A lightweight micro / nano porous three-dimensional high-temperature protective material and its preparation method

By adding nano-sol composite smoke suppressant and flame retardant and thermal expansion microsphere foaming agent to cellulose ionic liquid solution, a lightweight micro-nano porous three-dimensional high-heat protective material is prepared, which solves the problems of high processing difficulty, low production efficiency and reduced thermal protection performance in the existing technology. It achieves lightweight, high-efficiency porous three-dimensional high-heat protection effect and is suitable for protective clothing in high-temperature industries such as fire protection and petrochemicals.

CN119753926BActive Publication Date: 2026-11-17SHAANXI YUANFENG TEXTILE TECH RES
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411887715.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-12-20
Publication Date
2026-11-17
Estimated Expiration
2044-12-20

AI Technical Summary

Technical Problem

Existing high-heat protection materials suffer from problems such as high processing difficulty, low production efficiency, reduced heat protection performance, poor air permeability, and the generation of toxic fumes during combustion in fiber microstructure construction, multi-layer fabric composite and coating impregnation technologies, making it difficult to achieve both lightweight and high-heat protection.

Method used

The flame-retardant pre-woven fiber preparation method involves adding nano-sol composite smoke suppressant and flame retardant and thermal expansion microsphere foaming agent to a cellulose ionic liquid solution. After spinning, blending, weaving and high-temperature treatment, a multi-layer base fabric is formed, creating a micro-nano porous three-dimensional structure. Combined with flame retardant, smoke suppressant and comfort layer design, it achieves lightweight and high-heat protection.

Benefits of technology

It has achieved a lightweight, high-efficiency porous three-dimensional high-temperature protective material with good heat insulation performance, smoke suppression effect and comfort, and is suitable for protective clothing in high-temperature industries such as fire protection and petrochemical industry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119753926B_ABST
    Figure CN119753926B_ABST
Patent Text Reader

Abstract

This invention provides a lightweight micro-nano porous three-dimensional high-heat protective material and its preparation method. First, a flame-retardant pre-fiber is prepared by adding a thermally expanding microsphere foaming agent and a nano-sol composite smoke-suppressing and flame-retardant agent to a cellulose ionic liquid solution. Next, the flame-retardant pre-fiber is mixed with high-performance flame-retardant fibers, flame-retardant water-absorbing fibers, and flame-retardant hydrophobic fibers, respectively, to spin different blended yarns. Then, the blended yarns are used to weave a multi-layered three-dimensional base fabric with an outer flame-retardant layer, a middle super-absorbent layer, and an inner hydrophobic comfort layer. Finally, the base fabric is brushed and then heated at high temperature, causing the thermally expanding microsphere foaming agent in the fiber matrix to expand, thus obtaining the lightweight micro-nano porous three-dimensional high-heat protective material. This invention features a short, environmentally friendly, and easily industrialized preparation process. The prepared protective material is lightweight, exhibits excellent smoke-suppressing and flame-retardant properties, and possesses excellent heat insulation and moisture absorption properties. It is comfortable to wear and can be widely applied in the development of lightweight high-heat protective clothing for high-temperature industries such as fire fighting, metallurgy, and petrochemicals.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of preparation of high-heat-protective multifunctional textile materials, specifically to a lightweight micro-nano porous three-dimensional high-heat-protective material and its preparation method. Background Technology

[0002] High-heat protective clothing is one of the most widely used types of protective clothing. It refers to protective equipment designed to prevent the clothing itself from igniting or to slow down and extinguish combustion in extreme heat environments. Extreme heat environments mainly include intense flame convection and radiation heat, heat from contact with high-temperature burning materials or objects, molten metal splashes, steam jets, high-temperature gas convection heat, and high-temperature liquid splashes. The heat insulation principle of high-heat protective clothing is primarily to reduce the rate at which heat is transferred to the skin, thereby delaying the time it takes for burns to occur. It isolates heat sources and open flames from the body, preventing overheating injuries, heatstroke, burns, and other injuries. It avoids harm from high or ultra-high temperature heat sources, protecting the wearer's safety. It is widely used in workwear in industries such as firefighting, military, emergency rescue, petrochemicals, natural gas, and food processing.

[0003] Currently, high-temperature protective materials are mainly achieved through three technical measures: fiber microstructure construction, multi-layer fabric composite design, and coating and impregnation.

[0004] In terms of fiber microstructure construction, the most typical technical means is to prepare various microstructured or aerogel fibers. For example, patent CN114481357A discloses a microstructured fiber, which consists of a cladding layer and a core layer. After the fiber is formed, heating is used to give the fiber a microstructure. Alternatively, supercritical or freeze-drying technology can be used to obtain aerogel fibers with a porous network structure. Finally, the prepared microstructured or aerogel fibers are processed into various fabrics using weaving, non-woven, or knitting techniques.

[0005] In the design of multi-layered fabric composites, adhesives or fabric structure design are mainly used. For example, CN112221027B discloses a flame-retardant and heat-insulating fabric for fire escape emergency. This fabric is composed of three single-layer fabrics: a hydrogel dressing layer, a heat-insulating non-woven fabric layer, and a flame-retardant non-woven fabric layer, which are connected by adhesive bonding or heat-fusion reinforcement. CN116423938A discloses a multi-dimensional composite thermal protection fabric. This fabric has three layers: an inorganic fiber primary protective layer, a thermal and moisture comfort regulating layer, and an aerogel secondary thermal protective layer, from the outside to the inside. The thermal and moisture comfort regulating layer is interwoven with the other two layers to form a whole.

[0006] Regarding the use of coating and impregnation technology, CN108221397B provides a method for preparing fire-resistant and heat-insulating metallized coated fabric, which involves calendering and humidifying a flame-retardant base fabric, coating it with a flame-retardant polyurethane silver paste solution, and then drying it to obtain a fire-resistant and heat-insulating metallized coated fabric.

[0007] Existing technologies that improve the thermal protection performance of fabrics by constructing fiber microstructures, designing multilayer fabric composites, and using coating and impregnation techniques have the following main technical shortcomings.

[0008] First, after preparing microstructured or aerogel fiber raw materials, the numerous micropores in the fiber structure lead to a decrease in the fiber's tensile, elastic, and frictional properties, making the spinning and weaving of microstructured or aerogel fibers difficult and hindering large-scale industrial production. Furthermore, during the long textile processing steps, mechanical friction and compression can damage the fiber's microstructure, resulting in a sharp decline in the thermal protection properties of the final fabric.

[0009] Secondly, existing technologies for preparing micro / nano structures or aerogel fibers involve long processes, especially for aerogel fiber preparation. Currently, the most mature technologies employ supercritical or freeze-drying methods, which require stringent reaction conditions and are difficult to implement continuously in processes such as solvent replacement and drying, resulting in low production efficiency and hindering large-scale industrial applications. Furthermore, the mechanical fragility and structural instability of traditional aerogel fibers limit their widespread use in practical applications. Additionally, multilayer fabric composites mostly rely on simple physical stacking, which increases the total mass of the fabric but offers limited improvement in thermal protection, making it difficult to achieve lightweight, high-heat protection.

