A medium-entropy alloy, its preparation method and application
By adding Al, Ti, and W elements to the CoCrNi alloy and combining hot extrusion and heat treatment processes, the microstructure of the alloy was optimized, solving the problem of its low yield strength and tensile strength. This resulted in a high-strength, high-plasticity, and corrosion-resistant medium-entropy alloy suitable for structural materials in seawater or acidic environments.
Patent Information
- Application Number
- CN202411439837.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-15
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-10-15
AI Technical Summary
The low yield strength and tensile strength of CoCrNi medium-entropy alloys limit their widespread application.
The microstructure and properties of the CoCrNi alloy are optimized by adding trace elements of Al, Ti and W and controlling the formation of precipitates through hot extrusion, cold rolling and heat treatment processes.
It achieves a combination of high strength and high plasticity in the alloy, possessing excellent mechanical properties and corrosion resistance, making it suitable as a structural material for seawater or acidic environments.
Smart Images

Figure CN119320901B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of metal alloy materials technology, and in particular to a medium-entropy alloy, its preparation method, and its application. Background Technology
[0002] In recent years, multi-principal element alloys, as a novel type of metallic alloy material, have attracted widespread attention due to their unique four core effects, exhibiting excellent mechanical and physicochemical properties. This new type of metallic alloy has shown great application potential in numerous fields and has rapidly become a cutting-edge research hotspot in materials science. Among the many multi-principal element alloy systems, the CoCrNi medium-entropy alloy stands out due to its excellent room-temperature tensile plasticity and high fracture toughness. However, its relatively low yield strength and tensile strength limit its wider application to some extent. Summary of the Invention
[0003] Based on the above, this invention provides a medium-entropy alloy, its preparation method, and its applications. This invention precisely controls the formation of precipitated phases by adding trace elements of Al, Ti, and W to the alloy matrix (CoCrNi). Furthermore, to further optimize the alloy's microstructure and properties, this invention combines hot extrusion, cold rolling, and heat treatment processes to control the grain size and precipitated phase distribution, thereby optimizing and improving the alloy's performance.
[0004] To achieve the above objectives, the present invention provides the following solution:
[0005] One of the technical solutions of this invention is a medium-entropy alloy with the chemical formula Co. 54 Cr 25 Ni 10 Al3Ti3W5 (at.%).
[0006] The second technical solution of the present invention is a method for preparing the above-mentioned medium-entropy alloy, comprising the following steps:
[0007] According to Co 54 Cr 25 Ni 10 Al3Ti3W5 atomic percentage: Co, Cr, Ni, Al, Ti and W metallic elements are mixed and vacuum arc melted to obtain button ingots;
[0008] The button ingots are induction melted and then cast to obtain medium-entropy alloy ingots;
[0009] The medium-entropy alloy ingot is subjected to homogenization annealing, followed by heat holding, hot extrusion, and cooling to obtain the medium-entropy alloy.
[0010] The third technical solution of this invention is the application of the above-mentioned medium-entropy alloy in the preparation of structural materials for use in seawater or acidic environments.
[0011] The fourth technical solution of the present invention is a structural material, the raw materials of which include the above-mentioned medium-entropy alloy.
[0012] The present invention discloses the following technical effects:
[0013] (1) The present invention designs a Co-rich low stacking fault energy medium entropy alloy, so that the deformation mechanism of the alloy is dominated by stacking faults, thereby maintaining high strength while maintaining excellent elongation.
[0014] (2) Through appropriate composition design, under the combined action of Cr, Ti and W elements, the alloy has excellent mechanical properties while maintaining certain corrosion resistance. It has a high pitting potential in 3.5wt.% NaCl and a low corrosion current density in 0.5M H2SO4 solution.
[0015] (3) This invention applies the hot extrusion process commonly used in traditional alloys to the preparation of as-cast medium-entropy alloys. By adjusting the preparation and post-processing techniques, this invention obtains a medium-entropy alloy with high strength and high plasticity while maintaining certain corrosion resistance, which can be used as a structural material in seawater or acidic environments. Attached Figure Description
[0016] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0017] Figure 1 (a) Vickers hardness, (b) engineering stress-strain curves, and (c) strength and elongation variation curves for samples HE, HE-873-1, HE-973-1, HE-1073-1, and HE-1173-1.
[0018] Figure 2 (a) Vickers hardness, (b) engineering tensile stress-strain curves, (c) strength and elongation variation curves, and (d) strength-elongation product and yield strength comparison with data in the literature for samples HE, HE-973-1, HE-973-8, HE-973-12 and HE-973-16.
[0019] Figure 3XRD results of (a) HE-873-1, HE-973-1, HE-1073-1 and HE-1173-1 samples, and (b) XRD results of HE-973-8, HE-973-12 and HE-973-16 samples.
[0020] Figure 4 SEM images of samples (a) HE, (b) HE-873-1, (c) HE-973-1, (d) HE-1073-1, and (e) HE-1173-1; and a magnified SEM image of sample HE-1173-1. EDS results for the region indicated by the red box in (f): (g) Co, (h) Cr, (i) Ni, (j) Al, (k) Ti, and (l) W.
[0021] Figure 5 SEM images of samples (a) HE-973-8, (b) HE-973-12 and (c) HE-973-16.
[0022] Figure 6 (a) TEM bright-field image of HE-973-12 sample, (b) TEM dark-field image of region R1 in (a) and (c) SAED result; (d) TEM bright-field image of annealed twin and (e) SAED result of region R2 in (d); (f) TEM bright-field image of stacking fault.
[0023] Figure 7 The following are the results of the EDS surface scan of the corresponding regions of HE-973-12 sample: (a) high-angle annular dark field, (b) Fourier transform results of region R3 and (c) R4, and (a) EDS surface scan results of the corresponding regions: (d) Co, (e) Cr, (f) Ni, (g) Al, (h) Ti, (i) W.
[0024] Figure 8 (a) The true stress-strain and strain hardening rate curves of the HE-973-12 specimen, (b) Schematic diagram of microstructure changes during deformation, (c)-(e) KAM diagrams of the HE-973-12 specimen under different strains and (f)-(h) BC diagrams.
[0025] Figure 9 (a) Engineering stress-strain curves; (b) Vickers hardness for samples HE, HE+CR, HE+CR+1273K 1min and HE+CR+1273K 1min+973K 12h.
[0026] Figure 10 XRD results for the HE+CR, HE+CR+1273K 1min and HE+CR+1273K 1min+973K 12h samples.
[0027] Figure 11 SEM images of (a) HE+CR, (b) HE+CR+1273K 1min and (c) HE+CR+1273K 1min+973K 12h samples; EDS image of the area shown in the red box in (c): (d) Co, (e) Cr, (f) Ni, (g) Al, (h) Ti, (i) W.
