount of active material contained in the electrochemical device may be increased by minimizing the volume of the electrochemical device while electrically insulating the positive and negative electrodes.

[0039] The porous polymer substrate may include holes having an average diameter of about 0.01 μm or more and 1 μm or less, such as circular, round and elliptical shapes. For example, the size of the holes included in the porous polymer substrate may be about 0.01 μm or more and 0.09 μm or less, about 0.02 μm or more and 0.08 μm or less, about 0.03 μm or more and 0.07 μm or less, or about 0.04 μm or more and 0.06 μm or less. According to one embodiment, the size of the hole may be about 0.02 μm or more and 0.06 μm or less. When the pore size of the porous polymer substrate is adjusted within the above range, the permeability and ionic conductivity of the entire separator prepared may be controlled.

[0040] The permeability of porous polymer substrate can be about 10 seconds / 100cc or more and 100 seconds / 100cc or less. For example, the permeability of porous polymer substrate can be about 10 seconds / 100cc or more and 90 seconds / 100cc or less, 20 seconds / 100cc or more and 80 seconds / 100cc or less, 30 seconds / 100cc or more and 70 seconds / 100cc or less, or 40 seconds / 100cc or more and 60 seconds / 100cc or less. For example, the permeability of porous polymer substrate can be about 50 seconds / 100cc or more and 70 seconds / 100cc or less. When the permeability of porous polymer substrate is within the above range, the permeability of the separator prepared can be set in the range suitable for ensuring the output characteristics and cycle characteristics of the electrochemical device.

[0041] Permeability (seconds / 100cc) means the time (in seconds) it takes for 100cc of air to pass through a predetermined area of ​​a porous polymer substrate or separator at a constant pressure. Permeability can be measured using a Gurley air permeability tester according to ASTM D726-58, ASTM D726-94, or JIS-P8117. For example, a 4110N instrument from Gurley can be used to measure the permeability of 100cc of air at 0.304 kPa air or 1.215 kN / m 2 The pressure of water passing through 1 square inch (or 6.54 cm 2 For example, the time it takes for 100cc of air to pass through a 1 square inch sample at room temperature under a constant pressure of 4.8 inches of water can be measured using an ASAHI SEIKO EG01-55-1MR instrument.

[0042] The porosity of the porous polymer substrate can be about 10 volume % or more and 60 volume % or less. For example, the porosity of the porous polymer substrate can be about 15 volume % or more and 55 volume % or less, 20 volume % or more and 50 volume % or less, 25 volume % or more and 45 volume % or less, or 30 volume % or more and 40 volume % or less. For example, the porosity of the porous polymer substrate can be about 30 volume % or more and 50 volume % or less. When the porosity of the porous polymer substrate is within the above range, the ionic conductivity of the prepared separator can be set within a range suitable for ensuring the output characteristics and cycle characteristics of the electrochemical device.

[0043] Porosity refers to the ratio of the volume of the pores to the total volume of the porous polymer substrate. Porosity can be measured by methods known in the art. For example, porosity can be measured by Brunauer Emmett Teller (BET) measurement using nitrogen adsorption, capillary flow porometer, or water or mercury permeation method.

[0044] The porous coating is formed on at least one side of the porous polymer substrate and comprises a first polymer binder and inorganic particles. The first polymer binder and the inorganic particles can each be introduced with different ligands. The statement "introducing" ligand in the first polymer binder or the inorganic particles means that the ligand is chemically bonded to the polymer binder or the inorganic particles. To the extent that the ligand has the coordination binding ability to metal ions, the method of chemical coupling of the ligand is not limited, and any method known in the art can be used. The first polymer binder can be a polymer binder wherein the ligand is chemically bonded to the predetermined part of the repeating unit. The inorganic particles can be chemically bonded to the ligand via the functional group exposed on the surface of the particles, or can form a chemical bond with the ligand via a predetermined functional group after the surface of the inorganic particles is modified with the functional group.

[0045] The first polymer binder and inorganic particles can comprise different ligands, and can form coordination bonds to metal ions or form coordination bonds to single metal ions separately.For example, the first polymer binder and inorganic particles form coordination bonds to single metal ions simultaneously.For example, a first polymer binder and one or more inorganic particles can form coordination bonds to a metal ion simultaneously.The porous coating that can form coordination bonds to single metal ions can easily form complexes with metal ions, and even after complex formation, also keep stable structure.

[0046] The first polymer binder and inorganic particles can be chemically bonded to one or more ligands selected from the first ligand with a single degree of toothing and the second ligand with two or more degrees of toothing, independently of one another. For example, the first ligand with a degree of toothing and the second ligand with two degrees of toothing can form a coordination bond to a single metal ion simultaneously. The first ligand and the second ligand can be chemically bonded to one or more of the first polymer binder and inorganic particles independently of one another. Preferably, the first polymer binder can be chemically bonded to the first ligand, and inorganic particles can be chemically bonded to the second ligand, and vice versa.

[0047] The first ligand can be at least one selected from the following: imidazole, pyrazole, triazole, tetrazole, indazole, benzimidazole, azaindole, purine, and derivatives thereof. The first ligand can include an aromatic heterocycle and form a coordination bond with a metal ion at one position. The type of derivative is not limited as long as the derivative can form a coordination bond with the metal ion and form a chemical bond with the first polymer binder or inorganic particles. For example, the first ligand can be imidazole or a derivative thereof.

