Preparation method of ETFE fluorine diaphragm plate with excellent comprehensive performance

By plating aluminum-zinc alloy film on color steel roof and preparing composite coating, the corrosion and deterioration of existing color steel roofs in harsh environments is solved, and the high durability and reliability of the materials are achieved, adapting to modern climatic conditions and Reduce maintenance costs.

CN119388811AInactive Publication Date: 2025-02-07QINHUANGDAO QINSHUO TECHNOLOGY DEVELOPMENT CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411500361.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-25
Publication Date
2025-02-07
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing color steel roof is prone to corrosion and deterioration in harsh outdoor environments, resulting in short service life, aesthetics and safety impacts. The existing coating protection technology is difficult to cope with severe climatic conditions and environmental challenges.

Method used

Using a metal plate with an aluminum-zinc alloy film layer as the substrate, the substrate surface energy is improved through plasma treatment, and then the composite plating layer is prepared, including silica-carbon tube plating, indium tin oxide plating, wear-resistant layer, ETFE fluorine film layer and The wear-resistant hydrophobic layer improves the corrosion resistance, heat insulation, wear resistance and other properties of the material through the multi-layer film structure design.

Benefits of technology

It significantly improves the durability and reliability of the material, extends service life, reduces maintenance and replacement costs, adapts to modern climatic conditions, and performs well in coastal and highly corrosive and highly irradiated areas.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119388811A_ABST
    Figure CN119388811A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of an ETFE fluorofilm plate with excellent comprehensive performance, and belongs to the technical field of manufacturing of high-performance building materials. According to the preparation method, a metal plate plated with an aluminum-zinc alloy film layer serves as a substrate, and the upper surface and the lower surface of the substrate are each provided with a composite plating layer. The composite coating comprises a silicon dioxide-carbon tube coating, an indium tin oxide coating, a wear-resistant layer, an ETFE fluorine film layer and a wear-resistant hydrophobic layer. The ETFE fluorine diaphragm plate prepared by the method not only has excellent corrosion resistance and excellent heat insulation performance, but also has good scratch-resistant protection and weather resistance, and particularly, the coated wear-resistant hydrophobic layer effectively reduces the adhesion of moisture on the surface of the diaphragm plate, improves the self-cleaning performance of the diaphragm plate, reduces the maintenance cost, and is suitable for large-scale popularization and application. The introduction of the layer not only protects the surface of the film, but also enhances the stability of the film in the long-term use process. The ETFE fluorine film plate prepared by the method is suitable for various high-performance building requirements, and shows a wide application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of high-performance building material manufacturing, in particular to a method for preparing an ETFE fluorine membrane plate with excellent comprehensive performance. Background Art

[0002] In harsh outdoor environments, metal materials face a variety of severe physical and chemical reactions. These reactions, under the combined effects of external factors such as wind, sand, rain, ultraviolet radiation and salt spray, cause serious corrosion and degradation of metal materials, ultimately leading to material failure. This process not only affects the physical properties of the metal, but also seriously reduces its service life, thereby increasing the cost of maintenance and replacement.

[0003] At present, as a metal material widely used in the construction field, color steel roofs generally have a short service life, especially in coastal areas and under high corrosion and high radiation climate conditions. According to market survey data, due to the implementation of national standards and climate deterioration, many color steel roofs will show obvious rust after 2 to 5 years of use, affecting their appearance and safety. This phenomenon shows that the existing coating protection technology is difficult to effectively cope with the increasingly severe climate conditions and environmental challenges.

[0004] Therefore, in the face of harsh outdoor environments and the material problems caused by them, it is urgent to develop a new type of composite material to adapt to modern climate conditions, especially for coastal areas and areas with high corrosion and high radiation, to improve the durability and reliability of the material and provide strong support for the development of the construction industry. Summary of the invention

[0005] The purpose of the present invention is to solve the above problems in the prior art and to provide a method for preparing an ETFE fluorine film plate with excellent comprehensive performance.

[0006] The object of the present invention can be achieved by the following technical scheme: a method for preparing an ETFE fluorine film plate with excellent comprehensive performance, wherein the ETFE fluorine film plate adopts a metal plate coated with an aluminum-zinc alloy film layer as a substrate, and the upper surface and the lower surface of the substrate are both provided with a composite coating, and the composite coating comprises a silicon dioxide-carbon tube coating layer, an indium tin oxide coating layer, a wear-resistant layer, an ETFE fluorine film layer and a wear-resistant hydrophobic layer. The method for preparing the ETFE fluorine film plate comprises the following steps:

[0007] S1 Substrate surface treatment: After cleaning and drying the substrate, plasma technology is used to treat the substrate surface with oxygen to obtain a pre-coated plate;

[0008] The reason for using aluminum-zinc alloy film is: Enhanced anti-corrosion performance: The aluminum-zinc alloy film performs well in anti-corrosion because it combines the corrosion resistance of aluminum and the sacrificial protection of zinc. Zinc, as a sacrificial anode, can corrode in a corrosive environment before other metals such as iron, thereby protecting the metal substrate. Aluminum forms a dense oxide film that effectively isolates water and oxygen to prevent further oxidation of the metal. Improved durability and stability: In the composite coating design of ETFE fluorofilm panels, the corrosion resistance of the substrate is crucial. The aluminum-zinc alloy not only protects the substrate from corrosion, but also improves the mechanical stability and durability of the entire structure. This is critical to maintaining the integrity and performance of the ETFE fluorofilm layer and other functional coatings (such as silica-carbon tube coatings, indium tin oxide coatings, etc.).

