Airless spraying texture water-in-water artistic coating with efficient mildew resistance and preparation method of airless spraying texture water-in-water artistic coating

By developing airless spray-textured water-in-water artistic paint, using specific formulas and processes, the existing paint has been solved in the complex construction, easy to leak sand and serious layering, and has achieved efficient and environmentally friendly construction effects and long-term anti-mold function.

CN119978867AActive Publication Date: 2025-05-13BEIXIN JIABAOLI COATINGS (GUANGDONG) CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202510109809.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-01-23
Publication Date
2025-05-13
Estimated Expiration
2045-01-23

AI Technical Summary

Technical Problem

The existing water-in-water and sand-in-water coatings have complex processes, easy sand leakage, serious layering, low construction efficiency and uneven spraying during the construction process, which is difficult to meet the needs of modern construction industries for high efficiency, energy-saving and environmental protection.

Method used

Develop an airless spray-textured water-in-water artistic paint, using a combination of color-touching base paint formula A, mildew-proof base paint formula B, continuous phase formula C and water, and through specific formula ratios and process steps, an efficient anti-mold and strong texture coating is formed.

Benefits of technology

It can create a texture of imitation stone without the need for additional sand-like paint. The construction process is simple and efficient, reducing construction difficulty and cost, and has long-term and efficient anti-mold function. It is suitable for airless spraying tools, improving construction efficiency and coating stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119978867A_ABST
    Figure CN119978867A_ABST
Patent Text Reader

Abstract

The invention relates to an airless spraying texture water-in-water art coating with efficient mildew resistance and a preparation method thereof, and relates to the technical field of coatings, and the airless spraying texture water-in-water art coating comprises a toning base paint formula A, a mildew-resistant base paint formula B, a continuous phase formula C, water and the like. The invention provides an airless spraying texture water-in-water art coating with efficient mildew resistance, and the art coating has the following characteristics: firstly, the art coating has a certain texture, can directly form a stone-like effect, and does not need additional sand-containing texture paint; secondly, the construction process is efficient, simple and convenient, and construction difficulty and time cost are reduced; meanwhile, the coating should have efficient mildew-proof performance, and it is ensured that the coating keeps attractive, healthy and environmentally friendly in the long-term use process; finally, in order to further improve the construction efficiency, the coating is suitable for an airless spraying tool, the rapid and uniform spraying effect is achieved, and the defects in the prior art are overcome.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coatings, and in particular to an airless spraying textured water-in-water art coating with high-efficiency mildew resistance and a preparation method thereof. Background Art

[0002] In the field of architectural decoration, decorative materials that pursue naturalness and beauty have always been favored. Water-in-water paint, as a paint that can simulate the texture of natural stone, has been widely used in the market in recent years. However, the construction process of traditional water-in-water paint is relatively complicated. It is usually necessary to spray water-in-water paint again on the basis of the pre-sprayed sand-containing texture paint to achieve the desired imitation stone effect. This multi-layer construction process not only increases the construction difficulty and time cost, but may also cause potential quality problems at the joints between layers.

[0003] On the other hand, although water-in-sand paint simplifies the construction process to a certain extent, it can directly form a stone-like texture because it contains sand particles, without the need for additional spraying of sand-containing texture paint. However, water-in-sand paint also has significant defects in practical applications. Due to its sand-containing characteristics, the "sand leakage" phenomenon is prone to occur during the construction process, that is, sand particles fall off from the paint, affecting the integrity and aesthetics of the coating. In addition, water-in-sand paint is also prone to stratification, which further reduces the stability and durability of the coating. At the same time, the high construction consumption also increases the material cost, limiting its wider application.

[0004] More importantly, most water-in-water and water-in-sand coatings on the market rely on special air spray tools for construction. This spraying method not only has relatively low construction efficiency, but may also affect the final effect of the coating due to uneven spraying. In the modern construction industry that pursues high efficiency, energy saving and environmental protection, this construction method obviously can no longer meet market demand.

[0005] Therefore, there is an urgent need to develop a new type of water-in-water artistic paint to meet the market demand for new, efficient and environmentally friendly building decoration materials. Summary of the invention

[0006] In order to solve the above problems, the present invention provides an airless spraying textured water-in-water art paint with high efficiency and mildew resistance and a preparation method thereof.

[0007] In a first aspect, the present invention provides an airless sprayable textured water-in-water art paint with high mildew resistance, wherein the airless sprayable textured water-in-water art paint comprises a coloring base paint formula A, a mildew-proof base paint formula B, a continuous phase formula C and water;

[0008] The toning base paint formula A comprises a toning base paint composed of a first section material, a second section material, and a third section material and a 5% lithium magnesium silicate protective colloid solution; the weight proportion of the 5% lithium magnesium silicate protective colloid solution is 23 to 28 parts, and the weight proportion of the toning base paint is 40 to 50 parts; the first section material comprises the following components in weight proportions: 29.4 to 31.5 parts of water, 0.1 to 0.3 parts of fungicide, 0.5 to 1.0 parts of antifreeze, 0.1 to 0.3 parts of defoamer, and 0.2 to 0.5 parts of dispersant; the second section material comprises the following components in weight proportions: The components in parts by weight are: 1-3 parts of titanium dioxide, 8-12 parts of calcined kaolin, 18-21 parts of heavy calcium, 0-6 parts of wood fiber, 0.7-1.1 parts of hydroxyethyl cellulose, 0-0.6 parts of hydrophobically modified hydroxyethyl cellulose, and 0.1-0.3 parts of pH regulator; the third stage material includes the following components in parts by weight: 0.1-0.3 parts of bactericide, 0.1-0.2 parts of mildewcide, 1.0-1.5 parts of film-forming aid, 20-24 parts of emulsion, 0.1-0.3 parts of defoamer, and 6-9 parts of 10% lithium magnesium silicate protective gel solution;

[0009] The mildew-proof base paint formula B comprises a mildew-proof base paint composed of the fourth section material, the fifth section material, and the sixth section material and a 5% lithium magnesium silicate protective colloid solution; the weight proportion of the 5% lithium magnesium silicate protective colloid solution is 23 to 28 parts, and the weight proportion of the mildew-proof base paint is 40 to 50 parts; the fourth section material comprises the following components in weight proportions: 27.15 to 36.85 parts of water, 0.1 to 0.3 parts of fungicide, 0.5 to 1.0 parts of antifreeze agent, 0.1 to 0.3 parts of defoamer, and 0.2 to 0.5 parts of dispersant; the The fifth stage material includes the following components in parts by weight: 5-8 parts of titanium dioxide, 13-17 parts of calcined kaolin, 0.7-1.1 parts of hydroxyethyl cellulose, 0.5-1.0 parts of hydrophobically modified hydroxyethyl cellulose, and 0.1-0.3 parts of pH regulator; the sixth stage material includes the following components in parts by weight: 0.1-0.3 parts of bactericide, 0.2-2.5 parts of mildewcide, 1.4-1.8 parts of film-forming aid, 28-35 parts of emulsion, 0.1-0.3 parts of defoamer, and 7-10 parts of 10% lithium magnesium silicate protective gel solution;

[0010] The continuous phase formula C comprises the following components in parts by weight: 30.3-30.4 parts of water, 58-62 parts of emulsion, 1-3 parts of antifreeze agent, 2-5 parts of film-forming aid, 0.2-0.5 parts of defoamer, 0.2-0.5 parts of bactericide, 0.1-0.2 parts of mildewicide, 0.1-0.2 parts of pH adjuster, and 3.8 parts of associative alkali swelling thickener diluted with water; the associative alkali swelling thickener diluted with water is composed of 0.8 parts by weight of associative alkali swelling thickener and 3 parts by weight of water.