[0048] The second ligand can be at least one selected from the following: nitrilotriacetic acid (NTA), iminodiacetic acid (IDA), ethylenediaminetetraacetic acid (EDTA), 1,2-cyclohexanediamine-N,N,N',N'-tetraacetic acid, and derivatives thereof. The second ligand can be acetic acid, and can include two or more carboxyl groups to form coordination bonds with metal ions at two or more positions. The type of derivative is not limited, as long as the derivative can form a coordination bond with the metal ion and form a chemical bond with the first polymer binder or inorganic particles. Preferably, the second ligand can be selected from nitrilotriacetic acid, iminodiacetic acid, or derivatives thereof.

[0049] For example, the first polymer binder can be chemically bonded to the first part, and the inorganic particles can be chemically bonded to the second part. The second part may be more unstable in the electrochemical device compared with the first part. The second part may have a side reaction with the electrolyte in the electrochemical device. Therefore, the second part is typically bonded to the surface of the inorganic particles rather than being bonded to the first polymer binder that can be dissolved or swollen by the electrolyte to maintain the adsorption capacity to the metal ions.

[0050] According to one embodiment, the first polymer binder may include nitrilotriacetic acid as a ligand, and the inorganic particles may include imidazoles as a ligand. The metal ions may be included in the electrochemical device and may be generated during the charge and discharge process of the electrochemical device. For example, the metal ions may be transition metal ions derived from the positive electrode. For example, the metal ions may be divalent transition metal ions, such as manganese, nickel or cobalt, dissolved from the positive electrode active material. The divalent ions may be coordinated to six positions of each ion by one nitrilotriacetic acid and two imidazoles. The metal ions are coordinated to form a complex by the first polymer binder and the inorganic particles, so that their migration to the negative electrode and the side reaction with the electrolyte solution can be suppressed.

[0051] The porous coating layer may also include a second polymer binder. The second polymer binder does not include a ligand. The first polymer binder and the second polymer binder may combine the inorganic particles contained in the porous coating layer and provide adhesion to the porous coating layer. The first polymer binder includes the above-mentioned ligand and is used to adsorb metal ions so that the adhesion may be lower than the adhesion of the second polymer binder. The second polymer binder may provide the safety of the separator by maintaining the stable adhesion of the porous coating layer to the porous polymer substrate. For example, the content of the first polymer binder may be greater than or equal to the content of the second polymer binder. For example, the first polymer binder and the second polymer binder may be included in a weight ratio of about 7:3 to 5:5. When the content of the polymer binder is adjusted within the above range, a porous coating layer having good metal ion adsorption and stable adhesion to the porous substrate may be formed.

[0052] The first polymer binder and the second polymer binder may be selected from an acrylic polymer binder, a fluorine-based polymer binder, or a combination thereof. Preferably, the first polymer binder may be an acrylic polymer, and the second polymer binder may be a fluorine-based polymer binder.

[0053] The acrylic polymer binder may have repeating units comprising one or more monomers selected from the group consisting of (meth)acrylic acid, (meth)acrylic acid ester, propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, n-pentyl acrylate, isopentyl acrylate, n-ethylhexyl acrylate, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, methyl methacrylate, ethyl methacrylate, propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, n-pentyl methacrylate, isopentyl methacrylate, n-ethylhexyl acrylate, 2-hydroxyethyl acrylate, methyl methacrylate, ethyl methacrylate, propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, n-pentyl methacrylate, isopentyl methacrylate, n-ethylhexyl acrylate, 2-hydroxyethyl acrylate, acrylate, n-ethylhexyl methacrylate, 2-ethylhexyl methacrylate, hydroxyethyl methacrylate, (meth)acrylonitrile, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, ethyl (meth)acrylate, methyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, tert-butyl (meth)acrylate, amyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, lauryl (meth)acrylate, tetradecyl (meth)acrylate and pentafluorophenyl acrylate.

[0054] For example, the acrylic polymer binder may include one or more selected from the group consisting of polyacrylic acid, methyl acrylate, ethyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, ethylhexyl acrylate, methyl methacrylate, styrene-butadiene rubber, nitrile rubber, acrylonitrile-butadiene rubber, and acrylonitrile-butadiene-styrene rubber.

[0055] Fluorine-based polymer binders can be based on polyvinylidene fluoride. For example, fluorine-based polymer binders can be selected from one or more of polyvinylidene fluoride, polyhexafluoropropylene, polytetrafluoroethylene and polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP), polyvinylidene fluoride-trichloroethylene (PVDF-TCE) and polyvinylidene fluoride-chlorotrifluoroethylene (PVDF-CTFE), more particularly, copolymers containing polyvinylidene fluoride.

[0056] At least one of the first polymer binder and the second polymer binder may be in the form of particles. For example, the polymer binder may have a spherical or elliptical shape, but is not limited thereto. The average particle size (D50) of the polymer binder may be about 100 nm or more and 2000 nm or less. For example, the average particle size (D50) of the polymer binder may be about 200 nm to 1000 nm or 300 nm to 800 nm. When the particle size of the polymer binder particles is adjusted within the above range, the migration path of lithium ions and the adhesion of the porous coating to the porous substrate may be ensured at the same time.

[0057] The weight average molecular weight (Mw) of the first polymer binder and the second polymer binder can be about 40,000 or more and 500,000 or less. For example, the weight average molecular weight of the polymer binder can be about 50,000 or more and 450,000 or less, 100,000 or more and 400,000 or less, 150,000 or more and 350,000 or less, or 200,000 or more and 300,000 or less. For example, the weight average molecular weight of the first polymer binder can be about 40,000 to 100,000, and the weight average molecular weight of the second polymer binder can be about 40,000 to 200,000. When the weight average molecular weight of the polymer binder is adjusted within the above range, the polymer binder is uniformly dispersed to form a porous coating that simultaneously realizes the adsorption capacity of metal ions and the bonding capacity of porous polymer substrates.

