A multilayer polyetherimide energy storage composite dielectric film and its application
By introducing 4-N,N-dimethylaminophenylboronic acid and tetrafluorotetracyanoquinoline dimethane into a polyetherimide film to form a multilayer electronic layer, the problem of high conductivity loss of polyetherimide-based energy storage composite media at high temperatures is solved, achieving high-efficiency energy storage performance and long-term stability.
Patent Information
- Application Number
- CN202411529686.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-30
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-10-30
AI Technical Summary
Polyetherimide-based energy storage composite media suffer from high conductivity loss and poor energy storage performance at high temperatures. Existing modification strategies lead to space charge accumulation and electric field distortion in the media, affecting long-term durability.
A multilayer polyetherimide energy storage composite dielectric film was constructed by introducing 4-N,N-dimethylaminophenylboronic acid as a scattering electron layer and tetrafluorotetracyanoquinoline dimethane as a trapping electron layer to form a bifunctional symmetrical three-layer structure. The position and thickness of the electron layer were controlled to hinder carrier injection and transport, thereby enhancing the stability of the dielectric.
At 150℃ and 620kV/mm, the charge-discharge efficiency reached 93.26% and the discharge energy density reached 6.14J/cm3, significantly improving the energy storage performance and stability of the composite medium.
Smart Images

Figure CN119410010B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of energy storage dielectric materials and their preparation technology. Background Technology
[0002] The rapid development of ultra-high voltage direct current (UHVDC) transmission, new energy power generation, and electric vehicles has created a significant demand for high-efficiency, low-cost, and environmentally friendly energy storage technologies. Polymer-based dielectric capacitors, with their high power density, large open-circuit voltage, and good safety, have become an important energy storage device. However, under complex operating conditions such as strong electric fields and high temperatures, dielectric capacitors still face the problem of deteriorated energy storage performance. This is because, under extreme conditions, the insulation of the energy storage medium material decreases and conductivity losses increase.
[0003] Polyetherimide (PEI) contains imide groups in its molecular structure. The carbon-nitrogen and carbon-oxygen bonds in these groups have high bond energies, making them resistant to breakage at high temperatures. Furthermore, they possess numerous aromatic ring structures, resulting in high rigidity and excellent temperature resistance, making them a promising candidate for high-temperature energy storage dielectrics. However, despite PEI's good temperature resistance, its conductivity loss increases sharply at 150°C, severely degrading its energy storage performance. Current research has confirmed that introducing traps is an effective modification strategy to improve energy storage performance, particularly through doping with organic semiconductor molecules, which has shown great potential. However, introducing too many traps leads to space charge accumulation in the dielectric and causes electric field distortion, degrading the dielectric's long-term durability. Therefore, there is an urgent need to develop high-performance energy storage dielectric materials suitable for complex operating conditions and long-term durability while minimizing the amount of traps introduced. Summary of the Invention
[0004] The purpose of this invention is to solve the problems of high high-temperature dielectric loss and poor energy storage performance of existing polyetherimide-based energy storage composite media, and to provide a multilayer polyetherimide energy storage composite media film and its application.
[0005] This invention incorporates 4-N,N-dimethylaminophenylboronic acid (4-NB), a filler with electron-scattering properties, into polyetherimide (PEI) as an electron-scattering layer, and tetrafluorotetracyanoquinoline dimethyl ether (F4TCNQ), a filler with electron-trapping properties, into PEI as an electron-trapping layer. By controlling the position and thickness of the electron-scattering and electron-trapping layers, a bifunctional symmetrical three-layer composite dielectric (multilayer polyetherimide energy storage composite dielectric film) with both electron-scattering and electron-trapping properties is constructed. The electron-scattering and electron-trapping layers effectively hinder carrier injection and transport, reducing the conductivity current. Furthermore, the strong interaction between the bifunctional layers also contributes to improving the breakdown field strength, ultimately enhancing the energy storage performance of the composite dielectric. Results show that the prepared composite dielectric achieves a discharge energy density of 6.14 J / cm² at 150℃, 620 kV / mm, and a charge-discharge efficiency of 93.26%. 3 .
[0006] A multilayer polyetherimide energy storage composite dielectric film has a three-layer structure, consisting of an electron-scattering layer and an electron-trapping layer. One structure has two surface layers as electron-scattering layers and a middle layer as an electron-trapping layer; another structure has two surface layers as electron-trapping layers and a middle layer as an electron-scattering layer. The electron-scattering layer is composed of polyetherimide and 4-N,N-dimethylaminophenylboronic acid; the electron-trapping layer is composed of polyetherimide and tetrafluorotetracyanoquinoline dimethane.
[0007] The multilayer polyetherimide energy storage composite dielectric film has two surface layers that scatter electrons and an intermediate layer that traps electrons. Its preparation method is specifically carried out according to the following steps:
[0008] 1. Polyetherimide and 4-N,N-dimethylaminophenylboronic acid are dissolved in N-methylpyrrolidone, and then vacuum defoaming is performed to obtain a bubble-free 4-NB / PEI mixed solution.
[0009] 2. Polyetherimide and tetrafluorotetracyanoquinoline dimethyl ether are dissolved in N-methylpyrrolidone and then subjected to vacuum defoaming treatment to obtain a bubble-free F4TCNQ / PEI mixed solution.
[0010] 3. Apply the bubble-free 4-NB / PEI mixed solution to the substrate by scraping, and then dry it to form the lower surface composite film, which is the electron scattering layer.
[0011] 4. Apply the bubble-free F4TCNQ / PEI mixed solution to the lower surface composite film by scraping, and then dry it to form the middle layer composite film, which is the electron-capturing layer.
[0012] 5. The bubble-free 4-NB / PEI mixed solution is coated onto the intermediate composite film and then dried to form the upper composite film, which is the electron scattering layer; thus, a three-layer composite dielectric film is constructed, which is the multilayer polyetherimide energy storage composite dielectric film.
[0013] A multilayer polyetherimide energy storage composite dielectric film has two surface layers that trap electrons and an intermediate layer that scatters electrons. Its preparation method specifically includes the following steps:
[0014] 1. Polyetherimide and 4-N,N-dimethylaminophenylboronic acid are dissolved in N-methylpyrrolidone, and then vacuum defoaming is performed to obtain a bubble-free 4-NB / PEI mixed solution.
[0015] 2. Polyetherimide and tetrafluorotetracyanoquinoline dimethyl ether are dissolved in N-methylpyrrolidone and then subjected to vacuum defoaming treatment to obtain a bubble-free F4TCNQ / PEI mixed solution.
[0016] 3. Apply the bubble-free F4TCNQ / PEI mixed solution to the substrate by scraping, and then dry it to form the lower surface composite film, which is the electron-capturing layer.
[0017] 4. Apply the bubble-free 4-NB / PEI mixed solution to the lower surface composite film by scraping, and then dry it to form the intermediate composite film, which is the electron scattering layer.
[0018] 5. The bubble-free F4TCNQ / PEI mixed solution is coated onto the intermediate composite film and then dried to form the upper composite film, which is the electron-capturing layer; thus, a three-layer composite dielectric film is constructed, which is a multilayer polyetherimide energy storage composite dielectric film.