[0028] Figure 12 BC plot, IPF plot and GND plot of samples (a)(d)(g)HE+CR, (b)(e)(h)HE+CR+1273K 1min and (c)(f)(i)HE+CR+1273K1min+973K 12h.
[0029] Figure 13 (a) TEM image of the sample subjected to HE+CR+1273K 1min+973K 12h, (b) magnified view of region S1 in (a), (c) dark field image of (b); (b) corresponding EDS results: (d) Co, (e) Cr, (f) Ni, (g) Al, (h) Ti, (i) W; (j) SAED result of region S2 in (b); (k) high-resolution image of W-rich phase, (l) FFT result of region S3 in (k).
[0030] Figure 14 The following are the TEM images of the grain boundaries of the HE+CR+1273K 1min+973K 12h samples: (a) TEM image, (b) magnified view of region S4 in (a), (c) SAED result of region S6 in (b), (d) SAED result of region S5 in (b), and the corresponding EDS results for (b): (e) Co, (f) Cr, (g) Ni, (h) Al, (i) Ti, (j) W.
[0031] Figure 15 (a)E for HE-973-12 and HE+CR+1273K 1min+973K 12h samples and samples in the literature pit The comparison, (b) 1 / E pit -1 / (E pit -E corr )curve.
[0032] Figure 16 (a) Nyquist plot, (b) Bode impedance plot, (c) Bode phase angle plot, and (d) equivalent circuit diagram for As cast (cast specimen), HE-973-12, and HE+CR+1273K 1min+973K 12h specimens.
[0033] Figure 17SEM and corresponding EDS results for samples (a)(b)(c) As cast, (d)(e)(f) HE-973-12 and (g)(h)(i) HE+CR+1273K1min+973K12h.
[0034] Figure 18 XPS fitting results of passivation film formation in 3.5 wt.% NaCl solution for samples (a)-(e) As cast (cast sample), (f)-(j) HE-973-12, (k)-(o) HE+CR+1273K1min+973K12h.
[0035] Figure 19 (a) Open circuit potential versus time curve, (b) Tafel curve, (c) Comparison of corrosion current density and corrosion potential of the sample in this invention with alloys in the literature.
[0036] Figure 20 SEM and corresponding EDS results for samples (a)(b)(c) As cast, (d)(e)(f) HE-973-12 and (g)(h)(i) HE+CR+1273K1min+973K12h. Detailed Implementation
[0037] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as a limitation of the present invention, but rather as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0038] It should be understood that the terminology used in this invention is merely for describing particular embodiments and is not intended to limit the invention. Furthermore, with respect to numerical ranges in this invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Any stated value or intermediate value within a stated range, as well as each smaller range between any other stated value or intermediate value within said range, is also included in this invention. The upper and lower limits of these smaller ranges may be independently included or excluded from the range.
[0039] Unless otherwise stated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. While only preferred methods and materials have been described herein, any methods and materials similar or equivalent to those described herein may be used in the implementation or testing of this invention. All references to this specification are incorporated by way of citation to disclose and describe methods and / or materials associated with those references. In the event of any conflict with any incorporated reference, the content of this specification shall prevail.
[0040] Various modifications and variations can be made to the specific embodiments described in this specification without departing from the scope or spirit of the invention, as will be apparent to those skilled in the art. Other embodiments derived from this specification will also be apparent to those skilled in the art. This specification and embodiments are merely exemplary.
[0041] The terms “include,” “including,” “have,” “contain,” etc., used in this article are all open-ended terms, meaning that they include but are not limited to.
[0042] The first aspect of this invention provides a medium-entropy alloy with the chemical formula Co. 54 Cr 25 Ni 10 Al3Ti3W5 (at.%).
[0043] A second aspect of the present invention provides a method for preparing the above-mentioned medium-entropy alloy, comprising the following steps:
[0044] According to Co 54 Cr 25 Ni 10 Al3Ti3W5 atomic percentage: Co, Cr, Ni, Al, Ti and W metallic elements are mixed and vacuum arc melted to obtain button ingots (40g / piece);
[0045] Ten of the above-mentioned button ingots were induction melted and then cast to obtain a medium-entropy alloy ingot (cylindrical Ф29.3×50mm);
[0046] The medium-entropy alloy ingot is subjected to homogenization annealing, followed by heat holding, hot extrusion, and cooling to obtain the medium-entropy alloy.
[0047] In some embodiments of the present invention, the vacuum arc melting temperature is 2300-3800K, the time is 45s, and the number of times is 5; the induction melting temperature is 1700-2000K, and the time is 1min; the homogenization annealing temperature is 1473±1K, and the time is 24h; the heat preservation temperature is 1523±1K, and the time is 1h.
[0048] In some embodiments of the present invention, the hot extrusion speed is 22±5 mm / s, and the extrusion ratio is 11.88. The cooling is specifically air cooling to room temperature.
[0049] In some embodiments of the present invention, the cooling process further includes steps of cold rolling and / or heat treatment.
[0050] In some embodiments of the present invention, the parameters for the cold rolling are set as follows: roll diameter of 175 mm, maximum rolling force of 66838 N, rolling speed of 915.8 mm / s, rolling temperature of room temperature (293 K), reduction of 0.2 mm / pass, and 18-21 rolling passes depending on the thickness of the sample before rolling, resulting in a 60% thinning, and no lubrication during the rolling process. In some embodiments of the present invention, the heat treatment is performed at a temperature of 873 K-1073 K for 1-12 hours.
[0051] In some embodiments of the present invention, the heat treatment is first performed at 1273K for 1 minute, followed by treatment at 873K-1073K for 1-12 hours.
[0052] The heat treatment process also includes a water quenching cooling step.
[0053] A third aspect of the present invention provides the application of the above-mentioned medium-entropy alloy in the preparation of structural materials for use in seawater or acidic environments.
[0054] A fourth aspect of the present invention provides a structural material, the raw material of which includes the above-mentioned medium-entropy alloy.
[0055] Unless otherwise specified, the technical solutions described in this invention are all conventional solutions in the field, and the reagents or raw materials used are all purchased from commercial channels or are publicly available unless otherwise specified.