[0058] In the present disclosure, the weight average molecular weight of the polymer binder can be measured by gel permeation chromatography (GPC) (PL GPC220, Agilent Technologies). For example, the weight average molecular weight can be determined by using trichlorobenzene (TCB) as a solvent in a PL Olexis (Polymer Laboratories) column (column temperature: 160°C), and using an Agilent high temperature RI detector (using cubic function correction, reference: polystyrene) under the conditions of a sample concentration of 1.0 mg / mL, a flow rate of 1.0 mL / min, and an injection volume of 200 μl.

[0059] Based on the total weight of the porous coating, the porous coating may contain about 40% to 80% by weight of inorganic particles. For example, based on the total weight of the porous coating, the content of the inorganic particles may be about 45% by weight or more and 75% by weight or less, 50% by weight or more and 70% by weight or less, or 55% by weight or more and 65% by weight or less. For example, based on the total weight of the porous coating, the content of the inorganic particles may be about 60% by weight or more and 80% by weight or less. The porous coating containing inorganic particles within the above ranges can reduce the thermal shrinkage of the porous polymer substrate and prevent short - circuiting of the electrodes due to the shrinkage of the separator.

[0060] The inorganic particles can be electrochemically stable. There is no particular limitation on the inorganic particles as long as no oxidation and / or reduction reaction occurs within the operating voltage range of the electrochemical device (e.g., based on Li / Li + is 0V to 5V). For example, using inorganic particles with a high dielectric constant can help increase the dissociation of electrolyte salts (such as lithium salts) in the liquid electrolyte, thereby improving the ionic conductivity of the electrolyte. For the above reasons, the inorganic particles can include high - dielectric - constant inorganic particles with a dielectric constant of 5 or greater, such as 10 or greater. Non - limiting examples of inorganic particles with a dielectric constant of 5 or greater include BaTiO3, Pb(Zr,Ti)O3 (PZT), Pb 1-x La x Zr 1-y Ti y O3 (PLZT, 0 < x < 1, 0 < y < 1), Pb(Mg 1 / 3 Nb 2 / 3 )O3 - PbTiO3 (PMN - PT), hafnium dioxide (HfO2), SrTiO3, SnO2, CeO2, MgO, NiO, CaO, ZnO, ZrO2, SiO2, Y2O3, Al2O3, Al(OH)3, SiC, AlOOH, TiO2, and mixtures thereof.

[0061] In addition, inorganic particles having lithium - ion transfer ability (i.e., inorganic particles containing the element lithium but not storing lithium and having the ability to transfer lithium ions) can be used as the inorganic particles. Non - limiting examples of inorganic particles having lithium - ion transfer ability include lithium phosphate (Li3PO4), lithium titanium phosphate (Li x Ti y (PO4)3, 0 < x < 2, 0 < y < 3), lithium aluminum titanium phosphate (Li x Al y Ti z (PO4)3, 0 < x < 2, 0 < y < 1, 0 < z < 3), (LiAlTiP) x O ySeries of glasses (0 < x < 4, 0 < y < 13), such as 14Li2O-9Al2O3-38TiO2-39P2O5, lithium lanthanum titanate (Li x La y TiO3, 0 < x < 2, 0 < y < 3), lithium germanium thiophosphate (Li x Ge y P z S w , 0 < x < 4, 0 < y < 1, 0 < z < 1, 0 < w < 5), such as Li 3.25 Ge 0.25 P 0.75 S4, lithium nitride (Li x N y , 0 < x < 4, 0 < y < 2), such as Li3N, SiS2 series of glasses (Li x Si y S z , 0 < x < 3, 0 < y < 2, 0 < z < 4), such as Li3PO4-Li2S-SiS2, and P2S5 series of glasses (Li x P y S z , 0 < x < 3, 0 < y < 3, 0 < z < 7), such as LiI-Li2S-P2S5, or a mixture of two or more of them.

[0062] In addition, inorganic particles with flame retardancy can be used to endow the separator with flame retardant properties or prevent the rapid increase in temperature inside the electrochemical element. Non-limiting examples of inorganic particles with flame retardancy include Sb2O3, Sb2O4, Sb2O5, SrTiO3, SnO2, CeO2, MgO, Mg(OH)2, NiO, CaO, ZnO, Zn2SnO4, ZnSnO3, ZnSn(OH)6, ZrO2, Y2O3, SiO2, Al2O3, AlOOH, Al(OH)3, SiC, TiO2, H3BO3, HBO2, and mixtures thereof.

[0063] The average particle size (D50) of the inorganic particles can be about 10nm or more and 10,000nm or less. For example, the average particle size (D50) of the inorganic particles can be about 100nm or more and 9,000nm or less, 1,000nm or more and 8,000nm or less, 2,000nm or more and 7,000nm or less, 3,000nm or more and 6,000nm or less, or 4,000nm or more and 5,000nm or less. For example, the average particle size of the inorganic particles can be about 100nm or more and 700nm or less. When the average particle size of the inorganic particles is less than 10nm, due to the increase in specific surface area, an additional polymer binder for bonding between the inorganic particles is required, which is disadvantageous in terms of resistance. When the average particle size of the inorganic particles exceeds 10,000nm, the uniformity of the surface of the coating may be reduced, and damage to the porous polymer substrate or electrode may occur during lamination.