[0009] Through oxygen plasma treatment, the energy of the substrate surface is increased, which makes the surface more affinity and better able to combine with the coating material applied subsequently; the increased surface energy helps to improve the wettability and adhesion of the coating; plasma treatment also changes the microstructure of the substrate surface and increases its roughness, thereby increasing the mechanical interlocking strength between the coating and the substrate.

[0010] S2 Preparation of silica-carbon tube coating: S2.1 Preparation of silica-carbon tube composite sol: Acid treatment: Heat the multi-walled carbon nanotubes in a mixed solution of nitric acid solution and sulfuric acid solution; Rinse the acid-treated multi-walled carbon nanotubes with deionized water and then dry them in a vacuum oven; Add the multi-walled carbon nanotubes to an ethanol solution containing a dispersant and use ultrasonic treatment; Add the treated multi-walled carbon nanotube solution to the silica sol, add a pH adjusting solution, adjust the pH value to 9-10, and finally stir until uniform; the dispersant is polyvinyl pyrrolidone; The pH adjusting solution is a sodium hydroxide solution with a concentration of 0.1M; S2.2 Coating: Coat the prepared silica-carbon tube composite sol on the pre-coated plate, and after the coating is completed, perform a curing treatment to obtain a silica-carbon tube film plate;

[0011] The silica-carbon tube composite coating can adjust the surface roughness, which is crucial for the adhesion of the upper indium tin oxide coating. Appropriate surface roughness can increase the mechanical anchoring of the coating. Compared with the simple use of silica, the addition of multi-walled carbon nanotubes is mainly to utilize its excellent mechanical properties and high strength to enhance the overall structural strength and toughness of the composite film. When carbon nanotubes are used as a reinforcing agent in composite materials, they can significantly improve the tensile strength, flexural strength and impact resistance of the material.

[0012] S3 Preparation of indium tin oxide coating: S3.1 Preheating: preheating the silicon dioxide-carbon tube sheet to 150-200°C; S3.2 Preparation of nanoporous structure membrane: using magnetron sputtering equipment to deposit indium tin oxide material on the surface of the preheated silicon dioxide-carbon tube sheet, and promoting the formation of nanopores by gradually introducing oxygen and using pulse sputtering during the sputtering process; S3.3 Annealing: after the sputtering process is completed, naturally cool at room temperature, and then perform annealing at a temperature of 200-400°C. After the annealing is completed, an indium tin oxide membrane plate is obtained;

[0013] The presence of oxygen affects the nucleation and growth mechanisms of the film. Oxygen can promote the adsorption and diffusion of atoms on the substrate surface, help form a more uniform film, and affect the formation of nanopores. During the annealing process, external oxygen helps to further optimize the crystal structure of the film. The presence of oxygen can promote oxygen redistribution at high temperatures, remove defects in the film, and improve the density and crystallinity of the film.

[0014] The choice of preparing nanoporous structure membranes and their advantages over traditional smooth membranes are mainly reflected in the following aspects: Improve optical reflection and scattering efficiency: Nanoporous structure membranes can enhance the optical scattering and reflection capabilities of the material surface. This structure can effectively reflect and scatter infrared light in the incident light, which helps to reduce the absorption of thermal energy. In this way, nanoporous structure membranes can significantly reduce the thermal effect of sunlight, provide better thermal insulation performance, and enhance surface properties: Improve the lightweight of materials: Nanoporous structures help reduce the weight of materials by introducing voids into the material, which is very beneficial for applications that need to reduce the weight of the structure to improve energy efficiency and reduce costs. Enhance interlayer adhesion: The nanoporous structure can increase the contact area with the wear-resistant layer through its unique surface morphology, thereby improving the mechanical hooking effect between the layers and enhancing the overall adhesion and stability of the membrane layer.

[0015] S4 prepares the wear-resistant layer: S4.1 prepares the wear-resistant coating: the wear-resistant slurry is composed of polyurethane, polytetrafluoroethylene powder, silicon carbide particles, two-component epoxy resin and anhydrous ethanol, S4.2 coating: the wear-resistant slurry is coated on the indium tin oxide coated plate, and after the coating is completed, the curing operation and the sandblasting surface treatment operation are performed to obtain the wear-resistant film plate;

[0016] Polyurethane: Function: Polyurethane can withstand frequent expansion and contraction without breaking, providing basic structural support and durability for the coating. In addition, polyurethane has good wear resistance and impact resistance, which enables it to effectively protect the underlying materials when facing physical impact.

[0017] PTFE powder: Function: PTFE has an extremely low friction coefficient. In wear-resistant coatings, it can significantly reduce surface friction, reduce wear and increase the service life of the coating. This substance makes the surface smoother when in contact with other objects, reducing the loss caused by friction.

[0018] Silicon carbide particles: Adding silicon carbide particles to the coating can greatly improve the hardness and wear resistance of the surface, making it able to resist high-load wear. Silicon carbide also has good thermal conductivity, which helps the coating to maintain stable performance in high-temperature environments.

[0019] Two-component epoxy resin: Function: Epoxy resin has excellent mechanical strength and adhesion. It provides a strong bond that can firmly bind the coating to the substrate material. Epoxy resin also has excellent chemical stability and chemical corrosion resistance, and is suitable for use in a variety of environments.

[0020] Anhydrous ethanol: Function: In the process of coating preparation, anhydrous ethanol is used as a solvent to help the coating components mix evenly and promote the fluidity and construction of the coating. Anhydrous ethanol evaporates quickly, which helps the coating to dry and solidify quickly, thereby shortening the construction period.

[0021] Through the combined effect of these substances, the wear-resistant coating not only has excellent mechanical and chemical properties, but can also adapt to a variety of environmental conditions.