[0010] Third, heat-protective fabrics obtained using coating and impregnation techniques have poor breathability. The coating is easily damaged during processing and wearing, and the fabric is not washable, leading to a decline in its heat protection performance. Furthermore, existing high-temperature resistant and flame-retardant protective materials, such as CN109208154A, which uses a blend of 30%–65% acrylonitrile fiber, 30%–65% flame-retardant regenerated cellulose fiber, and 5%–25% para-aramid fiber to create an acrylonitrile-based blended flame-retardant, high-temperature resistant, and antistatic fabric, produce large amounts of toxic and corrosive fumes when burning due to the presence of acrylonitrile. Inhalation of these toxic gases, leading to unconsciousness and suffocation, is a major cause of injury and death in fires. Therefore, the smoke suppression performance of flame-retardant and high-temperature resistant protective materials urgently needs improvement.

[0011] It is evident that existing technologies for developing thermal protection fabrics, which utilize microstructures or aerogel fibers, present significant processing challenges, low production efficiency, and performance degradation. Multi-layered fabrics offer limited improvement in thermal protection, making it difficult to achieve a balance between lightweight and high-heat protection. Furthermore, they produce toxic fumes during combustion, and their smoke suppression and comfort aspects require further improvement. Summary of the Invention

[0012] To address the shortcomings of the existing technology, the purpose of this invention is to provide a method for preparing a lightweight micro-nano porous three-dimensional high-temperature protective material.

[0013] This invention provides a method for preparing a lightweight micro / nano porous three-dimensional high-temperature protective material, comprising the following steps:

[0014] Step 1: Preparation of flame-retardant pre-fibers: First, nano-sol composite smoke suppressant and flame retardant agent and crosslinking agent are added sequentially to cellulose ionic liquid solution and stirred to obtain crosslinked flame-retardant cellulose ionic liquid solution; then, a certain proportion of thermal expansion microsphere foaming agent is added to the crosslinked flame-retardant cellulose ionic liquid solution and stirred to obtain spinning solution; then, the spinning solution is filtered and degassed sequentially and placed in a wet spinning equipment, and the spinning solution is extruded from the spinneret under a nitrogen pressure of 0.5 MPa. After solidification, hot stretching, cutting, oiling, and packaging, flame-retardant pre-fibers are obtained.

[0015] The average particle size of the nano-sol composite flame retardant is 200nm to 300nm; the nano-sol composite smoke suppressant and flame retardant includes a mixture of bisphenol modified phosphate oligomer, hydroxymethylammonium phosphate, phosphonomethoxy, ferrous oxalate, calcium phosphomolybdate, and dihydroxy metal composite oxide-magnesium aluminum hydroxide.

[0016] Step 2, Spinning of blended yarn: The flame-retardant pre-made fiber is mixed with high-performance flame-retardant fiber, flame-retardant super absorbent fiber and flame-retardant ultrafine hydrophobic fiber respectively. The three mixtures are then processed sequentially through oiling and humidification, premixing, cleaning and carding, drawing, roving, spinning, winding, doubling, twisting and steaming to spin yarn I, yarn II and yarn III respectively.

[0017] Step 3, Preparation of base fabric: Through fabric structure design, yarn I, yarn II and yarn III are sequentially warped, sizing, reeded, woven and repaired to obtain a multi-layer base fabric. The outermost layer of this multi-layer base fabric is a flame-retardant layer composed of yarn I, the middle layer is a super absorbent layer composed of yarn II, and the innermost layer is a hydrophobic and comfortable layer composed of yarn III.

[0018] Step 4: Preparation of lightweight high-heat protective material: After the base fabric prepared in step 3 is desized, dyed, and stretched and set, the inner surface of the fabric is then brushed and then subjected to high temperature treatment, so that the thermal expansion microsphere foaming agent added to the flame retardant pre-fiber matrix expands under heat to form a multi-dimensional lightweight high-heat protective material.

[0019] Furthermore, in step 1, the cross-linked flame-retardant cellulose ionic liquid solution contains 15 to 25 parts of nano-sol composite smoke-suppressing and flame-retardant agent, 3 to 5 parts of cross-linking agent, and the remainder is cellulose ionic liquid solution.

[0020] Furthermore, in step 1, the spinning solution contains 10 to 25 parts of thermally expanding microsphere foaming agent with an average particle size of 300 nm to 400 nm; the remainder is a cross-linked flame-retardant cellulose ionic liquid solution.

[0021] Furthermore, the nanosol composite smoke suppressant and flame retardant in step 1 includes a mixture of various compounds such as bisphenol modified phosphate oligomer, hydroxymethylammonium phosphate, phosphonomethoxy, ferrous oxalate, calcium phosphomolybdate, and dihydroxy metal composite oxide-magnesium aluminum hydroxide.

[0022] Further, in step 1, the nano-sol composite smoke suppressant and flame retardant contains 10-20 parts of bisphenol-modified phosphate oligomer, 10-20 parts of hydroxymethylammonium phosphate, 20-35 parts of phosphoric acid methoxy, 8-15 parts of ferrous oxalate, 15-25 parts of calcium phosphomolybdate, and 8-15 parts of dihydroxy metal composite oxide-magnesium aluminum hydroxide; the average particle size of the nano-sol composite smoke suppressant and flame retardant is 200 nm to 300 nm.

[0023] Further, the crosslinking agent in step 1 contains 45 to 65 parts of ammonium bicarbonate and 35 to 55 parts of ammonium acetate.

[0024] Furthermore, in the hot drawing process described in step 1, the hot drawing temperature is 110℃~120℃, and the drawing ratio is 1.5 times~3.0 times.

[0025] Furthermore, the high-performance flame-retardant fiber mentioned in step 2 includes a mixture of various fibers such as aramid fiber, polyphenylene sulfide fiber, polyimide fiber, meta-aramid and para-aramid.

[0026] Furthermore, in step 2, yarn I contains 30 to 50 parts of flame-retardant pre-woven fiber, 20 to 40 parts of aramid fiber, 25 to 45 parts of polyphenylene sulfide fiber, and 25 to 40 parts of polyimide fiber.

[0027] Furthermore, in step 2, yarn II contains 25 to 45 parts flame-retardant superabsorbent fiber, 30 to 50 parts flame-retardant pre-woven fiber, 20 to 50 parts meta-aramid, and 5 to 15 parts para-aramid.

[0028] Furthermore, in step 2, the yarn III contains 25 to 45 parts of flame-retardant ultrafine hydrophobic fiber, 30 to 50 parts of flame-retardant pre-woven fiber, 20 to 50 parts of meta-aramid, and 5 to 15 parts of para-aramid.

[0029] Furthermore, in step 2, the linear density of yarn I is 11.81 tex × 2 to 15.54 tex × 2, the linear density of yarn II is 9.84 tex × 2 to 11.81 tex × 2, and the linear density of yarn III is 11.81 tex × 2 to 13.12 tex × 2.

[0030] Furthermore, the temperature of the steaming process in step 2 is 80℃~100℃.