[0011] Furthermore, the weight ratio of the tinting base paint formula A, the anti-mildew base paint formula B, the continuous phase formula C and the water is (60-65):(5-10):(20-30):(3-7).

[0012] Furthermore, the tinting base paint formula A comprises a tinting base paint composed of a first section material, a second section material, and a third section material and a 5% lithium magnesium silicate protective colloid solution; the weight of the 5% lithium magnesium silicate protective colloid solution is 25 parts, and the weight of the tinting base paint is 45 parts; the first section material comprises the following components in weight: 31.4 parts of water, 0.15 parts of fungicide, 0.8 parts of antifreeze, 0.2 parts of defoamer, and 0.3 parts of dispersant; the third section material comprises 25 parts of tinting base paint, 25 parts of tinting base paint, and 45 parts of tinting base paint. The second stage material includes the following components in parts by weight: 2 parts of titanium dioxide, 10 parts of calcined kaolin, 18 parts of heavy calcium, 3 parts of wood fiber, 0.7 parts of hydroxyethyl cellulose, 0.6 parts of hydrophobically modified hydroxyethyl cellulose, and 0.15 parts of pH regulator; the third stage material includes the following components in parts by weight: 0.2 parts of bactericide, 0.1 parts of mildewcide, 1.2 parts of film-forming aid, 22 parts of emulsion, 0.2 parts of defoamer, and 9 parts of 10% lithium magnesium silicate protective gel solution; or,

[0013] The toning base paint formula A comprises a toning base paint composed of a first section material, a second section material, and a third section material and a 5% lithium magnesium silicate protective colloid solution; the weight portion of the 5% lithium magnesium silicate protective colloid solution is 25 parts, and the weight portion of the toning base paint is 45 parts; the first section material comprises the following components in weight portions: 29.4 parts of water, 0.15 parts of fungicide, 0.8 parts of antifreeze agent, 0.2 parts of defoamer, and 0.3 parts of dispersant; the second section material The material includes the following components in parts by weight: 2 parts of titanium dioxide, 10 parts of calcined kaolin, 18 parts of heavy calcium, 6 parts of wood fiber, 0.7 parts of hydroxyethyl cellulose, 0.6 parts of hydrophobically modified hydroxyethyl cellulose, and 0.15 parts of pH regulator; the third stage material includes the following components in parts by weight: 0.2 parts of bactericide, 0.1 parts of mildewcide, 1.2 parts of film-forming aid, 22 parts of emulsion, 0.2 parts of defoamer, and 9 parts of 10% lithium magnesium silicate protective gel solution; or,

[0014] The toning base paint formula A comprises a toning base paint composed of a first section material, a second section material, and a third section material and a 5% lithium magnesium silicate protective colloid solution; the weight portion of the 5% lithium magnesium silicate protective colloid solution is 25 parts, and the weight portion of the toning base paint is 45 parts; the first section material comprises the following components in weight portions: 31.4 parts of water, 0.15 parts of fungicide, 0.8 parts of antifreeze agent, 0.2 parts of defoamer, and 0.3 parts of dispersant; the second section material The material includes the following components in parts by weight: 2 parts of titanium dioxide, 10 parts of calcined kaolin, 18 parts of heavy calcium, 3 parts of wood fiber, 0.7 parts of hydroxyethyl cellulose, 0.6 parts of hydrophobically modified hydroxyethyl cellulose, and 0.15 parts of pH regulator; the third stage material includes the following components in parts by weight: 0.2 parts of bactericide, 0.1 parts of mildewcide, 1.2 parts of film-forming aid, 22 parts of emulsion, 0.2 parts of defoamer, and 6 parts of 10% lithium magnesium silicate protective gel solution; or,

[0015] The toning base paint formula A comprises a toning base paint composed of a first section material, a second section material, and a third section material and a 5% lithium magnesium silicate protective colloid solution; the weight portion of the 5% lithium magnesium silicate protective colloid solution is 25 parts, and the weight portion of the toning base paint is 45 parts; the first section material comprises the following components in weight portions: 31.4 parts of water, 0.15 parts of fungicide, 0.8 parts of antifreeze agent, 0.2 parts of defoamer, and 0.3 parts of dispersant; the second section material The material includes the following components in parts by weight: 2 parts of titanium dioxide, 10 parts of calcined kaolin, 21 parts of heavy calcium, 0 parts of wood fiber, 0.7 parts of hydroxyethyl cellulose, 0.6 parts of hydrophobically modified hydroxyethyl cellulose, and 0.15 parts of pH regulator; the third stage material includes the following components in parts by weight: 0.2 parts of bactericide, 0.1 parts of mildewcide, 1.2 parts of film-forming aid, 22 parts of emulsion, 0.2 parts of defoamer, and 9 parts of 10% lithium magnesium silicate protective gel solution; or,

[0016] The toning base paint formula A comprises a toning base paint composed of a first section material, a second section material, and a third section material and a 5% lithium magnesium silicate protective colloid solution; the weight portion of the 5% lithium magnesium silicate protective colloid solution is 25 parts, and the weight portion of the toning base paint is 45 parts; the first section material comprises the following components in weight portions: 31.5 parts of water, 0.15 parts of fungicide, 0.8 parts of antifreeze agent, 0.2 parts of defoamer, and 0.3 parts of dispersant; the third section material comprises 25 parts of 5% lithium magnesium silicate protective colloid solution, and the weight portion of the toning base paint is 45 parts. The second stage material includes the following components in parts by weight: 2 parts of titanium dioxide, 10 parts of calcined kaolin, 18 parts of heavy calcium, 3 parts of wood fiber, 1.1 parts of hydroxyethyl cellulose, 0 parts of hydrophobically modified hydroxyethyl cellulose, and 0.15 parts of pH regulator; the third stage material includes the following components in parts by weight: 0.2 parts of bactericide, 0.2 parts of mildewcide, 1.2 parts of film-forming aid, 22 parts of emulsion, 0.2 parts of defoamer, and 9 parts of 10% lithium magnesium silicate protective gel solution.

