A Josephson knot and its preparation method
By using SOI masks and high-temperature oxidation processes to fabricate Josephson junctions, the problems of photoresist residue and softening were solved, enabling efficient fabrication of single-crystal alumina barrier layers and improving the low-temperature performance of Josephson junctions.
Patent Information
- Application Number
- CN202311142948.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-06
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-09-06
AI Technical Summary
Existing technologies for fabricating Josephson junctions suffer from performance degradation due to photoresist residue and softening or degradation at high temperatures, and cannot fabricate single-crystal alumina barrier layers, affecting the selection of superconductor deposition processes.
SOI mask is used instead of photoresist. First and second superconducting layers are formed on the substrate through SOI mask, and single crystal alumina barrier layer is formed by oxidation at high temperature to avoid photoresist residue and high temperature softening risk. Josephson junction is formed by oblique evaporation deposition process.
It enables the fabrication of Josephson junctions without photoresist residue, expands the selection of superconductor deposition methods, and improves the low-temperature performance of Josephson junctions, especially by reducing low-temperature losses using a single-crystal alumina barrier layer.
Smart Images

Figure CN119584845B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of quantum chip technology, and in particular to a Josephson junction and its fabrication method. Background Technology
[0002] Josephson junctions, as key components in superconducting quantum circuits, are typically constructed by sandwiching a very thin barrier layer (thickness ≤ the coherence length of a Cooper pair) between two superconductors, such as an S (superconductor)-I (semiconductor or insulator)-S (superconductor) structure, abbreviated as SIS. Superconducting electrons in a Josephson junction can tunnel from one side through the semiconductor or insulator film to the other. Current techniques for fabricating Josephson junctions often use photoresist, for example, by coating a substrate with photoresist, exposing and developing it to form a patterned window, and then fabricating the Josephson junction on the exposed area of this patterned window on the substrate. However, residual photoresist can adversely affect the performance of the Josephson junction, and there is a risk of softening or degradation of the photoresist during heated superconductor deposition processes. Summary of the Invention
[0003] The purpose of this application is to provide a Josephson junction and its fabrication method, so as to avoid the adverse effects of photoresist residue on the performance of the Josephson junction and the risk of photoresist softening or degradation during superconductor deposition processes that require heating. The specific technical solution is as follows:
[0004] The first aspect of this application provides a method for preparing a Josephson knot, characterized in that it includes:
[0005] An SOI mask and a substrate are provided, wherein the SOI mask has a first etching window and a second etching window extending through the SOI mask, and the first etching window and the second etching window have at least one intersecting region;
[0006] The SOI mask is fixed onto the substrate;
[0007] A first superconducting layer is formed on the substrate exposed by the first etched window;
[0008] An alumina barrier layer is formed on the first superconducting layer;
[0009] A second superconducting layer is formed on the substrate exposed by the second etch window to obtain a Josephson junction in the intersection region.
[0010] In some embodiments of this application, providing the SOI mask includes:
[0011] An SOI wafer is provided, the SOI wafer comprising a first silicon layer, a silicon dioxide layer and a second silicon layer stacked sequentially;
[0012] The first silicon layer is patterned and etched to form the first etching window and the second etching window;
[0013] The second silicon layer and the silicon dioxide layer are patterned and etched to form a cavity that exposes the first etching window and the second etching window, thereby obtaining the SOI mask.
[0014] In some embodiments of this application, the alumina barrier layer is a single-crystal alumina barrier layer.
[0015] In some embodiments of this application, the material of the first superconducting layer is selected from aluminum, and the formation of an alumina barrier layer on the first superconducting layer includes: placing the substrate in a sealed environment, heating the sealed environment to a high temperature, and introducing oxygen at the high temperature to oxidize the surface of the first superconducting layer to form a single-crystal alumina barrier layer.