[0019] A multilayer polyetherimide energy storage composite dielectric film is used as the dielectric material of a dielectric capacitor; the dielectric capacitor is used in high-voltage flexible DC transmission converter valves, new energy power generation filters, or new energy vehicle inverters.
[0020] A multilayer polyetherimide energy storage composite dielectric film is used in energy storage devices under high temperature and high field conditions. It achieves a discharge energy density of 6.14 J / cm³ at a charge / discharge efficiency of 93.26% under conditions of 150℃ and 620 kV / mm. 3 .
[0021] Compared with the prior art, the present invention has the following advantages:
[0022] I. This invention introduces 4-N,N-dimethylaminophenylboronic acid, a molecular semiconductor with scattering electrons, into a polyetherimide polymer to construct an electron-scattering layer (4-NB / PEI), and introduces tetrafluorotetracyanoquinoline dimethyl etherimide, a molecular semiconductor with trapping electrons, into the polyetherimide polymer to construct an electron-trapping layer (F4TCNQ / PEI). Using either 4-NB / PEI or F4TCNQ / PEI layers as the surface layer and another type of composite dielectric as the intermediate layer, a bifunctional three-layer symmetrical polyetherimide film is constructed. This multilayer structure possesses both electron-scattering and electron-trapping functions, synergistically suppressing low-energy electron injection and high-energy electron transport while reducing the number of traps, and shows good potential in reducing carrier accumulation. Final example results show that the all-organic energy storage composite dielectric prepared in this invention achieves a discharge energy density of 6.14 J / cm² at 150℃, 620 kV / mm, and a charge-discharge efficiency of 93.26%. 3 ;
[0023] II. In this invention, 4-N,N-dimethylaminophenylboronic acid, which has the property of scattering electrons, is introduced into polyetherimide polymer. The introduced small molecule has a high proportion of negative surface electrostatic potential, which can play a strong scattering role for electrons. It can reduce the collisional ionization of electrons in the electron transport path, weaken the energy of electrons, and reduce the injection and transport of electrons.
[0024] Third, this invention introduces tetrafluorotetracyanoquinoline dimethyl ether into polyetherimide polymers, which has electron-trapping and scattering properties. The introduced small molecule has a high proportion of positive surface electrostatic potential, which can play a strong role in trapping electrons and avoid high-energy electron transport.
[0025] IV. The multilayer polyetherimide energy storage composite film prepared by this invention can utilize its multilayer structure to scatter and capture electrons, thereby suppressing low-energy electron injection and high-energy electron transport in the bulk. Furthermore, the electrostatic attraction between the dual-functional layers creates strong interfacial forces, enhancing the stability of the composite medium. The interlayer filler contact redistributes the filler electrostatic potential, strengthens intermolecular forces, and enhances the ability to resist high-energy electron impacts, thereby reducing the energy loss of the composite medium. This solves the problems of poor high-temperature energy storage characteristics and high dielectric loss of existing polyetherimides.
[0026] Fifth, this invention belongs to a fully organic system, which is suitable for large-scale production. Moreover, the multi-layer structure is a symmetrical structure, which can reduce the difficulty of production and provide a new research and development idea for the preparation of high-temperature, high-field and long-term service energy storage fully organic composite films. Attached Figure Description
[0027] Figure 1(a) is the surface electrostatic potential cloud diagram and potential statistics diagram of 4-N,N-dimethylaminophenylboronic acid; (b) is the surface electrostatic potential cloud diagram and potential statistics diagram of tetrafluorotetracyanoquinoline dimethane.
[0028] Figure 2 (a) shows the cross-sectional morphology and elemental distribution of the FNF-3 film, (b) shows the cross-sectional morphology and elemental distribution of the FNF-4 film, (c) shows the cross-sectional morphology and elemental distribution of the FNF-5 film, (d) shows the cross-sectional morphology and elemental distribution of the NFN-3 film, (e) shows the cross-sectional morphology and elemental distribution of the NFN-4 film, and (f) shows the cross-sectional morphology and elemental distribution of the NFN-5 film.
[0029] Figure 3 (a) shows the XRD patterns of the composite media obtained in different embodiments, and (b) shows the XRD patterns of 4-N,N-dimethylaminophenylboronic acid and tetrafluorotetracyanoquinoline dimethane and the comparative examples.
[0030] Figure 4 (a) shows the infrared spectra of the composite media obtained in different embodiments, and (b) shows the infrared spectra of 4-N,N-dimethylaminophenylboronic acid and tetrafluorotetracyanoquinoline dimethane and the comparative examples.
[0031] Figure 5 (a) shows the dielectric constant and dielectric loss of the composite media obtained in different embodiments as a function of frequency at 150°C; (b) shows the dielectric constant and dielectric loss of the comparative example as a function of frequency at 150°C.
[0032] Figure 6 (a) is a Weibull distribution diagram of the breakdown field strength of the composite medium obtained in different embodiments at 150°C, and (b) is a Weibull distribution diagram of the breakdown field strength of the comparative example at 150°C.
[0033] Figure 7 (a) is a graph showing the change of electrical conductivity current with electric field strength at 150°C for composite media obtained in different embodiments; (b) is a graph showing the change of electrical conductivity current with electric field strength at 150°C for comparative examples.
[0034] Figure 8 (a) is a graph showing the energy storage characteristics of the composite medium obtained in different embodiments at 150°C, and (b) is a graph showing the energy storage characteristics of the comparative example at 150°C.
[0035] Figure 9(a) Schematic diagram of the interface charge of a thin film with a 3 μm thick electron-scattering layer as the surface layer and an electron-capturing layer as the middle layer; (b) Schematic diagram of the interface charge of a thin film with a 4 μm thick electron-scattering layer as the surface layer and an electron-capturing layer as the middle layer; (c) Schematic diagram of the interface charge of a thin film with a 5 μm thick electron-scattering layer as the surface layer and an electron-capturing layer as the middle layer; (d) Schematic diagram of the interface charge of a thin film with a 5 μm thick electron-capturing layer as the surface layer and an electron-scattering layer as the middle layer.
[0036] Figure 10 (a) is the AC box model diagram of 4-N,N-dimethylaminophenylboronic acid and tetrafluorotetracyanoquinoline dimethane, and (b) is the interaction energy data diagram of 4-N,N-dimethylaminophenylboronic acid and tetrafluorotetracyanoquinoline dimethane. Detailed Implementation
[0037] Specific Implementation Method 1: This implementation method is a multilayer polyetherimide energy storage composite dielectric film with a three-layer structure, consisting of an electron scattering layer and an electron trapping layer; one structure has two surface layers as electron scattering layers and a middle layer as electron trapping layer; another structure has two surface layers as electron trapping layers and a middle layer as electron scattering layer; the electron scattering layer is composed of polyetherimide and 4-N,N-dimethylaminophenylboronic acid; the electron trapping layer is composed of polyetherimide and tetrafluorotetracyanoquinoline dimethane.
[0038] Specific Implementation Method Two: This implementation method differs from Specific Implementation Method One in that the volume ratio of 4-N,N-dimethylaminophenylboronic acid to polyetherimide in the electron scattering layer is 0.008:1; and the volume ratio of tetrafluorotetracyanoquinoline dimethyl etherimide in the electron trapping layer is 0.006:1. The other steps are the same as in Specific Implementation Method One.