[0017] Further, the mildew-proof base paint formula B includes a mildew-proof base paint composed of the fourth section material, the fifth section material, and the sixth section material and a 5% magnesium lithium silicate protective colloid solution; the weight proportion of the 5% magnesium lithium silicate protective colloid solution is 25 parts, and the weight proportion of the mildew-proof base paint is 45 parts; the fourth section material includes the following components in weight proportions: 34.55 parts of water, 0.15 parts of fungicide, 0.8 parts of antifreeze, 0.2 parts of defoamer, and 0.3 parts of dispersant; the fifth section material includes the following components in weight proportions: 6 parts of titanium dioxide, 15 parts of calcined kaolin, 0.8 parts of hydroxyethyl cellulose, 0.7 parts of hydrophobically modified hydroxyethyl cellulose, and 0.2 parts of pH regulator; the sixth section material includes the following components in weight proportions: 0.2 parts of fungicide, 2.5 parts of mildew-proof agent, 1.4 parts of film-forming aid, 28 parts of emulsion, 0.2 parts of defoamer, and 9 parts of 10% magnesium lithium silicate protective colloid solution; or,

[0018] The mildew-proof base paint formula B comprises a mildew-proof base paint composed of the fourth section material, the fifth section material, and the sixth section material and a 5% lithium magnesium silicate protective colloid solution; the weight proportion of the 5% lithium magnesium silicate protective colloid solution is 25 parts, and the weight proportion of the mildew-proof base paint is 45 parts; the fourth section material comprises the following components in weight proportions: 27.15 parts of water, 0.15 parts of fungicide, 0.8 parts of antifreeze agent, 0.2 parts of defoamer, and 0.3 parts of dispersant; the fifth section material comprises the following components in weight proportions: 6 parts of titanium dioxide, 15 parts of calcined kaolin, 0.8 parts of hydroxyethyl cellulose, 0.7 parts of hydrophobically modified hydroxyethyl cellulose, and 0.2 parts of pH regulator; the sixth section material comprises the following components in weight proportions: 0.2 parts of fungicide, 2.5 parts of mildew-proof agent, 1.8 parts of film-forming aid, 35 parts of emulsion, 0.2 parts of defoamer, and 9 parts of 10% lithium magnesium silicate protective colloid solution; or,

[0019] The mildew-proof base paint formula B includes a mildew-proof base paint composed of a fourth section material, a fifth section material, and a sixth section material and a 5% lithium magnesium silicate protective colloid solution; the weight proportion of the 5% lithium magnesium silicate protective colloid solution is 25 parts, and the weight proportion of the mildew-proof base paint is 45 parts; the fourth section material includes the following components in weight proportions: 36.85 parts of water, 0.15 parts of a fungicide, 0.8 parts of an antifreeze agent, 0.2 parts of a defoamer, and 0.3 parts of a dispersant; the fifth section material includes the following components in weight proportions: 6 parts of titanium dioxide, 15 parts of calcined kaolin, 0.8 parts of hydroxyethyl cellulose, 0.7 parts of hydrophobically modified hydroxyethyl cellulose, and 0.2 parts of a pH regulator; the sixth section material includes the following components in weight proportions: 0.2 parts of a fungicide, 0.2 parts of a mildew-proof agent, 1.4 parts of a film-forming aid, 28 parts of an emulsion, 0.2 parts of a defoamer, and 9 parts of a 10% lithium magnesium silicate protective colloid solution.

[0020] Further, the continuous phase formula C comprises the following components in parts by weight: 30.4 parts of water, 60 parts of emulsion, 2 parts of antifreeze agent, 3 parts of film-forming aid, 0.3 parts of defoamer, 0.3 parts of bactericide, 0.1 parts of mildewcide, 0.1 parts of pH adjuster, 3.8 parts of associative alkali swelling thickener diluted with water; the associative alkali swelling thickener diluted with water is composed of 0.8 parts by weight of associative alkali swelling thickener and 3 parts by weight of water; or,

[0021] The continuous phase formula C comprises the following components in parts by weight: 30.3 parts of water, 60 parts of emulsion, 2 parts of antifreeze agent, 3 parts of film-forming aid, 0.3 parts of defoamer, 0.3 parts of bactericide, 0.2 parts of mildewcide, 0.1 parts of pH adjuster, and 3.8 parts of associative alkali swelling thickener diluted with water; the associative alkali swelling thickener diluted with water is composed of 0.8 parts by weight of associative alkali swelling thickener and 3 parts by weight of water.

[0022] In a second aspect, the present invention provides a method for preparing the airless sprayable textured water-in-water art paint with high-efficiency mildew resistance as described in any one of the first aspects, the preparation method comprising the following steps:

[0023] Preparing a tinted base paint formula A;

[0024] Preparing mildew-proof base paint formula B;

[0025] Prepare continuous phase formulation C;

[0026] The color-adjusting base paint formula A, the anti-mildew base paint formula B, the continuous phase formula C and the water are mixed to obtain the airless spray textured water-in-water art paint.

[0027] Further, the step of preparing the toning base paint formula A comprises the following process:

[0028] 1) Stir the water, dispersant, defoamer, bactericide and antifreeze in the first stage at 300 r / min for 3 minutes to mix well.

[0029] 2) Weigh the second stage powder, add titanium dioxide and calcined kaolin slowly one by one, mix for 3 minutes, then slowly add hydroxyethyl cellulose and hydrophobically modified hydroxyethyl cellulose and stir for 3 minutes, then slowly add pH adjuster, adjust the speed to 1500r / min appropriately, and disperse for 25 minutes.

[0030] 3) Reduce the speed to 1000r / min, gradually add bactericide, mildewproof agent, film-forming aid, add emulsion and defoamer after mixing, stir for 5 minutes, then add 10% concentration of protective glue solution, speed 1500r / min, stir and mix for 15 minutes before discharging

[0031] 4) Granulation stage: Weigh 25 parts by weight of a 5% concentration protective glue solution into a dispersion tank, weigh 45 parts by weight of a tinting base paint A and add it to the protective glue solution, pre-cut and granulate on a disperser, the speed is gradually increased from 300 r / min by 200 r / min, and the gradient stirring time is 3 min.

[0032] Furthermore, the step of preparing the mildew-proof base paint formula B comprises the following process:

[0033] 1) Stir the water, dispersant, defoamer, bactericide and antifreeze in the first stage at 300 r / min for 3 minutes to mix well.

[0034] 2) Weigh the second stage powder, titanium dioxide, calcined kaolin, heavy calcium and wood fiber, slowly add them one by one, mix for 3 minutes, then slowly add hydroxyethyl cellulose and hydrophobically modified hydroxyethyl cellulose and stir for 3 minutes, then slowly add pH regulator, adjust the speed to 1800r / min appropriately, and disperse for 25 minutes.

