A self-fired silicon nitride ceramic substrate and its preparation method
Thick film green ceramic tapes with a three-layer structure of boron nitride/silicon nitride/boron nitride were prepared by roll-to-roll casting technology, which solved the problems of warping and edge bending of silicon nitride ceramic substrates, and realized high flatness and high strength of in-sintering silicon nitride ceramic substrates, thereby improving production efficiency and reducing costs.
Patent Information
- Application Number
- CN202510208181.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-02-25
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2045-02-25
AI Technical Summary
Existing silicon nitride ceramic substrates are prone to warping and edge bending after sintering, resulting in uneven metallization layers or heating elements. Furthermore, traditional correction and polishing processes lead to low production efficiency and high costs, making it difficult to meet the requirements of mass production.
Thick film green ceramic tapes with a three-layer structure of boron nitride/silicon nitride/boron nitride were prepared using roll-to-roll casting technology. By casting boron nitride and silicon nitride slurries, combined with debinding and sintering processes, an instant-fired silicon nitride ceramic substrate was prepared.
It achieves high flatness and high strength of silicon nitride ceramic substrates, with warpage less than 3/1000, flexural strength exceeding 800MPa, and thermal conductivity exceeding 80W/(m•K), reducing dust hazards and process costs, and improving production efficiency.
Smart Images

Figure CN120038831B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of semiconductor ceramic substrate technology, specifically to a calcinable silicon nitride ceramic substrate and its preparation method. Background Technology
[0002] Silicon nitride ceramic substrates possess excellent thermal conductivity, mechanical properties, low coefficient of thermal expansion, and high thermal shock resistance, making them a key alternative material for high-power third-generation semiconductors. However, large-area, thin ceramic substrates are prone to warping and edge bending after sintering, potentially leading to uneven thickness or shape of the metallization layer or heating element, affecting their direct use. Currently, production primarily relies on secondary correction and grinding to ensure the flatness of the ceramic substrate to meet application requirements. The correction process, i.e., secondary sintering, has the disadvantage of causing secondary grain growth, reducing the product's flexural strength. Furthermore, secondary sintering reduces production efficiency and increases labor and energy costs, hindering mass production and marketability. Most companies use grinding processes to ensure substrate flatness, requiring sufficient grinding allowance in the sintered product, thus increasing production and material costs. When the ceramic substrate is large or thin, defects such as cracking and breakage are easily generated during grinding.
[0003] Therefore, this application is submitted. Summary of the Invention
[0004] The purpose of this invention is to provide an instant-fired silicon nitride ceramic substrate and its preparation method. The method employs roll-to-roll casting technology to sequentially cast boron nitride, silicon nitride, and boron nitride to obtain a thick film green ceramic tape with a three-layer structure of boron nitride / silicon nitride / boron nitride. Finally, the instant-fired silicon nitride ceramic substrate with good flatness and high strength is prepared by debinding and sintering.
[0005] To solve the above-mentioned technical problems, the present invention adopts the following solution: A method for preparing a readily sinterable silicon nitride ceramic substrate includes the following steps: Step 1: After preparing boron nitride slurry and silicon nitride slurry, defoaming treatment is performed separately to obtain boron nitride casting slurry and silicon nitride casting slurry; Step 2: Boron nitride casting paste, silicon nitride casting paste, and boron nitride casting paste are sequentially cast from roll to roll to obtain green ceramic tape; Step 3: Post-processing. After debinding and sintering, the green ceramic strip is used to obtain an instant-fired silicon nitride ceramic substrate.
[0006] Furthermore, when preparing the boron nitride slurry, 60-65% boron nitride powder, 5-10% binder I, 1-5% dispersant I, 1-5% defoamer, and 25-35% anhydrous ethanol are mixed and ball-milled for 10-20 hours by mass percentage.
[0007] Furthermore, the boron nitride powder has a purity >99.8% and an average particle size D. 50 The diameter is 15~25µm, and the specific surface area is 5~10m². 2 / g; The adhesive I is one of polyvinyl butyral, methylcellulose, ethylcellulose, and polyacrylic acid; The dispersant I is one of polyacrylate, polyacrylamide, polyelectrolyte ammonium, and trioleic acid glyceride; The defoaming agent is one of polypropylene glycol, polysiloxane, isooctyl alcohol, and diethylhexanol.