[0022] The sandblasting surface treatment is to increase the roughness and better combine with the ETFE fluoro film.

[0023] S5 ETFE fluorofilm bonding: Adopt ETFE fluorofilm bonding production line, use adhesive to bond ETFE fluorofilm to wear-resistant film plate, and obtain initial ETFE fluorofilm plate; ETFE fluorofilm bonding production line, from the starting point to the end point of the production line, arrange substrate unwinding machine, front material storage rack, pretreatment equipment, coating machine, heating machine in sequence, and film material unwinding machine is arranged in parallel with heating machine, and film plate laminating machine, shaping machine, rear material storage rack, protective film laminating machine, leveling machine and leveling machine are arranged in sequence behind heating machine and film material unwinding machine, one side of protective film laminating machine is connected to protective film unwinding machine by input, and the other side of protective film laminating machine is connected to automatic winding machine by output;

[0024] Regarding the bonding problem of ETFE fluorofilm, the high transparency and smooth surface of ETFE fluorofilm will visually expose any poor bonding, such as bubbles, wrinkles or uneven adhesive distribution. The surface energy of ETFE fluorofilm is low, which means that its surface is not easy to form a good bond with the adhesive. The low surface energy makes it difficult for the adhesive to wet the film surface, thus affecting the bonding strength. In order to solve the above problems, a specially designed production line is designed. The advantages of the production line are as follows:

[0025] Overall automation and precise control: The automated design of the production line reduces human operating errors and improves product consistency and quality. The automated process can more accurately control parameters at each stage, such as the amount of adhesive applied, compounding pressure and temperature, thereby improving bonding quality.

[0026] Sophisticated coater design: The coater can precisely control the coating thickness and uniformity of the adhesive, ensuring that there are no bubbles or wrinkles on the film surface. Fine control of the coating process helps avoid uneven distribution of the adhesive, thereby improving the visual and functional properties of the final product.

[0027] Optimal configuration of heating machine and laminating machine: The heating machine ensures that the adhesive is cured at the optimal temperature, optimizes the bonding effect, and prevents high temperature from damaging the ETFE fluoro film. The laminating machine effectively combines the ETFE fluoro film with the substrate under controlled conditions, further ensuring the overall quality of the composite layer.

[0028] Subsequent processing equipment: protective film laminating machine, leveling machine and leveling machine and other subsequent processing equipment ensure the surface protection and dimensional accuracy of the composite material, and improve the overall quality and aesthetics of the product. Protective film lamination can prevent scratches or damage to the ETFE fluorine film during subsequent processing and transportation.

[0029] Automatic winder: The automatic winder ensures that the material at the end of the production line can be neatly wound up, reducing material waste and possible manual operation errors, and improving production efficiency and material utilization.

[0030] These advantages indicate that the use of an ETFE fluorofilm bonding production line can effectively solve the technical problems that may be encountered during the pasting process of the ETFE fluorofilm, while improving production efficiency and product quality, giving it a competitive advantage in the high-end market.

[0031] S6 Preparation of wear-resistant hydrophobic layer: S7.1 Preparation of wear-resistant hydrophobic coating: The wear-resistant hydrophobic coating is composed of polydimethylsiloxane, MTEOS curing agent, nano-silica particles, a catalyst and a solvent, and the solvent is cyclopentane or n-hexane; the catalyst is a platinum compound catalyst; S7.2 Coating: Remove the protective film covered by the protective film composite machine, coat the wear-resistant hydrophobic coating on the initial ETFE fluoromembrane plate, and then perform a curing operation to obtain the ETFE fluoromembrane plate.

[0032] Polydimethylsiloxane (PDMS): PDMS is a silicon-based polymer with extremely low surface energy, which makes the coating have excellent hydrophobic properties. When PDMS is coated on a surface, it can significantly reduce the contact angle of water and other liquids with the surface, allowing water droplets to easily bead up on the surface and roll off, thereby achieving a hydrophobic effect. In addition, PDMS can resist minor wear and tear due to its high flexibility and elasticity, which increases the wear resistance of the coating, allowing it to maintain performance under physical wear conditions.

[0033] MTEOS curing agent: Methyltriethoxysilane (MTEOS) is a silane curing agent used to cure PDMS. It forms a three-dimensional network structure by cross-linking with PDMS, which enhances the mechanical strength and chemical stability of the coating. This cured network structure provides good wear resistance and long-term environmental stability.

[0034] Nano-silica particles: Nano-silica particles play a key role in enhancing the wear resistance of this coating. These particles are evenly distributed in the PDMS matrix, increasing the hardness and stiffness of the coating. During the physical friction process, these hard particles can effectively resist surface wear and protect the coating and substrate. Nano-silica also helps to enhance the hydrophobicity of the coating because they provide a micro-structured surface. These tiny structures increase the roughness of the surface, making it more difficult for water droplets to contact the actual surface of the coating, thereby enhancing the hydrophobic effect.

[0035] Catalyst (platinum compounds): Platinum compounds are used as catalysts to accelerate the curing reaction between PDMS and MTEOS, ensuring that the coating can be completely cured in a short period of time to form a wear-resistant and hydrophobic layer with a complete structure.

[0036] The use of catalysts optimizes the crosslinking density and rate, further improving the overall performance of the coating.

[0037] Solvent (cyclopentane or n-hexane): The selected solvents such as cyclopentane or n-hexane are mainly used to adjust the viscosity of the coating. These solvents will evaporate after the coating process, leaving a uniformly distributed cured coating.

[0038] Through the synergistic effect of the above components, the wear-resistant hydrophobic layer not only has excellent hydrophobic properties, but also can maintain structural and functional stability under physical wear conditions.