[0035] 3) Reduce the speed to 1000r / min, gradually add bactericide, mildewproof agent, film-forming aid, add emulsion and defoamer after mixing, stir for 5 minutes, then add 10% concentration of protective glue solution, speed 1500r / min, stir and mix for 15 minutes before discharging

[0036] 4) Granulation stage: Weigh 25 parts by weight of a 5% concentration protective glue solution into a dispersion tank, weigh 45 parts by weight of a tinting base paint A and add it to the protective glue solution, pre-cut and granulate on a disperser, the speed is gradually increased from 300 r / min by 200 r / min, and the gradient stirring time is 3 min.

[0037] Further, the step of preparing the continuous phase formula C comprises the following process:

[0038] Add most of the water to the dispersion tank, with a speed of 250r / min, first add the emulsion, stir and disperse at low speed for 5 minutes, then add the antifreeze agent, film-forming aid, defoaming agent, stir for 10 minutes, then add the bactericide, mildewproof agent and pH adjuster in turn, stir at low speed for 5 minutes, and finally slowly add the associative alkali swelling thickener solution diluted with water, stir and disperse for 10 minutes.

[0039] The above technical solution provided by the embodiment of the present invention has at least the following advantages compared with the prior art:

[0040] The embodiment of the present invention provides an airless spray textured water-in-water art paint with high efficiency and mildew resistance. The paint has the following characteristics: first, it should have a certain texture and can directly form a stone-like effect without the need for additional sand-containing textured paint; second, the construction process should be efficient and simple to reduce the construction difficulty and time cost; at the same time, the paint should have high efficiency and mildew resistance to ensure that the coating remains beautiful and healthy and environmentally friendly during long-term use; finally, in order to further improve the construction efficiency, the paint should be suitable for airless spray tools to achieve a fast and uniform spraying effect. Specifically:

[0041] 1) The present invention obtains a water-in-water artistic paint with a stone-like texture;

[0042] 2) The artistic coating provided by the present invention has the characteristics of high efficiency, convenient construction and low consumption;

[0043] 3) The artistic coating provided by the present invention has a long-term and efficient anti-mildew function;

[0044] 4) The artistic paint provided by the present invention can obtain various effects by using different spraying tools and air pressure, "one product with multiple effects":

[0045] How to obtain the water-in-water effect of stone imitation in the present invention, and at the same time have the characteristics of high efficiency, simplicity and low consumption in construction:

[0046] To obtain a good water-in-water imitation stone effect, it is necessary to spray out an obvious uneven surface structure to obtain texture. Therefore, it is necessary to reduce the deformation of the color dots during the entire spraying process, enhance the ability to resist deformation, and reduce the volume change of the paint film drying shrinkage to obtain an uneven surface structure and better texture. The following two points are mainly used to design color dots with better toughness. The first point is to use hydrophobic modified hydroxyethyl cellulose and hydroxyethyl cellulose. Choosing a suitable combination of lithium magnesium silicate and cellulose can obtain color dots with stronger toughness and increase its dosage, so that the reaction "gel" is more complete. The hydrophobic modified hydroxyethyl cellulose and lithium magnesium silicate form a "gel" and also associate with the emulsion, making the formed three-dimensional network structure more firm and complete, and enhancing the ability to resist pressure. The second point is to use wood fiber + high-content powder. Wood fiber is similar to the role of "rebar". High-content powder makes the color dots stronger, thus resisting the high pressure of airless spraying, so that the color dots have good integrity and low deformation during the spraying process. In addition, wood fiber plays a skeleton role in the film-forming process. At the same time, more powder synergistically fills the strength (similar to the role of "coarse aggregate") and increases the volume solid content, so that the volume change of the color dots after shrinkage during the drying process of the paint film is reduced, making the texture strong and meeting the demand for better texture with low consumption.

[0047] How the present invention achieves long-term and efficient mildew-proof function:

[0048] By designing a base paint with a high mildewproofing agent content, the particle size is controlled to be very small during granulation, so that it can be evenly present in the paint film as a minimal white color point of the base paint, and the paint film can play the role of a mildewproofing agent warehouse. A certain stacking density is required to release the mildewproofing agent in time to exert the mildewproofing function. Specifically, the emulsion content is high, the mildewproofing agent content is relatively high, and a "microcapsule" structure is formed after drying. The degree of encapsulation of the mildewproofing agent by the emulsion and powder can be used to control the ease and duration of the mildewproofing agent release, thereby achieving the effect of sustained release of the mildewproofing agent and obtaining long-term and efficient mildewproofing function.

[0049] How to achieve various effects with different spraying tools, "one product with multiple effects"

[0050] When using airless spraying, the principle is to extrude the material so that the material coming out of the nozzle is all water-in-water paint, so the substrate can be fully covered. When the discharge pressure is low, the color dots can resist the extrusion damage caused by the pressure through their own strength and toughness. At the same time, the force of contact with the substrate is small, which can well maintain its own uniform three-dimensional "rounded" shape, with small deformation, and obtain a better texture. Moreover, the color dots are about the same size as the paint can, maintaining consistent and clear color dots. When the air pressure is increased, the color dots that appear will be broken due to the high pressure and will be smaller when they come out of the nozzle. In addition, the force of contact with the substrate will also be greater, which will cause a slightly larger deformation, weaken the three-dimensional sense, and weaken the texture presented. When the product is diluted with water for construction, because the viscosity is reduced, the same unit discharge mass can be obtained at a lower air pressure, but the toughness of the color dots in the product remains unchanged, and the force of contact with the substrate is reduced, so the color dots are deformed less, and a more obvious three-dimensional sense or texture can be obtained. Therefore, customers can obtain various effects by changing the construction process, with a large operating space, and achieve "one product with multiple effects". BRIEF DESCRIPTION OF THE DRAWINGS

[0051] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.

[0052] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0053] Figure 1 This is a rendering of an airless spray textured water-in-water art paint with high efficiency and mildew resistance provided in Example 1 of the present invention.

[0054] Figure 2This is a picture showing the effect of a highly effective and mildew-proof airless spray textured water-in-water art paint provided in Example 1 of the present invention being stored at room temperature for 30 days without color bleeding.

[0055] Figure 3 This is a picture showing the effect of a highly effective and mildew-proof airless sprayable textured water-in-water art paint stored at 50°C for 30 days without color bleeding, as provided in Example 1 of the present invention.

[0056] Figure 4 This is a can opening state diagram of an airless spray textured water-in-water art paint with high mildew resistance provided in Example 1 of the present invention after being stored at 50°C for 30 days. DETAILED DESCRIPTION

[0057] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0058] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0059] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are intended only to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples that do not specify specific conditions are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.