[0008] Furthermore, when preparing silicon nitride slurry, 55-60% silicon nitride powder, 5-10% sintering aid, 0.5-1.5% dispersant II, and 15-20% organic solvent are placed in a ball mill by weight percentage and ball milled once to obtain a dispersion slurry; 5-10% binder II and 1-5% plasticizer are placed in the dispersion slurry and ball milled a second time to obtain silicon nitride slurry.
[0009] Furthermore, the silicon nitride powder has a purity >99.8% and an average particle size D. 50 Its diameter is 0.4~0.8µm, and its specific surface area is 10~15m². 2 / g; The sintering aid is a mixture of magnesium oxide and yttrium oxide, with an average particle size D. 50 The ranges are 0.1~0.5µm and 1.0~1.5µm, respectively. The dispersant II is one of herring oil, castor oil, and triethanolamine; The adhesive II is polyvinyl butyral; The plasticizer is at least one of dibutyl phthalate and polyethylene glycol; The organic solvent is at least two of toluene, isopropanol, anhydrous ethanol, and xylene.
[0010] Furthermore, silicon nitride magnetic balls are added into the ball mill, with the volume of the silicon nitride magnetic balls occupying 1 / 3 of the internal volume of the ball mill. The rotation speed is 100~200 r / min, the first ball milling time is 10~20 h, and the second ball milling time is 20~30 h.
[0011] Furthermore, the viscosity of the boron nitride casting slurry is 1000~2000 cps, and the viscosity of the silicon nitride casting slurry is 5000~10000 cps.
[0012] Furthermore, the casting speed of the boron nitride casting slurry is 0.5~2m / min, and the casting speed of the silicon nitride casting slurry is 0.1~2m / min; the green ceramic tape has a three-layer structure of boron nitride / silicon nitride / boron nitride, with a total thickness of 0.44~1.2mm, a boron nitride thickness of 0.02~0.1mm, and a silicon nitride thickness of 0.4~1.0mm.
[0013] Furthermore, during glue removal, the temperature is 450~600℃, the heating rate is 0.5~2℃ / min, and the holding time is 5~10h; During sintering, the sintering temperature is 1700~1900℃, the heating rate is 1~5℃ / min, and the holding time is 1~5h.
[0014] A ready-to-fire silicon nitride ceramic substrate is prepared by the above-mentioned method for preparing a ready-to-fire silicon nitride ceramic substrate. The silicon nitride ceramic substrate has a warpage of <3 / 1000, a flexural strength of >800MPa, and a thermal conductivity of >80W / (m•K).
[0015] The beneficial effects of this invention are as follows: This invention uses roll-to-roll casting technology to replace the current traditional powder coating process. A boron nitride thin film is cast on each of the two sides of the silicon nitride thick film to obtain a thick film green ceramic tape with a three-layer structure of boron nitride / silicon nitride / boron nitride. The transformation process of boron nitride slurry from rheotype to viscoelasticity improves the dispersion uniformity and stability of boron nitride powder. At the same time, the reduction of the powder coating process not only reduces the harm of dust to the human body and reduces process costs, but also reduces the introduction of residual stress and contaminants in the green body. The boron nitride thin film forms a stable BN skeleton on both surfaces of the silicon nitride thick film, reducing the thermal stress of debinding and sintering and improving warpage defects. Finally, a ready-to-fire silicon nitride substrate is prepared by debinding and sintering, with a warpage of <3 / 1000, flexural strength >800MPa, and thermal conductivity >80W / (m•K). Attached Figure Description
[0016] Figure 1 This is a photograph of the silicon nitride ceramic substrate used in Example 2. Figure 2 This is a microscopic cross-sectional view of the silicon nitride ceramic substrate in Example 2. Detailed Implementation
[0017] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. All other embodiments obtained by those skilled in the art based on the described embodiments of the present invention without creative effort are within the scope of protection of the present invention.
[0018] Furthermore, for clarity and brevity, descriptions of well-known structures, functions, and configurations may have been omitted. Those skilled in the art will recognize that various changes and modifications can be made to the examples described herein without departing from the spirit and scope of this disclosure.
[0019] Techniques, methods, and equipment known to those skilled in the art may not be discussed in detail, but where appropriate, such techniques, methods, and equipment should be considered part of the specification.