[0016] In some embodiments of this application, the material of the first superconducting layer is selected from any superconducting metal other than aluminum, and the formation of an alumina barrier layer on the first superconducting layer includes: after depositing an aluminum layer on the first superconducting layer, placing the substrate in a sealed environment, heating the sealed environment to a high temperature, and introducing oxygen at the high temperature to oxidize the aluminum layer to form a single-crystal alumina barrier layer.
[0017] In some embodiments of this application, the enclosed environment is heated to 280°C to 500°C.
[0018] In some embodiments of this application, the material of the first superconducting layer is selected from any superconducting metal other than aluminum, and the formation of an alumina barrier layer on the first superconducting layer includes: after depositing an aluminum layer on the first superconducting layer, placing the substrate in a sealed environment, oxidizing the deposited aluminum layer at room temperature in the sealed environment to form an amorphous alumina barrier layer, and converting the amorphous alumina barrier layer into a monocrystalline alumina barrier layer by high-temperature annealing.
[0019] In some embodiments of this application, the high-temperature annealing treatment is performed at a temperature of 800°C to 2000°C.
[0020] In some embodiments of this application, the material of the first superconducting layer is selected from any superconducting metal other than aluminum, and the formation of an alumina barrier layer on the first superconducting layer includes: heating the substrate to a high temperature, depositing aluminum on the first superconducting layer at the high temperature while simultaneously introducing oxygen to form a single-crystal alumina barrier layer.
[0021] In some embodiments of this application, the substrate is heated to 700°C to 800°C, and the aluminum deposition rate is... to
[0022] In some embodiments of this application, the first etching window and the second etching window are perpendicular to each other, and the first superconducting layer and the second superconducting layer are formed by an oblique evaporation deposition process, with the evaporation directions being perpendicular to each other.
[0023] In some embodiments of this application, the preparation method further includes: separating the SOI mask and the substrate.
[0024] A second aspect of this application provides a Josephson knot obtained according to any of the foregoing methods.
[0025] The beneficial effects of this application are:
[0026] This application provides a Josephson junction and its fabrication method. This method utilizes an SOI mask instead of photoresist, avoiding the adverse effects of photoresist residue on the Josephson junction's performance. Since photoresist is not heat-resistant, this method also avoids the risk of photoresist softening or degrading at high temperatures during heat-requiring superconductor deposition processes, expanding the range of superconductor deposition methods that can be used, such as magnetron sputtering and chemical vapor deposition.
[0027] Of course, implementing any product or method of this application does not necessarily require achieving all of the advantages described above at the same time. Attached Figure Description
[0028] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other embodiments can be obtained based on these drawings.
[0029] Figure 1 A schematic flowchart illustrating the method for preparing the Josephson junction provided in this application;
[0030] Figure 2 Schematic diagrams of the structure of the SOI mask provided in this application before and after patterning;
[0031] Figure 3 This is a schematic diagram of the process steps of one embodiment of this application;
[0032] Figure 4 This is a schematic diagram of the process steps for another embodiment of this application;
[0033] Figure 5 This is a schematic diagram of the process steps for another embodiment of this application;
[0034] Reference numerals: 100: SOI mask; 110: First silicon layer; 111: First etching window; 112: Second etching window; 120: Silicon dioxide layer; 130: Second silicon layer; 20: Substrate; 30: First superconducting layer; 40: Alumina barrier layer; 50: Second superconducting layer. Detailed Implementation
[0035] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. All other embodiments obtained by those skilled in the art based on this application are within the scope of protection of this application.
[0036] In the description of this application, it should be understood that the terms "center", "upper", "lower", "left", "right", etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this application.
[0037] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of that feature. In the description of this application, "multiple" means at least two, such as two, three, etc., unless otherwise explicitly specified.