[0039] Preferably, in step S1, during the surface treatment process, the purity of oxygen is greater than 99.5%, and the oxygen flow rate is 50-100 sccm.

[0040] Preferably, in step S2.1, the concentration of the nitric acid solution is 68%, and the concentration of the sulfuric acid solution is 98%; the ratio of the nitric acid solution to the sulfuric acid solution is 1:3; the heating treatment temperature is 110-140°C; the outer diameter of the multi-walled carbon nanotubes is 10-15nm, and the length is 1-3μm; the particle diameter in the silica sol is not more than 10nm; in the acidification treatment, the heating treatment temperature is 110-140°C; in the silica-carbon tube composite sol, the weight ratio of multi-walled carbon nanotubes: ethanol: dispersant: silica sol is 5-6:20-22:1.5-2:68-70; in step S2.2, the coating is carried out by spin coating, and the curing treatment temperature is 100-200°C.

[0041] Selection and conditions of acid treatment: Use and ratio of nitric acid and sulfuric acid (68% nitric acid and 98% sulfuric acid, ratio of 1:3): The combination of nitric acid and sulfuric acid is used to treat multi-walled carbon nanotubes. The main purpose is to remove impurities on the surface of carbon tubes and introduce functional groups (such as carboxyl groups). These functional groups help the subsequent dispersion process and bonding with silica. Sulfuric acid provides a strong oxidizing effect, while nitric acid can further introduce more functional groups and increase the activity of carbon tubes. Heating treatment temperature (110-140℃): This temperature range is sufficient to promote acid reaction, but it does not cause excessive damage or structural destruction of carbon tubes, thereby maintaining the structural integrity and functionality of carbon nanotubes.

[0042] Preparation of silica-carbon tube composite sol: Use ultrasonic treatment: Ultrasonic treatment is used to enhance the dispersibility of carbon nanotubes in the solution and prevent aggregation. Ultrasonic waves can generate tiny bubbles, whose explosion can break the van der Waals force between carbon tubes, thereby improving their uniform distribution in the solution. Adjust pH to 9-10: At a higher pH value, the stability of silica sol is better, and it is also conducive to the ionization of functional groups on the surface of carbon nanotubes, further improving the interaction and adhesion between carbon nanotubes and silica particles.

[0043] Coating and curing: Spin coating is an efficient coating technology that can form a uniform film on the substrate. The thickness and uniformity of the film layer can be adjusted by controlling the spin coating speed and time.

[0044] Curing temperature (100-200℃): Curing within this temperature range can ensure that the organic components in the composite material are fully cross-linked and cured, and also avoid material degradation that may be caused by high temperature. The curing process enhances the mechanical strength and chemical stability of the film layer, ensuring its durability and functionality in the application.

[0045] Preferably, in step S3.2, the parameters during the sputtering process are set as follows: argon flow rate: set to 40-45sccm to ensure good sputtering efficiency; oxygen flow rate: set to 2-3sccm at the beginning; every 3-5 minutes, the oxygen flow rate increases by 1 to 2sccm; while observing the growth of the film layer and the performance changes, adjust the size and frequency of the increment according to the observation results; when the oxygen flow rate reaches the preset target value of 10-11sccm, maintain this flow rate until the end of the sputtering process; the pulse frequency is 500Hz, and the pulse width is 100μs.

[0046] Preheat to 150-200℃: Preheating can reduce the difference in thermal expansion between the substrate and the film layer, preventing cracks in the coating during or after sputtering. Preheating helps to increase the energy of the substrate surface, making it easier for the indium tin oxide particles to form a uniform and compact structure during deposition.

[0047] Magnetron sputtering and oxygen introduction: Argon flow rate 40-45sccm: Argon, as an inert gas, is mainly used to provide sufficient ion impact force to sputter the target material (indium tin oxide) from the target surface. This flow range ensures good sputtering efficiency while maintaining the stability of the sputtering process. Gradually increase the oxygen flow rate: The low oxygen flow rate at the beginning helps to form more indium tin oxide (ITO) deposition. As the sputtering proceeds, gradually increasing the oxygen flow rate can adjust the degree of oxidation of the film layer and help form a nanoporous structure. The nanoporous structure can increase the surface roughness and specific surface area of ​​the coating, which is very important for improving the optical and electrical properties of the coating. Pulse sputtering method: Pulse frequency 500Hz, pulse width 100μs: Pulse sputtering allows the target material to be sputtered at very precise time intervals, so that the deposition of the material can be strictly controlled. This fine control helps to manufacture a uniform nanoporous structure, thereby improving the uniformity and quality of the film layer. During the pulse sputtering process, the short-term high energy release helps the material particles to be more densely and evenly stacked on the substrate. This not only increases the density of the film, but also helps to evenly distribute the nanopores, improving the overall structural stability and functionality of the film. Since pulsed sputtering allows operation at lower average power, it can effectively reduce thermal stress during film generation. This decompression effect helps avoid cracks and other defects in the film, thereby improving the mechanical stability and durability of the coating.

[0048] Preferably, in step S4.1, the weight ratio of polyurethane: polytetrafluoroethylene powder: silicon carbide particles: two-component epoxy resin: anhydrous ethanol is 60:10:15:5:10; the particle size of the silicon carbide particles is 5-10 microns; in step S4.2, the curing temperature is 80-120°C.

[0049] Preferably, in step S5, the thickness of the ETFE fluoro film is 100 um, and the fireproof grade is A2; the adhesive adopts a polymer adhesive, and the thickness of the bonding layer formed by the adhesive is 40 um; the target temperature of the heating machine is 200°C.