[0031] Furthermore, the fabric structure described in step 3 is formed by interlacing the middle layer with the outer and inner layers through the methods of inner warp knotting outer weft and outer warp knotting inner weft; wherein, the fabric structure of the outer layer, middle layer, and inner layer is a plain weave or a twill weave.

[0032] Furthermore, in step 3, the warp density of the fabric is 660 threads / 10cm to 710 threads / 10cm, and the weft density is 575 threads / 10cm to 625 threads / 10cm.

[0033] Furthermore, the yarn arrangement ratio of the outer layer, middle layer, and inner layer fabrics in step 3 is 1:1:1 to 4:2:3.

[0034] Furthermore, the drying temperature for the sizing process described in step 3 is 100℃~120℃.

[0035] Furthermore, the base fabric described in step 3 has a unit area mass of 300 g / m². 2 ~360g / m 2 .

[0036] Furthermore, in step 4, the abrasive skin has a mesh size of 400-500, a machine speed of 12-18 m / min, a grinding roller speed of 850-950 rpm, and a pressure of 0.2 MPa-0.4 MPa.

[0037] Furthermore, the high-temperature treatment in step 4 is carried out at a temperature of 140℃ to 160℃.

[0038] On the other hand, the present invention also provides a lightweight micro-nano porous three-dimensional high-temperature protective material prepared by the aforementioned preparation method.

[0039] The beneficial effects of this invention are as follows:

[0040] The lightweight micro-nano porous three-dimensional high-heat protective material described in this invention features flame-retardant pre-fibers where the hot drawing temperature (110℃~120℃), sizing and drying temperature (100℃~120℃), and steaming temperature (80℃~100℃) are all lower than the thermal expansion temperature (130℃~150℃) of the thermal expansion microsphere foaming agent during preparation and processing. During the spinning and weaving of the flame-retardant pre-fibers to form the base fabric, no expansion occurs, reducing the processing difficulty caused by the poor physical and mechanical properties of microstructures or aerogel fibers. Simultaneously, it avoids the long processing flow from spinning to weaving of microstructures or aerogel fibers, preventing damage to the micro-nano structure during carding, drawing, and twisting processes, thus ensuring thermal protection performance. This solves the technical problem of large-scale industrialization of traditional micro-nano structured materials such as aerogel fibers due to their mechanical fragility and structural instability.

[0041] The lightweight micro-nano porous three-dimensional high-temperature protective material of this invention creatively involves high-temperature heating treatment of the final heat protection material, causing the flame-retardant pre-fabricated fibers in the formed material to expand. At the same time, the high-temperature treatment temperature is 140℃~160℃, which is far lower than the minimum heat resistance temperature of the pre-fabricated flame-retardant fiber matrix and other fibers. It does not cause irreversible damage to the protective material, but only causes thermal expansion of the flame-retardant pre-fabricated fibers to form a lightweight micro-nano porous three-dimensional high-temperature protective material.

[0042] The high-heat protective material developed in this invention involves the thorough mixing of fibers during each spinning process, resulting in a uniform distribution of flame-retardant pre-fabricated fibers. Microscopically, the material exhibits a uniform distribution of various micro- and nano-sized closed-cell (closed-pore) and interconnected (open-pore) mixed pore structures. Air within these mixed pore structures forms unique gas chambers with the bubble walls, and the unique properties of air contribute to the material's low density and low thermal conductivity, thus enhancing its thermal insulation performance. Macroscopically, the invention's unique multi-layered composite structure allows heat to dissipate through multiple reflections within the multi-layered structure when exposed to a heat source, further improving the material's thermal insulation. Simultaneously, the invention creatively and effectively combines the constructed micro- and nano-porous structures with the macroscopic multi-structure of the protective material. Through a synergistic effect across dimensions (micro-, meso-, and macro-), the thermal insulation performance of the protective material is significantly improved, overcoming the limitation of simply increasing the number of material layers in developing multi-layered composite fabrics where the improvement in thermal protection performance is not significant.

[0043] The flame-retardant pre-woven fiber of this invention undergoes a direct chemical cross-linking reaction between the thermally expanding microsphere foaming agent, the nano-sol flame retardant, and the fiber matrix. When the self-made flame-retardant pre-woven fiber is not subjected to heat expansion treatment, its performance is almost the same as that of commonly used textile fibers. When the flame-retardant pre-woven fiber is blended with other fibers, it is mixed through multiple processes, resulting in a uniform distribution of the flame-retardant pre-woven fiber. Theoretically, there is no upper limit to the amount that can be added, and 100% can be achieved. After high-temperature treatment, the material can distribute more micro-nano porous structures, making the protective material lightweight and achieving high-heat protection.

[0044] In the preparation of flame-retardant pre-woven fibers, this invention adds ferrous oxalate, calcium phosphomolybdate, and a dihydroxyl metal composite oxide—magnesium aluminum hydroxide—to the nano-sol composite smoke-suppressing halogen-free flame retardant. This smoke-suppressing flame retardant promotes char formation through cross-linking in the condensed phase, converting carbon in the polymer into carbon monoxide and carbon dioxide. This dilutes combustible gases and smoke, thereby reducing the amount of soot formed and exerting a smoke-suppressing effect. Alternatively, the alumina and magnesium oxide formed during heating have a large surface area and can adsorb smoke dust. Therefore, this invention creatively alters the combustion mode through a synergistic effect of flame retardancy and smoke suppression, utilizing principles such as coverage effect, transfer effect, free radical inhibition, and accelerated char formation. By reducing the content of combustibles, it reduces smoke production, achieving a composite smoke-suppressing and flame-retardant effect through synergistic action.

[0045] In the structural design of the three-dimensional high-heat protective material, this invention incorporates a flame-retardant layer, a moisture-absorbing layer, and a comfort layer from the outside in. The outermost flame-retardant layer prevents the flame from burning and spreading, and prevents molten dripping, thus ensuring the structural integrity and functional maintenance of the protective clothing during operation in hot environments. The super-absorbent fibers in the middle moisture-absorbing layer can absorb and store the sweat produced by the human body. The innermost comfort layer is composed of microfibers, which, after being brushed, form a plush texture on the surface of the material, making it soft, comfortable, and skin-friendly to the touch, thereby improving the comfort of the protective material.

[0046] It is evident that the preparation process of this invention is short, environmentally friendly, and easy to industrialize. The prepared protective material is lightweight, has excellent smoke suppression and flame retardancy, and excellent heat insulation and moisture absorption properties. It is comfortable to wear and can be widely used in the development of lightweight high-heat protective clothing in high-temperature industries such as fire fighting and petrochemicals. Attached Figure Description

[0047] To more clearly illustrate the technical solutions of the embodiments of this application, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of this application and should not be regarded as a limitation of the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.

[0048] Figure 1This is a SEM image of the flame-retardant pre-fabricated fiber in Example 1.