[0038] Current technologies typically use photoresist in the fabrication of Josephson junctions. The use of photoresist generally presents the following problems: First, photoresist residue is prone to form in the area where the Josephson junction contacts the substrate. Even though photoresist can be dissolved through a washing process, it cannot be completely removed. Residual photoresist can adversely affect the performance of the Josephson junction. Second, photoresist is not heat-resistant and risks softening or degradation at high temperatures, making it unsuitable for thin-film deposition methods requiring heating, such as magnetron sputtering and chemical vapor deposition, when depositing superconducting layers.
[0039] Furthermore, existing techniques for fabricating alumina barrier layers involve room-temperature oxidation of Al(111) to obtain amorphous alumina barrier layers. Monocrystalline alumina barrier layers have fewer defects and lower losses compared to amorphous alumina barrier layers, resulting in better low-temperature performance for Josephson junctions with monocrystalline alumina barrier layers. However, fabricating monocrystalline alumina barrier layers or converting amorphous alumina barrier layers to monocrystalline alumina barrier layers requires high temperatures, exceeding the operating temperature of photoresist, which would soften or degrade the photoresist. Therefore, photoresist-based fabrication methods cannot yield Josephson junctions with monocrystalline alumina barrier layers.
[0040] SOI (Silicon-on-Insulator) technology introduces a buried oxide layer between the top silicon layer and the back substrate. This application uses an SOI mask instead of photoresist to fabricate Josephson junctions, avoiding the adverse effects of photoresist residue on the junction's performance and the risk of photoresist softening or degradation during heated superconductor deposition processes. Furthermore, the fabrication method of this application yields a single-crystal alumina barrier layer, reducing losses at low temperatures and resulting in better low-temperature performance of the fabricated Josephson junction.
[0041] refer to Figure 1 The first aspect of this application provides a method for preparing a Josephson junction, characterized by comprising:
[0042] S1: Provide an SOI mask 100 and a substrate 20. The SOI mask 100 has a first etching window 111 and a second etching window 112 that penetrate the SOI mask 100. The first etching window 111 and the second etching window 112 have at least one intersecting region.
[0043] S2: Fix the SOI mask 100 onto the substrate 20;
[0044] S3: A first superconducting layer 30 is formed on the substrate 20 exposed by the first etching window 111;
[0045] S4: An alumina barrier layer 40 is formed on the first superconducting layer 30;
[0046] S5: A second superconducting layer 50 is formed on the substrate 20 exposed by the second etching window 112 to obtain a Josephson junction in the intersection region.
[0047] refer to Figure 2 In some embodiments of this application, providing the SOI mask 100 in step S1 includes:
[0048] An SOI wafer is provided, comprising a first silicon layer 110, a silicon dioxide layer 120, and a second silicon layer 130 stacked sequentially (reference). Figure 2 (a));
[0049] The first silicon layer 110 is patterned and etched to form a first etching window 111 and a second etching window 112;
[0050] Patterned etching of the second silicon layer 130 and silicon dioxide layer 120 forms a cavity exposing the first etching window 111 and the second etching window 112, resulting in an SOI mask 100 (reference). Figure 2 (b)).
[0051] For example, the SOI mask 100 can be specifically fabricated using the following method: An SOI wafer is provided; photoresist is uniformly applied to the surface of the first silicon layer 110 of the SOI wafer to expose a first etching window 111 and a second etching window 112; the first silicon layer 110 is etched down to the silicon dioxide layer 120; the photoresist is removed by stripping to obtain the first etching window 111 and the second etching window 112; 2 μm of SiO2 and 9 μm of Si3N are deposited on the surface of the second silicon layer 130 of the SOI wafer. 4; Photoresist is uniformly applied to the surface of the second silicon layer 130 of the SOI wafer to expose the back cavity pattern; 2μm SiO2 and 9μm Si3N4 are etched to transfer the back cavity pattern to the SiO2 and Si3N4 layers; deep silicon etching is performed on the second silicon layer 130 to the silicon dioxide layer 120; the photoresist is removed by stripping, and the SiO2, Si3N4 and silicon dioxide layers 120 are wet-removed to form a cavity exposing the first etching window 111 and the second etching window 112, thus obtaining the SOI mask 100.