[0064] The porous coating can be formed by coating at least one surface of a porous polymer substrate with a coating slurry comprising a first polymer binder, inorganic particles and a dispersion medium. The coating slurry may also include a second polymer binder. For example, the separator may be prepared by applying the coating slurry to at least one side of the porous polymer substrate and then drying to remove the dispersion medium. The porous coating may have a porous structure comprising a gap volume in which inorganic particles are connected by a first polymer binder or a first polymer binder and a second polymer binder. The porous coating adheres to the porous polymer substrate while allowing lithium ions to pass therethrough, thereby preventing thermal shrinkage of the porous polymer substrate.

[0065] The coating slurry may include a dispersion medium for dissolving or dispersing at least a portion of the polymer binder and dispersing the inorganic particles. By controlling the type and content of the dispersion medium, a coating slurry in which the inorganic particles are uniformly dispersed may be used. The example of the dispersion medium includes water, ethanol, acetone, isopropyl alcohol (IPA), dimethylacetamide (DMAc), dimethylformamide (DMF), N-methyl-2-pyrrolidone (NMP), acetonitrile, and combinations thereof. The above-mentioned type of dispersion medium may be used to form a porous coating in which the inorganic particles are uniformly dispersed.

[0066] The viscosity of the coating slurry may be about 100cps or more and 1,000cps or less. For example, the viscosity of the coating slurry may be about 200cps or more and 900cps or less, 300cps or more and 800cps or less, 400cps or more and 700cps or less, or 500cps or more and 600cps or less. For example, the viscosity of the coating slurry may be about 300cps or more and 800cps or less. When the viscosity of the coating slurry exceeds 1,000cps, a slurry (D99 about 100μm) with a very large particle size (D99) is formed, which makes it difficult to manufacture the separator by continuous application on a porous polymer substrate, making it difficult to ensure productivity.

[0067] The coating slurry may also contain additives such as dispersants, surfactants, defoamers, flame retardants and wetting agents to improve dispersibility and flame retardancy and improve the uniformity of the porous coating formed. Examples of dispersants include one or more selected from oil-soluble polyamines, oil-soluble amine compounds, fatty acids, fatty alcohols, sorbitan fatty acid esters, tannic acid, pyrogallic acid and polyacrylic acid. By using the above-mentioned types of dispersants, the stability of the coating slurry can be improved and the uniformity of the porous coating formed by the coating slurry can be ensured.

[0068] Based on the total weight of the coating slurry, the additive may be included in an amount of 0 wt % or more and 5 wt % or less. For example, the content of the additive may be about 0.01 wt % or more and 4 wt % or less, 0.1 wt % or more and 3 wt % or less, or 1 wt % or more and 2 wt % or less. For example, the content of the additive may be about 3 wt % or more and 5 wt % or less. When the content of the additive is adjusted within the above range, uniform dispersion and stability of the inorganic particles contained in the coating slurry may be achieved.

[0069] After forming the porous coating, the dispersion medium contained in the coating slurry can be removed by drying or heating. For example, the porous coating can include about 5ppm or less dispersion medium. For example, the porous coating can be composed of a first polymer binder and inorganic particles, or composed of a first polymer binder, a second polymer binder and inorganic particles. In the process of removing the dispersion medium, a plurality of holes can be formed on the surface and inside of the porous coating. The hole can include the interstitial volume formed between the inorganic particles, and can have a structure in which a three-dimensional network is formed to allow fluid to pass.

[0070] The thickness of the porous coating layer may be about 1 μm or more and 15 μm or less. For example, the thickness of the porous coating layer may be about 2 μm or more and 14 μm or less, 3 μm or more and 13 μm or less, 4 μm or more and 12 μm or less, 5 μm or more and 11 μm or less, 6 μm or more and 10 μm or less, or 7 μm or more and 9 μm or less. For example, the thickness of the porous coating layer may be about 1 μm or more and 5 μm or less. When the thickness of the porous coating layer is adjusted within the above range, the shrinkage of the porous polymer substrate may be minimized and stable adhesion to the porous polymer substrate may be achieved.

[0071] The permeability of the separator for electrochemical device can be about 50 seconds / 100cc or more and 150 seconds / 100cc or less. For example, the permeability of the separator can be 60 seconds / 100cc or more and 140 seconds / 100cc or less, 70 seconds / 100cc or more and 130 seconds / 100cc or less, 80 seconds / 100cc or more and 120 seconds / 100cc or less, or 90 seconds / 100cc or more and 110 seconds / 100cc or less. For example, the permeability of the separator can be about 100 seconds / 100cc or more and 120 seconds / 100cc or less. When the permeability of the separator is within the above range, the output, stability and cycle characteristics of the electrochemical device can be ensured.

[0072] According to another embodiment of the present disclosure, the electrochemical device includes a positive electrode, a negative electrode and a separator between the positive electrode and the negative electrode, wherein the separator is the separator of the above embodiment. The electrochemical device can be manufactured by inserting an electrode assembly including a positive electrode, a negative electrode and a separator between the positive electrode and the negative electrode into a housing or a bag, and sealing the housing or the bag. Before the housing or the bag is sealed, the electrode assembly can be impregnated with an electrolyte solution by injecting an electrolyte solution. The shape of the housing or the bag is not limited. For example, the electrochemical device can be a cylindrical, prismatic, coin-shaped or pouch-shaped lithium secondary battery.