[0039] Specific Implementation Method 3: This implementation method differs from Specific Implementation Method 1 or 2 in that the thickness of the multilayer polyetherimide energy storage composite medium film is 5μm to 13μm; the ratio of the thickness of a single surface layer to the total thickness of the multilayer polyetherimide energy storage composite medium film is (3-5):13. Other steps are the same as in Specific Implementation Method 1 or 2.
[0040] Specific Implementation Method Four: The difference between this implementation method and Specific Implementation Methods One to Three is that the two surface layers of the multilayer polyetherimide energy storage composite dielectric film are electron scattering layers, and the middle layer is an electron trapping layer. Its preparation method is specifically carried out according to the following steps:
[0041] 1. Polyetherimide and 4-N,N-dimethylaminophenylboronic acid are dissolved in N-methylpyrrolidone, and then vacuum defoaming is performed to obtain a bubble-free 4-NB / PEI mixed solution.
[0042] 2. Polyetherimide and tetrafluorotetracyanoquinoline dimethyl ether are dissolved in N-methylpyrrolidone and then subjected to vacuum defoaming treatment to obtain a bubble-free F4TCNQ / PEI mixed solution.
[0043] 3. Apply the bubble-free 4-NB / PEI mixed solution to the substrate by scraping, and then dry it to form the lower surface composite film, which is the electron scattering layer.
[0044] 4. Apply the bubble-free F4TCNQ / PEI mixed solution to the lower surface composite film by scraping, and then dry it to form the middle layer composite film, which is the electron-capturing layer.
[0045] 5. A bubble-free 4-NB / PEI mixed solution is coated onto the intermediate composite film using a scraping method, followed by drying to form the upper composite film, which is the electron scattering layer; this constructs a three-layer composite dielectric film, namely a multilayer polyetherimide energy storage composite dielectric film. Other steps are the same as in specific embodiments one to three.
[0046] Specific Implementation Method Five: The difference between this implementation method and Specific Implementation Methods One to Four is that the two surface layers of the multilayer polyetherimide energy storage composite dielectric film are electron-capturing layers, and the middle layer is an electron-scattering layer. Its preparation method is specifically carried out according to the following steps:
[0047] 1. Polyetherimide and 4-N,N-dimethylaminophenylboronic acid are dissolved in N-methylpyrrolidone, and then vacuum defoaming is performed to obtain a bubble-free 4-NB / PEI mixed solution.
[0048] 2. Polyetherimide and tetrafluorotetracyanoquinoline dimethyl ether are dissolved in N-methylpyrrolidone and then subjected to vacuum defoaming treatment to obtain a bubble-free F4TCNQ / PEI mixed solution.
[0049] 3. Apply the bubble-free F4TCNQ / PEI mixed solution to the substrate by scraping, and then dry it to form the lower surface composite film, which is the electron-capturing layer.
[0050] 4. Apply the bubble-free 4-NB / PEI mixed solution to the lower surface composite film by scraping, and then dry it to form the intermediate composite film, which is the electron scattering layer.
[0051] 5. The bubble-free F4TCNQ / PEI mixed solution is coated onto the intermediate composite film and then dried to form the upper composite film, which is the electron-capturing layer; thus, a three-layer composite dielectric film is constructed, which is a multilayer polyetherimide energy storage composite dielectric film. Other steps are the same as in specific embodiments one to four.
[0052] Specific Implementation Method Six: This implementation method differs from Specific Implementation Methods One to Five in the following ways: In step one, the volume ratio of 4-N,N-dimethylaminophenylboronic acid to polyetherimide is 0.008:1; in step one, the total mass of polyetherimide and 4-N,N-dimethylaminophenylboronic acid to the volume ratio of N-methylpyrrolidone is (0.15g~0.18g):1mL; in step two, the volume ratio of tetrafluorotetracyanoquinoline dimethylane to polyetherimide is 0.006:1; in step two, the total mass of polyetherimide and tetrafluorotetracyanoquinoline dimethylane to the volume ratio of N-methylpyrrolidone is (0.15g~0.18g):1mL. The other steps are the same as in Specific Implementation Methods One to Five.
[0053] Specific Implementation Method Seven: This implementation method differs from Specific Implementation Methods One to Six in that the vacuum degassing treatment method described in steps one and two is as follows: a gradient vacuum treatment is adopted, firstly, the environment is kept at a vacuum level of 500 mbar and a temperature of 30°C for 5 to 15 minutes, then at a vacuum level of 100 mbar and a temperature of 30°C for 5 to 15 minutes, and finally at a vacuum level of 10 mbar and a temperature of 30°C for 5 to 15 minutes. The other steps are the same as in Specific Implementation Methods One to Six.
[0054] Specific Implementation Method Eight: The difference between this implementation method and Specific Implementation Methods One through Seven is that the drying method described in steps Three, Four, and Five is as follows:
[0055] ① In an environment with a relative humidity of 40%, keep warm at 70℃ for 4 hours, and then keep warm at 120℃ for 2 hours;
[0056] ② In an environment with a relative humidity of 30%, keep warm at 150℃ for 2 hours, and then keep warm at 200℃ for 2 hours;
[0057] ③ In an environment with a relative humidity of 20%, keep warm at 200℃ for 4 hours under a nitrogen atmosphere;
[0058] ④ Cool the film to room temperature in a nitrogen atmosphere, controlling the nitrogen flow along the coating direction. Other steps are the same as in specific embodiments one to seven.
[0059] Specific Implementation Method Nine: This implementation method uses a multilayer polyetherimide energy storage composite dielectric film as the dielectric material of a dielectric capacitor; the dielectric capacitor is used in high-voltage flexible DC transmission converter valves, new energy power generation filters, or new energy vehicle electric vehicle inverters.
[0060] Specific Implementation Method Ten: This implementation method describes a multilayer polyetherimide energy storage composite dielectric film for energy storage under high temperature and high field conditions. It achieves a discharge energy density of 6.14 J / cm² at a charge / discharge efficiency of 93.26% under conditions of 150℃ and 620 kV / mm. 3 .
[0061] The beneficial effects of the present invention are verified using the following embodiments:
[0062] Example 1: A multilayer polyetherimide energy storage composite dielectric film has two surface layers that trap electrons and an intermediate layer that scatters electrons. Its preparation method is specifically carried out according to the following steps:
[0063] 1. Under conditions of 60℃ and a stirring speed of 300 r / min, PolyK company product [model number missing] was used. 1000 polyetherimide and 4-N,N-dimethylaminophenylboronic acid were dissolved in N-methylpyrrolidone and then subjected to vacuum defoaming treatment to obtain a bubble-free 4-NB / PEI mixed solution.
[0064] In step one, the volume ratio of 4-N,N-dimethylaminophenylboronic acid to polyetherimide is 0.008:1;
[0065] In step one, the total mass ratio of polyetherimide and 4-N,N-dimethylaminophenylboronic acid to the volume ratio of N-methylpyrrolidone is 0.16 g: 1 mL.