[0020] In all examples shown and discussed herein, any specific values should be interpreted as merely exemplary and not as limitations. Therefore, other examples of exemplary embodiments may have different values.
[0021] Preparation of boron nitride slurry: By mass percentage, 65% boron nitride powder, 5% polyvinyl butyral, 1.5% trioleic acid glyceride, 2.5% polypropylene glycol, and 26% anhydrous ethanol are mixed and ball-milled at 50 r / min for 5 h to obtain boron nitride slurry.
[0022] Preparation of silicon nitride slurry: By mass percentage, 60% silicon nitride powder, 6% magnesium oxide and yttrium oxide mixture (mass ratio of magnesium oxide to yttrium oxide is 1:1), 1.5% castor oil, 19.5% toluene and anhydrous ethanol (mass ratio of toluene to anhydrous ethanol is 1:2) are mixed and placed in a ball mill. Silicon nitride ceramic balls are added to 1 / 3 of the ball mill's internal volume. After ball milling at 200 r / min for 10 h, a silicon nitride dispersion slurry is obtained. Then, 10% polyvinyl butyral and 3% dibutyl phthalate are added to the silicon nitride dispersion slurry, and ball milling is continued at 100 r / min for 20 h to obtain a silicon nitride slurry.
[0023] Degassing treatment: The silicon nitride slurry was placed in degassing tank II, the thermal circulation was turned on, the temperature was controlled at 35°C, and the vacuum degree was evacuated to -98Kpa. The slurry was stirred at a low speed of 20r / min for 4h until the viscosity of the slurry was 7000~8000cps. Finally, it was aged for 5h to obtain silicon nitride casting slurry. This silicon nitride casting slurry was used to prepare the instant-fired silicon nitride ceramic substrate in Examples 1-4.
[0024] Example 1 A method for preparing a self-fired silicon nitride ceramic substrate includes the following steps: (1) Place the boron nitride slurry in degassing tank I, turn on the heat circulation, control the temperature at 20℃, and evacuate to a vacuum degree of -98Kpa. Stir at a speed of 20r / min for 1h until the slurry viscosity is 1000cps. Finally, age for 2h to obtain boron nitride casting slurry. (2) Roll-to-roll sequential casting is adopted. 100-mesh screens are installed at the discharge ports of degassing tanks I and II. Plastic hoses are used to connect casting machine cutter heads I and II respectively. First, degassing tank I and cutter head I are connected for casting. The scraper height is adjusted to 0.1~0.2mm and the casting speed is 2m / min. The casting machine oven is divided into 5 temperature zones, with gradient temperatures of 25, 45, 65, 85 and 100℃ respectively. After drying, a boron nitride film with a thickness of 20µm is finally obtained. (3) Then convert to degassing tank II and blade II for casting, adjust the scraper height to 0.5~1.0mm, the casting speed to 0.5m / min, and the casting machine oven temperature to 25, 45, 65, 85 and 100℃ respectively. After drying, a silicon nitride thick film with a thickness of 0.4mm is obtained on the boron nitride film surface. (4) Then switch back to degassing tank I and cutter head I to cast another layer of boron nitride film with the same thickness as in step (2), and finally obtain a green blank with a boron nitride / silicon nitride / boron nitride structure with a thickness of 0.44 mm; (5) Cut the green blank into 200*250mm specifications, then remove the glue, set the glue removal temperature to 600℃, the heating rate to 0.5℃ / min, and the holding time to 2h; finally, sinter at 1900℃ with air pressure, the heating rate to 5℃ / min, and the holding time to 2h, to obtain the instant-fired silicon nitride ceramic substrate.
[0025] In Example 1, the boron nitride film thickness was 20 µm. The prepared instant-fired ceramic substrate exhibited adhesion, which led to separation and substrate cracking. The warpage was 5 / 1000, the flexural strength was 790 MPa, and the thermal conductivity was 80 W / (m•K).