[0073] The positive electrode and the negative electrode can be coated by applying an electrode active material on at least one surface of each current collector and drying. The current collector can be a material that has conductivity without causing chemical changes in the electrochemical device. Examples of current collectors for the positive electrode include aluminum, nickel, titanium, fired carbon, and stainless steel; and aluminum or stainless steel subjected to surface treatment with carbon, nickel, titanium or silver, but are not limited thereto. Examples of current collectors for the negative electrode include copper, nickel, titanium, fired carbon, and stainless steel; and copper or stainless steel subjected to surface treatment with carbon, nickel, titanium or silver, but are not limited thereto. The current collector can be in various forms, such as a thin metal plate, a film, a foil, a mesh, a porous material, or a foam.

[0074] The positive electrode includes a positive current collector and a positive electrode active material layer containing a positive electrode active material, a conductive material, and a binder resin on at least one surface of the current collector. The positive electrode active material includes layered compounds such as lithium manganese composite oxides (e.g., LiMn2O4 and LiMnO2), lithium cobalt oxide (LiCoO2), and lithium nickel oxide (LiNiO2), or compounds substituted with one or more transition metal elements; compounds represented by the formula Li 1+x Mn 2-x O4 (where x is from 0 to 0.33), LiMnO3, LiMn2O3, or LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, LiV3O4, V2O5, Cu2V2O7; Ni-site type lithium nickel oxides represented by the formula LiNi 1-x M x O2 (where M = Co, Mn, Al, Cu, Fe, Mg, B, or Ga, and x = 0.01 to 0.3); lithium manganese composite oxides represented by the formula LiMn 1-x M x O2 (where M = Co, Ni, Fe, Cr, Zn, or Ta, and x = 0.01 to 0.1) or Li2Mn3MO8 (where M = Fe, Co, Ni, Cu, or Zn); LiMn2O4 in which some Li in the formula is replaced by alkaline earth metal ions; disulfide compounds; Fe2(MoO4)3, and these can be used alone or in a mixture of two or more of them. For example, the positive electrode active material may contain one or more transition metal elements.

[0075] The negative electrode includes a negative current collector and a negative electrode active material layer containing a negative electrode active material, a conductive material, and a binder resin on at least one surface of the current collector. The negative electrode active material in the negative electrode includes carbon such as lithium metal oxides, hard carbon, and graphite carbon; silicon-based materials such as Li x Fe2O3 (0 ≤ x ≤ 1), Li x WO2 (0 ≤ x ≤ 1), Si, SiO x (0 < x < 2), SiC, and Si alloys; metal composite oxides such as Sn x Me 1-x Me' y O z(Me: Mn, Fe, Pb, Ge; Me': Al, B, P, Si, elements of Group 1, Group 2 and Group 3 of the periodic table, halogens; 0 < x ≤ 1; 1 ≤ y ≤ 3; 1 ≤ z ≤ 8); lithium metal; lithium alloy; tin-based alloy; metal oxides such as SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4 and Bi2O5; conductive polymers such as polyacetylene; Li-Co-Ni-based materials; and titanium oxides, which can be used alone or in a mixture of two or more of them.

[0076] The conductive material can be any one of the conductive materials selected from the following or a mixture of two or more conductive materials: graphite, carbon black, carbon fiber or metal fiber, metal powder, conductive whisker, conductive metal oxide, carbon nanotube, activated carbon and polyphenylene derivative. The carbon nanotube has a cylindrical graphite sheet with a diameter of nanoscale and an sp 2 bonded structure, and exhibits conductor or semiconductor characteristics according to the rolling angle and structure of the graphite sheet. The carbon nanotube can be classified into single-walled carbon nanotube (SWCNT), double-walled carbon nanotube (DWCNT) and multi-walled carbon nanotube (MWCNT) based on the number of bonds constituting its wall, and the carbon nanotube can be appropriately selected based on the application of the dispersion. For example, the conductive material can be one selected from the following: natural graphite, artificial graphite, super-p, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, Denka black, aluminum powder, nickel powder, zinc oxide, potassium titanate and titanium oxide, or a mixture of two or more of them.

[0077] The binder resin that can be used herein can be any binder resin commonly used for the electrodes of electrochemical devices. Non-limiting examples of the binder resin include polyvinylidene fluoride-copoly-hexafluoropropylene, polyvinylidene fluoride-copoly-trichloroethylene, poly(methyl methacrylate), poly(ethylhexyl acrylate), poly(butyl acrylate), polyacrylonitrile, polyvinylpyrrolidone, polyvinyl acetate, polyethylene-copoly-vinyl acetate, poly(ethylene oxide), polyarylate, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, cyanoethyl sucrose, pullulan and carboxymethyl cellulose, but are not limited thereto.

[0078] The electrolyte can be obtained by making a material having such as A+ B - A salt of the structure of is obtained by dissolving or dissociating in an organic solvent, wherein A + Including alkali metal cations such as Li + 、Na + or K + , or a combination thereof, and B - Including anions such as PF6 - 、BF4 - , Cl - Br - ,I - 、ClO4 - 、AsF6 - 、CH3CO2 - CF3SO3 - 、N(CF3SO2)2 - or C(CF2SO2)3 - , or a combination thereof, the organic solvent being, for example, propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, tetrahydrofuran, N-methyl-2-pyrrolidone (NMP), ethyl methyl carbonate (EMC), γ-butyrolactone, or a mixture thereof.