[0050] Preferably, in step S6, in the wear-resistant hydrophobic coating, the weight ratio of polydimethylsiloxane:MTEOS curing agent:nano-silicon dioxide particles:catalyst is 70-72:9-10:12-15:0.95-1.03; during the curing operation, the curing temperature is 60-80°C.

[0051] Polydimethylsiloxane 70-72%: This ratio ensures that polydimethylsiloxane, as the main matrix, occupies the main volume of the coating, thereby ensuring basic hydrophobicity and flexibility.

[0052] MTEOS curing agent 9-10%: The MTEOS curing agent at this ratio is sufficient to react with polydimethylsiloxane to form a sufficient network structure, but not excessive enough to cause the coating to become too hard and brittle.

[0053] Nano-silica particles 12-15%: Within this ratio range, the content of nano-silica particles can effectively enhance the structural strength of the coating while maintaining appropriate dispersion and surface properties. Too much may cause particle aggregation, affecting the uniformity and appearance of the coating.

[0054] Catalyst 0.95-1.03%: Catalyst content within this range ensures the efficiency of the curing reaction and promotes the coating to quickly form a cross-linked structure at the preset curing temperature, while excessive catalyst may cause the reaction rate to be too fast, affecting the quality and performance of the coating.

[0055] The setting of these parameters is aimed at balancing the mechanical properties, chemical stability and processing performance of the coating during application, thereby ensuring the overall performance and application effect of the coating. This parameter ratio is optimized based on the chemical characteristics of the material and the expected application performance.

[0056] Compared with the prior art, the present invention has the following beneficial effects:

[0057] Excellent anti-corrosion performance: Aluminum-zinc alloy plate is used as the substrate. By setting a composite coating on the surface of the substrate, the corrosion resistance of the material is greatly improved, which prevents the metal substrate from being oxidized and corroded in harsh environments, thereby extending the service life of the membrane plate.

[0058] Excellent thermal insulation performance: The indium tin oxide layer coated on the surface of the membrane can effectively reflect infrared rays in sunlight and reduce heat radiation. This function is particularly important in hot weather, which can significantly improve the thermal insulation effect of the membrane, reduce indoor temperature, save energy consumption, and improve the comfort of living and working environment.

[0059] Scratch protection: Adding a wear-resistant layer to the surface of the membrane not only improves its scratch resistance, but also effectively protects the inner indium tin oxide infrared insulation layer to prevent the degradation of insulation performance due to scratches. This design ensures the stability and reliability of the membrane during long-term use.

[0060] Good weather resistance: The ETFE fluoro film bonding production line is used to tightly attach the ETFE fluoro film layer to the substrate to ensure the stability and durability of the film under different climatic conditions. The ETFE fluoro film material itself has excellent weather resistance and can effectively resist the damage of external factors such as ultraviolet rays, wind and rain.

[0061] Application of wear-resistant hydrophobic layer: Coating with a wear-resistant hydrophobic layer effectively reduces the adhesion of water on the membrane surface, improves its self-cleaning performance, and reduces maintenance costs. The introduction of this layer not only protects the membrane surface, but also enhances its stability during long-term use.

[0062] In summary, the ETFE fluorofilm sheet of the present invention exhibits excellent performance through the design of a multi-layer film structure, combined with multiple functions such as anti-corrosion, heat insulation, and wear resistance. This innovative design not only improves the adaptability of the film sheet in various extreme environments, but also greatly prolongs its service life, reduces maintenance costs, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0063] Figure 1 This is a comparison chart of product performance in salt spray resistance test.

[0064] Figure 2 This is a comparison chart of metal adhesion test performance.

[0065] Figure 3 This is a comparison chart of metal adhesion test in a salt spray environment.

[0066] Figure 4 This is a cost comparison chart.

[0067] Figure 5 This is a schematic diagram of the ETFE fluorofilm bonding production line.

[0068] Figure 6 This is a comparison chart of UV resistance aging test.

[0069] Figure 7 This is a comparison chart of the T-bend test. DETAILED DESCRIPTION

[0070] The following are specific embodiments of the present invention and the accompanying drawings to further describe the technical solution of the present invention, but the present invention is not limited to these embodiments.

[0071] A method for preparing an ETFE fluorine film plate with excellent comprehensive performance, wherein the ETFE fluorine film plate adopts a national standard aluminum-zinc plate as a substrate, and a composite coating is provided on the upper surface and the lower surface of the substrate, wherein the composite coating comprises a silicon dioxide-carbon tube coating, an indium tin oxide coating, a wear-resistant layer, an ETFE fluorine film layer and a wear-resistant hydrophobic layer. The method for preparing the ETFE fluorine film plate comprises the following steps:

[0072] S1 Substrate surface treatment: S1.1 Cleaning: First, use a degreasing agent such as acetone or ethanol to thoroughly clean the aluminum-zinc alloy-plated substrate to remove grease, dust and other surface impurities. Rinse: Rinse the cleaned substrate thoroughly with deionized water to remove any residual cleaning agent and loose contaminants. Drying: Use hot air to blow dry and ensure that the substrate surface is completely dry. S1.2 Plasma treatment: Plasma generation: Place the treated dry substrate in the plasma reaction chamber. Oxygen purification: Ensure that the purity of the oxygen used is greater than 99.5% to optimize the surface activation effect. Oxygen flow adjustment: Set the oxygen flow rate in the range of 50-100sccm, which helps control the density of the plasma and the uniformity of the reaction. Power setting: According to the specifications of the equipment, adjust the power setting to produce the required plasma intensity. Processing time: The plasma treatment time is between 3-5 minutes; S1.3 Post-treatment: Cooling: After the treatment is completed, let the substrate cool naturally at room temperature. Clean again: Rinse briefly with deionized water to remove any surface residues that may be generated by plasma treatment. Final drying: Dry the substrate thoroughly again to prepare for the next coating treatment.