[0052] This application does not impose any particular limitation on the thickness of the first silicon layer 110, the silicon dioxide layer 120, and the second silicon layer 130 in the SOI wafer, as long as the purpose of this application can be achieved. For example, the thickness of the first silicon layer 110 can be 0.1 to 100 μm, the thickness of the silicon dioxide layer 120 can be 0.4 to 4 μm, and the thickness of the second silicon layer 130 can be 300 to 725 μm.
[0053] In some embodiments of this application, the first etching window 111 and the second etching window 112 in the SOI mask 100 provided in step S1 have at least one intersecting region. For example, the number of intersecting regions can be one, two, or three. Specifically, there can be one or more first etching windows 111 and one or more second etching windows 112. At least one Josephson junction, such as a single-junction Josephson junction or a double-junction Josephson junction, can be obtained in a single fabrication process. This application does not impose any particular limitation on the shape of the intersecting region, as long as it achieves the purpose of this application. For example, the first etching window 111 and the second etching window 112 can be elongated, with equal widths and perpendicular intersection, making the shape of the intersecting region square.
[0054] In some embodiments of this application, in step S2, the surface of the first silicon layer 110 of the SOI mask 100 is bonded to the substrate 20. This application does not impose any particular limitation on the method by which the SOI mask 100 is fixed to the substrate 20 in step S2, as long as the purpose of this application is achieved. For example, the following method can be adopted: placing the SOI mask 100 and the substrate 20 in two clamps; observing under a microscope to align the surface of the first silicon layer 110 of the SOI mask 100 with the substrate 20; and fixing the clamps with screws to further secure the SOI mask 100 and the substrate 20.
[0055] This application does not impose any particular restriction on the type of substrate 20, as long as it achieves the purpose of this application. The substrate 20 typically includes a substrate, and this application does not impose any particular restriction on the type of substrate, as long as it achieves the purpose of this application. For example, the substrate can be selected from any of a silicon substrate, a sapphire substrate, and a silicon carbide substrate.
[0056] In some embodiments of this application, the material of the first superconducting layer 30 in step S3 is selected from aluminum. In other embodiments of this application, the material of the first superconducting layer 30 in step S3 is selected from any superconducting metal other than aluminum, such as, but not limited to, any of niobium, tantalum, rhenium, titanium nitride, or niobium titanium nitride. This application does not impose any particular limitation on the thin film deposition method for forming the first superconducting layer 30, as long as it achieves the purpose of this application. For example, the aforementioned thin film deposition method may include, but is not limited to, any of electron beam evaporation, magnetron sputtering, thermal evaporation, or atomic layer vapor deposition. This application does not impose any particular limitation on the thickness of the first superconducting layer 30, as long as it achieves the purpose of this application.
[0057] In some embodiments of this application, forming the alumina barrier layer 40 in step S4 includes forming a single-crystal alumina barrier layer or an amorphous alumina barrier layer. In some embodiments of this application, forming the alumina barrier layer 40 requires first depositing an aluminum layer. This application does not particularly limit the method of depositing the aluminum layer, as long as it achieves the purpose of this application; for example, it may include, but is not limited to, any of electron beam evaporation, magnetron sputtering, thermal evaporation, or atomic layer vapor deposition. This application does not particularly limit the thickness of the alumina barrier layer 40, as long as it achieves the purpose of this application.
[0058] In some embodiments of this application, the material of the first superconducting layer 30 in step S3 is selected from aluminum, and the formation of an alumina barrier layer 40 on the first superconducting layer 30 in step S4 includes: placing the substrate 20 in a sealed environment, introducing oxygen into the sealed environment, and oxidizing the surface of the first superconducting layer 30 at room temperature to form an amorphous alumina barrier layer 40.