[0079] The electrochemical device including the electrode assembly may be a lithium secondary battery. The battery may be used as a unit cell, and may be used as a battery module including a unit cell and a battery pack including a battery module. The battery pack may be used as a power source for various electrical devices. Examples of the device include small devices such as computers, mobile phones, and power tools; electric vehicles powered by electric motors, including electric vehicles (EV), hybrid electric vehicles (HEV), and plug-in hybrid electric vehicles (PHEV); electric two-wheeled vehicles, including electric bicycles (E-bike) and electric scooters (E-scooters); electric golf carts; and medium to large devices, such as power storage systems, but not limited thereto.

[0080] Another embodiment of the present invention provides a method for preparing a separator for an electrochemical device, the method comprising forming a porous coating layer comprising a first polymer binder and inorganic particles on at least one surface of a porous polymer substrate. The contents overlapping with those described in the separator for an electrochemical device are replaced with the description of the aforementioned embodiment.

[0081] The step of forming the porous coating layer can include preparing a coating slurry comprising a first polymer binder, inorganic particles and a dispersion medium, and applying the coating slurry to at least one surface of the porous polymer substrate, followed by drying. The first polymer binder and the inorganic particles can each be introduced with different ligands. The coating slurry can also include a second polymer binder that is not introduced into a ligand.

[0082] The step of forming the porous coating layer may further include subjecting at least one surface of the porous polymer substrate to a corona discharge treatment before applying the coating slurry to the porous polymer substrate. The step of subjecting at least one surface of the porous polymer substrate to a corona discharge treatment can prevent the bonding force between the porous polymer substrate surface and the coating surface from being reduced at high temperatures, and prevent the bonding force between the polymer substrate surface and the coating surface from being reduced due to the electrolyte.

[0083] At least one surface of a porous polymer substrate can be subjected to corona discharge treatment in air at a voltage of about 0.1 kV or greater and 10 kV or less. For example, the corona discharge treatment can be carried out at the following voltages: 0.2 kV or greater and 9 kV or less, 0.3 kV or greater and 8 kV or less, 0.4 kV or greater and 7 kV or less, 0.5 kV or greater and 6 kV or less, 0.6 kV or greater and 5 kV or less, 0.7 kV or greater and 4 kV or less, 0.8 kV or greater and 3 kV or less, 0.9 kV or greater and 2 kV or less, or 1.0 kV or greater and 2 kV or less. Preferably, the corona discharge treatment can be carried out in air at a voltage of 1.8 kV. When the applied voltage of the corona discharge treatment is adjusted within the above range, a suitable number of functional groups can be formed on the surface of the polymer substrate, and typically prevent damage to the surface of the polymer substrate.

[0084] The step of forming a porous coating layer may include applying a coating slurry to a porous polymer substrate to form a coating layer. For example, the coating layer may be formed by, but is not limited to, a rod coater, a wire rod coater, a roller coater, a spray coater, a spin coater, an inkjet coater, a screen coater, a reverse coater, a gravure coater, a knife coater, a slot die coater, a hot melt coater, a comma coater, and a direct metering coater. Preferably, the step of forming a porous coating layer may include using a rod coater or a slot die coater to simultaneously coat two surfaces of the porous polymer substrate with the coating slurry.

[0085] The step of forming a porous coating may include applying a coating slurry to a porous polymer substrate, followed by drying or heating the coating to evaporate the dispersion medium contained in the coating. The removal of the dispersion medium may be performed at a temperature that allows only the dispersion medium contained in the coating to evaporate without modifying the polymer binder contained in the coating. For example, the removal of the dispersion medium may be achieved by heating the coating to a predetermined temperature, but ensuring that the temperature of the coating surface does not exceed 60°C. When the coating is heated under the above conditions, the thermal energy may be first used to heat the dispersion medium and change the phase, and may not be used to modify the polymer binder.

[0086] Hereinafter, the present disclosure will be described in more detail with reference to specific embodiments and experimental examples. The following embodiments and experimental examples merely illustrate the present disclosure, and the present disclosure is not limited to the following embodiments and experimental examples.

[0087] Example 1

[0088] Preparation of coating slurry

[0089] The first polymer binder is prepared by introducing nitrilotriacetic acid (NTA) as a ligand into an acrylate-based polymer binder. Specifically, at room temperature (25°C), 11g of pentafluorophenyl acrylate (PFA) is dissolved in 200mL of anhydrous dimethylformamide (DMF), and then mixed with a solution of 12g of amine-substituted nitrilotriacetic acid (NH2(CH2)4NTA) dissolved in 10mL of distilled water. Another 210mL of triethylamine (TEA) is added to the mixed solution, and then heated at 50°C for 6 hours. The mixed solution is dialyzed in distilled water to remove dimethylformamide, and dried in a vacuum oven at 40°C for 1 hour, thereby producing 8.5g of the first polymer binder (weight average molecular weight: 58,000) containing nitrilotriacetic acid.

[0090] The second polymer binder used here is commercially available polyvinylidene fluoride-hexafluoropropylene (weight average molecular weight: 100,000, HFP substitution degree 10%).

[0091] N-(3-triethoxysilylpropyl)-4,5-dihydroimidazole and tetraethylorthosilicate (TEOS) were introduced into ethanol and condensed under hydrochloric acid and sodium chloride catalysts to oligomerize. The oligomerized silanes were then mixed and copolymerized under triethylamine catalyst to obtain gel-like imidazole-substituted silica particles. The gel was washed with water and ethanol in this order using a centrifuge and then dried in a vacuum oven at 40° C. for 24 hours, thereby producing imidazole-introduced silica in a solid state (average particle size (D50): 500 nm).