[0049] Figure 2 This is a SEM image of the micro-nano flame-retardant fibers formed by high-temperature expansion in Example 1. Detailed Implementation

[0050] The technical solution of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0051] In this invention, the flame-retardant superabsorbent fiber was purchased from UK Technical Absorbent Products Ltd., and the flame-retardant ultrafine hydrophobic fiber was purchased from Qingdao Xinwei Textile Development Co., Ltd.; the thermal expansion microsphere foaming agent was purchased from Polychem, USA, model 186DU20; the bisphenol modified phosphate oligomer (BDP) was purchased from Jiangsu Haian Petrochemical Plant; the hydroxymethylammonium phosphate was purchased from Wuhan Lanabai Pharmaceutical Chemical Co., Ltd.; the zinc stannate was purchased from Hubei Xingyan New Material Technology Co., Ltd.; the phosphonoheterocyclic methoxy group was purchased from Shandong Xindongneng Chemical Co., Ltd.; the ferrous oxalate was purchased from Jinan Kaichuang Chemical Co., Ltd.; the calcium phosphomolybdate was purchased from Shanghai Youpeng Chemical Co., Ltd.; the dihydroxy metal composite oxide-magnesium aluminum hydroxide was purchased from Hebei Yuechao Wear-resistant Materials Co., Ltd.; the ammonium bicarbonate was purchased from Shandong Xinyi Biotechnology Co., Ltd.; and the ammonium acetate was purchased from Weifang Youlan Chemical Co., Ltd.

[0052] Example 1

[0053] This embodiment provides a method for preparing a lightweight micro / nano porous three-dimensional high-temperature protective material, the steps of which include:

[0054] Step 1: Preparation of flame-retardant pre-fibers: First, nano-sol composite smoke suppressant and flame retardant agent and crosslinking agent are added sequentially to cellulose ionic liquid solution and stirred to obtain crosslinked flame-retardant cellulose ionic liquid solution; then, a certain proportion of thermal expansion microsphere foaming agent is added to the crosslinked flame-retardant cellulose ionic liquid solution and stirred to obtain spinning solution; then, the spinning solution is filtered and degassed sequentially and placed in a wet spinning equipment, and the spinning solution is extruded from the spinneret under a nitrogen pressure of 0.5 MPa. After solidification, hot stretching, cutting, oiling, and packaging, flame-retardant pre-fibers are obtained.

[0055] Step 2, Spinning of blended yarn: The flame-retardant pre-made fiber is mixed with high-performance flame-retardant fiber, flame-retardant super absorbent fiber and flame-retardant ultrafine hydrophobic fiber respectively. The three mixtures are then processed sequentially through oiling and humidification, premixing, cleaning and carding, drawing, roving, spinning, winding, doubling, twisting and steaming to spin yarn I, yarn II and yarn III respectively.

[0056] Step 3, Preparation of base fabric: Through fabric structure design, yarn I, yarn II and yarn III are sequentially warped, sizing, reeded, woven and repaired to obtain a multi-layer base fabric. The outermost layer of this multi-layer base fabric is a flame-retardant layer composed of yarn I, the middle layer is a super absorbent layer composed of yarn II, and the innermost layer is a hydrophobic and comfortable layer composed of yarn III.

[0057] Step 4: Preparation of lightweight high-heat protective material: After the base fabric prepared in step 3 is desized, dyed, and stretched and set, the inner surface of the fabric is then brushed and then subjected to high temperature treatment, so that the thermal expansion microsphere foaming agent added to the flame retardant pre-fiber matrix expands under heat to form a multi-dimensional lightweight high-heat protective material.

[0058] In step 1, the cross-linked flame-retardant cellulose ionic liquid solution contains 20 parts of nano-sol composite smoke-suppressing and flame-retardant agent, 5 parts of cross-linking agent, and the remainder is cellulose ionic liquid solution.

[0059] The spinning solution in step 1 contains 25 parts of thermally expanding microsphere foaming agent with an average particle size of 300 nm; the remainder is a cross-linked flame-retardant cellulose ionic liquid solution.

[0060] The nano-sol composite smoke suppressant and flame retardant in step 1 contains 10 parts of bisphenol modified phosphate oligomer, 20 parts of hydroxymethylammonium phosphate, 30 parts of phosphonocyclic methoxy, 10 parts of ferrous oxalate, 15 parts of calcium phosphomolybdate, and 15 parts of dihydroxy metal composite oxide-magnesium aluminum hydroxide. The average particle size of the nano-sol composite smoke suppressant and flame retardant is 200 nm.

[0061] The crosslinking agent in step 1 contains 55 parts ammonium bicarbonate and 45 parts ammonium acetate.

[0062] In the hot drawing process described in step 1, the hot drawing temperature is 120℃ and the drawing ratio is 2.0 times.

[0063] In step 2, yarn I contains 50 parts flame-retardant pre-woven fiber, 25 parts polyphenylene sulfide fiber, and 25 parts polyimide fiber.

[0064] The yarn II described in step 2 contains 25 parts flame-retardant superabsorbent fiber, 45 parts flame-retardant pre-fabricated fiber, 20 parts meta-aramid, and 10 parts para-aramid.

[0065] The yarn III described in step 2 contains 25 parts flame-retardant ultrafine hydrophobic fiber, 45 parts flame-retardant pre-made fiber, 20 parts meta-aramid, and 10 parts para-aramid.

[0066] In step 2, the linear density of yarn I is 14.76 tex × 2, the linear density of yarn II is 9.84 tex × 2, and the linear density of yarn III is 13.12 tex × 2.

[0067] The temperature for the steaming process in step 2 is 100℃.

[0068] The fabric structure described in step 3 is formed by interlacing the middle layer with the outer and inner layers through the methods of inner warp knotting outer weft and outer warp knotting inner weft.

[0069] The fabric described in step 3 has a warp density of 700 threads / 10cm and a weft density of 615 threads / 10cm.

[0070] The yarn arrangement ratio of the outer, middle, and inner layers of fabric in step 3 is 4:2:3.

[0071] The drying temperature for the sizing process described in step 3 is 120℃.

[0072] The base fabric mentioned in step 3 has a unit area mass of 360 g / m². 2 The unit area mass ratio of the outer, middle, and inner layers of fabric is 3:2:2.

[0073] In step 4, the abrasive skin has a mesh size of 400, a machine speed of 18 meters per minute, a grinding roller speed of 950 revolutions per minute, and a pressure of 0.4 MPa.

[0074] The high-temperature treatment in step 4 is performed at a temperature of 160°C.

[0075] Figure 1 This is a SEM image of the flame-retardant pre-fabricated fiber in Example 1; Figure 2 This is a SEM image of the micro-nano flame-retardant fibers formed by high-temperature expansion in Example 1.

[0076] Depend on Figure 1 It is known that the flame-retardant pre-fabricated fiber before high-temperature treatment has a uniform texture, high molecular orientation, and excellent mechanical properties, and is not much different from conventional textile fibers.

[0077] Depend on Figure 2 It is known that flame-retardant pre-fabricated fibers treated at high temperatures exhibit micro-nano porous structures in their cross-sections, which is beneficial for improving the thermal protection performance of high-temperature protective materials.