[0066] 2. Under the conditions of 60℃ and a stirring speed of 300r / min, polyetherimide and tetrafluorotetracyanoquinoline dimethyl ether were dissolved in N-methylpyrrolidone, and then vacuum defoaming was performed to obtain a bubble-free F4TCNQ / PEI mixed solution.
[0067] In step two, the volume ratio of tetrafluorotetracyanoquinoline dimethyl ether to polyetherimide is 0.006:1;
[0068] In step two, the total mass ratio of polyetherimide and tetrafluorotetracyanoquinoline dimethyl ether to N-methylpyrrolidone is 0.16 g: 1 mL.
[0069] 3. Pour the bubble-free 4-NB / PEI mixed solution evenly onto a clean and flat glass plate. Raise the coating knife to a height of 4.5μm and scrape it horizontally at a speed of 5cm / s. Then dry it to form a dense lower surface composite film with a thickness of 3μm, which is the electron scattering layer.
[0070] 4. Pour the bubble-free F4TCNQ / PEI mixed solution evenly onto the lower surface composite film, raise the coating knife to a height of 10.5μm, and scrape horizontally at a speed of 5cm / s. Then dry the film to form a dense intermediate composite film with a thickness of 7μm, which is the electron-trapping layer.
[0071] 5. The bubble-free 4-NB / PEI mixed solution is uniformly poured onto the intermediate composite film. The coating blade is raised to a height of 4.5 μm and horizontally coated at a speed of 5 cm / s. After drying, a dense upper composite film with a thickness of 3 μm is formed, which is the electron scattering layer. A dense three-layer composite dielectric film with a thickness of 13 μm is constructed, which is the multilayer polyetherimide energy storage composite dielectric film (denoted as NFN-3).
[0072] The vacuum degassing treatment method described in Step 1 and Step 2 is as follows: Gradient vacuum treatment is adopted. First, the vacuum environment of 500 mbar and 30°C is set for 10 min, then the vacuum environment of 100 mbar and 30°C is set for 10 min, and finally the vacuum environment of 10 mbar and 30°C is set for 10 min.
[0073] The drying process described in steps three, four, and five is as follows:
[0074] ① In an environment with a relative humidity of 40%, keep warm at 70℃ for 4 hours, and then keep warm at 120℃ for 2 hours;
[0075] ② In an environment with a relative humidity of 30%, keep warm at 150℃ for 2 hours, and then keep warm at 200℃ for 2 hours;
[0076] ③ In an environment with a relative humidity of 20%, keep warm at 200℃ for 4 hours under a nitrogen atmosphere;
[0077] ④ Place the film in a nitrogen atmosphere and cool it to room temperature, while controlling the nitrogen gas flow along the coating direction.
[0078] Example 2: The difference between this example and Example 1 is as follows: In step three, a bubble-free 4-NB / PEI mixed solution is evenly poured onto a clean, flat glass plate. The coating blade is raised to a height of 6 μm and horizontally coated at a speed of 5 cm / s. After drying, a dense lower surface composite film with a thickness of 4 μm is formed, which is the electron-scattering layer. In step four, a bubble-free F4TCNQ / PEI mixed solution is evenly poured onto the lower surface composite film. The coating blade is raised to a height of 6.5 μm and horizontally coated at a speed of 5 cm / s. After drying... Dry processing is performed to form a dense intermediate composite film with a thickness of 5 μm, which is the electron-capturing layer. In step five, a bubble-free 4-NB / PEI mixed solution is uniformly poured onto the intermediate composite film. The coating blade is raised to a height of 6 μm and horizontally coated at a speed of 5 cm / s. After drying, a dense upper surface composite film with a thickness of 4 μm is formed, which is the electron-scattering layer. A dense three-layer composite dielectric film with a thickness of 13 μm is constructed, which is the multilayer polyetherimide energy storage composite dielectric film (denoted as NFN-4).
[0079] Example 3: The difference between this example and Example 1 is as follows: In step three, a bubble-free 4-NB / PEI mixed solution is evenly poured onto a clean, flat glass plate. The coating blade is raised to a height of 6.5 μm and horizontally coated at a speed of 5 cm / s. After drying, a dense lower surface composite film with a thickness of 5 μm is formed, which is the electron-scattering layer. In step four, a bubble-free F4TCNQ / PEI mixed solution is evenly poured onto the lower surface composite film. The coating blade is raised to a height of 4.5 μm and horizontally coated at a speed of 5 cm / s. After drying... Drying process is performed to form a dense intermediate composite film with a thickness of 3 μm, which is the electron-capturing layer. In step five, a bubble-free 4-NB / PEI mixed solution is uniformly poured onto the intermediate composite film. The coating blade is raised to a height of 6.5 μm and horizontally coated at a speed of 5 cm / s. After drying, a dense upper surface composite film with a thickness of 5 μm is formed, which is the electron-scattering layer. A dense three-layer composite dielectric film with a thickness of 13 μm is constructed, which is the multilayer polyetherimide energy storage composite dielectric film (denoted as NFN-5).
[0080] Example 4: A multilayer polyetherimide energy storage composite dielectric film has two surface layers that trap electrons and an intermediate layer that scatters electrons. Its preparation method is specifically carried out according to the following steps:
[0081] 1. Under conditions of 60℃ and a stirring speed of 300 r / min, PolyK company product [model number missing] was used. 1000 polyetherimide and 4-N,N-dimethylaminophenylboronic acid were completely dissolved in N-methylpyrrolidone, and then vacuum defoaming was performed to obtain a bubble-free 4-NB / PEI mixed solution.
[0082] In step one, the volume ratio of 4-N,N-dimethylaminophenylboronic acid to polyetherimide is 0.008:1;
[0083] In step one, the total mass ratio of polyetherimide and 4-N,N-dimethylaminophenylboronic acid to the volume ratio of N-methylpyrrolidone is 0.16 g: 1 mL.
[0084] 2. Under the conditions of 60℃ and a stirring speed of 300r / min, polyetherimide and tetrafluorotetracyanoquinoline dimethyl ether were completely dissolved in N-methylpyrrolidone, and then vacuum defoaming was performed to obtain a bubble-free F4TCNQ / PEI mixed solution.
[0085] In step two, the volume ratio of tetrafluorotetracyanoquinoline dimethyl ether to polyetherimide is 0.006:1;
[0086] In step two, the total mass ratio of polyetherimide and tetrafluorotetracyanoquinoline dimethyl ether to N-methylpyrrolidone is 0.16 g: 1 mL.
[0087] 3. Pour the bubble-free F4TCNQ / PEI mixed solution evenly onto a clean and flat glass plate. Raise the coating knife to a height of 4.5μm and scrape it horizontally at a speed of 5cm / s. Then dry it to form a dense lower surface composite film with a thickness of 3μm, which is the electron trapping layer.
[0088] 4. Pour the bubble-free 4-NB / PEI mixed solution evenly onto the lower surface composite film, raise the coating knife to a height of 10.5μm, and scrape horizontally at a speed of 5cm / s. Then dry the film to form a dense intermediate composite film with a thickness of 7μm, which is the electron scattering layer.