[0092] At room temperature (25° C.), 15.2 g of a first polymer binder (an acrylic binder into which NTA was introduced), 15.2 g of a second polymer binder (PVDF-HFP), 26.9 g of inorganic particles (silica into which imidazole was introduced), and 0.76 g of PAA as an additive were added to 124 mL of NMP and stirred with a vibrator for 60 minutes to prepare a coating slurry.

[0093] Preparation of porous polymer substrates

[0094] As the porous polymer substrate, a polyethylene film (MI: 0.2 g / 10 min, Tm: 135° C., porosity: 45%, average pore size: 45 nm) having a size of 20 cm×30 cm and a thickness of 9 μm was used.

[0095] Preparation of separators

[0096] The coating slurry was coated on both surfaces of the polyethylene film using a bar coater to form a coating layer with a thickness of 3 μm (the composition of the porous coating layer was 20 wt % of the first polymer binder, 20 wt % of the second polymer binder and 60 wt % of the inorganic particles based on the total weight of the porous coating layer).

[0097] The process of applying a low-temperature air flow to the polyethylene film having the coating layer formed thereon and removing the dispersion medium was repeated 5 times to prepare a separator having a total thickness of 15 μm.

[0098] Example 2

[0099] Preparation of coating slurry

[0100] As the first polymer binder, commercially available polyvinyl imidazole (weight average molecular weight 100,000) was used.

[0101] As the second polymer binder, commercially available polyvinylidene fluoride-hexafluoropropylene was used as in Example 1.

[0102] Inorganic particles are prepared by introducing nitrilotriacetic acid as a ligand into silica. For example, 40.5 g of amine-substituted cationic silica gel and 33.5 g of nitrilotriacetic acid are added to 500 mL of pyridine to prepare a dispersion. The dispersion is stirred and reacted at 90° C. for 3 hours under a reflux system, then cooled to room temperature, and 0.5 M sodium bicarbonate is added to neutralize unreacted nitrilotriacetic acid. The reactant is washed in this order with distilled water, ethanol and diethyl ether using a centrifuge, and then dried at room temperature for 24 hours, thereby producing a solid silicon dioxide (average particle size (D50): 700 nm) into which nitrilotriacetic acid is introduced.

[0103] At room temperature (25° C.), 15.2 g of a first polymer binder (polyvinyl imidazole), 15.2 g of a second polymer binder (PVDF-HFP), 26.9 g of inorganic particles (silica in which NTA was introduced), and 0.76 g of PAA as an additive were added to 124 mL of NMP and stirred with a vibrator for 60 minutes to prepare a coating slurry.

[0104] Preparation of separators

[0105] The same porous polymer substrate used in Example 1 was used, and a separator was prepared in the same manner as in Example 1.

[0106] Comparative Example 1

[0107] The separator was prepared in the same manner as in Example 1, except that an acrylic binder introduced with NTA was used as the first polymer binder, PVDF-HFP was used as the second polymer binder, and silica introduced with NTA was used as the inorganic particles when preparing the coating slurry. (The composition of the porous coating layer was 20 wt % of the first polymer binder, 20 wt % of the second polymer binder, and 60 wt % of the inorganic particles based on the total weight of the porous coating layer).

[0108] Comparative Example 2

[0109] The separator was prepared in the same manner as in Example 1, except that polyvinyl imidazole was used as the first polymer binder, PVDF-HFP was used as the second polymer binder, and imidazole-introduced silica was used as the inorganic particles when preparing the coating slurry. (Based on the total weight of the porous coating layer, the composition of the porous coating layer was 20 wt % of the first polymer binder, 20 wt % of the second polymer binder, and 60 wt % of the inorganic particles).

[0110] Comparative Example 3

[0111] The separator was prepared in the same manner as in Example 1, except that an acrylic binder introduced with NTA was used as the first polymer binder, PVDF-HFP was used as the second polymer binder, and silica was used as the inorganic particles when preparing the coating slurry. (The composition of the porous coating layer was 20 wt % of the first polymer binder, 20 wt % of the second polymer binder, and 60 wt % of the inorganic particles based on the total weight of the porous coating layer).

[0112] Comparative Example 4

[0113] The separator was prepared in the same manner as in Example 1, except that polyvinyl imidazole was used as the first polymer binder, PVDF-HFP was used as the second polymer binder, and the silica of Comparative Example 3 was used as the inorganic particles when preparing the coating slurry. (Based on the total weight of the porous coating layer, the composition of the porous coating layer was 20 wt % of the first polymer binder, 20 wt % of the second polymer binder, and 60 wt % of the inorganic particles).

[0114] Comparative Example 5

[0115] The separator was prepared in the same manner as in Example 1, except that polyvinyl imidazole and an acrylic binder introduced with NTA were used as the first polymer binder, PVDF-HFP was used as the second polymer binder, and the silica introduced in Comparative Example 3 was used as the inorganic particles when preparing the coating slurry. (The composition of the porous coating layer was 10 wt % of polyvinyl imidazole, 10 wt % of an acrylic binder introduced with NTA, 20 wt % of the second polymer binder, and 60 wt % of the inorganic particles, based on the total weight of the porous coating layer).