[0059] refer to Figure 3In some embodiments of this application, the material of the first superconducting layer 30 in step S3 is selected from aluminum, and the formation of an alumina barrier layer on the first superconducting layer 30 in step S4 includes: placing the substrate 20 in a sealed environment, heating the sealed environment to a high temperature, and introducing oxygen at the high temperature to oxidize the surface of the first superconducting layer 30, forming a single-crystal alumina barrier layer 40. In some embodiments of this application, the sealed environment is heated to 280°C to 500°C. The melting point of aluminum is 660°C, and when the temperature exceeds 277°C (550K), Al(111) can be oxidized to form single-crystal alumina.
[0060] In some embodiments of this application, the material of the first superconducting layer 30 in step S3 is selected from any superconducting metal other than aluminum. Step S4, forming an alumina barrier layer 40 on the first superconducting layer 30, includes: after depositing an aluminum layer on the first superconducting layer 30, placing the substrate 20 in a sealed environment, heating the sealed environment to a high temperature, and introducing oxygen at the high temperature to oxidize the aluminum layer to form a single-crystal alumina barrier layer 40. In some embodiments of this application, the sealed environment is heated to 280°C to 500°C. Aluminum has a melting point of 660°C, and when the temperature exceeds 277°C (550K), single-crystal alumina can be oxidized on Al(111).
[0061] In some embodiments of this application, the material of the first superconducting layer 30 in step S3 is selected from any superconducting metal other than aluminum, and the formation of an alumina barrier layer on the first superconducting layer 30 in step S4 includes: after depositing an aluminum layer on the first superconducting layer 30, placing the substrate 20 in a sealed environment, and oxidizing the deposited aluminum layer at room temperature in the sealed environment to form an amorphous alumina barrier layer 40. The room temperature oxidation can be achieved by introducing oxygen into the sealed environment.
[0062] refer to Figure 4 In some embodiments of this application, the material of the first superconducting layer 30 in step S3 is selected from any superconducting metal other than aluminum. Step S4, forming an alumina barrier layer 40 on the first superconducting layer 30, includes: after depositing an aluminum layer on the first superconducting layer 30, placing the substrate 20 in a sealed environment, and oxidizing the deposited aluminum layer at room temperature in the sealed environment to form an amorphous alumina barrier layer. Room temperature oxidation can be achieved by introducing oxygen into the sealed environment. The amorphous alumina barrier layer is then converted into a single-crystal alumina barrier layer 40 through a high-temperature annealing treatment. In some embodiments of this application, the high-temperature annealing temperature is between 800°C and 2000°C. Because a high-temperature annealing treatment is required, the melting point of the material of the first superconducting layer must be higher than the annealing temperature.
[0063] In some embodiments of this application, the material of the first superconducting layer 30 in step S3 is selected from any superconducting metal other than aluminum. Step S4, forming an alumina barrier layer 40 on the first superconducting layer 30, includes: setting the temperature of the substrate 20 to room temperature, depositing aluminum on the first superconducting layer 30 while simultaneously introducing oxygen to form an amorphous alumina barrier layer 40. In some embodiments of this application, the aluminum deposition rate is... to
[0064] refer to Figure 5 In some embodiments of this application, the material of the first superconducting layer 30 in step S3 is selected from any superconducting metal other than aluminum. Step S4, forming an alumina barrier layer 40 on the first superconducting layer 30, includes: heating the substrate 20 to a high temperature, depositing aluminum on the first superconducting layer 30 at the high temperature while simultaneously introducing oxygen to form a single-crystal alumina barrier layer 40. In some embodiments of this application, the substrate 20 is heated to 700°C to 800°C, and the aluminum deposition rate is... to
[0065] In some embodiments of this application, a Josephson junction is formed in the intersecting region in step S5. Specifically, the first superconducting layer 30 and the alumina barrier layer 40 are formed on the substrate 20 at the location exposed by the first etch window 111, and the second superconducting layer 50 is formed on the substrate 20 at the location exposed by the second etch window 112. At the location exposed in the intersecting region of the first etch window 111 and the second etch window 112 on the substrate 20, the structure is a first superconducting layer / alumina barrier layer / second superconducting layer, i.e., a Josephson junction is obtained. The number of intersecting regions of the first etch window 111 and the second etch window 112 is the number of Josephson junctions. This application does not have any particular limitation on the material of the second superconducting layer 50 in step S5, as long as it can achieve the purpose of this application. For example, the material of the second superconducting layer 50 can be, but is not limited to, any of aluminum, niobium, tantalum, rhenium, titanium nitride, or niobium titanium nitride. This application does not impose any particular limitation on the thin film deposition method for forming the second superconducting layer 50, as long as it achieves the purpose of this application. For example, the aforementioned thin film deposition method may include, but is not limited to, any of electron beam evaporation, magnetron sputtering, thermal evaporation, or atomic layer vapor deposition. This application does not impose any particular limitation on the thickness of the second superconducting layer 50, as long as it achieves the purpose of this application.