[0078] Example 2

[0079] This embodiment provides a method for preparing a lightweight micro / nano porous three-dimensional high-temperature protective material, the steps of which include:

[0080] Step 1: Preparation of flame-retardant pre-fibers: First, nano-sol composite smoke suppressant and flame retardant agent and crosslinking agent are added sequentially to cellulose ionic liquid solution and stirred to obtain crosslinked flame-retardant cellulose ionic liquid solution; then, a certain proportion of thermal expansion microsphere foaming agent is added to the crosslinked flame-retardant cellulose ionic liquid solution and stirred to obtain spinning solution; then, the spinning solution is filtered and degassed sequentially and placed in a wet spinning equipment, and the spinning solution is extruded from the spinneret under a nitrogen pressure of 0.5 MPa. After solidification, hot stretching, cutting, oiling, and packaging, flame-retardant pre-fibers are obtained.

[0081] Step 2, Spinning of blended yarn: The flame-retardant pre-made fiber is mixed with high-performance flame-retardant fiber, flame-retardant super absorbent fiber and flame-retardant ultrafine hydrophobic fiber respectively. The three mixtures are then processed sequentially through oiling and humidification, premixing, cleaning and carding, drawing, roving, spinning, winding, doubling, twisting and steaming to spin yarn I, yarn II and yarn III respectively.

[0082] Step 3, Preparation of base fabric: Through fabric structure design, yarn I, yarn II and yarn III are sequentially warped, sizing, reeded, woven and repaired to obtain a multi-layer base fabric. The outermost layer of this multi-layer base fabric is a flame-retardant layer composed of yarn I, the middle layer is a super absorbent layer composed of yarn II, and the innermost layer is a hydrophobic and comfortable layer composed of yarn III.

[0083] Step 4: Preparation of lightweight high-heat protective material: After the base fabric prepared in step 3 is desized, dyed, and stretched and set, the inner surface of the fabric is then brushed and then subjected to high temperature treatment, so that the thermal expansion microsphere foaming agent added to the flame retardant pre-fiber matrix expands under heat to form a multi-dimensional lightweight high-heat protective material.

[0084] In step 1, the cross-linked flame-retardant cellulose ionic liquid solution contains 25 parts of nano-sol composite smoke-suppressing and flame-retardant agent, 5 parts of cross-linking agent, and the remainder is cellulose ionic liquid solution.

[0085] In step 1, the spinning solution contains 10 parts of thermally expanding microsphere foaming agent with an average particle size of 350 nm; the remainder is a cross-linked flame-retardant cellulose ionic liquid solution.

[0086] The nano-sol composite smoke suppressant and flame retardant in step 1 contains 20 parts of bisphenol modified phosphate oligomer, 10 parts of hydroxymethylammonium phosphate, 20 parts of phosphonocyclic methoxy, 15 parts of ferrous oxalate, 25 parts of calcium phosphomolybdate, and 10 parts of dihydroxy metal composite oxide-magnesium aluminum hydroxide. The average particle size of the nano-sol composite smoke suppressant and flame retardant is 260 nm.

[0087] The crosslinking agent in step 1 contains 45 parts ammonium bicarbonate and 55 parts ammonium acetate.

[0088] In the hot drawing process described in step 1, the hot drawing temperature is 110℃ and the drawing ratio is 1.5 times.

[0089] In step 2, yarn I contains 30 parts flame-retardant pre-woven fiber, 35 parts polyphenylene sulfide fiber, and 35 parts polyimide fiber.

[0090] The yarn II described in step 2 contains 35 parts flame-retardant superabsorbent fiber, 35 parts flame-retardant pre-fabricated fiber, 20 parts meta-aramid, and 10 parts para-aramid.

[0091] The yarn III described in step 2 contains 30 parts flame-retardant ultrafine hydrophobic fiber, 40 parts flame-retardant pre-made fiber, 20 parts meta-aramid, and 10 parts para-aramid.

[0092] In step 2, the linear density of yarn I is 11.81 tex × 2, the linear density of yarn II is 9.84 tex × 2, and the linear density of yarn III is 11.81 tex × 2.

[0093] The temperature for the steaming process in step 2 is 80℃.

[0094] The fabric structure described in step 3 is formed by interlacing the middle layer with the outer and inner layers through the methods of inner warp knotting outer weft and outer warp knotting inner weft.

[0095] The fabric described in step 3 has a warp density of 660 threads / 10cm and a weft density of 575 threads / 10cm.

[0096] The yarn arrangement ratio of the outer, middle, and inner layers of fabric in step 3 is 3:2:3.

[0097] The drying temperature for the sizing process described in step 3 is 100℃.

[0098] The base fabric mentioned in step 3 has a unit area mass of 300 g / m². 2 The unit area mass ratio of the outer, middle, and inner layers of fabric is 3:2:3.

[0099] In step 4, the abrasive skin has a mesh size of 500, a machine speed of 12 meters per minute, a grinding roller speed of 850 revolutions per minute, and a pressure of 0.2 MPa.

[0100] The high-temperature treatment in step 4 is performed at a temperature of 140°C.

[0101] Example 3

[0102] This embodiment provides a method for preparing a lightweight micro / nano porous three-dimensional high-temperature protective material, the steps of which include:

[0103] Step 1: Preparation of flame-retardant pre-fibers: First, nano-sol composite smoke suppressant and flame retardant agent and crosslinking agent are added sequentially to cellulose ionic liquid solution and stirred to obtain crosslinked flame-retardant cellulose ionic liquid solution; then, a certain proportion of thermal expansion microsphere foaming agent is added to the crosslinked flame-retardant cellulose ionic liquid solution and stirred to obtain spinning solution; then, the spinning solution is filtered and degassed sequentially and placed in a wet spinning equipment, and the spinning solution is extruded from the spinneret under a nitrogen pressure of 0.5 MPa. After solidification, hot stretching, cutting, oiling, and packaging, flame-retardant pre-fibers are obtained.

[0104] Step 2, Spinning of blended yarn: The flame-retardant pre-made fiber is mixed with high-performance flame-retardant fiber, flame-retardant super absorbent fiber and flame-retardant ultrafine hydrophobic fiber respectively. The three mixtures are then processed sequentially through oiling and humidification, premixing, cleaning and carding, drawing, roving, spinning, winding, doubling, twisting and steaming to spin yarn I, yarn II and yarn III respectively.

[0105] Step 3, Preparation of base fabric: Through fabric structure design, yarn I, yarn II and yarn III are sequentially warped, sizing, reeded, woven and repaired to obtain a multi-layer base fabric. The outermost layer of this multi-layer base fabric is a flame-retardant layer composed of yarn I, the middle layer is a super absorbent layer composed of yarn II, and the innermost layer is a hydrophobic and comfortable layer composed of yarn III.

[0106] Step 4: Preparation of lightweight high-heat protective material: After the base fabric prepared in step 3 is desized, dyed, and stretched and set, the inner surface of the fabric is then brushed and then subjected to high temperature treatment, so that the thermal expansion microsphere foaming agent added to the flame retardant pre-fiber matrix expands under heat to form a multi-dimensional lightweight high-heat protective material.