[0026] Example 2 A method for preparing a readily sinterable silicon nitride ceramic substrate includes the following steps: (1) Place the boron nitride slurry in degassing tank I, turn on the heat circulation, control the temperature at 25℃, and evacuate to a vacuum degree of -98Kpa. Stir at a speed of 20r / min for 1h until the slurry viscosity is 1200cps. Finally, age for 2h to obtain boron nitride casting slurry. (2) Roll-to-roll sequential casting is adopted. First, the degassing tank I and the blade I are connected for casting. The height of the scraper is adjusted to 0.1~0.2mm and the casting speed is 1.5m / min. The oven gradient temperatures are set to 25, 45, 65, 85 and 100℃ respectively. After drying, a boron nitride film with a thickness of 40µm is finally obtained. (3) Then convert to degassing tank II and blade II for casting, adjust the scraper height to 0.5~1.0mm, the casting speed to 0.5m / min, and the casting machine oven temperature to 25, 45, 65, 85 and 100℃ respectively. After drying, a silicon nitride thick film with a thickness of 0.4mm is obtained on the boron nitride film surface. (4) Then switch back to degassing tank I and cutter head I to cast another layer of boron nitride film with the same thickness as in step (2), and finally obtain a green blank with a boron nitride / silicon nitride / boron nitride structure with a thickness of 0.48 mm; (5) Cut the green blank into 200*250mm specifications, then remove the glue, set the glue removal temperature to 600℃, the heating rate to 0.5℃ / min, and the holding time to 2h; finally, sinter at 1900℃ with air pressure, the heating rate to 5℃ / min, and the holding time to 2h, to obtain the instant-fired silicon nitride ceramic substrate.
[0027] The boron nitride film thickness in Example 2 was 40µm. The prepared instant-fired ceramic substrate had good flatness and no adhesion or cracking. The warpage was 2 / 1000, the flexural strength was 820MPa, and the thermal conductivity was 82W / (m•K).
[0028] Example 3 A method for preparing a readily sinterable silicon nitride ceramic substrate includes the following steps: (1) Place the boron nitride slurry in degassing tank I, turn on the heat circulation, control the temperature at 30℃, and evacuate to a vacuum degree of -98Kpa. Stir at a speed of 20r / min for 1h until the slurry viscosity is 1400cps. Finally, age for 2h to obtain boron nitride casting slurry. (2) Roll-to-roll sequential casting is adopted. First, the degassing tank I and the blade I are connected for casting. The height of the scraper is adjusted to 0.1~0.2mm and the casting speed is 1.0m / min. The oven gradient temperatures are set to 25, 45, 65, 85 and 100℃ respectively. After drying, a boron nitride film with a thickness of 60µm is finally obtained. (3) Then convert to degassing tank II and blade II for casting, adjust the scraper height to 0.5~1.0mm, the casting speed to 0.5m / min, and the casting machine oven temperature to 25, 45, 65, 85 and 100℃ respectively. After drying, a silicon nitride thick film with a thickness of 0.4mm is obtained on the boron nitride film surface. (4) Then switch back to degassing tank I and cutter head I to cast another layer of boron nitride film with the same thickness as in step (2), and finally obtain a green blank with a boron nitride / silicon nitride / boron nitride structure with a thickness of 0.52 mm; (5) Cut the green blank into 200*250mm specifications, then remove the glue, set the glue removal temperature to 600℃, the heating rate to 0.5℃ / min, and the holding time to 2h; finally, sinter at 1900℃ with air pressure, the heating rate to 5℃ / min, and the holding time to 2h, to obtain the instant-fired silicon nitride ceramic substrate.
[0029] In Example 3, the boron nitride film thickness was 60 µm. The prepared instant-fired ceramic substrate exhibited cracking and slight warping, with a warping degree of 8 / 1000, a flexural strength of 770 MPa, and a thermal conductivity of 81 W / (m•K).