[0060] The raw materials used in the examples and comparative examples in the experiment are as follows:

[0061] The antifreeze agent is preferably ethylene glycol;

[0062] The hydroxyethyl cellulose used was Ashland 250HHBR;

[0063] The hydrophobically modified hydroxyethyl cellulose used was Ashland HE10K;

[0064] The wood fiber used is BE600-30PU from Guangdong Longhu Technology Co., Ltd.;

[0065] The dispersant used was Arkema’s P30;

[0066] The titanium dioxide used was SR-237 from Shandong Dongjia Group Co., Ltd.;

[0067] The calcined kaolin used was DB80 from Sanfeng Chemical;

[0068] The heavy calcium powder used is ultrafine calcium carbonate CC918 produced by Guangxi Hezhou Kelong Powder Co., Ltd.;

[0069] The preferred pH adjuster is Dow's AMP-95;

[0070] The base paint emulsion chosen is RS-2788 from Badford;

[0071] The continuous phase emulsion selected was POLYSOL AP-4765 from Shanghai Showa Polymer Co., Ltd.;

[0072] The lithium magnesium silicate used is Hemmings 482;

[0073] The preferred defoamer is NXZ from Nopco;

[0074] The preferred film-forming aid is LOCA DA from Shengxingxing;

[0075] The preferred fungicide is Thor's ACTICIDE MBS 5050;

[0076] The preferred preservative is Troy's PW40;

[0077] The associative alkali swelling thickener selected is Dow's TT-935.

[0078] The relationship between the component dosages of the artistic coatings provided in Examples 1 to 2 and Comparative Examples 1 to 4 is shown in Table 1, Table 2, Table 3 and Table 4.

[0079] Table 1 Ratio of raw materials in the color base paint formula A

[0080]

[0081]

[0082] Table 2 Ratio of raw materials in formula B of anti-mildew base paint

[0083]

[0084] Table 3 Ratio of raw materials in continuous phase C

[0085]

[0086]

[0087] Table 4

[0088]

[0089] Table 5 10% lithium magnesium silicate protective gel solution formula composition

[0090] Components Weight percentage (%) water 89.7 Fungicides 0.3 Hemmings 482 10 Total 100

[0091] Table 6 5% lithium magnesium silicate protective gel solution formula composition table

[0092] Components Weight percentage (%) water 94.7 Fungicides 0.3 Hemmings 482 5 Total 100

[0093] The preparation method of the above-mentioned airless spray textured water-in-water art paint with high efficiency and mildew resistance comprises the following steps:

[0094] Production process of color base paint A:

[0095] 1) Stir the water, dispersant, defoamer, bactericide and antifreeze in the first stage at 300 r / min for 3 minutes to mix well.

[0096] 2) Weigh the second stage powder, add titanium dioxide and calcined kaolin slowly one by one, mix for 3 minutes, then slowly add hydroxyethyl cellulose and hydrophobically modified hydroxyethyl cellulose and stir for 3 minutes, then slowly add pH adjuster, adjust the speed to 1500r / min appropriately, and disperse for 25 minutes.

[0097] 3) Reduce the speed to 1000r / min, gradually add bactericide, mildewproof agent, film-forming aid, add emulsion and defoamer after mixing, stir for 5 minutes, then add 10% concentration of protective glue solution, speed 1500r / min, stir and mix for 15 minutes before discharging

[0098] Granulation stage: weigh 25 parts by weight of 5% concentration protective glue solution into a dispersion tank, weigh 45 parts by weight of color base paint A and add it to the protective glue solution, pre-cut and put it on a disperser for granulation, the speed is gradually increased from 300r / min by 200 speeds, the gradient stirring time is 3 minutes, and the size of the color dots is observed until it meets the requirements.

[0099] Production process of mold inhibitor "microcapsule" base paint formula B:

[0100] 1) Stir the water, dispersant, defoamer, bactericide and antifreeze in the first stage at 300 r / min for 3 minutes to mix well.

[0101] 2) Weigh the second stage powder, titanium dioxide, calcined kaolin, heavy calcium and wood fiber, slowly add them one by one, mix for 3 minutes, then slowly add hydroxyethyl cellulose and hydrophobically modified hydroxyethyl cellulose and stir for 3 minutes, then slowly add pH regulator, adjust the speed to 1800r / min appropriately, and disperse for 25 minutes.

[0102] 3) Reduce the speed to 1000r / min, gradually add bactericide, mildewproof agent, film-forming aid, add emulsion and defoamer after mixing, stir for 5 minutes, then add 10% concentration of protective glue solution, speed 1500r / min, stir and mix for 15 minutes before discharging

[0103] Granulation stage: weigh 25 parts by weight of 5% concentration protective glue solution into a dispersion tank, weigh 45 parts by weight of color base paint A and add it to the protective glue solution, pre-cut and put it on a disperser for granulation, the speed is gradually increased from 300r / min by 200 speeds, the gradient stirring time is 3 minutes, and the size of the color dots is observed until it meets the requirements.

[0104] Production process of continuous phase C:

[0105] Add most of the water to the dispersion tank, with a speed of 250r / min, first add the emulsion, stir and disperse at low speed for 5 minutes, then add the antifreeze agent, film-forming aid, defoaming agent, stir for 10 minutes, then add the bactericide, mildewproof agent and pH adjuster in turn, stir at low speed for 5 minutes, finally slowly add the associative alkali swelling thickener solution diluted with water (diluted with water at a ratio of 1:3), stir and disperse for 10 minutes.

[0106] The production process of the finished product formula is:

[0107] First add the granulated color base paint A and mildew-proof base paint B into the dispersion tank, rotate at 250r / min, slowly add the continuous phase C and water, and mix for 10 minutes.

[0108] Test Case

[0109] This example tests the performance of the artistic coatings provided in the embodiments and comparative examples.

[0110] Test method:

[0111] 1) Viscosity: After the product is produced, observe the temperature and test the viscosity in time.

[0112] 2) Color penetration: spray a certain amount of water-in-water paint on a certain area of ​​blue substrate and observe whether the color of the substrate is clear.

[0113] 3) Storage stability: For heat storage stability, place it in a 50℃ oven for 30 days, observe the viscosity change, construction status and paint film condition before and after heat storage, and pass if there is no abnormality. For freeze-thaw stability, place it in a -7℃ constant temperature box, take it out after 18 hours and place it at room temperature, and place it in a -7℃ constant temperature and humidity box after 6 hours. After three cycles, stir it to make it flowable, observe the construction status and paint film condition before and after freeze-thaw, and pass if there is no abnormality.