[0107] In step 1, the cross-linked flame-retardant cellulose ionic liquid solution contains 15 parts of nano-sol composite smoke suppressant and flame retardant, 3 parts of cross-linking agent, and the remainder is cellulose ionic liquid solution.

[0108] In step 1, the spinning solution contains 20 parts of thermally expanding microsphere foaming agent with an average particle size of 400 nm; the remainder is a cross-linked flame-retardant cellulose ionic liquid solution.

[0109] The nano-sol composite smoke suppressant and flame retardant in step 1 contains 15 parts of bisphenol modified phosphate oligomer, 15 parts of hydroxymethylammonium phosphate, 35 parts of phosphonocyclic methoxy, 8 parts of ferrous oxalate, 15 parts of calcium phosphomolybdate, and 12 parts of dihydroxy metal composite oxide-magnesium aluminum hydroxide. The average particle size of the nano-sol composite smoke suppressant and flame retardant is 300 nm.

[0110] The crosslinking agent in step 1 contains 65 parts ammonium bicarbonate and 35 parts ammonium acetate.

[0111] In the hot drawing process described in step 1, the hot drawing temperature is 120℃ and the drawing ratio is 3.0 times.

[0112] In step 2, yarn I contains 40 parts flame-retardant pre-woven fiber, 40 parts aramid fiber, and 20 parts polyimide fiber.

[0113] The yarn II described in step 2 contains 45 parts flame-retardant superabsorbent fiber, 40 parts flame-retardant pre-fabricated fiber, and 15 parts para-aramid.

[0114] The yarn III described in step 2 contains 35 parts flame-retardant ultrafine hydrophobic fiber, 40 parts flame-retardant pre-woven fiber, 20 parts meta-aramid, and 5 parts para-aramid.

[0115] In step 2, the linear density of yarn I is 11.81 tex × 2, the linear density of yarn II is 11.81 tex × 2 tex, and the linear density of yarn III is 11.81 tex × 2.

[0116] The temperature for the steaming process in step 2 is 90℃.

[0117] The fabric structure described in step 3 is formed by interlacing the middle layer with the outer and inner layers through the methods of inner warp knotting outer weft and outer warp knotting inner weft.

[0118] The fabric described in step 3 has a warp density of 710 threads / 10cm and a weft density of 590 threads / 10cm.

[0119] The yarn arrangement ratio of the outer, middle, and inner layers of fabric in step 3 is 1:1:1.

[0120] The drying temperature for the sizing process described in step 3 is 110℃.

[0121] The base fabric mentioned in step 3 has a unit area mass of 330 g / m². 2 The unit area mass ratio of the outer, middle, and inner layers of fabric is 3:2:2.

[0122] In step 4, the abrasive skin has a mesh size of 450, a machine speed of 15 meters per minute, a grinding roller speed of 900 revolutions per minute, and a pressure of 0.3 MPa.

[0123] The high-temperature treatment in step 4 is performed at a temperature of 150°C.

[0124] Example 4

[0125] This embodiment provides a method for preparing a lightweight micro / nano porous three-dimensional high-temperature protective material, the steps of which include:

[0126] Step 1: Preparation of flame-retardant pre-fibers: First, nano-sol composite smoke suppressant and flame retardant agent and crosslinking agent are added sequentially to cellulose ionic liquid solution and stirred to obtain crosslinked flame-retardant cellulose ionic liquid solution; then, a certain proportion of thermal expansion microsphere foaming agent is added to the crosslinked flame-retardant cellulose ionic liquid solution and stirred to obtain spinning solution; then, the spinning solution is filtered and degassed sequentially and placed in a wet spinning equipment, and the spinning solution is extruded from the spinneret under a nitrogen pressure of 0.5 MPa. After solidification, hot stretching, cutting, oiling, and packaging, flame-retardant pre-fibers are obtained.

[0127] Step 2, Spinning of blended yarn: The flame-retardant pre-made fiber is mixed with high-performance flame-retardant fiber, flame-retardant super absorbent fiber and flame-retardant ultrafine hydrophobic fiber respectively. The three mixtures are then processed sequentially through oiling and humidification, premixing, cleaning and carding, drawing, roving, spinning, winding, doubling, twisting and steaming to spin yarn I, yarn II and yarn III respectively.

[0128] Step 3, Preparation of base fabric: Through fabric structure design, yarn I, yarn II and yarn III are sequentially warped, sizing, reeded, woven and repaired to obtain a multi-layer base fabric. The outermost layer of this multi-layer base fabric is a flame-retardant layer composed of yarn I, the middle layer is a super absorbent layer composed of yarn II, and the innermost layer is a hydrophobic and comfortable layer composed of yarn III.

[0129] Step 4: Preparation of lightweight high-heat protective material: After the base fabric prepared in step 3 is desized, dyed, and stretched and set, the inner surface of the fabric is then brushed and then subjected to high temperature treatment, so that the thermal expansion microsphere foaming agent added to the flame retardant pre-fiber matrix expands under heat to form a multi-dimensional lightweight high-heat protective material.

[0130] In step 1, the cross-linked flame-retardant cellulose ionic liquid solution contains 20 parts of nano-sol composite smoke-suppressing and flame-retardant agent, 5 parts of cross-linking agent, and the remainder is cellulose ionic liquid solution.

[0131] The spinning solution in step 1 contains 20 parts of thermally expanding microsphere foaming agent with an average particle size of 300 nm; the remainder is a cross-linked flame-retardant cellulose ionic liquid solution.

[0132] The nano-sol composite smoke suppressant and flame retardant in step 1 contains 10 parts of bisphenol modified phosphate oligomer, 20 parts of hydroxymethylammonium phosphate, 30 parts of phosphonocyclic methoxy, 10 parts of ferrous oxalate, 15 parts of calcium phosphomolybdate, and 15 parts of dihydroxy metal composite oxide-magnesium aluminum hydroxide. The average particle size of the nano-sol composite smoke suppressant and flame retardant is 200 nm.

[0133] The crosslinking agent in step 1 contains 55 parts ammonium bicarbonate and 45 parts ammonium acetate.

[0134] In the hot drawing process described in step 1, the hot drawing temperature is 120℃ and the drawing ratio is 2.0 times.

[0135] In step 2, yarn I contains 45 parts flame-retardant pre-woven fiber, 20 parts aramid fiber, and 35 parts polyphenylene sulfide fiber.

[0136] The yarn II described in step 2 contains 30 parts flame-retardant superabsorbent fiber, 40 parts flame-retardant pre-fabricated fiber, 25 parts meta-aramid, and 5 parts para-aramid.

[0137] The yarn III described in step 2 contains 35 parts flame-retardant ultrafine hydrophobic fiber, 40 parts flame-retardant pre-woven fiber, 20 parts meta-aramid, and 5 parts para-aramid.

[0138] In step 2, the linear density of yarn I is 15.54 tex × 2, the linear density of yarn II is 10.74 tex × 2, and the linear density of yarn III is 11.81 tex × 2.

[0139] The temperature for the steaming process in step 2 is 90℃.