[0030] Example 4 A method for preparing a self-fired silicon nitride ceramic substrate includes the following steps: (1) Place the boron nitride slurry in degassing tank I, turn on the heat circulation, control the temperature at 30℃, and evacuate to a vacuum degree of -98Kpa. Stir at a speed of 20r / min for 1.5h until the slurry viscosity is 1600cps. Finally, age for 2h to obtain boron nitride casting slurry. (2) Roll-to-roll sequential casting is adopted. First, the degassing tank I and the blade I are connected for casting. The height of the scraper is adjusted to 0.1~0.2mm and the casting speed is 0.5m / min. The oven gradient temperatures are set to 25, 45, 65, 85 and 100℃ respectively. After drying, a boron nitride film with a thickness of 80µm is finally obtained. (3) Then convert to degassing tank II and blade II for casting, adjust the scraper height to 0.5~1.0mm, the casting speed to 0.5m / min, and the casting machine oven temperature to 25, 45, 65, 85 and 100℃ respectively. After drying, a silicon nitride thick film with a thickness of 0.4mm is obtained on the boron nitride film surface. (4) Then switch back to degassing tank I and cutter head I to cast another layer of boron nitride film with the same thickness as in step (2), and finally obtain a green blank with a boron nitride / silicon nitride / boron nitride structure with a thickness of 0.56 mm; (5) Cut the green blank into 200*250mm specifications, then remove the glue, set the glue removal temperature to 600℃, the heating rate to 0.5℃ / min, and the holding time to 2h; finally, sinter at 1900℃ with air pressure, the heating rate to 5℃ / min, and the holding time to 2h, to obtain the instant-fired silicon nitride ceramic substrate.
[0031] In Example 4, the boron nitride film thickness was 80 µm. The prepared instant-fired ceramic substrate exhibited numerous bumps, cracks, and severe warping, with a warping degree of 15 / 1000, a flexural strength of 670 MPa, and a thermal conductivity of 78 W / (m•K).
[0032] Comparative Example 1 A method for preparing silicon nitride ceramic substrates using a conventional powder coating process includes the following steps: (1) By mass percentage, 1% carboxymethyl cellulose and polyvinyl alcohol and 76% deionized water are mixed in a mixing tank and stirred at 50 r / min for 1 h to obtain a glue solution. Then, 20% boron nitride powder and 3% herring oil are added to the glue solution and stirred for 2 h to obtain boron nitride coating slurry. The speed is controlled at 80 r / min.
[0033] (2) Turn on the powder coating machine and convey the silicon nitride green blank with a thickness of 0.4 mm to the atomizer through the powder coating machine conveyor belt. The boron nitride powder coating slurry is evenly atomized onto the surface of the green blank through the atomizer. Then, the boron nitride powder coating slurry is dried and firmly adhered to the surface of the green blank through the 60℃ heating section to obtain a powder coating layer with a single-sided thickness of 20µm. Then, the green blank with one side coated is flipped over to coat the other side to obtain a double-sided powder-coated green blank with a thickness of 0.44 mm.
[0034] (3) The powder-coated green blanks are stacked and debonded. The debonding temperature is 600℃, the heating rate is 0.5℃ / min, and the holding time is 2h. Finally, they are sintered at 1900℃ with air pressure, the heating rate is 5℃ / min, and the holding time is 2h to obtain silicon nitride ceramic substrate.
[0035] In Comparative Example 1, the boron nitride powder coating layer was 20µm thick. The prepared silicon nitride ceramic substrate exhibited partial pitting and severe adhesion, with a warpage of 7 / 1000, a flexural strength of 720MPa, and a thermal conductivity of 76W / (m•K).
[0036] Comparative Example 2 A method for preparing silicon nitride ceramic substrates using a conventional powder coating process includes the following steps: (1) By mass percentage, 2% carboxymethyl cellulose, polyvinyl alcohol and 75% deionized water are mixed in a mixing tank and stirred at 50 r / min for 1 h to obtain a glue solution. Then, 20% boron nitride powder and 3% herring oil are added to the glue solution and stirred for 2 h to obtain boron nitride coating slurry. The speed is controlled at 80 r / min.
[0037] (2) Turn on the powder coating machine and convey the silicon nitride green blank with a thickness of 0.4 mm to the atomizer through the powder coating machine conveyor belt. The boron nitride powder coating slurry is evenly atomized onto the surface of the green blank through the atomizer. Then, the boron nitride powder is dried and firmly adhered to the surface of the green blank through the 60℃ heating section to obtain a powder coating layer with a single-sided thickness of 40µm. Then, the green blank with one side coated is flipped over to coat the other side to obtain a double-sided powder coating structure green blank with a thickness of 0.48 mm.
[0038] (3) The powder-coated green blanks are stacked and debonded. The debonding temperature is 600℃, the heating rate is 0.5℃ / min, and the holding time is 2h. Finally, they are sintered at 1900℃ with air pressure, the heating rate is 5℃ / min, and the holding time is 2h to obtain silicon nitride ceramic substrate.