[0066] In some embodiments of this application, the first etching window 111 and the second etching window 112 are perpendicular to each other, and the first superconducting layer 30 and the second superconducting layer 50 are formed by an oblique evaporation deposition process, with the evaporation directions being perpendicular to each other, so as to avoid the material of the first superconducting layer 30 being deposited on the substrate 20 exposed by the second etching window 112.
[0067] In some embodiments of this application, the preparation method further includes step S6: separating the SOI mask 100 and the substrate 20. This application does not impose any particular restrictions on the method of separating the SOI mask 100 and the substrate 20 in step S6, as long as it achieves the purpose of this application.
[0068] The second aspect of this application provides a Josephson junction obtained according to any of the foregoing methods. The Josephson junction provided by this application avoids the adverse effects of photoresist residue on its performance, and also avoids the risk of photoresist softening or degradation during superconductor deposition processes requiring heating. Furthermore, the Josephson junction using a single-crystal alumina barrier layer exhibits better low-temperature performance.
[0069] Example
[0070] The embodiments and comparative examples provided below illustrate the implementation of this application in more detail. Various tests and evaluations were conducted according to the methods described below. Furthermore, unless otherwise specified, "parts" and "%" are quality standards.
[0071] Example 1
[0072] refer to Figure 3 Example 1 of this application provides a method for preparing a Josephson junction, the structure of which is aluminum / single-crystal alumina / aluminum. The preparation method includes the following steps:
[0073] S11: Provides an SOI mask and a substrate. The SOI mask has a first etching window and a second etching window that penetrate the SOI mask. The first etching window and the second etching window have two intersecting regions and are perpendicular to each other.
[0074] S21: Reference Figure 3 (a) Fixing the SOI mask onto the substrate;
[0075] S31: Reference Figure 3 (b) Aluminum of 30-50 nm is deposited by oblique evaporation in an electron beam evaporation chamber to form a first superconducting layer on the substrate exposed by the first etching window. The aluminum deposition method can also be magnetron sputtering, thermal evaporation, etc.
[0076] S41: Reference Figure 3 (c) The substrate and SOI mask obtained in S31 are transferred to the oxidation cavity. After the oxidation cavity is heated to 280-500°C, oxygen is introduced to oxidize the surface of the first superconducting layer and form a 1-3 nm single crystal alumina barrier layer on the first superconducting layer.
[0077] S51: Reference Figure 3(d) The substrate and SOI mask obtained in S41 are transferred back to the electron beam evaporation chamber, and 60-100 nm of aluminum is deposited by oblique evaporation. The direction of oblique evaporation is perpendicular to that in S31, so that a second superconducting layer is formed on the substrate exposed by the second etching window, and a Josephson junction is obtained in the intersection region. The above-mentioned aluminum deposition method can also be magnetron sputtering, thermal evaporation, etc.