[0056] The technical solutions provided by the present invention will be described in detail below with reference to the embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0057] Example 1
[0058] 1. Experimental Materials and Procedures (Co) 54 Cr 25 Ni 10 Preparation of Al3Ti3W5 (at.%) medium entropy alloy
[0059] Hot extrusion: Medium-entropy alloy button ingots are obtained by arc melting of elemental metals Co, Cr, Ni, Al, Ti, and W (purity >99.5 wt.%). Before preparation, the oxide film on the surface of each raw material is removed, and weighing is performed using an electronic balance with an accuracy of 0.0002 g, with the mass error controlled within ±0.002 g. The weighed samples are ultrasonically cleaned with ethanol, air-dried, and then sealed in vacuum bags to prevent oxidation. Button ingots are prepared by vacuum arc melting (using a vacuum arc melting and casting equipment, model WK-Ⅱ). During melting, the metal materials are arranged in descending order of melting point to ensure complete melting. To ensure full fusion of the alloy elements, the arc is gently shaken during melting, and after cooling, the sample is flipped and melted again. Each button ingot is flipped and melted at least 5 times (each melting temperature is 3800±100 K, time is 45 s). The obtained button ingots were then cast into cylindrical medium-entropy alloy ingots (cast state, Ф29.3×50mm) using an induction melting furnace (KZG-2, Kusite, induction melting temperature 1800±100K, time 1min) and a copper mold. To ensure uniform composition, the obtained samples were homogenized and annealed at 1473K for 24h in an argon atmosphere. The medium-entropy alloy ingots were then encased in a steel sleeve and held at 1523K for 1h. Finally, they were extruded using a four-column hydraulic press (HP32-315, Jiangsu Tiankai) at an extrusion speed of 22±5mm / s. After air cooling to room temperature, a long rod with a diameter of 16mm and a length of approximately 600mm was obtained. The diameter of the medium-entropy alloy portion was approximately 8.5mm, resulting in an extrusion ratio of approximately 11.88.
[0060] Post-processing: Post-processing is divided into three types: heat treatment (i.e., annealing), cold rolling (i.e., rolling), and cold rolling + heat treatment; the equipment used for post-processing of materials includes annealing furnaces and cold rolling mills.
[0061] Before heat treatment, the cut samples are sealed in glass tubes under an argon atmosphere using a vacuum sealing device to prevent oxidation during the heat treatment process. The samples obtained from the hot extrusion are named HE. Samples that undergo post-processing after hot extrusion are named according to their preparation process. For samples that only undergo heat treatment, the naming rule is HE-heat treatment temperature-heat treatment time, i.e.: HE-873-1, HE-973-1, HE-1073-1, HE-1173-1, HE-973-4, HE-973-8, HE-973-12, HE-973-16 (for example, HE-873-1 indicates that the hot-extruded sample was directly heat-treated at a temperature of 873K for 1 hour; the unit of heat treatment time is hours). For samples that undergo only cold rolling, the naming convention is HE+CR. For samples that are first cold rolled (specifically, the cold rolling process is as follows: roll diameter 175mm, maximum rolling force 66838N, rolling speed 915.8mm / s, rolling temperature room temperature (293K), reduction 0.2mm / pass, with 18-21 rolling passes depending on the thickness of the sample before rolling, cold rolling to 40% of the original thickness of the sample, without lubrication during the rolling process) and then heat treated, the naming convention is HE+CR+heat treatment process, i.e., HE+CR+973K 1h, HE+CR+1073K 1h, HE+CR+1173K 1h, HE+CR+1273K 1min, HE+CR+1173K 1h+973K 12h, HE+CR+1273K 1min+973K 12h (e.g., HE+CR+973K) 1h indicates that the hot-extruded sample is first cold-rolled, and then heat-treated at a temperature of 973K for 1 hour.
[0062] 2. Co prepared by annealing-controlled hot extrusion 54 Cr 25 Ni 10 Properties and microstructure of Al3Ti3W5 (i.e., post-treatment is only heat treatment)
[0063] 2.1 Heat treatment process on Co 54 Cr 25 Ni 10 Influence of Al3Ti3W5 alloy on mechanical properties
[0064] Figure 1 Figure (a) shows the Vickers hardness of samples HE, HE-873-1, HE-973-1, HE-1073-1, and HE-1173-1. The results show that the hardness of the alloy first increases and then decreases with increasing annealing temperature. At an annealing temperature of 1073 K, the hardness of the alloy increases to approximately 327 HV, and decreases to approximately 282 HV as the annealing temperature is further increased to 1173 K. Figure 1 Figures (b) and (c) show the engineering stress-strain curves and the strength and elongation of samples HE, HE-873-1, HE-973-1, HE-1073-1, and HE-1173-1, respectively. The samples exhibit good comprehensive mechanical properties, with high yield strength, ultimate tensile strength, and good ductility. Similar to the change in hardness, the strength of the samples initially increases and then decreases with increasing annealing temperature. The sample annealed at 973K for 1 hour exhibits the optimal combination of strength and ductility, with a yield strength of approximately 800 MPa, a tensile strength of approximately 1279 MPa, and an elongation of approximately 46.6%. These results indicate a correlation between the mechanical properties of the extruded heat-treated samples and the annealing temperature.
[0065] Since the HE-973-1 sample exhibited the best overall mechanical properties, the annealing time dependence at 973K was further investigated. Annealing times were set to 8 hours, 12 hours, and 16 hours. Figure 2 (a) shows the Vickers hardness of samples HE, HE-973-1, HE-973-8, HE-973-12, and HE-973-16. With increasing holding time, the Vickers hardness reaches its maximum at approximately 366 HV after 8 hours of holding. Engineering stress-strain curves show that annealing at 973 K for 12 hours exhibits the best mechanical properties, with yield strength and ultimate tensile strength continuously increasing to approximately 960 MPa and 1439 MPa, respectively, while ductility decreases to approximately 36%. Overall, compared to the reported CoCrNi ternary alloy, the hot-extruded samples exhibit superior mechanical properties and demonstrate a good combination of strength and ductility in the precipitate-strengthened alloy. Figure 2 (d)
[0066] 2.2 Heat treatment process on Co 54 Cr 25 Ni 10 Influence of Al3Ti3W5 alloy microstructure
[0067] 2.2.1 XRD and SEM Analysis
[0068] like Figure 3 As shown in (a), the XRD results of samples HE-873-1, HE-973-1, HE-1073-1, and HE-1173-1 reveal a single FCC structure. Similarly, samples heat-treated at 973 K for different times also show a single FCC structure. Figure 3 (b)
[0069] To characterize the microstructure of the samples, SEM tests were also performed on the heat-treated samples. Figure 4 and Figure 5).like Figure 4 As shown in (a)-(e), annealing significantly promotes precipitation at grain boundaries, a phenomenon that becomes more pronounced at increasing temperatures. The precipitated phases exhibit two distinct elemental enrichments: the larger black precipitates are rich in Al and Ti, while the smaller white precipitates are rich in W. Figure 4 (f)-(l)).