[0089] 5. The bubble-free F4TCNQ / PEI mixed solution is uniformly poured onto the intermediate composite film. The coating blade is raised to a height of 4.5μm and horizontally coated at a speed of 5cm / s. After drying, a dense upper composite film with a thickness of 3μm is formed, which is the electron-trapping layer. A dense three-layer composite dielectric film with a thickness of 13μm is constructed, which is the multilayer polyetherimide energy storage composite dielectric film (denoted as FNF-3).
[0090] The vacuum degassing treatment method described in Step 1 and Step 2 is as follows: Gradient vacuum treatment is adopted. First, the vacuum environment of 500 mbar and 30°C is set for 10 min, then the vacuum environment of 100 mbar and 30°C is set for 10 min, and finally the vacuum environment of 10 mbar and 30°C is set for 10 min.
[0091] The drying process described in steps three, four, and five is as follows:
[0092] ① In an environment with a relative humidity of 40%, keep warm at 70℃ for 4 hours, and then keep warm at 120℃ for 2 hours;
[0093] ② In an environment with a relative humidity of 30%, keep warm at 150℃ for 2 hours, and then keep warm at 200℃ for 2 hours;
[0094] ③ In an environment with a relative humidity of 20%, keep warm at 200℃ for 4 hours under a nitrogen atmosphere;
[0095] ④ Place the film in a nitrogen atmosphere and cool it to room temperature, while controlling the nitrogen gas flow along the coating direction.
[0096] Example 5: The difference between this example and Example 4 is as follows: In step three, the bubble-free F4TCNQ / PEI mixed solution is evenly poured onto a clean and flat glass plate. The coating blade is raised to a height of 6 μm and horizontally coated at a speed of 5 cm / s. After drying, a dense lower surface composite film with a thickness of 4 μm is formed, which is the electron-trapping layer. In step four, the bubble-free 4-NB / PEI mixed solution is evenly poured onto the lower surface composite film. The coating blade is raised to a height of 6.5 μm and horizontally coated at a speed of 5 cm / s. After drying... The process involves processing to form a dense intermediate composite film with a thickness of 5 μm, which is the electron scattering layer. In step five, a bubble-free F4TCNQ / PEI mixed solution is uniformly poured onto the intermediate composite film. The coating blade is raised to a height of 6 μm and horizontally coated at a speed of 5 cm / s. After drying, a dense upper surface composite film with a thickness of 4 μm is formed, which is the electron trapping layer. A dense three-layer composite dielectric film with a thickness of 13 μm is constructed, which is the multilayer polyetherimide energy storage composite dielectric film (denoted as FNF-4). Other steps and parameters are the same as in Example 4.
[0097] Example 6: The difference between this example and Example 4 is as follows: In step three, the bubble-free F4TCNQ / PEI mixed solution is evenly poured onto a clean and flat glass plate. The coating blade is raised to a height of 6.5 μm and horizontally coated at a speed of 5 cm / s. After drying, a dense lower surface composite film with a thickness of 5 μm is formed, which is the electron-trapping layer. In step four, the bubble-free 4-NB / PEI mixed solution is evenly poured onto the lower surface composite film. The coating blade is raised to a height of 4.5 μm and horizontally coated at a speed of 5 cm / s. After drying... The process involves processing to form a dense intermediate composite film with a thickness of 3 μm, which is the electron scattering layer. In step five, a bubble-free F4TCNQ / PEI mixed solution is uniformly poured onto the intermediate composite film. The coating blade is raised to a height of 6.5 μm and horizontally coated at a speed of 5 cm / s. After drying, a dense upper surface composite film with a thickness of 5 μm is formed, which is the electron trapping layer. A dense three-layer composite dielectric film with a thickness of 13 μm is constructed, which is the multilayer polyetherimide energy storage composite dielectric film (denoted as FNF-5). Other steps and parameters are the same as in Example 4.
[0098] Comparative Example 1: The preparation method of PEI dielectric thin film is carried out according to the following steps:
[0099] 1. Under conditions of 60℃ and a stirring speed of 300 r / min, PolyK's Ultem product... 1000 polyetherimide was completely dissolved in N-methylpyrrolidone, and then vacuum defoaming was performed to obtain a bubble-free PEI solution.
[0100] In step one, the mass ratio of polyetherimide to N-methylpyrrolidone is 0.16 g: 1 mL;
[0101] 2. Pour the bubble-free PEI solution evenly onto a clean and flat glass plate, raise the coating knife to a height of 19.5 μm, and scrape it horizontally at a speed of 5 cm / s. Then dry it to form a dense PEI dielectric film with a thickness of 13 μm (denoted as PEI).
[0102] The vacuum degassing treatment method described in step one is as follows: Gradient vacuum treatment is adopted. First, the vacuum environment of 500 mbar and 30°C is set for 10 min, then the vacuum environment of 100 mbar and 30°C is set for 10 min, and finally the vacuum environment of 10 mbar and 30°C is set for 10 min.
[0103] The drying process described in step two is as follows:
[0104] ① In an environment with a relative humidity of 40%, keep warm at 70℃ for 4 hours, and then keep warm at 120℃ for 2 hours;
[0105] ② In an environment with a relative humidity of 30%, keep warm at 150℃ for 2 hours, and then keep warm at 200℃ for 2 hours;
[0106] ③ In an environment with a relative humidity of 20%, keep warm at 200℃ for 4 hours under a nitrogen atmosphere;
[0107] ④ Place the film in a nitrogen atmosphere and cool it to room temperature, while controlling the nitrogen gas flow along the coating direction.
[0108] Comparative Example 2: The preparation method of F4TCNQ / PEI composite dielectric film is carried out according to the following steps:
[0109] 1. Under conditions of 60℃ and a stirring speed of 300 r / min, PolyK company product [model number missing] was used. 1000 polyetherimide and tetrafluorotetracyanoquinoline dimethyl ether were completely dissolved in N-methylpyrrolidone, and then vacuum defoaming was performed to obtain a bubble-free F4TCNQ / PEI mixed solution.
[0110] In step one, the volume ratio of tetrafluorotetracyanoquinoline dimethyl ether to polyetherimide is 0.006:1;
[0111] In step one, the total mass ratio of polyetherimide and tetrafluorotetracyanoquinoline dimethyl ether to N-methylpyrrolidone is 0.16 g: 1 mL.
[0112] 2. Pour the bubble-free F4TCNQ / PEI mixed solution evenly onto a clean, flat glass plate. Raise the coating blade to a height of 19.5 μm and scrape it horizontally at a speed of 5 cm / s. Then dry the plate to form a dense F4TCNQ / PEI composite dielectric film with a thickness of 13 μm (denoted as F). 0.6 );
[0113] The vacuum degassing treatment method described in step one is as follows: Gradient vacuum treatment is adopted. First, the vacuum environment of 500 mbar and 30°C is set for 10 min, then the vacuum environment of 100 mbar and 30°C is set for 10 min, and finally the vacuum environment of 10 mbar and 30°C is set for 10 min.
[0114] The drying process described in step two is as follows:
[0115] ① In an environment with a relative humidity of 40%, keep warm at 70℃ for 4 hours, and then keep warm at 120℃ for 2 hours;
[0116] ② In an environment with a relative humidity of 30%, keep warm at 150℃ for 2 hours, and then keep warm at 200℃ for 2 hours;
[0117] ③ In an environment with a relative humidity of 20%, keep warm at 200℃ for 4 hours under a nitrogen atmosphere;
[0118] ④ Place the film in a nitrogen atmosphere and cool it to room temperature, while controlling the nitrogen gas flow along the coating direction.