[0078] S61: Reference Figure 3 (e) Remove the substrate and SOI mask obtained in S51 from the electron beam evaporation chamber and separate the SOI mask and substrate.
[0079] Example 2
[0080] refer to Figure 4 Embodiment 2 of this application provides a method for preparing a Josephson junction, the structure of which is rhenium / single-crystal alumina / aluminum. The preparation method includes the following steps:
[0081] S12: Provide an SOI mask and a substrate. The SOI mask has a first etching window and a second etching window that penetrate the SOI mask. The first etching window and the second etching window have two intersecting regions and are perpendicular to each other.
[0082] S22: Reference Figure 4 (a) Fixing the SOI mask onto the substrate;
[0083] S32: Reference Figure 4 (b) Rhenium of 30-50 nm is deposited by oblique evaporation in an electron beam evaporation chamber to form a first superconducting layer on the substrate exposed by the first etching window. The above-mentioned rhenium deposition method can also be magnetron sputtering, thermal evaporation, etc.
[0084] S42: Reference Figure 4 (c) A 0.2 nm layer of aluminum is obliquely evaporated and deposited on the first superconducting layer and then transferred to the oxide cavity. Reference Figure 4 (d) Oxygen is introduced into the oxidation chamber at room temperature to oxidize the deposited aluminum and form amorphous aluminum oxide. The oxidation chamber is heated and annealed at a temperature of 800-2000°C to convert the amorphous aluminum oxide into a single-crystal aluminum oxide barrier layer. The above-mentioned aluminum deposition method can also be atomic layer vapor deposition, magnetron sputtering, etc.
[0085] S52: Reference Figure 4 (e) The substrate and SOI mask obtained in S42 are transferred back to the electron beam evaporation chamber, and 60-100 nm of aluminum is deposited by oblique evaporation. The direction of oblique evaporation is perpendicular to that in S32, so that a second superconducting layer is formed on the substrate exposed by the second etching window, and a Josephson junction is obtained in the intersection region. The above-mentioned aluminum deposition method can also be magnetron sputtering, thermal evaporation, etc.
[0086] S62: Reference Figure 4 (f) Remove the substrate and SOI mask obtained by S52 from the electron beam evaporation chamber and separate the SOI mask and substrate.
[0087] Example 3
[0088] refer to Figure 5 Example 3 of this application provides a method for preparing a Josephson junction, the structure of which is niobium / single-crystal alumina / aluminum. The preparation method includes the following steps:
[0089] S13: Provide an SOI mask and a substrate. The SOI mask has a first etching window and a second etching window that penetrate the SOI mask. The first etching window and the second etching window have two intersecting regions and are perpendicular to each other.
[0090] S23: Reference Figure 5 (a) Fixing the SOI mask onto the substrate;
[0091] S33: Reference Figure 5 (b) 30-50 nm of niobium is deposited by oblique evaporation in an electron beam evaporation chamber to form a first superconducting layer on the substrate exposed by the first etching window. The above-mentioned niobium deposition method can also be magnetron sputtering, thermal evaporation or other methods.
[0092] S43: Reference Figure 5 (c) Heat the substrate to 750°C and set the intrinsic vacuum to 5 × 10⁻⁶. -6 torr, with Aluminum of 0.1–1 nm is deposited on the first superconducting layer at a rate of 1 nm, while oxygen is introduced to form a single-crystal alumina barrier layer. After cooling, the oxygen introduction is stopped.
[0093] S53: Reference Figure 5 (d) Aluminum of 60-100 nm is deposited by oblique evaporation. The direction of oblique evaporation is perpendicular to that in S33, so that a second superconducting layer is formed on the substrate exposed by the second etching window, and a Josephson junction is obtained in the intersection region. The above-mentioned aluminum deposition method can also be magnetron sputtering, thermal evaporation, etc.