[0070] Among the samples heat-treated at different temperatures after extrusion, the sample annealed at 973K for 1 hour exhibited the best mechanical properties. This may be attributed to the precipitation of the L12 phase. Phase diagram calculations showed that a large amount of L12 phase precipitated within the grains at intermediate temperatures, providing a second-phase strengthening effect. Based on this, heat treatment experiments were conducted at 973K for different times. Figure 5 SEM images of samples HE-973-8, HE-973-12, and HE-973-16 are shown. The precipitates at the grain boundaries do not change significantly with increasing annealing time. The grain size fluctuates in the range of 9–13 μm (excluding twins), and this degree of variation does not lead to significant differences in intensity. However, the content and size of the L12 phase change with annealing time, and the intensity fluctuations should be attributed to changes in the size and quantity of the L12 phase.
[0071] 2.2.2 TEM analysis of HE-973-12 sample
[0072] To further determine the microstructure of intragranular and grain boundary precipitates, TEM, HRTEM, SAED, and EDS measurements were performed on the HE-973-12 sample. Figure 6 and Figure 7 ). Figure 6 Image (a) shows a bright-field TEM image within the crystal. The magnified dark-field TEM image in region R1 and the corresponding SAED pattern are shown below. Figure 6 As shown in (b) and (c), numerous spherical nanoprecipitates were found within the FCC structure matrix and identified as an ordered L12 phase (see Figure 1). Figure 6 (c) The superlattice diffraction spots marked by the green dashed circles in the middle. Figure 6 As shown in (d) and (e), annealed twins also exist inside the matrix. Figure 6Figure (f) shows the presence of numerous stacking faults within the crystal. In low-stack-fault-energy Ni-based single-crystal superalloys, the deformation mechanism changes with increasing hot compression temperature. At 873 K, the deformation mechanism shifts from antiphase boundary shear to stacking fault shear; at 1073 K, the deformation mechanism is primarily controlled by stacking fault shear, accompanied by reactions of stacking faults in different directions and Lomer-Cottrell (LC) locking; above 1173 K, although some stacking faults still exist, the main deformation mechanism is dislocation bypassing. In this invention, the sample to be hot-extruded was first held at 1523 K for one hour, then removed from the annealing furnace and hot-extruded in the atmosphere. Due to the rapid cooling of the sample in air, this process can be considered a medium-temperature compression deformation, leading to the formation of numerous stacking faults.
[0073] like Figure 7 As shown, the TEM, FFT, and EDS results at the grain boundaries reveal two element-rich regions: one rich in Al and Ti (Co2AlTi), and the other rich in W (Co3W). In the Co-Al-Ti-W system, discontinuous precipitation of the Co3W and Co2AlTi phases at the grain boundaries was observed at 1023 K.
[0074] The strengthening mechanism and deformation mechanism of the sample were analyzed. The deformation process of the HE-973-12 sample is as follows: Figure 8 As shown. Before deformation, the HE-973-12 sample contained intragranular and grain boundary precipitates, and stacking faults were present prior to plastic deformation. In the initial stage of deformation, due to the low stacking fault energy, a large number of stacking faults were generated, leading to the formation of numerous structurally stable LC locks. These locks acted as barriers to dislocation movement, resulting in a significant increase in the work hardening rate during the early stages of plastic deformation. Furthermore, the LC locks could serve as Frank-Reed dislocation sources, providing more dislocations to accommodate subsequent plastic deformation. This, in turn, led to the accumulation and entanglement of more dislocations around the LC locks, slowing down the rate of decrease in the later work hardening rate. Figure 8 (a)). Because many nanoscale L12 particles exist along the dislocation slip path, it becomes more difficult for dislocations to move within the grain during tensile deformation until the shear stress is sufficient for the dislocations to cut through the precipitated phase. When dislocation slip encounters large particles, the dislocations aggregate around the grain boundaries (a). Figure 8 (c) and (f)). As plastic deformation proceeds, the volume fraction of dislocations gradually increases ( Figure 8 (d), (g)). Near fracture, the volume fraction of dislocations becomes higher, leading to rapid propagation of slip bands and the appearance of microcracks at grain boundaries. Figure 8In the middle (e), (h)), and begin to connect with each other. Therefore, fracture should occur along grain boundaries and a few slip bands, resulting in a mixed transverse-transgranular fracture mode ( Figure 8 (h) In general, maintaining work hardening during plastic deformation can induce excellent tensile properties, which should be attributed to the synergistic activation of dislocations and stacking faults. The trend of work hardening rate variation observed in other samples is similar to that of sample HE-973-12. The work hardening effect is affected by the different proportions of dislocation density, precipitates, grain boundaries and stacking faults, resulting in different plastic deformation behaviors.
[0075] This section investigates the effect of heat treatment on Co prepared by hot extrusion. 54 Cr 25 Ni 10 Influence of heat treatment temperature and time on the properties and microstructure of Al3Ti3W5 medium-entropy alloys. Orthogonal experiments were conducted on the alloy to investigate the relationship between microstructure and mechanical properties, as well as the corresponding deformation mechanism. The following conclusions were drawn:
[0076] (1) Three types of precipitates were observed in the hot-extruded and subsequently heat-treated samples: L12 nanoparticles within the FCC grains, W-rich precipitates at grain boundaries, and Al and Ti-rich precipitates. Hot extrusion refined the grains while promoting stacking fault accumulation. The content of various precipitates could be adjusted by changing the heat treatment temperature and time.
[0077] (2) The optimized heat treatment parameters were set to 973K for 12 hours. The yield strength and tensile strength of the HE-973-12 sample increased to approximately 960 MPa and 1439 MPa, respectively, accompanied by a relatively high plastic strain of approximately 36%. A good combination of high strength and high plasticity was achieved. Calculations of the strengthening mechanism showed that the L12-type second-phase strengthening mechanism made the main contribution to the increase in yield strength. The collective strengthening effect from L12 precipitation strengthening, grain boundary precipitation strengthening, grain boundary strengthening, and solid solution strengthening increased the yield strength of the HE-973-12 sample to approximately 960 MPa.
[0078] (3) During deformation, the HE-973-12 sample activated high-density stacking faults in different directions, leading to the formation of stacking fault networks and immovable LC locks, providing an effective source for work hardening capacity and thus achieving a significant strength-plasticity synergy. The L12 precipitates were sheared by dislocations, which facilitated long-distance dislocation slip through the matrix. Conversely, dislocations were accumulated at the interface between the grain boundary precipitates and the matrix, which increased work hardening capacity in the early stages of plastic deformation but also led to stress concentration.
[0079] 3. Co prepared by cold rolling and heat treatment controlled by hot extrusion 54 Cr25 Ni 10 Performance and microstructure of Al3Ti3W5
[0080] 3.1 The effect of cold rolling and heat treatment processes on Co 54 Cr 25 Ni 10 Influence of Al3Ti3W5 alloy on mechanical properties
[0081] The hot-extruded samples were first thinned by 60% by rolling (cold rolling parameters: roll diameter 175mm, maximum rolling force 66838N, rolling speed 915.8mm / s, rolling temperature room temperature (293K), reduction 0.2mm / pass, 18-21 rolling passes depending on the initial sample thickness, no lubrication during rolling), followed by heat treatment (temperature and time as described above). The heat-treated samples were then cooled by water quenching and cut into dog-bone shaped tensile specimens for quasi-static tensile testing at room temperature. The heat treatment process and corresponding yield strength, tensile strength, and elongation are shown in Table 1.