[0119] Comparative Example 3: The preparation method of the 4-NB / PEI composite dielectric film is carried out according to the following steps:
[0120] 1. Under conditions of 60℃ and a stirring speed of 300 r / min, PolyK company product [model number missing] was used. 1000 polyetherimide and 4-N,N-dimethylaminophenylboronic acid were completely dissolved in N-methylpyrrolidone, and then vacuum defoaming was performed to obtain a bubble-free 4-NB / PEI mixed solution.
[0121] In step one, the volume ratio of 4-N,N-dimethylaminophenylboronic acid to polyetherimide is 0.008:1;
[0122] In step one, the total mass ratio of polyetherimide and 4-N,N-dimethylaminophenylboronic acid to the volume ratio of N-methylpyrrolidone is 0.16 g: 1 mL.
[0123] 2. Pour the bubble-free 4-NB / PEI mixed solution evenly onto a clean, flat glass plate. Raise the coating blade to a height of 19.5 μm and scrape it horizontally at a speed of 5 cm / s. Then dry the plate to form a dense 4-NB / PEI composite dielectric film with a thickness of 13 μm (denoted as N). 0.8 );
[0124] The vacuum degassing treatment method described in step one is as follows: Gradient vacuum treatment is adopted. First, the vacuum environment of 500 mbar and 30°C is set for 10 min, then the vacuum environment of 100 mbar and 30°C is set for 10 min, and finally the vacuum environment of 10 mbar and 30°C is set for 10 min.
[0125] The drying process described in step two is as follows:
[0126] ① In an environment with a relative humidity of 40%, keep warm at 70℃ for 4 hours, and then keep warm at 120℃ for 2 hours;
[0127] ② In an environment with a relative humidity of 30%, keep warm at 150℃ for 2 hours, and then keep warm at 200℃ for 2 hours;
[0128] ③ In an environment with a relative humidity of 20%, keep warm at 200℃ for 4 hours under a nitrogen atmosphere;
[0129] ④ Place the film in a nitrogen atmosphere and cool it to room temperature, while controlling the nitrogen gas flow along the coating direction.
[0130] The composite media obtained in Examples 1-6 and Comparative Examples 1-3 were characterized in terms of structure and performance, and the results are as follows:
[0131] Figure 1 (a) is the surface electrostatic potential cloud diagram and potential statistics diagram of 4-N,N-dimethylaminophenylboronic acid; (b) is the surface electrostatic potential cloud diagram and potential statistics diagram of tetrafluorotetracyanoquinoline dimethane.
[0132] Depend on Figure 1 It can be seen that the electrostatic potential near the tetrafluorophenyl and cyanide groups in F4TCNQ is positive, indicating a strong electron affinity at these positions. In contrast, the electrostatic potential near the boric acid and benzene rings in 4-NB is negative, exhibiting significant electron scattering characteristics. The surface potential distribution areas of the two fillers also differ considerably. F4TCNQ has a high proportion of positive electrostatic potential area, reaching 63.78%, and a high proportion of 32.72% in the strong positive potential range (20-45 kcal / mol), indicating that the filler as a whole exhibits electron-capturing characteristics. 4-NB has a high proportion of electrostatic potential area in the -30-0 kcal / mol range, reaching 60%, and the potential values in the regions with a high proportion of positive electrostatic potential are relatively low; therefore, the filler as a whole exhibits electron scattering characteristics.
[0133] Figure 2 (a) shows the cross-sectional morphology and elemental distribution of the FNF-3 film, (b) shows the cross-sectional morphology and elemental distribution of the FNF-4 film, (c) shows the cross-sectional morphology and elemental distribution of the FNF-5 film, (d) shows the cross-sectional morphology and elemental distribution of the NFN-3 film, (e) shows the cross-sectional morphology and elemental distribution of the NFN-4 film, and (f) shows the cross-sectional morphology and elemental distribution of the NFN-5 film.
[0134] Depend on Figure 2It can be seen that the cross-section of the multilayer composite medium is smooth and free of impurities, with an overall thickness maintained at 13 μm. Furthermore, the thickness of the functional layer conforms to the design thickness of the experimental scheme with minimal error, indicating that the coating process can achieve the construction of a multilayer modified structure. The cross-sectional image of the composite medium shows that the interface is clearer when the surface layer thickness is small, but decreases with increasing surface layer thickness. This may be due to uneven expansion and contraction of different thickness layers during drying, leading to a more obvious interface. Alternatively, it may be due to uneven stress distribution during the brittle fracture test before the SEM experiment, resulting in cracks in the interface region and a more obvious interface. Energy dispersive spectroscopy (EDS) was used to characterize the elemental composition distribution of the multilayer structure. B element was used to characterize the distribution of 4-NB, and F element was used to characterize the distribution of F4TCNQ. Taking NFN-4 as an example, a large amount of B element is distributed in the surface layer, and a large amount of F element is distributed in the middle layer, proving that the constructed multilayer structure is an NFN structure, and the filler distribution conforms to the design scheme. A small amount of B element is distributed in the intermediate layer and a small amount of F element is distributed in the surface layer. This may be due to the migration of a small amount of filler or it may be due to the test error caused by stray signals from the test instrument.
[0135] Figure 3 (a) shows the XRD patterns of the composite media obtained in different embodiments, and (b) shows the XRD patterns of 4-N,N-dimethylaminophenylboronic acid and tetrafluorotetracyanoquinoline dimethane and the comparative examples.
[0136] Depend on Figure 3 It can be seen that no sharp and high-intensity characteristic peaks appeared in the composite medium, proving that the prepared multilayer composite medium has high purity and no impurities introduced. Compared with pure PEI, the peak of the multilayer composite medium in the 10°-30° range showed a leftward shift, mainly due to the reduction of PEI molecular chain stacking caused by the introduction of 4-NB. The spectrum also shows that the leftward shift of the peak increases with the increase of the 4-NB layer thickness, which is due to the increase of 4-NB content in the medium.
[0137] Figure 4 (a) shows the infrared spectra of the composite media obtained in different embodiments, and (b) shows the infrared spectra of 4-N,N-dimethylaminophenylboronic acid and tetrafluorotetracyanoquinoline dimethane and the comparative examples.
[0138] Depend on Figure 4 It can be seen that at 1776cm -1 and 1712cm -1 The characteristic peak at 1367 cm⁻¹ is due to the C=O stretching vibration of imide. -1 and 725cm -1 The characteristic peak at 1240 cm⁻¹ is due to the CN stretching vibration of the imide ring. -1 and 1100cm-1 The characteristic peak at 1450 cm⁻¹ is due to the stretching vibration of COC. The composite medium did not show characteristic peak information for F4TCNQ in FTIR, but because 4-NB has a characteristic peak at 1450 cm⁻¹... -1 There are broad peaks on both sides caused by the variable-angle vibration of N(CH3)2, so the composite structure has a peak length of 1250-1500 cm⁻¹. -1 The sharpness of the characteristic peaks decreased, which may be due to the degeneracy behavior that occurs during testing caused by the introduction of 4-NB.