[0140] The fabric structure described in step 3 is formed by interlacing the middle layer with the outer and inner layers through the methods of inner warp knotting outer weft and outer warp knotting inner weft.

[0141] The fabric described in step 3 has a warp density of 685 threads / 10cm and a weft density of 625 threads / 10cm.

[0142] The yarn arrangement ratio of the outer, middle, and inner layers of fabric in step 3 is 4:2:3.

[0143] The drying temperature for the sizing process described in step 3 is 110℃.

[0144] The base fabric mentioned in step 3 has a unit area mass of 360 g / m². 2 The unit area mass ratio of the outer, middle, and inner layers of fabric is 4:2:3.

[0145] In step 4, the abrasive skin has a mesh size of 450, the machine speed is 18 meters / minute, the grinding roller speed is 900 revolutions / minute, and the pressure is 0.4 MPa.

[0146] The high-temperature treatment in step 4 is performed at a temperature of 160°C.

[0147] Comparative Example 1

[0148] A method for preparing a three-dimensional high-heat protective material, wherein after the inner surface of the fabric is brushed in step 4, no high-temperature treatment is performed, and the rest is the same as in Example 1.

[0149] Comparative Example 2

[0150] A method for preparing a lightweight micro-nano porous three-dimensional high-temperature protective material, wherein in step 1, the mass ratio of bisphenol modified phosphate oligomer, hydroxymethyl phosphate amidourea, and phosphonocyclic methoxy is 1:2:3 in the nano-sol composite smoke suppressant and flame retardant, and other process conditions are the same as in Example 1.

[0151] Comparative Example 3

[0152] A method for preparing a lightweight micro-nano porous three-dimensional high-temperature protective material, wherein in step 1, the mass ratio of bisphenol modified phosphate oligomer, hydroxymethylammonium phosphate, phosphonocyclic methoxy, ferrous oxalate, calcium phosphomolybdate, and dihydroxy metal composite oxide-magnesium aluminum hydroxide in the nanosol composite smoke suppressant and flame retardant is 1:1:1:1:1:1, and other process conditions are the same as in Example 1.

[0153] Comparative Example 4

[0154] A method for preparing a lightweight micro-nano porous three-dimensional high-temperature protective material, wherein in step 1, the cross-linking agent in the cross-linked flame-retardant cellulose ionic liquid solution is 0 parts, and other process conditions are the same as in Example 1.

[0155] The lightweight micro-nano porous three-dimensional high-temperature protective materials prepared in Examples 1-4 and Comparative Examples 1-4 were washed 100 times in an A2 type automatic washing machine with neutral detergent according to the 4N method in GB / T 8629-2017. Their flame-retardant and heat-insulating properties were then tested according to standards GB 8965.1-2020 "Flame-retardant Protective Clothing" and GB 38453-2019 "Heat-insulating Protective Clothing". The smoke-suppressing performance (maximum specific optical density) of the protective materials was characterized according to GB / T10671-2008 "Specific Optical Density Test Method for Smoke Production of Solid Materials". The measured data for each technical indicator are shown in Table 1.

[0156] Table 1. Test results of various indicators of lightweight micro / nano porous three-dimensional high-temperature protective materials

[0157]

[0158] By comparing and analyzing the test data of the lightweight micro-nano porous three-dimensional high-temperature protective materials prepared in Example 1 and Comparative Example 1, it can be seen that when the final protective material is not subjected to high-temperature treatment, the thermally expandable material uniformly distributed in the material does not expand, resulting in a sharp decrease in the thermal protection coefficient of the protective material. The thermal protection coefficient of the protective material after thermal expansion (Example 1) is 1878 kW·s / m. 2 The thermal protection coefficient of the unexpanded protective material (Comparative Example 2) is 1189 kW·s / m. 2As can be seen, the thermal protection coefficient of the protective material can be increased by 58.7% after the final fabric is expanded by high-temperature treatment, demonstrating a significant technical advantage. Simultaneously, comparative analysis of the thermal insulation performance revealed that the protective material (Comparative Example 1) without high-temperature treatment had a convective thermal conductivity rating of B2, a radiative thermal conductivity rating of C2, and a contact thermal conductivity rating of F2. After expansion by high-temperature treatment, the protective material (Example 1) achieved a convective thermal conductivity rating of B3, a radiative thermal conductivity rating of C3, and a contact thermal conductivity rating of F3, demonstrating a clear technical advantage. Furthermore, comparative analysis of the thermal protection and insulation performance of Examples 1-4 showed a positive correlation between the technical index values ​​and the content of flame-retardant prefabricated fibers. This indicates that the flame-retardant prefabricated fibers prepared using this invention significantly improve the overall performance of the protective material without increasing technical difficulty.

[0159] By comparing and analyzing the test data of the protective materials prepared in Example 1 and Comparative Example 2, it can be seen that when no smoke-suppressing flame retardant (ferrous oxalate, calcium phosphomolybdate, and dihydroxyl metal composite oxide-magnesium aluminum hydroxide) is added to the flame retardant, the maximum specific optical density of the protective material (Comparative Example 2) after combustion is 3.42 times that of the material with added smoke-suppressing flame retardant. It is evident that this invention, through the synergistic effect of flame retardancy and smoke suppression, utilizes flame retardant principles such as coverage effect, transfer effect, free radical inhibition, and accelerated char formation to change the combustion mode, reducing smoke production by decreasing the content of combustibles, and achieving a composite smoke-suppressing and flame-retardant effect through synergistic action (Example 1).

[0160] By comparing and analyzing the flame retardant and thermal protection test data of the protective materials prepared in Example 1 and Comparative Example 3, it can be seen that when the flame retardant components are set to the same mass (Comparative Example 3), the flame retardant and thermal insulation performance of the protective material is far inferior to that of Example 1. It can be seen that there is a flame retardant synergistic effect among the components of the flame retardant, and the content also affects the flame retardant and thermal protection performance of the composite fabric.

[0161] By comparing and analyzing the test data of the protective materials prepared in Example 1 and Comparative Example 4, it can be seen that when no crosslinking agent is added to the cellulose ionic liquid solution system, the flame retardant and smoke suppression properties of the prepared protective material (Comparative Example 4) are significantly reduced after 100 washes. It can be seen that the addition of crosslinking agent (Example 1) not only makes the self-made flame retardant pre-fiber have excellent mechanical properties and good spinnability without heat expansion treatment, and theoretically there is no upper limit to the amount added, but also allows the fabric to distribute more micro-nano porous structures after subsequent high-temperature treatment, making the fabric lightweight and highly heat-protective, and can also improve the wash resistance of the material, extend the service life, and reduce the cost of use.

[0162] Principles and steps not explicitly described in this invention are all obtainable by those skilled in the art through conventional technical means, and therefore will not be elaborated upon. Obviously, those skilled in the art can make various modifications and variations to this invention without departing from its spirit and scope. Therefore, if these modifications and variations fall within the scope of the claims of this invention and their equivalents, this invention also intends to include these modifications and variations.