[0082] Table 1: Yield strength, tensile strength, and elongation of samples with different treatment processes
[0083]
[0084] Note: "\" in the table indicates that it cannot be stretched.
[0085] For samples that underwent only one heat treatment, those heat-treated at 973K and 1073K for one hour exhibited significant brittleness, making tensile mechanical property testing impossible. This was because the heat treatment temperature was too low, resulting in incomplete recrystallization and the presence of numerous slip bands left from rolling, leading to a loss of plasticity. After attempting higher heat treatment temperatures and longer treatment times, it was found that while the alloy's plasticity improved (attributable to recrystallization), its strength significantly decreased. Therefore, a heat treatment method of high-temperature followed by low-temperature treatment was subsequently adopted. The high-temperature heat treatment facilitated recovery and recrystallization, while also promoting the precipitation of the Co3W phase. The subsequent heat treatment at a moderate temperature further promoted the precipitation of the precipitated phase, achieving the goal of second-phase strengthening. The results showed that the HE+CR+1173K 1h+973K 12h sample was unable to be stretched. The first annealing at 1173K for 1h was insufficient, resulting in incomplete recrystallization. The second annealing at 973K for 12h caused a large precipitation of the L12 phase, leading to a sharp decrease in plasticity. In contrast, the HE+CR+1273K 1min+973K 12h sample exhibited a tensile strength of 1774 MPa and an elongation of 10.8%. Compared to the HE-973-12 sample, the elongation decreased by 25%, but the yield strength and tensile strength increased by 464 MPa and 335 MPa, respectively.
[0086] like Figure 9 The figures show the engineering stress-strain curves and hardness of the selected sample and the hot-extruded sample (HE). It can be seen that the Co prepared by hot extrusion... 54 Cr 25 Ni 10 The Al3Ti3W5 alloy exhibited a high strength of 2000 MPa after rolling. However, significant work softening was observed. Dislocations in the cold-rolled sample reached saturation, causing the sample to lose its work hardening ability. After heat treatment at 1273 K for 1 min, the rolled sample underwent complete recrystallization, with the tensile strength decreasing from 2000 MPa to 1675 MPa, while the elongation increased to 22.3%. After precipitation heat treatment at 973 K for 12 hours, the tensile strength increased to 1774 MPa, with an elongation of 10.8%.
[0087] 3.2 The effect of cold rolling and heat treatment processes on Co 54 Cr 25 Ni 10 Influence of Al3Ti3W5 alloy microstructure
[0088] To clarify the relationship between the microstructure and mechanical properties of alloys, it is necessary to characterize the alloy's microstructure. First, the phase composition of the sample is analyzed, such as... Figure 10The XRD test results of the HE+CR, HE+CR+1273K 1min and HE+CR+1273K 1min+973K 12h samples are shown, indicating that the samples after cold rolling and cold rolling followed by annealing all exhibit a single-phase FCC structure.
[0089] like Figure 11 The image shown is a SEM image of the sample. The hot-extruded sample, after rolling, exhibits densely interwoven slip bands. After annealing, the HE+CR+1273K 1min and HE+CR+1273K 1min+973K 12h samples show dense white precipitates. EDS results for the HE+CR+1273K 1min+973K 12h sample indicate that these dense white precipitates are W-rich precipitates. Compared to the annealed sample only, the W-rich phase in the rolled-annealed sample precipitates not only at grain boundaries but also within the grains along the slip bands formed during rolling (e.g., ...). Figure 10 (As shown by the yellow dashed line in (b)). The high dislocation density and localized stress concentration in the slip band can reduce the energy barrier for nucleation, thereby promoting the nucleation of the precipitate. In addition, the dislocation network may also provide diffusion channels, accelerating the migration and aggregation of atoms in the slip band region, further promoting the formation of the precipitate. Compared with the W-rich phase (299.1 nm) in the HE-973-12 sample that only underwent annealing, the W-rich phase (106.652 nm) in HE+CR+1273K1min+973K12h was smaller. This is because recrystallization and the precipitation of a large number of precipitates occurred simultaneously, and the higher nucleation rate caused the precipitate to come into contact with other boundaries (such as grains or another precipitate) early in the growth process, thus stopping its growth.
[0090] like Figure 12The EBSD images of the samples are shown, displaying the BC, IPF, and GND images of the rolled and annealed samples. The rolled sample exhibits dense slip bands, elongated grains, and fragmentation, along with a high dislocation density. Generally, based on orientation difference, grain boundaries of 2° < θ < 15° and θ ≥ 15° are termed low-angle grain boundaries (LAGB) and high-angle grain boundaries (HAGB), respectively. The annealed samples all showed very low LAGB content (HE+CR+1273K 1min: 3.74%; HE+CR+1273K 1min+973K 12h: 2.83%), indicating that they achieved complete recrystallization. The annealed samples exhibited a non-uniform structure, consisting of large grains and small grains, with the average grain size decreasing from ~13 μm in the HE sample to 6.64 μm in the HE+CR+1273K1min+973K12h sample. The high dislocation density generated during rolling provided stored energy for subsequent heat treatment, which became the driving force for the nucleation and growth of new grains at the recrystallization temperature. The energy provided by the high dislocation density helped overcome the atomic arrangement instability within the original grains, promoting the formation of new grains. During recrystallization, the high nucleation rate led to the simultaneous growth of a large number of grains. Due to the presence of numerous nucleation points, the new grains came into contact with each other before growth, halting their growth and resulting in an overall reduction in grain size. Simultaneously, a large number of annealing twins appeared in the HE+CR+1273K1min and HE+CR+1273K1min+973K12h samples, with twin boundaries accounting for 30.8% and 36.8%, respectively.
[0091] To further characterize the microstructure of the HE+CR+1273K 1min+973K 12h sample, TEM, HRTEM, SAED, and EDS tests were performed. Figure 13 ).like Figure 13 As shown in (a), the annealed sample exhibits numerous annealed twins, along with a large number of black submicron-sized precipitates within the grains and at the grain boundaries. The S1 region within the selected grain was magnified. Figure 13 In (b), this region shows black precipitates and twin morphology. The corresponding EDS test results ( Figure 13 The black precipitate shown in (d)-(i) is a W-rich phase, corresponding to the high-resolution image. Figure 13 (k) and its Fourier transform results Figure 13 The middle (l) shows that the phase is a Co3W phase. This is consistent with the results obtained from SEM testing. Figure 11Consistent with this, the Co3W phase precipitated not only at grain boundaries but also within the grains. In addition, annealing twins and nano-L12 precipitates were also observed. Figure 13 (c) and (j)).