[0116] Comparative Example 6

[0117] The separator was prepared in the same manner as in Example 1, except that when preparing the coating slurry, the first polymer binder was not used, PVDF-HFP was used as the second polymer binder, and NTA-introduced silica was used as the inorganic particles. (Based on the total weight of the porous coating layer, the composition of the porous coating layer was 40 wt % of the second polymer binder and 60 wt % of the inorganic particles).

[0118] Comparative Example 7

[0119] The separator was prepared in the same manner as in Example 1, except that when preparing the coating slurry, the first polymer binder was not used, PVDF-HFP was used as the second polymer binder, and silica introduced with imidazole was used as the inorganic particles. (Based on the total weight of the porous coating layer, the composition of the porous coating layer was 40 wt % of the second polymer binder and 60 wt % of the inorganic particles).

[0120] Comparative Example 8

[0121] The separator was prepared in the same manner as in Example 1, except that when preparing the coating slurry, the first polymer binder was not used, PVDF-HFP was used as the second polymer binder, and NTA-introduced silica and imidazole-introduced silica were used as inorganic particles. (Based on the total weight of the porous coating layer, the composition of the porous coating layer was 40 wt% of the second polymer binder, 30 wt% of NTA-introduced silica, and 30 wt% of imidazole-introduced silica).

[0122] Experimental Example: Determination of the Characteristics of the Separator

[0123] The properties of the separators prepared in Examples and Comparative Examples were determined and shown in Table 1 below.

[0124] Permeability measurement

[0125] The permeability was measured using a Gurley densometer (Gurley, 4110N) to determine the flow rate of 100 cc of air through a 28.6 mm diameter and 645 mm area. 2 The time taken for the separators to be

[0126] Measurement of battery life characteristics

[0127] The amount of lithium manganese composite oxide: conductive material (Denka black): binder (PVdF) was weighed into a weight ratio of 95:2.5:2.5, added to N-methylpyrrolidone (NMP) and mixed to prepare a positive electrode active material slurry, which was then coated on a 20 μm thick aluminum foil to a thickness of 200 μm, followed by roll pressing and drying to prepare a positive electrode.

[0128] A Li metal plate having a thickness of 200 μm was used as a negative electrode, and the positive electrode and the negative electrode were stacked with the separator of the example or the comparative example in between, and then inserted into an aluminum bag.

[0129] An electrolyte containing 3 mol of vinylene carbonate (VC), 1.5 mol of propane sultone (PS), 1 mol of ethylene sulfate (ESa), and 1 mol of lithium salt LiPF6 as additives in a solvent in which ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed in a weight ratio of 3 / 7 in an amount of 1 g was injected into an aluminum bag, and the bag was sealed to prepare a battery.

[0130] The prepared battery was subjected to single charge and discharge at a rate of 0.1 C in a voltage range of 3.0 V to 4.4 V, followed by 300 charge and discharge cycles at a rate of 1.0 C each, in a 25° C. room to determine the life characteristics. The life characteristics were expressed as a capacity retention ratio by calculating the ratio of the discharge capacity after 300 cycles to the initial discharge capacity.

[0131] In addition, the resistance was measured before and after 300 cycles to determine the resistance increase rate.

[0132] [Table 1]

[0133]

[0134] As shown in Table 1, for example, the capacity retention rate after 300 cycles in the example is relatively higher than that in the comparative example, and the resistance increase rate after 300 cycles in the example is relatively lower than that in the comparative example.

[0135] From the foregoing, it will be understood that, for illustrative purposes, various embodiments of the present disclosure are described herein, and various modifications may be made without departing from the scope and spirit of the present disclosure. Therefore, the various embodiments disclosed herein are not intended to be limiting, with the true scope and spirit being indicated by the appended claims.

Claims

1. A separator for an electrochemical device, comprising: a porous polymer substrate; as well as a porous coating layer comprising a first polymer binder and inorganic particles and formed on at least one surface of the porous polymer substrate, The first polymer binder and the inorganic particles are each introduced with different ligands. 2 . The separator according to claim 1 , wherein the first polymer binder and the inorganic particles form a coordination bond to a single metal ion. 3 . The separator according to claim 1 , wherein the first polymer binder and the inorganic particles are each independently chemically bonded to one or more ligands selected from a first ligand having a single degree of toothing and a second ligand having two or more degrees of toothing. 4 . The separator according to claim 3 , wherein the first ligand is at least one selected from the group consisting of imidazole, pyrazole, triazole, tetrazole, indazole, benzimidazole, azaindole, purine, and derivatives thereof. 5 . The separator according to claim 3 , wherein the second ligand is at least one selected from the group consisting of nitrilotriacetic acid, iminodiacetic acid, ethylenediaminetetraacetic acid, 1,2-cyclohexanediaminetetraacetic acid, and derivatives thereof. The separator according to claim 5 , wherein the inorganic particles have the second ligand chemically bonded to surfaces thereof. 7 . The separator according to claim 1 , wherein the inorganic particles are included at 40 wt % to 80 wt % based on the total weight of the porous coating layer.

8. The separator according to claim 1, wherein the porous coating further comprises a second polymer binder, and The content of the first polymer binder is greater than or equal to the content of the second polymer binder.

9. An electrochemical device comprising: positive electrode; negative electrode; and A separator disposed between the positive electrode and the negative electrode, The separator is the separator for an electrochemical device according to claim 1.

10. The electrochemical device according to claim 9, wherein metal ions are generated during charging and discharging of the electrochemical device. The electrochemical device according to claim 10 , wherein the metal ions are transition metal ions derived from the positive electrode.