[0114] 4) Color dot toughness, adjust the product viscosity to be consistent, use air spray, control the spray gun distance and air pressure, spray the same quality of water-in-water paint, and observe the color dot size and texture comparison after drying

[0115] 5) Anti-mildew performance test: spray a certain mass of water-in-water paint on the calcium silicate board twice, cure it at room temperature for 7 days, and then place it in a curing box with a humidity of 80% and a temperature of 30°C. Observe the board's performance in the first month, the second month, the third month, the fourth month, the fifth month, and the sixth month to see if there is mold growth.

[0116] The test results are shown in Table 7 below.

[0117] Table 7

[0118]

[0119] Compared with Example 1:

[0120] Example 2: The amount of wood fiber is higher, the physical cross-linking is more sufficient, and the pressure resistance is higher, so the deformation is smaller and the texture is stronger;

[0121] Comparative Example 1: The amount of protective glue used is insufficient, and the degree of "gelation" formed with cellulose is insufficient, resulting in a low density of the three-dimensional network structure, which makes the color point toughness poor;

[0122] Comparative Example 2: Wood fiber can form a macroscopic rigid three-dimensional network structure in the color dots, and obtain good resistance to pressure deformation. In Comparative Example 2, no wood fiber is added, resulting in poor toughness of the color dots;

[0123] Comparative Example 3: The emulsion content in the mildew-proof base paint is too high, and the mildew-proof agent is too densely wrapped, resulting in untimely release of the mildew-proof agent, resulting in the presence of spot mold;

[0124] Comparative Example 4: Only hydroxyethyl cellulose was used. The product had insufficient high shear resistance under high pressure, which made the colored dots easily broken. Although the overall antifungal agent content was consistent with that in Example 1, the antifungal performance was not as durable as that in Example 1 because the antifungal agent in Comparative Example 4 was more easily consumed and lost.

[0125] In addition, the effect diagram of an airless spray textured water-in-water art paint with high mildew resistance provided in Example 1 of the present invention is as follows: Figure 1 As shown, the effect of no color bleeding after 30 days of storage at room temperature is as follows Figure 2 As shown, the effect of no color bleeding after 30 days storage at 50℃ is as follows Figure 3 As shown, the state of the opened can after storage at 50℃ for 30 days is as follows Figure 4 shown.

[0126] The foregoing is merely a specific embodiment of the present invention, which enables those skilled in the art to understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features claimed herein.

Claims

1. An airless sprayable textured water-in-water art paint with high mildew resistance, characterized in that: The airless spray textured water-in-water art paint comprises a color-adjusting base paint formula A, an anti-mildew base paint formula B, a continuous phase formula C and water; The color-adjusting base paint formula A comprises a color-adjusting base paint composed of a first-stage material, a second-stage material, and a third-stage material, and a 5% lithium magnesium silicate protective glue solution; The weight proportion of the 5% lithium magnesium silicate protective gel solution is 23-28 parts, and the weight proportion of the toning base paint is 40-50 parts; the first section material includes the following components in weight proportions: 29.4-31.5 parts of water, 0.1-0.3 parts of fungicide, 0.5-1.0 parts of antifreeze, 0.1-0.3 parts of defoamer, and 0.2-0.5 parts of dispersant; the second section material includes the following components in weight proportions: 1-3 parts of titanium dioxide, 8-12 parts of calcined kaolin, and 10-20 parts of molten iron. 1-0.6 parts of cellulose, 0.7-1.1 parts of hydroxyethyl cellulose, 0.1-0.6 parts of hydrophobically modified hydroxyethyl cellulose, and 0.1-0.3 parts of pH regulator; the third stage material includes the following components in parts by weight: 0.1-0.3 parts of bactericide, 0.1-0.2 parts of mildewcide, 1.0-1.5 parts of film-forming aid, 20-24 parts of emulsion, 0.1-0.3 parts of defoamer, and 6-9 parts of 10% lithium magnesium silicate protective gel solution; The mildew-proof base paint formula B comprises a mildew-proof base paint composed of the fourth section material, the fifth section material, and the sixth section material and a 5% lithium magnesium silicate protective colloid solution; the weight proportion of the 5% lithium magnesium silicate protective colloid solution is 23 to 28 parts, and the weight proportion of the mildew-proof base paint is 40 to 50 parts; the fourth section material comprises the following components in weight proportions: 27.15 to 36.85 parts of water, 0.1 to 0.3 parts of fungicide, 0.5 to 1.0 parts of antifreeze agent, 0.1 to 0.3 parts of defoamer, and 0.2 to 0.5 parts of dispersant; the The fifth stage material includes the following components in parts by weight: 5-8 parts of titanium dioxide, 13-17 parts of calcined kaolin, 0.7-1.1 parts of hydroxyethyl cellulose, 0.5-1.0 parts of hydrophobically modified hydroxyethyl cellulose, and 0.1-0.3 parts of pH regulator; the sixth stage material includes the following components in parts by weight: 0.1-0.3 parts of bactericide, 0.2-2.5 parts of mildewcide, 1.4-1.8 parts of film-forming aid, 28-35 parts of emulsion, 0.1-0.3 parts of defoamer, and 7-10 parts of 10% lithium magnesium silicate protective gel solution; The continuous phase formula C comprises the following components in parts by weight: 30.3-30.4 parts of water, 58-62 parts of emulsion, 1-3 parts of antifreeze agent, 2-5 parts of film-forming aid, 0.2-0.5 parts of defoamer, 0.2-0.5 parts of bactericide, 0.1-0.2 parts of mildewicide, 0.1-0.2 parts of pH adjuster, and 3.8 parts of associative alkali swelling thickener diluted with water; the associative alkali swelling thickener diluted with water is composed of 0.8 parts by weight of associative alkali swelling thickener and 3 parts by weight of water.

2. The airless sprayable textured water-in-water art paint with high mildew resistance according to claim 1 is characterized in that: The weight ratio of the color-adjusting base paint formula A, the anti-mildew base paint formula B, the continuous phase formula C and the water is (60-65):(5-10):(20-30):(3-7).