[0092] This invention also performed TEM tests on the grain boundary region of the HE+CR+1273K 1min+973K 12h sample, and the results are as follows. Figure 14 As shown, two precipitated phases appeared at the grain boundaries. EDS results indicate that they are a W-rich phase and an Al / Ti-rich phase, respectively. Figure 14 SAED results for the Al and Ti-rich phases (e)-(j) show that it is a Co2AlTi phase. Figure 14 In the middle (c), the SAED results of the W-rich phase are superimposed with the diffraction spots of the L12 phase, but it is still possible to distinguish that it is the Co3W phase. Figure 14 (d)). In summary, the microstructure test results of the HE+CR+1273K 1min+973K 12h sample show a microstructure including fine grains, annealing twins and precipitates (intragranular: nano-L12+submicron Co3W; grain boundaries: submicron Co3W+Co2AlTi).
[0093] Through analysis of various strengthening and plastic deformation mechanisms, this invention summarizes a series of events occurring during sample deformation. Before deformation, the HE+CR+1273K 1min+973K 12h sample contains intragranular (L12 phase and Co3W) and grain boundary (Co3W and Co2AlTi) precipitates, and dislocations are present before plastic deformation. At the beginning of deformation, due to the low stacking fault energy, a large number of stacking faults are generated, forming a stacking fault network. LC locking and the interactions between stacking faults provide a highly efficient source of work hardening ability. They can fix dislocations, preventing them from moving to grain boundaries or phase boundaries and causing catastrophic stress concentration. Simultaneously, they can act as Frank-Reed dislocation sources, generating new dislocations to adapt to subsequent deformation, resulting in a significant strength-ductility synergistic effect. Because many nanoscale L12 particles exist on the dislocation slip path, it becomes more difficult for dislocations to move within the grains during tensile deformation until the shear stress is sufficient for the dislocations to cut through the precipitates. When dislocation slip encounters submicron-sized precipitates Co3W and Co2AlTi, dislocations and stacking faults accumulate at the interface between the FCC matrix and the precipitates. When dislocation motion encounters grain boundaries or twin boundaries, it accumulates at the interface. Near fracture, the volume fractions of dislocations and stacking faults become higher, leading to rapid propagation of slip bands, while microcracks appear at the grain boundaries and begin to connect. Overall, maintaining work hardening during plastic deformation can induce excellent tensile properties, which should be attributed to the synergistic activation of dislocations and stacking faults.
[0094] This section focuses on the effect of rolling heat treatment on Co prepared by hot extrusion. 54 Cr 25 Ni 10 Influence of microstructure on the properties of Al3Ti3W5 medium-entropy alloys. Heat treatment experiments with different processes were conducted on the rolled alloys. The relationship between microstructure and mechanical properties, as well as the corresponding deformation mechanisms, were investigated. The following conclusions were drawn:
[0095] (1) The hot-extruded sample is first rolled and then heat-treated, which can effectively refine the grains and promote the precipitation of submicron-sized Co3W phase. Finally, the preferred HE+CR+1273K 1min+973K 12h sample exhibits a microstructure containing fine grains, annealed twins and precipitated phases (intragranular: nano-sized L12 + submicron-sized Co3W; grain boundary: submicron-sized Co3W + Co2AlTi).
[0096] (2) The optimized process parameters were: after rolling 60%, annealing at 1273K for 1 min, followed by annealing at 973K for 12 h. Compared with the HE-973-12 sample, the HE+CR+1273K 1 min+973K 12 h sample showed a 25% decrease in elongation, but an increase in yield strength and tensile strength of 464 MPa and 335 MPa, respectively. A good combination of high strength and toughness was achieved. Calculations of the strengthening mechanism showed that second-phase strengthening and dislocation strengthening made the main contributions to the increase in yield strength.
[0097] (3) During the deformation process of the HE+CR+1273K 1min+973K 12h sample, high-density stacking faults were activated in different directions, leading to the formation of stacking fault networks and immovable LC locks, providing an effective source for work hardening capacity and thus achieving a significant strength-toughness synergy. The L12 precipitate was sheared by dislocations, which facilitated long-distance dislocation slip through the matrix. Conversely, dislocations were accumulated at the interface between the submicron-sized Co2AlTi and Co3W precipitates and the matrix, which increased work hardening capacity in the early stages of plastic deformation but also led to stress concentration.
[0098] 4. High strength and high toughness Co 54 Cr 25 Ni 10 Corrosion resistance of Al3Ti3W5 medium-entropy alloy
[0099] 4.1 Electrochemical corrosion behavior in 3.5 wt.% NaCl solution
[0100] 4.1.1 Electrochemical Analysis
[0101] To more accurately assess the corrosion resistance of the samples, a penalty function was set according to the evaluation index proposed by Nascimento et al. for assessing the corrosion resistance of alloys in NaCl solution.
[0102]
[0103] Where Z is the value of the penalty function, and α1 and α2 are commutative constants whose values are arbitrary and depend on the relative weights assigned to each performance metric by the designer. (E) pit and E pit -E corr Since they have the same weight, α1 and α2 are equal. When the E of an alloy pit and E corr The smaller the value of the penalty function Z, the better its corrosion resistance in NaCl solution. For example... Figure 15 As shown in (b), the horizontal and vertical axes are plotted with 1 / E as the horizontal axis and the vertical axis as the vertical axis. pit and 1 / (E pit -E corr The graph shows that the closer the alloy is to the lower left corner, the smaller the penalty function Z value, and the better its corrosion resistance. Therefore, the Ascast (cast sample), HE+973-12, and HE+CR+1273K 1min+973K 12h samples exhibit good corrosion resistance in NaCl solution. In summary, Ascast, HE-973-12, and HE+CR+1273K 1min+973K 12h show superior pitting potential, indicating good corrosion resistance in NaCl solution.