Claims

1. A method for preparing a lightweight micro / nano porous three-dimensional high-temperature protective material, characterized in that the steps include... include: (1) Preparation of flame-retardant pre-woven fibers: First, nano-sol composite smoke suppressant and flame retardant agent and crosslinking agent are added sequentially to a cellulose ionic liquid solution and stirred to obtain a crosslinked flame-retardant cellulose ionic liquid solution; then, a certain proportion of thermally expanding microsphere foaming agent is added to the crosslinked flame-retardant cellulose ionic liquid solution and stirred to obtain a spinning solution; then, the spinning solution is filtered and defoamed sequentially and placed in a wet spinning equipment, and the spinning solution is extruded from the spinneret under a nitrogen pressure of 0.5 MPa. After solidification, hot stretching, cutting, oiling, and packaging processes, flame-retardant pre-woven fibers are obtained; wherein, the nano-sol composite smoke suppressant and flame retardant agent and crosslinking agent are added sequentially to a cellulose ionic liquid solution and stirred to obtain a crosslinked flame-retardant cellulose ionic liquid solution; then, a certain proportion of thermally expanding microsphere foaming agent is added to the crosslinked flame-retardant cellulose ionic liquid solution and stirred to obtain a spinning solution; then, the nano-sol composite smoke suppressant and flame retardant agent and crosslinking agent are added sequentially to a cellulose ionic liquid solution and stirred to obtain a crosslinked flame-retardant cellulose ionic liquid ... The nano-sol composite smoke suppressant and flame retardant comprises a mixture of various components including bisphenol-modified phosphate oligomer, hydroxymethyl phosphate amidourea, phosphatidyl methoxy, ferrous oxalate, calcium phosphomolybdate, and dihydroxy metal composite oxide-magnesium aluminum hydroxide. The nano-sol composite smoke suppressant and flame retardant contains 10-20 parts of bisphenol-modified phosphate oligomer, 10-20 parts of hydroxymethyl phosphate amidourea, 20-35 parts of phosphatidyl methoxy, 8-15 parts of ferrous oxalate, 15-25 parts of calcium phosphomolybdate, and 8-15 parts of dihydroxy metal composite oxide-magnesium aluminum hydroxide, with an average particle size of 200 nm-300 nm. (2) Spinning of blended yarn: The flame-retardant pre-made fiber is mixed with high-performance flame-retardant fiber, flame-retardant super absorbent fiber and flame-retardant ultrafine hydrophobic fiber respectively. The three mixtures are then processed in sequence through oiling and humidification, premixing, cleaning and combing, drawing, roving, spinning, winding, doubling, twisting and steaming processes to spin yarn I, yarn II and yarn III respectively. (3) Preparation of base fabric: Through the design of fabric structure, yarn I, yarn II and yarn III are warped, sized, threaded with reed, woven and repaired in sequence to obtain multi-layer base fabric. The outer layer of the multi-layer base fabric is a flame-retardant layer composed of yarn I, the middle layer is a super absorbent layer composed of yarn II, and the inner layer is a hydrophobic and comfortable layer composed of yarn III. (4) Preparation of lightweight high-heat protective material: After the base fabric prepared in step 3 is desized, dyed and stretched and shaped, the inner surface of the base fabric is then roughened and finally treated at high temperature, so that the thermal expansion microsphere foaming agent added to the flame retardant pre-fiber matrix is ​​heated and expanded to form a multi-dimensional lightweight high-heat protective material.

2. The method for preparing a lightweight micro / nano porous three-dimensional high-temperature protective material according to claim 1, characterized in that, The cross-linked flame-retardant cellulose ionic liquid solution contains 15 to 25 parts of nano-sol composite smoke suppressant and flame retardant, 3 to 5 parts of cross-linking agent, and the remainder is cellulose ionic liquid solution.

3. The method for preparing a lightweight micro / nano porous three-dimensional high-temperature protective material according to claim 1, characterized in that, The spinning solution contains 10 to 25 parts of thermally expanding microsphere foaming agent with an average particle size of 300 nm to 400 nm; the remainder is a cross-linked flame-retardant cellulose ionic liquid solution.

4. The method for preparing a lightweight micro / nano porous three-dimensional high-temperature protective material according to claim 1, characterized in that, The crosslinking agent contains 45 to 65 parts of ammonium bicarbonate and 35 to 55 parts of ammonium acetate, with a hot stretching temperature of 110°C to 120°C and a stretching ratio of 1.5 to 3.0 times; the high-performance flame-retardant fiber includes a mixture of various fibers such as aramid fiber, polyphenylene sulfide fiber, polyimide fiber, meta-aramid fiber, and para-aramid fiber.

5. The method for preparing a lightweight micro / nano porous three-dimensional high-temperature protective material according to claim 1, characterized in that, The yarn I contains 30 to 50 parts of flame-retardant pre-woven fiber, 20 to 40 parts of aramid fiber, 25 to 45 parts of polyphenylene sulfide fiber, and 25 to 40 parts of polyimide fiber. The yarn II contains 25 to 45 parts flame-retardant superabsorbent fiber, 30 to 50 parts flame-retardant pre-woven fiber, 20 to 50 parts meta-aramid, and 5 to 15 parts para-aramid. The yarn III contains 25 to 45 parts flame-retardant ultrafine hydrophobic fiber, 30 to 50 parts flame-retardant pre-made fiber, 20 to 50 parts meta-aramid, and 5 to 15 parts para-aramid.

6. The method for preparing a lightweight micro / nano porous three-dimensional high-temperature protective material according to claim 1, characterized in that, The linear density of yarn I is 11.81tex×2 to 15.54tex×2, the linear density of yarn II is 9.84tex×2 to 11.81tex×2, and the linear density of yarn III is 11.81tex×2 to 13.12tex×2. The temperature of the steaming process is 80℃ to 100℃.

7. The method for preparing a lightweight micro / nano porous three-dimensional high-temperature protective material according to claim 1, characterized in that, The base fabric has a warp density of 660 to 710 threads / 10cm and a weft density of 575 to 625 threads / 10cm; the yarn arrangement ratio of the outer, middle, and inner base fabric layers is 1:1:1 to 4:2:3; the drying temperature for the sizing process is 100℃ to 120℃; and the unit area mass of the base fabric is 300g / m². 2 ~360g / m 2 The abrasive skin has a mesh size of 400-500, a machine speed of 12-18 m / min, a grinding roller speed of 850-950 rpm, and a pressure of 0.2-0.4 MPa; the high-temperature treatment temperature is 140-160℃.

8. A lightweight micro-nano porous three-dimensional high-temperature protective material prepared by the preparation method according to any one of claims 1-7.

Citation Information

Patent Citations

  • A method for preparing a fire-resistant and heat-insulating metallized coated fabric

    CN108221397B

  • Modacrylic fiber blended flame-retardant high-temperature-resistant antistatic fabric and preparation method thereof

    CN109208154A

  • A flame-retardant and heat-insulating fabric for fire escape emergency and its production device

    CN112221027B

  • Thermal protection fabric with multi-dimensional composite structure and preparation method of thermal protection fabric

    CN116423938A

  • Preparation method of flame-retardant cellulose fiber

    CN109208103A