[0073] S2 Preparation of silica-carbon tube film layer: S2.1 Preparation of silica-carbon tube composite sol: Acid treatment: Heat the multi-walled carbon nanotubes in a mixed solution of nitric acid solution and sulfuric acid solution; Rinse the acid-treated multi-walled carbon nanotubes with deionized water and then dry them in a vacuum oven; Add the multi-walled carbon nanotubes to an ethanol solution containing a dispersant and use ultrasonic treatment; Add the treated multi-walled carbon nanotube solution to the silica sol, add a pH adjusting solution, adjust the pH value to 9, and finally stir until uniform; the dispersant is polyvinyl pyrrolidone; The pH adjusting solution is a sodium hydroxide solution with a concentration of 0.1M; S2.2 Coating: Coat the prepared silica-carbon tube composite sol on an aluminum-zinc alloy substrate. After the coating is completed, perform a curing treatment to obtain a silica-carbon tube sheet; The thickness of the silica-carbon tube film layer is 20um;

[0074] The concentration of the nitric acid solution is 68%, and the concentration of the sulfuric acid solution is 98%; the ratio of the nitric acid solution to the sulfuric acid solution is 1:3; the heating treatment temperature is 140°C; the outer diameter of the multi-walled carbon nanotubes is 10-15nm, and the length is 1-3μm; the particle diameter in the silica sol is not greater than 10nm; in the silica-carbon tube composite sol, the weight ratio of the multi-walled carbon nanotubes: ethanol: dispersant: silica sol is 6:21:1.8:70; in step S2.2, the coating is carried out by spin coating, and the curing treatment temperature is 150°C.

[0075] S3 Preparation of indium tin oxide coating layer: S3.1 Preheating: preheat the silicon dioxide-carbon tube sheet to 180°C; S3.2 Preparation of nanoporous structure membrane: using magnetron sputtering equipment to deposit indium tin oxide material on the surface of the preheated silicon dioxide-carbon tube sheet, and gradually introducing oxygen and using pulse sputtering to promote the formation of nanopores during the sputtering process; S3.3 Annealing: after the sputtering process is completed, it is naturally cooled at room temperature, and then annealed at 300°C. After the annealing is completed, an indium tin oxide plate is obtained; the thickness of the indium tin oxide coating is 40um;

[0076] The parameters during the sputtering process were set as follows: argon flow rate: set to 45 sccm to ensure good sputtering efficiency; oxygen flow rate: set to 2-3 sccm at the beginning; the oxygen flow rate increased by 1 sccm every 5 minutes; when the oxygen flow rate reached the preset target value of 10 sccm, this flow rate was maintained until the end of the sputtering process; the pulse frequency was 500 Hz and the pulse width was 100 μs.

[0077] S4 Preparation of wear-resistant layer: S4.1 Preparation of wear-resistant coating: The wear-resistant slurry is composed of polyurethane, polytetrafluoroethylene powder, silicon carbide particles, two-component epoxy resin and anhydrous ethanol, S4.2 Coating: Coat the wear-resistant slurry on the indium tin oxide coated plate. After coating, perform curing and sandblasting surface treatment to obtain a wear-resistant film plate; the thickness of the wear-resistant layer is 10um;

[0078] In step S4.1, the weight ratio of polyurethane: polytetrafluoroethylene powder: silicon carbide particles: two-component epoxy resin: anhydrous ethanol is 60:10:15:5:10; the particle size of the silicon carbide particles is 5-10 microns; in step S4.2, the curing temperature is 110°C.

[0079] S5 bonding ETFE fluorine film: Figure 5As shown, an ETFE fluoro film bonding production line is adopted, and the ETFE fluoro film is bonded to the wear-resistant film plate by using a polymer adhesive to obtain an initial ETFE fluoro film plate; the ETFE fluoro film bonding production line, from the starting point to the end point of the production line, is sequentially arranged with a substrate unwinding machine, a front material storage rack, a pretreatment device, a coating machine, and a heating machine, and a film material unwinding machine is arranged in parallel with the heating machine, and a film plate laminating machine, a shaping machine, a rear material storage rack, a protective film laminating machine, a leveling machine, and a leveling machine are sequentially arranged behind the heating machine and the film material unwinding machine, and one side of the protective film laminating machine is connected to the protective film unwinding machine at an input, and the other side of the protective film laminating machine is connected to the automatic winding machine at an output;

[0080] The thickness of the ETFE fluorine film is 100um, and the fire protection grade is A2; the adhesive adopts a polymer adhesive, and the thickness of the bonding layer formed by the adhesive is 40um; the target temperature of the heating machine is 200℃.

[0081] The workflow of the ETFE fluorofilm bonding production line is a series of precisely controlled steps designed to effectively prepare and process ETFE fluorofilm panels. The following are the detailed steps of the main equipment working together on the production line:

[0082] Substrate Unwinder: This equipment is used to unwind the substrate material of the wear-resistant membrane from the coil, which is the starting point of the production line. The unwinding of the substrate is the first step in the entire production process, providing the necessary raw materials for subsequent processing.

[0083] Front material rack: The unfolded substrate material is temporarily stored here. The main function of this area is to ensure the continuous supply of raw materials to the production line, and at the same time, it serves as a buffer to reduce production interruptions that may be caused by insufficient supply. Pretreatment equipment: Before the substrate material enters the coating machine, the pretreatment equipment is used to clean, remove dust and preheat the substrate. This step is crucial to improve the adhesion of the adhesive and ensure the effect and quality of the bonding process.