[0094] S63: Reference Figure 5 (e) Remove the substrate and SOI mask obtained from S53 from the electron beam evaporation chamber and separate the SOI mask and substrate.
[0095] The above description is only a preferred embodiment of this application and is not intended to limit this application. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the scope of protection of this application.
Claims
1. A method of fabricating a Josephson junction, characterized by, include: An SOI mask and a substrate are provided, wherein the SOI mask has a first etching window and a second etching window extending through the SOI mask, and the first etching window and the second etching window have at least one intersecting region; The SOI mask is fixed onto the substrate; A first superconducting layer is formed on the substrate exposed by the first etched window; An alumina barrier layer is formed on the first superconducting layer; A second superconducting layer is formed on the substrate exposed by the second etched window to obtain a Josephson junction in the intersection region; The alumina barrier layer is a single-crystal alumina barrier layer.
2. The production method according to claim 1, characterized by, The provision of the SOI mask includes: An SOI wafer is provided, the SOI wafer comprising a first silicon layer, a silicon dioxide layer and a second silicon layer stacked sequentially; The first silicon layer is patterned and etched to form the first etching window and the second etching window; The second silicon layer and the silicon dioxide layer are patterned and etched to form a cavity that exposes the first etching window and the second etching window, thereby obtaining the SOI mask.
3. The preparation method according to claim 1, characterized in that, The material of the first superconducting layer is selected from aluminum. The process of forming an alumina barrier layer on the first superconducting layer includes: placing the substrate in a sealed environment, heating the sealed environment to a high temperature, and introducing oxygen at the high temperature to oxidize the surface of the first superconducting layer to form a single-crystal alumina barrier layer.
4. The method of claim 1, wherein, The material of the first superconducting layer is selected from any superconducting metal other than aluminum. The process of forming an aluminum oxide barrier layer on the first superconducting layer includes: depositing an aluminum layer on the first superconducting layer, placing the substrate in a sealed environment, heating the sealed environment to a high temperature, and introducing oxygen at the high temperature to oxidize the aluminum layer to form a single-crystal aluminum oxide barrier layer.
5. The production method according to claim 3 or 4, characterized by, The sealed environment is heated to 280°C to 500°C.
6. The method of claim 1, wherein, The material of the first superconducting layer is selected from any superconducting metal other than aluminum. The process of forming an alumina barrier layer on the first superconducting layer includes: depositing an aluminum layer on the first superconducting layer, placing the substrate in a sealed environment, oxidizing the deposited aluminum layer at room temperature in the sealed environment to form an amorphous alumina barrier layer, and converting the amorphous alumina barrier layer into a monocrystalline alumina barrier layer by high-temperature annealing.
7. The production method according to claim 6, wherein The high-temperature annealing treatment is performed at temperatures ranging from 800°C to 2000°C.
8. The method of claim 1, wherein, The material of the first superconducting layer is selected from any superconducting metal other than aluminum. The formation of an alumina barrier layer on the first superconducting layer includes: heating the substrate to a high temperature, depositing aluminum on the first superconducting layer at the high temperature while simultaneously introducing oxygen to form a single-crystal alumina barrier layer.
9. The production method according to claim 8, characterized by, The substrate is heated to 700°C to 800°C, and the aluminum deposition rate is 0.1 Å / s to 1 Å / s.
10. The preparation method according to claim 1, characterized in that, The first etching window and the second etching window are perpendicular to each other. The first superconducting layer and the second superconducting layer are formed by oblique evaporation deposition process, and the evaporation directions are perpendicular to each other.
11. The method of claim 1, wherein, The preparation method further includes: separating the SOI mask and the substrate.
12. A Josephson knot obtained by the preparation method according to any one of claims 1 to 11.
Citation Information
Patent Citations
Mask and manufacturing method thereof, and manufacturing method of Josephson junction
CN116682721A