3. The airless sprayable textured water-in-water art paint with high mildew resistance according to claim 1 is characterized in that: The color-adjusting base paint formula A comprises a color-adjusting base paint composed of a first-stage material, a second-stage material, and a third-stage material, and a 5% lithium magnesium silicate protective glue solution; The weight proportion of the 5% lithium magnesium silicate protective colloid solution is 25 parts, and the weight proportion of the toning base paint is 45 parts; the first section material includes the following components in weight proportions: 31.4 parts of water, 0.15 parts of fungicide, 0.8 parts of antifreeze, 0.2 parts of defoamer, and 0.3 parts of dispersant; the second section material includes the following components in weight proportions: 2 parts of titanium dioxide, 10 parts of calcined kaolin, 18 parts of heavy calcium, 3 parts of wood fiber, 0.7 parts of hydroxyethyl cellulose, 0.6 parts of hydrophobically modified hydroxyethyl cellulose, and 0.15 parts of pH regulator; the third section material includes the following components in weight proportions: 0.2 parts of fungicide, 0.1 parts of mildewcide, 1.2 parts of film-forming aid, 22 parts of emulsion, 0.2 parts of defoamer, and 9 parts of 10% lithium magnesium silicate protective colloid solution; or, The color-adjusting base paint formula A comprises a color-adjusting base paint composed of a first-stage material, a second-stage material, and a third-stage material, and a 5% lithium magnesium silicate protective glue solution; The weight proportion of the 5% lithium magnesium silicate protective colloid solution is 25 parts, and the weight proportion of the toning base paint is 45 parts; the first section material includes the following components in weight proportions: 29.4 parts of water, 0.15 parts of fungicide, 0.8 parts of antifreeze, 0.2 parts of defoamer, and 0.3 parts of dispersant; the second section material includes the following components in weight proportions: 2 parts of titanium dioxide, 10 parts of calcined kaolin, 18 parts of heavy calcium, 6 parts of wood fiber, 0.7 parts of hydroxyethyl cellulose, 0.6 parts of hydrophobically modified hydroxyethyl cellulose, and 0.15 parts of pH regulator; the third section material includes the following components in weight proportions: 0.2 parts of fungicide, 0.1 parts of mildewcide, 1.2 parts of film-forming aid, 22 parts of emulsion, 0.2 parts of defoamer, and 9 parts of 10% lithium magnesium silicate protective colloid solution; or, The color-adjusting base paint formula A comprises a color-adjusting base paint composed of a first-stage material, a second-stage material, and a third-stage material, and a 5% lithium magnesium silicate protective glue solution; The weight proportion of the 5% lithium magnesium silicate protective colloid solution is 25 parts, and the weight proportion of the toning base paint is 45 parts; the first section material includes the following components in weight proportions: 31.4 parts of water, 0.15 parts of fungicide, 0.8 parts of antifreeze, 0.2 parts of defoamer, and 0.3 parts of dispersant; the second section material includes the following components in weight proportions: 2 parts of titanium dioxide, 10 parts of calcined kaolin, 18 parts of heavy calcium, 3 parts of wood fiber, 0.7 parts of hydroxyethyl cellulose, 0.6 parts of hydrophobically modified hydroxyethyl cellulose, and 0.15 parts of pH regulator; the third section material includes the following components in weight proportions: 0.2 parts of fungicide, 0.1 parts of mildewcide, 1.2 parts of film-forming aid, 22 parts of emulsion, 0.2 parts of defoamer, and 6 parts of 10% lithium magnesium silicate protective colloid solution; or, The color-adjusting base paint formula A comprises a color-adjusting base paint composed of a first-stage material, a second-stage material, and a third-stage material, and a 5% lithium magnesium silicate protective glue solution; The weight proportion of the 5% lithium magnesium silicate protective colloid solution is 25 parts, and the weight proportion of the toning base paint is 45 parts; the first section material includes the following components in weight proportions: 31.4 parts of water, 0.15 parts of fungicide, 0.8 parts of antifreeze, 0.2 parts of defoamer, and 0.3 parts of dispersant; the second section material includes the following components in weight proportions: 2 parts of titanium dioxide, 10 parts of calcined kaolin, 21 parts of heavy calcium, 0 parts of wood fiber, 0.7 parts of hydroxyethyl cellulose, 0.6 parts of hydrophobically modified hydroxyethyl cellulose, and 0.15 parts of pH regulator; the third section material includes the following components in weight proportions: 0.2 parts of fungicide, 0.1 parts of mildewcide, 1.2 parts of film-forming aid, 22 parts of emulsion, 0.2 parts of defoamer, and 9 parts of 10% lithium magnesium silicate protective colloid solution; or, The color-adjusting base paint formula A comprises a color-adjusting base paint composed of a first-stage material, a second-stage material, and a third-stage material, and a 5% lithium magnesium silicate protective glue solution; The weight proportion of the 5% lithium magnesium silicate protective colloid solution is 25 parts, and the weight proportion of the toning base paint is 45 parts; the first section material includes the following components in weight proportions: 31.5 parts of water, 0.15 parts of fungicide, 0.8 parts of antifreeze agent, 0.2 parts of defoamer, and 0.3 parts of dispersant; the second section material includes the following components in weight proportions: 2 parts of titanium dioxide, 10 parts of calcined kaolin, 18 parts of heavy calcium, 3 parts of wood fiber, 1.1 parts of hydroxyethyl cellulose, 0 parts of hydrophobically modified hydroxyethyl cellulose, and 0.15 parts of pH regulator; the third section material includes the following components in weight proportions: 0.2 parts of fungicide, 0.2 parts of mildewcide, 1.2 parts of film-forming aid, 22 parts of emulsion, 0.2 parts of defoamer, and 9 parts of 10% lithium magnesium silicate protective colloid solution.

4. The airless sprayable textured water-in-water art paint with high mildew resistance according to claim 1 is characterized in that: The mildew-proof base paint formula B comprises a mildew-proof base paint composed of the fourth section material, the fifth section material, and the sixth section material and a 5% lithium magnesium silicate protective colloid solution; the weight proportion of the 5% lithium magnesium silicate protective colloid solution is 25 parts, and the weight proportion of the mildew-proof base paint is 45 parts; the fourth section material comprises the following components in weight proportions: 34.55 parts of water, 0.15 parts of fungicide, 0.8 parts of antifreeze agent, 0.2 parts of defoamer, and 0.3 parts of dispersant; the fifth section material comprises the following components in weight proportions: 6 parts of titanium dioxide, 15 parts of calcined kaolin, 0.8 parts of hydroxyethyl cellulose, 0.7 parts of hydrophobically modified hydroxyethyl cellulose, and 0.2 parts of pH regulator; the sixth section material comprises the following components in weight proportions: 0.2 parts of fungicide, 2.5 parts of mildew-proof agent, 1.4 parts of film-forming aid, 28 parts of emulsion, 0.2 parts of defoamer, and 9 parts of 10% lithium magnesium silicate protective colloid solution; or, The mildew-proof base paint formula B comprises a mildew-proof base paint composed of the fourth section material, the fifth section material, and the sixth section material and a 5% lithium magnesium silicate protective colloid solution; the weight proportion of the 5% lithium magnesium silicate protective colloid solution is 25 parts, and the weight proportion of the mildew-proof base paint is 45 parts; the fourth section material comprises the following components in weight proportions: 27.15 parts of water, 0.15 parts of fungicide, 0.8 parts of antifreeze agent, 0.2 parts of defoamer, and 0.3 parts of dispersant; the fifth section material comprises the following components in weight proportions: 6 parts of titanium dioxide, 15 parts of calcined kaolin, 0.8 parts of hydroxyethyl cellulose, 0.7 parts of hydrophobically modified hydroxyethyl cellulose, and 0.2 parts of pH regulator; the sixth section material comprises the following components in weight proportions: 0.2 parts of fungicide, 2.5 parts of mildew-proof agent, 1.8 parts of film-forming aid, 35 parts of emulsion, 0.2 parts of defoamer, and 9 parts of 10% lithium magnesium silicate protective colloid solution; or, The mildew-proof base paint formula B includes a mildew-proof base paint composed of a fourth section material, a fifth section material, and a sixth section material and a 5% lithium magnesium silicate protective colloid solution; the weight proportion of the 5% lithium magnesium silicate protective colloid solution is 25 parts, and the weight proportion of the mildew-proof base paint is 45 parts; the fourth section material includes the following components in weight proportions: 36.85 parts of water, 0.15 parts of a fungicide, 0.8 parts of an antifreeze agent, 0.2 parts of a defoamer, and 0.3 parts of a dispersant; the fifth section material includes the following components in weight proportions: 6 parts of titanium dioxide, 15 parts of calcined kaolin, 0.8 parts of hydroxyethyl cellulose, 0.7 parts of hydrophobically modified hydroxyethyl cellulose, and 0.2 parts of a pH regulator; the sixth section material includes the following components in weight proportions: 0.2 parts of a fungicide, 0.2 parts of a mildew-proof agent, 1.4 parts of a film-forming aid, 28 parts of an emulsion, 0.2 parts of a defoamer, and 9 parts of a 10% lithium magnesium silicate protective colloid solution.