[0104] To better analyze the corrosion behavior of the medium-entropy alloy in NaCl solution, electrochemical impedance spectroscopy was performed on the samples to quantitatively analyze the passivation behavior of the alloy. Figure 16 The image shows the fitting results for the EIS data. Figure 16 In Figure (a), the Nyquist plot shows that, generally, the larger the radius of curvature of a capacitor, the better its corrosion resistance. The HE-973-12 sample exhibits the largest radius of curvature, demonstrating the best corrosion resistance. Figure 16 (b) shows the Bode impedance diagram, which reveals that the HE-973-12 sample exhibits the highest impedance at both high and low frequencies. Figure 16 (c) is the Bode phase angle diagram, and the larger peak width shows that the HE-973-12 and As cast samples have better corrosion resistance. Figure 16(d) shows the equivalent circuit diagram used when fitting the EIS circuit. Because the curve HE+CR+1273K 1min+973K 12h in the Nyquist plot exhibits a combination of circular arcs and approximately straight lines, different equivalent circuits were used for fitting the three samples. For the Ascast and HE-973-12 samples, the equivalent circuit diagram used was as follows: Figure 16 The equivalent circuit shown in ① of diagram (d) is replaced by the equivalent circuit shown in ② for the HE+CR+1273K 1min+973K 12h sample. In this invention, R s R represents the resistance of an electrolyte solution, reflecting the solution's electrical conductivity. c This refers to the resistance of the passivation layer, representing its ability to impede current flow. R ct Q is the charge transfer resistance, which represents the degree of resistance to the charge transfer process at the electrode surface. Furthermore, Q... c and Q dl These are phase angle elements representing the capacitance of the passivation layer and the electric double layer, respectively, describing their capacitive properties and response behavior under an alternating electric field. To obtain better fitting results, a constant phase element (CPE) is used to adjust Q in the actual fitting process. c and Q dl The specific parameters were simulated. The impedance of the CPE is defined as follows:
[0105] Z CPE =[Y0(jω) n ] -1
[0106] Where ω is the angular frequency, Y0 is the pseudo capacitance of CPE, j is the imaginary unit, and the value of n represents the degree to which CPE deviates from the ideal capacitance characteristics, ranging between 0 and 1.
[0107] Table 2 Electrochemical parameters of the equivalent fitting circuit
[0108]
[0109] Use such as Figure 16 The fitting results for the equivalent circuit shown in (d) are shown in Table 2. The variance χ² of the fitted data is used. 2 The accuracy of the fitting results was tested, and the χ² value was found to be... 2The values are all small, indicating a good fit. Since the Rct value depends on the Faraday process of oxidation or reduction caused by electron transfer, it can indicate the speed of the corrosion process. A larger Rct indicates a slower corrosion reaction. The HE-973-12 sample showed a larger Rct than the HE+CR+1273K 1min+973K 12h sample, while the Rct value of the HE+CR+1273K 1min+973K 12h sample was greater than that of the As cast sample. This is consistent with the i... (The sentence is incomplete and requires further context to translate accurately.) corr The results are consistent. Rc represents the resistance of the corrosion product layer. The Rc values of the three samples are not high, indicating that the corrosion layer does not significantly impede the current. However, the Rc value of the HE+CR+1273K 1min+973K 12h sample is slightly higher, which may indicate that its corrosion layer is thicker or denser.
[0110] 4.1.2 Microstructure after corrosion
[0111] In corrosive environments, including air, corrosion-resistant alloys can automatically form a protective or passivating film. This passivating film effectively slows down the corrosion process by isolating the alloy from direct contact with the surrounding environment, acting as an electron barrier for charge transfer, and preventing the diffusion of corrosive ions to the alloy surface. The specific composition and structure of the passivating film directly affect the corrosion resistance of the alloy. Therefore, by analyzing the passivating film on the surface of corroded samples, a deeper understanding of the corrosion mechanism of the alloy can be achieved. Thus, samples after Tafel testing were characterized by SEM and EDS. Figure 17 As shown, the three samples exhibit different degrees of corrosion morphology. The As cast sample surface only showed a small portion of passivation film, while a large number of pitting corrosion pits were present. Figure 17 As shown by the yellow arrow in (a), the passivation film on the HE-973-12 sample is more extensive, while the HE+CR+1273K1min+973K12h sample is almost entirely a passivation film. All three samples exhibit significant enrichment of Al, Ti, and W on their passivation films.
[0112] To further characterize the passivation film formed on the samples during the corrosion process, XPS measurements were performed. The XPS results were analyzed using Advantage software and its built-in database. After subtracting the Shirley baseline, the high-resolution XPS spectra were decomposed and convolved. Figure 18 The characteristic spectra and fitting results for Co 2p, Cr 2p, Al 2p, Ti 2p, and W 4f are shown. Since no energy level corresponding to Ni was detected in the passivation film, it indicates that there are no Ni compounds in the passivation films of these samples. The results show that the passivation films on all three samples are composed of compounds of elements such as Co, Cr, Al, Ti, and W.
[0113] 4.2Co 54 Cr 25 Ni 10 Electrochemical corrosion behavior of Al3Ti3W5 medium-entropy alloy in 0.5M H2SO4 solution
[0114] 4.2.1 Electrochemical Analysis
[0115] like Figure 19 Polarization curves of As cast, HE-973-12, and HE+12731min+97312h samples in 0.5M H2SO4 solution. Analysis of polarization curves. Figure 19 The corrosion current density (i) obtained in (b) corr ), corrosion potential (E) corr ) and pitting potential (E) pit As shown in Table 3.
[0116] Table 3. Electrochemical experimental results of Tafel curves
[0117]
[0118] like Figure 19 As shown in (a), the As cast sample exhibits the most positive open-circuit potential at room temperature, meaning it is the least likely to initiate corrosion. As shown in Table 3, among the three samples, the highest corrosion current density is 41.6 μA / cm². 2 The minimum is 22.06 uA / cm. 2 This is at a lower level compared to alloys with similar compositions (e.g.) Figure 19 As shown in (c), the maximum corrosion potential is -0.296mV and the minimum is -0.307mV, which is at a medium level, indicating that the alloy is not easily corroded in the H2SO4 solution environment.
[0119] 4.2.2 Microstructure after corrosion
[0120] To further investigate the corrosion mechanism of the alloy in 0.5M H2SO4 solution, this invention performed SEM and EDS tests on three samples—As cast, HE-973-12, and HE+12731min+97312h—that had completed Tafel testing. Figure 20 As shown, the three samples exhibit different degrees of corrosion morphology. The As cast sample has the shallowest corrosion, with only a small portion of the sample surface showing a passivation film, but it also has multiple pitting corrosion pits (such as...). Figure 20 As shown by the yellow arrow in (a), the annealed sample has a more extensive passivation film, while the sample that was rolled and then annealed is almost entirely a passivation film. The passivation films of the three samples have the same composition, mainly composed of oxides of Al, Ti, and W.
[0121] This section studies Co 54 Cr 25 Ni 10 The corrosion resistance of Al3Ti3W5 medium-entropy alloys, especially the performance of samples under different heat treatment processes, was investigated. Through electrochemical corrosion behavior studies in 3.5 wt.% NaCl and 0.5 M H2SO4 solutions, this invention found that as-cast samples (As cast), annealed samples only (HE-973-12), and samples subjected to rolling and heat treatment (HE+CR+1273K1min+973K12h) all exhibited excellent corrosion resistance.