[0139] Figure 5 (a) shows the dielectric constant and dielectric loss of the composite media obtained in different embodiments as a function of frequency at 150°C; (b) shows the dielectric constant and dielectric loss of the comparative example as a function of frequency at 150°C.
[0140] Depend on Figure 5 It can be seen that the relative permittivity of multilayer composite dielectrics is relatively stable over a wide frequency range, with small fluctuations, and the loss factor remains at a low level. Among the NFN composite multilayer structures, NFN-3 has the highest relative permittivity, followed by NFN-4, and NFN-5 has the lowest. This is because F4TCNQ has strong polarization capability; as the thickness of the F4TCNQ / PEI composite dielectric layer increases, the proportion of F4TCNQ in the composite dielectric increases, thus the dielectric constant shows an upward trend. The same pattern is observed for FNF composite dielectrics, with FNF-5 having the highest relative permittivity, followed by NFN-4, and NFN-3 having the lowest.
[0141] Figure 6 (a) is a Weibull distribution diagram of the breakdown field strength of the composite medium obtained in different embodiments at 150°C, and (b) is a Weibull distribution diagram of the breakdown field strength of the comparative example at 150°C.
[0142] Depend on Figure 6It can be seen that in the NFN structure, NFN-4 has the highest characteristic breakdown field strength, reaching 671.4 kV / mm, NFN-5 is 663.8 kV / mm, and NFN-3 is the lowest at 661.3 kV / mm. With the increase of the 4-NB / PEI surface layer thickness, the breakdown field strength of the composite dielectric shows a pattern of first increasing and then decreasing. For the FNF structure, with the increase of the 4-NB / PEI surface layer thickness, the breakdown field strength of the composite dielectric gradually increases, reaching 665.2 kV / mm for the FNF-5 structure. The breakdown field strength of the NFN and FNF structure composite dielectrics exhibits drastically different patterns with surface layer thickness. For the NFN structure composite dielectric, when the surface layer thickness is small, the repulsive electron injection capability is weak, and a large number of electrons are injected into the composite dielectric. However, when the surface layer thickness is large, the ability of the intermediate layer to capture high-energy electrons is weak, and high-energy electrons that the repulsive electron layer fails to scatter will accelerate their transport within the dielectric, causing a decrease in the breakdown performance of the insulating dielectric. For the FNF structure composite dielectric, the surface layer is an F4TCNQ / PEI composite dielectric with electron-trapping properties, while the middle layer is a 4-NB / PEI composite dielectric with electron-scattering properties. As the thickness of the F4TCNQ / PEI surface layer gradually increases, the improvement in the breakdown field strength of the composite dielectric is mainly attributed to the increase in traps, thus enhancing the ability to trap electrons and suppress electron transport. Overall, the improved breakdown performance of the NFN structure is a combination of the surface barrier advantage and the bulk trap advantage of the composite dielectric. The surface layer has a significant advantage in suppressing electron injection, while the middle layer has a significant advantage in suppressing high-energy electron transport.
[0143] Figure 7 (a) is a graph showing the change of electrical conductivity current with electric field strength at 150°C for composite media obtained in different embodiments; (b) is a graph showing the change of electrical conductivity current with electric field strength at 150°C for comparative examples.
[0144] As shown in the figure, NFN-4 has the lowest conductivity current, followed by FNF-5. FNF-3 and FNF-4 have relatively high conductivity currents, but the differences are not significant. However, compared with the comparative example, the conductivity current values are lower, indicating that the multilayer composite dielectric has lower conductivity loss and can reduce the generation of a large amount of heat.
[0145] Figure 8 (a) is a graph showing the energy storage characteristics of the composite medium obtained in different embodiments at 150°C, and (b) is a graph showing the energy storage characteristics of the comparative example at 150°C.
[0146] As shown in the figure, for the NFN structure, with the increase of the thickness of the scattered electron surface layer, the maximum energy density with an efficiency ≥90% first increases and then decreases, and the variation trend is consistent with the DC breakdown performance. NFN-4 has a strong ability to inject repulsive electrons from the surface layer and to trap high-energy electrons in the intermediate layer, thus significantly improving its performance. The energy density of NFN-4 is 6.14 J / cm³.3 The corresponding polarization electric field is 620 kV / mm, and the energy storage density is 283.7% higher than that of pure PEI, and higher than that of F. 0.6 An increase of 26.3%, relative to N 0.8 The energy storage performance is improved by 17.9%. In the FNF structure, the thicker the surface layer with electron-attracting properties, the better the energy storage performance. This is because the increased number of traps enhances the ability to capture electrons, increases the dielectric strength of the medium, and reduces energy loss, thus increasing the energy storage density. However, the energy storage performance of FNF-5 can only reach 6.02 J / cm³. 3 It is 282% higher than pure PEI and higher than F. 0.6 An increase of 23.9%, relative to N 0.8 The performance was improved by 15.5%. Although there was an improvement, it is still not as good as NFN-4. In addition, the FNF structure did not show a significant effect in reducing trap introduction.
[0147] Figure 9 (a) Schematic diagram of the interface charge of a thin film with a 3 μm thick electron-scattering layer as the surface layer and an electron-capturing layer as the middle layer; (b) Schematic diagram of the interface charge of a thin film with a 4 μm thick electron-scattering layer as the surface layer and an electron-capturing layer as the middle layer; (c) Schematic diagram of the interface charge of a thin film with a 5 μm thick electron-scattering layer as the surface layer and an electron-capturing layer as the middle layer; (d) Schematic diagram of the interface charge of a thin film with a 5 μm thick electron-capturing layer as the surface layer and an electron-scattering layer as the middle layer.
[0148] As shown in the figure, in the NFN structure, charges of the opposite type to those on the electrode plates can form at the interface. The built-in electric field between the interface charges is opposite in direction to the applied electric field, which can hinder the transport of charge carriers within the composite dielectric. However, as the surface layer thickness increases, the interface charge decreases, and the magnitude of the built-in electric field changes. The intensity of the built-in electric field decreases with increasing surface layer thickness, and due to the smaller thickness of the intermediate layer, the probability of recombination of charges of different polarities increases, weakening the suppression of electron transport, thus leading to a performance degradation trend. For the FNF structure composite dielectric, the polarity and charge quantity of the interface charge change with surface layer thickness in the same way as the NPN structure, but the performance evolution is completely opposite. This is because although the interface charge decreases, with increasing thickness, more traps are introduced, and the trap trapping effect becomes the dominant factor. Therefore, with increasing surface layer thickness, the breakdown field strength of the composite dielectric shows an upward trend.
[0149] Figure 10 (a) is the AC box model diagram of 4-N,N-dimethylaminophenylboronic acid and tetrafluorotetracyanoquinoline dimethane; (b) is the interaction energy data diagram of 4-N,N-dimethylaminophenylboronic acid and tetrafluorotetracyanoquinoline dimethane.