5. The airless sprayable textured water-in-water art paint with high mildew resistance according to claim 1, characterized in that: The continuous phase formula C comprises the following components in parts by weight: 30.4 parts of water, 60 parts of emulsion, 2 parts of antifreeze agent, 3 parts of film-forming aid, 0.3 parts of defoamer, 0.3 parts of bactericide, 0.1 parts of mildewcide, 0.1 parts of pH adjuster, 3.8 parts of associative alkali swelling thickener diluted with water; the associative alkali swelling thickener diluted with water is composed of 0.8 parts by weight of associative alkali swelling thickener and 3 parts by weight of water; or, The continuous phase formula C comprises the following components in parts by weight: 30.3 parts of water, 60 parts of emulsion, 2 parts of antifreeze agent, 3 parts of film-forming aid, 0.3 parts of defoamer, 0.3 parts of bactericide, 0.2 parts of mildewcide, 0.1 parts of pH adjuster, and 3.8 parts of associative alkali swelling thickener diluted with water; the associative alkali swelling thickener diluted with water is composed of 0.8 parts by weight of associative alkali swelling thickener and 3 parts by weight of water.

6. A method for preparing the highly effective mildew-proof airless sprayable textured water-in-water art paint according to any one of claims 1 to 5, characterized in that: The preparation method comprises the following steps: Preparing a tinted base paint formula A; Preparing mildew-proof base paint formula B; Prepare continuous phase formulation C; The color-adjusting base paint formula A, the anti-mildew base paint formula B, the continuous phase formula C and the water are mixed to obtain the airless spray textured water-in-water art paint.

7. The method for preparing the airless sprayable textured water-in-water art paint with high efficiency and mildew resistance according to claim 6, characterized in that: The steps of preparing the tinted base paint formula A include the following process: 1) Stir the water, dispersant, defoamer, bactericide and antifreeze in the first stage at 300 r / min for 3 minutes to mix well. 2) Weigh the second stage powder, add titanium dioxide and calcined kaolin slowly one by one, mix for 3 minutes, then slowly add hydroxyethyl cellulose and hydrophobically modified hydroxyethyl cellulose and stir for 3 minutes, then slowly add pH adjuster, adjust the speed to 1500r / min appropriately, and disperse for 25 minutes. 3) Reduce the speed to 1000r / min, gradually add bactericide, mildewproof agent, film-forming aid, add emulsion and defoamer after mixing, stir for 5 minutes, then add 10% concentration of protective glue solution, speed 1500r / min, stir and mix for 15 minutes before discharging 4) Granulation stage: Weigh 25 parts by weight of a 5% concentration protective glue solution into a dispersion tank, weigh 45 parts by weight of a tinting base paint A and add it to the protective glue solution, pre-cut and granulate on a disperser, the speed is gradually increased from 300 r / min by 200 r / min, and the gradient stirring time is 3 min.

8. The method for preparing the airless spraying textured water-in-water art paint with high efficiency and mildew resistance according to claim 6, characterized in that: The steps of preparing the mildew-proof base paint formula B include the following process: 1) Stir the water, dispersant, defoamer, bactericide and antifreeze in the first stage at 300 r / min for 3 minutes to mix well. 2) Weigh the second stage powder, titanium dioxide, calcined kaolin, heavy calcium and wood fiber, slowly add them one by one, mix for 3 minutes, then slowly add hydroxyethyl cellulose and hydrophobically modified hydroxyethyl cellulose and stir for 3 minutes, then slowly add pH regulator, adjust the speed to 1800r / min appropriately, and disperse for 25 minutes. 3) Reduce the speed to 1000r / min, gradually add bactericide, mildewproof agent, film-forming aid, add emulsion and defoamer after mixing, stir for 5 minutes, then add 10% concentration of protective glue solution, speed 1500r / min, stir and mix for 15 minutes before discharging 4) Granulation stage: Weigh 25 parts by weight of a 5% concentration protective glue solution into a dispersion tank, weigh 45 parts by weight of a tinting base paint A and add it to the protective glue solution, pre-cut and granulate on a disperser, the speed is gradually increased from 300 r / min by 200 r / min, and the gradient stirring time is 3 min.

9. The method for preparing the airless sprayable textured water-in-water art paint with high-efficiency mildew resistance according to claim 6, characterized in that: The steps of preparing the continuous phase formula C include the following process: Add most of the water to the dispersion tank, with a speed of 250r / min, first add the emulsion, stir and disperse at low speed for 5 minutes, then add the antifreeze agent, film-forming aid, defoaming agent, stir for 10 minutes, then add the bactericide, mildewproof agent and pH adjuster in turn, stir at low speed for 5 minutes, and finally slowly add the associative alkali swelling thickener solution diluted with water, stir and disperse for 10 minutes.

Citation Information

Patent Citations

  • Formula and production method of waterproof breathable water-in-water multicolour coating

    CN105754442A

  • Novel waterborne water-in-water multi-color coating and method for preparing same

    CN106433472A

  • Plane pearlescent colorful artistic coating and preparation method thereof

    CN113493647A

  • Colorful paint and preparation method thereof

    CN114213926A

  • Anti-cracking sand-in-sand stone-like coating as well as preparation method and application thereof

    CN114276702A