[0084] Coating machine: The coating machine evenly applies adhesive on the substrate. The quality of coating directly affects the performance of the final product, so the uniformity and accuracy of the coating process must be ensured.

[0085] Heating machine: The coated substrate is heated by the heating machine to heat the adhesive, thus providing better conditions for the bonding process. The target temperature is set at 200°C, which helps to optimize the bonding ability of the adhesive. Film unwinding machine: This equipment is responsible for unwinding the ETFE fluoro film so that it can be laminated with the substrate coated with adhesive. The smoothness and continuity of the unwinding are very critical to the subsequent lamination process.

[0086] Membrane sheet laminating machine: In this stage, the substrate treated with adhesive is tightly bonded with the ETFE fluorofilm under appropriate pressure and temperature conditions. This process ensures the overall structure and performance of the membrane sheet.

[0087] Forming machine: Through the processing of the forming machine, the newly made ETFE fluorofilm sheet is cured and shaped in a controlled environment to ensure that the material meets the preset physical performance standards and dimensional requirements.

[0088] Post-stocking rack: The finalized membrane panels are temporarily stored here before entering the next processing stage. This ensures that there is enough time and space for the next step of compounding and finishing.

[0089] Protective film laminating machine: This equipment is used to laminate a protective film on the surface of the prepared ETFE fluoro film. This protective film can prevent the film from being scratched or damaged during subsequent processing and transportation.

[0090] Leveling machines and flattening machines: These machines are used to further sort and flatten the ETFE fluorofilm panels to ensure the flatness and dimensional accuracy of the products to meet the specific requirements of customers.

[0091] Protective film unwinder: used in conjunction with the protective film laminator to provide a continuous supply of protective film to keep the production process smooth.

[0092] Automatic Winder: The end point of the production line, used to wind up the film sheet after all the processing steps. This step marks the completion of the entire manufacturing process.

[0093] S6 Preparation of wear-resistant hydrophobic layer: S6.1 Preparation of wear-resistant hydrophobic coating: The wear-resistant hydrophobic coating is composed of polydimethylsiloxane, MTEOS curing agent, nano-silicon dioxide particles, catalyst and solvent, and the solvent is cyclopentane or n-hexane; the catalyst is a platinum compound catalyst; S6.2 Coating: Remove the protective film, coat the wear-resistant hydrophobic coating on the membrane plate, and then perform curing operation to obtain an ETFE fluoro membrane plate, and the thickness of the wear-resistant hydrophobic layer is 20um;

[0094] In the wear-resistant hydrophobic coating, the weight ratio of polydimethylsiloxane: MTEOS curing agent: nano-silica particles: catalyst is 70:0:14:1; during the curing operation, the curing temperature is 70°C.

[0095] The ETFE fluorine film prepared in the specific example was sent to the National Material Chemistry Testing Center for testing. Some of the test results are as follows:

[0096]

[0097]

[0098]

[0099] Comparison of similar products: Product performance comparison 1:

[0100]

[0101]

[0102] Product performance comparison 2: Salt spray resistance test (medium salt spray 4000 hours), the results are shown in 1.

[0103] Product performance comparison 3: Metal adhesion test, the results are as follows Figure 2 shown.

[0104] Product performance comparison 4: Metal adhesion test in salt spray environment, such as Figure 3 shown.

[0105] Cost comparison: Comparison of new construction and subsequent maintenance costs of ETFE fluorofilm panels and ordinary color steel panels, such as Figure 4 shown.

[0106] UV aging test comparison: ETFE fluorine film board and ordinary coating board are tested for UV aging resistance. Figure 6 shown.

[0107] T-bend test comparison: ETFE fluorine film board and polyester board and fluorocarbon board are tested for T-bend. Figure 7 shown.

[0108] The specific embodiments described herein are merely examples of the spirit of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in similar ways without departing from the spirit of the present invention or exceeding the defined scope.