[0150] Depend on Figure 10It is known that the interaction energy between F4TCNQ molecules is 4062.71 Ha, the interaction energy between 4-NB molecules is 611.87 Ha, and the interaction energy of the entire box is 4637.65 Ha. Therefore, the interlayer interaction energy is -0.06 Ha, or -36.93 kcal / mol. The negative interlayer interaction energy indicates a strong attraction between the 4-NB and F4TCNQ layers, which may be caused by van der Waals forces, hydrogen bonds, or covalent bonds. Strong interactions can increase the stability of multilayer structures, making the interlayer bonding tighter and reducing interlayer physical defects. Furthermore, strong interlayer interactions can also strongly bind electrons, hindering electron transport and reducing electrical conduction losses.
[0151] In summary, the multilayer polyetherimide energy storage composite medium prepared by this invention has low conductivity loss, good high-temperature breakdown strength, and good energy storage performance.
[0152] Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Anyone skilled in the art can make various modifications and alterations without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be determined by the claims.
Claims
1. A multilayer polyetherimide energy storage composite dielectric film, characterized in that... The multilayer polyetherimide energy storage composite dielectric film has a three-layer structure, consisting of an electron-scattering layer and an electron-trapping layer. One structure has two surface layers as electron-scattering layers and a middle layer as an electron-trapping layer; another structure has two surface layers as electron-trapping layers and a middle layer as an electron-scattering layer. The electron-scattering layer is composed of polyetherimide and 4-N,N-dimethylaminophenylboronic acid; the electron-trapping layer is composed of polyetherimide and tetrafluorotetracyanoquinoline dimethane. The volume ratio of 4-N,N-dimethylaminophenylboronic acid to polyetherimide in the electron scattering layer is 0.008:1; the volume ratio of tetrafluorotetracyanoquinoline dimethyl etherimide in the electron trapping layer is 0.006:
1. The thickness of the multilayer polyetherimide energy storage composite medium film is 5μm~13μm; the ratio of the thickness of a single surface layer to the total thickness of the multilayer polyetherimide energy storage composite medium film is (3~5):
13.
2. The multilayer polyetherimide energy storage composite dielectric film according to claim 1, characterized in that... The multilayer polyetherimide energy storage composite dielectric film has two surface layers that scatter electrons and an intermediate layer that traps electrons. Its preparation method is specifically carried out according to the following steps:
1. Polyetherimide and 4-N,N-dimethylaminophenylboronic acid are dissolved in N-methylpyrrolidone, and then vacuum defoaming is performed to obtain a bubble-free 4-NB / PEI mixed solution.
2. Polyetherimide and tetrafluorotetracyanoquinoline dimethyl ether are dissolved in N-methylpyrrolidone and then subjected to vacuum defoaming treatment to obtain a bubble-free F4TCNQ / PEI mixed solution.
3. Apply the bubble-free 4-NB / PEI mixed solution to the substrate by scraping, and then dry it to form the lower surface composite film, which is the electron scattering layer.
4. Apply the bubble-free F4TCNQ / PEI mixed solution to the lower surface composite film by scraping, and then dry it to form the middle layer composite film, which is the electron-capturing layer.
5. The bubble-free 4-NB / PEI mixed solution is coated onto the intermediate composite film and then dried to form the upper composite film, which is the electron scattering layer; thus, a three-layer composite dielectric film is constructed, which is the multilayer polyetherimide energy storage composite dielectric film.
3. The multilayer polyetherimide energy storage composite dielectric film according to claim 1, characterized in that... The multilayer polyetherimide energy storage composite dielectric film has two surface layers that trap electrons and an intermediate layer that scatters electrons. Its preparation method is specifically carried out according to the following steps:
1. Polyetherimide and 4-N,N-dimethylaminophenylboronic acid are dissolved in N-methylpyrrolidone, and then vacuum defoaming is performed to obtain a bubble-free 4-NB / PEI mixed solution.
2. Polyetherimide and tetrafluorotetracyanoquinoline dimethyl ether are dissolved in N-methylpyrrolidone and then subjected to vacuum defoaming treatment to obtain a bubble-free F4TCNQ / PEI mixed solution.
3. Apply the bubble-free F4TCNQ / PEI mixed solution to the substrate by scraping, and then dry it to form the lower surface composite film, which is the electron-capturing layer.
4. Apply the bubble-free 4-NB / PEI mixed solution to the lower surface composite film by scraping, and then dry it to form the intermediate composite film, which is the electron scattering layer.
5. The bubble-free F4TCNQ / PEI mixed solution is coated onto the intermediate composite film and then dried to form the upper composite film, which is the electron-capturing layer; thus, a three-layer composite dielectric film is constructed, which is a multilayer polyetherimide energy storage composite dielectric film.
4. A multilayer polyetherimide energy storage composite dielectric film according to claim 2 or 3, characterized in that... In step one, the volume ratio of 4-N,N-dimethylaminophenylboronic acid to polyetherimide is 0.008:1; the total mass of polyetherimide and 4-N,N-dimethylaminophenylboronic acid in step one is (0.15g~0.18g):1mL to N-methylpyrrolidone. In step two, the volume ratio of tetrafluorotetracyanoquinoline dimethyl ether to polyetherimide is 0.006:1; the total mass of polyetherimide and tetrafluorotetracyanoquinoline dimethyl ether to N-methylpyrrolidone in step two is (0.15g~0.18g):1mL.
5. A multilayer polyetherimide energy storage composite dielectric film according to claim 2 or 3, characterized in that... The vacuum degassing treatment method described in steps one and two is as follows: Gradient vacuum treatment is adopted. First, the vacuum environment is set at 500 mbar and 30°C for 5 min to 15 min, then at 100 mbar and 30°C for 5 min to 15 min, and finally at 10 mbar and 30°C for 5 min to 15 min.
6. A multilayer polyetherimide energy storage composite dielectric film according to claim 2 or 3, characterized in that... The drying process described in steps three, four, and five is as follows: ① In an environment with a relative humidity of 40%, keep warm at 70℃ for 4 hours, and then keep warm at 120℃ for 2 hours; ② In an environment with a relative humidity of 30%, keep warm at 150℃ for 2 hours, and then keep warm at 200℃ for 2 hours; ③ In an environment with a relative humidity of 20%, keep warm at 200℃ for 4 hours under a nitrogen atmosphere; ④ Place the film in a nitrogen atmosphere and cool it to room temperature, while controlling the nitrogen gas flow along the coating direction.
7. The application of the multilayer polyetherimide energy storage composite dielectric film as described in claim 1, characterized in that... A multilayer polyetherimide energy storage composite dielectric film is used as the dielectric material of a dielectric capacitor; the dielectric capacitor is used in high-voltage flexible DC transmission converter valves, new energy power generation filters, or new energy vehicle inverters.
8. The application of the multilayer polyetherimide energy storage composite dielectric film as described in claim 1, characterized in that... A multilayer polyetherimide energy storage composite dielectric film is used in energy storage devices under high temperature and high field conditions. It achieves a discharge energy density of 6.14 J / cm² at a charge / discharge efficiency of 93.26% under conditions of 150℃ and 620 kV / mm. 3 .
Citation Information
Patent Citations
PEI cast film with high energy storage density and high smoothness and preparation method thereof
CN116262855A
Polyetherimide-based energy storage composite dielectric film and preparation method and application thereof