[0122] (1) These samples exhibited high pitting potentials in 3.5 wt.% NaCl solution. In 0.5 M H2SO4 solution, they showed low corrosion current density and moderate corrosion potential. This indicates that the alloy has good corrosion resistance in NaCl solution and sulfuric acid environments. Comparing the corrosion performance and mechanical properties of the alloys, it can be found that the HE-973-12 and HE+CR+1273K 1min+973K 12h samples obtained in this invention possess both good mechanical properties and corrosion resistance.
[0123] (2) Through analysis of the microstructure after corrosion, we further confirmed the protective effect of the passivation film and the key role of alloying elements in corrosion resistance. In particular, the enrichment of Cr, Ti, and W contributes to the formation of a more stable passivation film, thus providing better protection. At the same time, the microstructure of the alloy, such as grain size, dislocation density, and precipitates, also has a significant impact on its corrosion resistance.
[0124] In summary, this invention designs a material with the component Co. 54 Cr 25 Ni 10 A medium-entropy alloy of Al3Ti3W5 was prepared by hot extrusion, followed by heat treatment or rolling and heat treatment processes to adjust the alloy's microstructure, including grain size, precipitates, and defects. These methods resulted in an alloy with excellent mechanical properties while maintaining good corrosion resistance. The main conclusions are as follows:
[0125] (1) For the hot-extruded samples that underwent heat treatment. Three types of precipitates were observed in the hot-extruded and subsequently annealed samples: coherent L12 nanoprecipitates within the FCC grains, W-rich and Al / Ti-rich precipitates at the grain boundaries. Hot extrusion refined the grains while promoting the accumulation of stacking faults. The content of various precipitates could be adjusted by changing the annealing temperature and annealing time. The yield strength and tensile strength of the optimal HE-973-12 sample increased to 960 MPa and 1439 MPa, respectively, accompanied by a relatively high plastic strain of approximately 36%. A good combination of high strength and plasticity was achieved. The L12 second-phase strengthening made the main contribution to the increase in yield strength. During the deformation process, the HE-973-12 sample activated high-density stacking faults in different directions, leading to the formation of stacking fault networks and immobile LC locks, providing an effective source for work hardening capacity, thus achieving a significant strength-toughness synergy. The L12 precipitates were sheared by dislocations, which facilitated long-distance dislocation slip through the matrix. Conversely, dislocations accumulate at the interface between the grain boundary precipitates and the matrix, which increases work hardening capacity in the early stages of plastic deformation, but also leads to stress concentration.
[0126] (2) The process of heat treatment after rolling can further enhance Co. 54 Cr 25 Ni 10 Mechanical properties of Al3Ti3W5 medium-entropy alloys were investigated. Results showed that this process effectively refined the grains and promoted the precipitation of submicron-sized Co3W phases. Ultimately, the preferred HE+CR+1273K 1min+973K 12h sample exhibited a microstructure containing fine grains, annealed twins, and precipitated phases (intragranular: nano-sized L12 phase + submicron Co3W phase; grain boundary: submicron-sized Co3W phase + Co2AlTi phase). Compared to the HE-973-12 sample, the HE+CR+1273K1min+973K 12h sample showed a 25% decrease in elongation, but an increase in yield strength and tensile strength of 464 MPa and 335 MPa, respectively. Calculations of the strengthening mechanism indicated that second-phase strengthening and dislocation strengthening made the main contributions to the increased yield strength. During the deformation process, the HE+CR+1273K 1min+973K 12h sample activated high-density stacking faults in different directions, ensuring that the alloy maintained a certain elongation under high strength.
[0127] (3) Samples under different processing conditions all exhibited corrosion resistance. Through electrochemical corrosion behavior studies in 3.5 wt.% NaCl and 0.5 MH₂SO₄ solutions, this invention found that the as-cast sample (As cast), the hot-extruded annealed sample (HE-973-12), and the hot-extruded rolled and heat-treated sample (HE+CR+1273K 1min+97312h) all exhibited excellent corrosion resistance. The NaCl solution showed a high pitting potential, demonstrating good pitting corrosion resistance. In 0.5 MH₂SO₄ solution, the low corrosion current density and moderate corrosion potential of the sample indicated that the alloy has good corrosion resistance in a sulfuric acid environment. Analysis of the microstructure after corrosion further confirmed the protective effect of the passivation film and the key role of alloying elements in corrosion resistance. In particular, the oxides and hydroxides of Cr, Ti, and W contribute to the formation of a more stable passivation film, thus providing better protection. Meanwhile, the microstructure of the alloy, such as grain size, dislocation density, and precipitates, also has a significant impact on its corrosion resistance.
[0128] The embodiments described above are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Various modifications and improvements made by those skilled in the art to the technical solutions of the present invention without departing from the spirit of the present invention should fall within the protection scope defined by the claims of the present invention.
Claims
1. A method for preparing a medium-entropy alloy, characterized in that, Includes the following steps: According to Co 54 Cr 25 Ni 10 Al3Ti3W5 atomic percentage: Co, Cr, Ni, Al, Ti and W metallic elements are mixed and vacuum arc melted to obtain button ingots; The button ingots were induction melted and then cast to obtain medium-entropy alloy ingots; The medium-entropy alloy ingot is subjected to homogenization annealing, followed by heat holding, hot extrusion, and cooling to obtain the medium-entropy alloy.
2. The method for preparing a medium-entropy alloy according to claim 1, characterized in that, The vacuum arc melting temperature is 2300-3800 K, the time is 45 s, and the number of times is 5; the induction melting temperature is 1700-2000 K, and the time is 1 min; the homogenization annealing temperature is 1473 ± 1 K, and the time is 24 h; the heat preservation temperature is 1523 ± 1 K, and the time is 1 h.
3. The method for preparing a medium-entropy alloy according to claim 1, characterized in that, The hot extrusion speed is 22 ± 5 mm / s, and the extrusion ratio is 11.
88.
4. The method for preparing a medium-entropy alloy according to claim 1, characterized in that, The cooling process also includes steps of cold rolling and / or heat treatment.
5. The method for preparing a medium-entropy alloy according to claim 4, characterized in that, The parameters for the cold rolling are set as follows: roll diameter is 175 mm, maximum rolling force is 66838 N, rolling speed is 915.8 mm / s, rolling temperature is room temperature, reduction is 0.2 mm / pass, rolling passes are 18-21, and rolling thinning is 60%.
6. The method for preparing a medium-entropy alloy according to claim 4, characterized in that, The heat treatment is performed at a temperature of 873K-1073K for 1-12 hours.
7. The method for preparing a medium-entropy alloy according to claim 4, characterized in that, The heat treatment consists of first treating at 1273K for 1 minute, followed by treating at 873K-1073K for 1-12 hours.
8. The application of a medium-entropy alloy prepared by the preparation method according to any one of claims 1-7 in the preparation of structural materials for use in seawater or acidic environments.