Claims

1. A method for preparing an ETFE fluorine film sheet with excellent comprehensive performance, characterized in that: The ETFE fluorine film plate uses a metal plate coated with an aluminum-zinc alloy film layer as a substrate, and the upper surface and the lower surface of the substrate are provided with a composite coating, and the composite coating includes a silicon dioxide-carbon tube coating, an indium tin oxide coating, a wear-resistant layer, an ETFE fluorine film layer and a wear-resistant hydrophobic layer. The preparation method of the ETFE fluorine film plate includes the following steps: S1 Substrate surface treatment: After cleaning and drying the substrate, plasma technology is used to treat the substrate surface with oxygen to obtain a pre-coated plate; S2 Preparation of silica-carbon tube coating: S2.1 Preparation of silica-carbon tube composite sol: Acid treatment: Heat the multi-walled carbon nanotubes in a mixed solution of nitric acid solution and sulfuric acid solution; Rinse the acid-treated multi-walled carbon nanotubes with deionized water and then dry them in a vacuum oven; Add the multi-walled carbon nanotubes to an ethanol solution containing a dispersant and use ultrasonic treatment; Add the treated multi-walled carbon nanotube solution to the silica sol, add a pH adjusting solution, adjust the pH value to 9-10, and finally stir until uniform; the dispersant is polyvinyl pyrrolidone; The pH adjusting solution is a sodium hydroxide solution with a concentration of 0.1M; S2.2 Coating: Coat the prepared silica-carbon tube composite sol on the pre-coated plate, and after the coating is completed, perform a curing treatment to obtain a silica-carbon tube film plate; S3: Preparing an indium tin oxide coating: S3.1: Preheating: Preheating the silicon dioxide-carbon tube sheet to 150-200° C.; S3.2 Preparation of nanoporous structure membrane: using magnetron sputtering equipment to deposit indium tin oxide material on the surface of the preheated silicon dioxide-carbon tube sheet, and gradually introducing oxygen and using pulse sputtering to promote the formation of nanopores during the sputtering process; S3.3 Annealing: after the sputtering process is completed, it is naturally cooled at room temperature, and then annealing treatment is performed at a temperature of 200-400°C. After the annealing is completed, an indium tin oxide membrane plate is obtained; S4 prepares the wear-resistant layer: S4.1 prepares the wear-resistant coating: the wear-resistant slurry is composed of polyurethane, polytetrafluoroethylene powder, silicon carbide particles, two-component epoxy resin and anhydrous ethanol, S4.2 coating: the wear-resistant slurry is coated on the indium tin oxide coated plate, and after the coating is completed, the curing operation and the sandblasting surface treatment operation are performed to obtain the wear-resistant film plate; S5 ETFE fluorofilm bonding: Adopt ETFE fluorofilm bonding production line, use adhesive to bond ETFE fluorofilm to wear-resistant film plate, and obtain initial ETFE fluorofilm plate; ETFE fluorofilm bonding production line, from the starting point to the end point of the production line, arrange substrate unwinding machine, front material storage rack, pretreatment equipment, coating machine, heating machine in sequence, and film material unwinding machine is arranged in parallel with heating machine, and film plate laminating machine, shaping machine, rear material storage rack, protective film laminating machine, leveling machine and leveling machine are arranged in sequence behind heating machine and film material unwinding machine, one side of protective film laminating machine is connected to protective film unwinding machine by input, and the other side of protective film laminating machine is connected to automatic winding machine by output; S6 Preparation of wear-resistant hydrophobic layer: S6.1 Preparation of wear-resistant hydrophobic coating: The wear-resistant hydrophobic coating is composed of polydimethylsiloxane, MTEOS curing agent, nano-silica particles, a catalyst and a solvent, and the solvent is cyclopentane or n-hexane; the catalyst is a platinum compound catalyst; S6.2 Coating: Remove the protective film covered by the protective film composite machine, coat the wear-resistant hydrophobic coating on the initial ETFE fluoromembrane plate, and then perform a curing operation to obtain the ETFE fluoromembrane plate.

2. The method for preparing the ETFE fluorine film sheet with excellent comprehensive performance as claimed in claim 1, characterized in that: In step S1, during the surface treatment process, the purity of oxygen is greater than 99.5%, and the oxygen flow rate is 50-100 sccm.

3. The method for preparing the ETFE fluorine film sheet with excellent comprehensive performance as claimed in claim 1, characterized in that: In step S2.1, the concentration of the nitric acid solution is 68%, and the concentration of the sulfuric acid solution is 98%; the ratio of the nitric acid solution to the sulfuric acid solution is 1:3; the heating treatment temperature is 110-140°C; the outer diameter of the multi-walled carbon nanotubes is 10-15nm, and the length is 1-3μm; the particle diameter in the silica sol is not more than 10nm; in the acidification treatment, the heating treatment temperature is 110-140°C; in the silica-carbon tube composite sol, according to the weight ratio, the multi-walled carbon nanotubes: ethanol: dispersant: silica sol is 5-6:20-22:1.5-2:68-70; in step S2.2, the coating is carried out by spin coating, and the curing treatment temperature is 100-200°C.

4. The method for preparing the ETFE fluorine film sheet with excellent comprehensive performance as claimed in claim 1, characterized in that: In step S3.2, the parameters during the sputtering process are set as follows: Argon flow rate: set to 40-45sccm to ensure good sputtering efficiency; Oxygen flow rate: set to 2-3sccm at the beginning; every 3-5 minutes, the oxygen flow rate increases by 1 to 2sccm; while observing the growth of the film layer and the performance changes, adjust the size and frequency of the increment according to the observation results; when the oxygen flow rate reaches the preset target value of 10-11sccm, maintain this flow rate until the end of the sputtering process; the pulse frequency is 500Hz and the pulse width is 100μs.

5. The method for preparing the ETFE fluorine film sheet with excellent comprehensive performance as claimed in claim 1, characterized in that: In step S4.1, the weight ratio of polyurethane: polytetrafluoroethylene powder: silicon carbide particles: two-component epoxy resin: anhydrous ethanol is 60:10:15:5:10; the particle size of the silicon carbide particles is 5-10 microns; in step S4.2, the curing temperature is 80-120°C.

6. The method for preparing the ETFE fluorine film sheet with excellent comprehensive performance as claimed in claim 1, characterized in that: In step S5, the thickness of the ETFE fluorine film is 100um, and the fire protection grade is A2; the adhesive adopts a polymer adhesive, and the thickness of the bonding layer formed by the adhesive is 40um; the target temperature of the heating machine is 200°C.

7. The method for preparing the ETFE fluorine film sheet with excellent comprehensive performance as claimed in claim 1, characterized in that: In step S6, in the wear-resistant hydrophobic coating, the weight ratio of polydimethylsiloxane: MTEOS curing agent: nano-silicon dioxide particles: catalyst is 70-72: 9-10: 12-15: 0.95-1.03; during the curing operation, the curing temperature is 60-80°C.

Citation Information

Cited By

  • Anti-dripping ETFE film for greenhouse and preparation method of anti-dripping ETFE film

    CN121536065A

  • Droplet-proof ETFE film for greenhouses and method for producing the same

    CN121536065B