[0039] In Comparative Example 2, the boron nitride powder coating layer was 40 µm thick. The prepared silicon nitride ceramic substrate exhibited some pitting, a small amount of adhesion and cracking. The warpage was 4 / 1000, the flexural strength was 750 MPa, and the thermal conductivity was 77 W / (m•K).
[0040] Comparative Example 3 A method for preparing silicon nitride ceramic substrates using a conventional powder coating process includes the following steps: (1) By mass percentage, 3% carboxymethyl cellulose and polyvinyl alcohol and 74% deionized water are mixed in a mixing tank and stirred at 50 r / min for 1 h to obtain a glue solution. Then, 20% boron nitride powder and 3% herring oil are added to the glue solution and stirred for 2 h to obtain boron nitride coating slurry. The speed is controlled at 80 r / min.
[0041] (2) Turn on the powder coating machine and convey the silicon nitride green blank with a thickness of 0.4 mm to the atomizer through the powder coating machine conveyor belt. The boron nitride powder coating slurry is evenly atomized onto the surface of the green blank through the atomizer. Then, the boron nitride powder is dried and firmly adhered to the surface of the green blank through the 60℃ heating section to obtain a powder coating layer with a single-sided thickness of 60µm. Then, the green blank with one side coated is flipped over to coat the other side to obtain a double-sided powder coating structure green blank with a thickness of 0.52 mm.
[0042] (3) The powder-coated green blanks are stacked and debonded. The debonding temperature is 600℃, the heating rate is 0.5℃ / min, and the holding time is 2h. Finally, they are sintered at 1900℃ with air pressure, the heating rate is 5℃ / min, and the holding time is 2h to obtain silicon nitride ceramic substrate.
[0043] In Comparative Example 3, the boron nitride powder coating layer was 60µm thick. The prepared silicon nitride ceramic substrate exhibited numerous pits and misalignments, with a warpage of 9 / 1000, a flexural strength of 710MPa, and a thermal conductivity of 78W / (m•K).
[0044] Comparative Example 4 A method for preparing silicon nitride ceramic substrates using a conventional powder coating process includes the following steps: (1) By mass percentage, 4% carboxymethyl cellulose and polyvinyl alcohol and 73% deionized water are mixed in a mixing tank and stirred at 50 r / min for 1 h to obtain a glue solution. Then, 20% boron nitride powder and 3% herring oil are added to the glue solution and stirred for 2 h to obtain boron nitride coating slurry. The speed is controlled at 80 r / min.
[0045] (2) Turn on the powder coating machine and convey the silicon nitride green blank with a thickness of 0.4 mm to the atomizer through the powder coating machine conveyor belt. The boron nitride powder coating slurry is evenly atomized onto the surface of the green blank through the atomizer. Then, the boron nitride powder is dried and firmly adhered to the surface of the green blank through the 60℃ heating section to obtain a powder coating layer with a single-sided thickness of 80µm. Then, the green blank with one side coated is flipped over to coat the other side to obtain a double-sided powder coating structure green blank with a thickness of 0.56 mm.
[0046] (3) The powder-coated green blanks are stacked and debonded. The debonding temperature is 600℃, the heating rate is 0.5℃ / min, and the holding time is 2h. Finally, they are sintered at 1900℃ with air pressure, the heating rate is 5℃ / min, and the holding time is 2h to obtain silicon nitride ceramic substrate.
[0047] In Comparative Example 4, the boron nitride powder coating thickness was 80 µm. The prepared silicon nitride ceramic substrate exhibited severe warping, with a warping degree of 20 / 1000, a flexural strength of 650 MPa, and a thermal conductivity of 74 W / (m•K).
[0048] Table 1 shows a comparison of the properties of the silicon nitride ceramic substrates prepared in the embodiments and comparative examples of this application: Table 1 Performance Comparison of Examples and Comparative Examples Referring to Table 1, compared with the conventional double-sided coating method used in Comparative Examples 1-4 for silicon nitride green blanks, the silicon nitride ceramic substrate prepared in Example 2 exhibits the least warpage, higher flexural strength and thermal conductivity, and shows no adhesion or cracking. Figure 1 and Figure 2 .
[0049] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes, and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.
Claims
1. A method for preparing a ready-to-fire silicon nitride ceramic substrate, characterized in that, Includes the following steps: Step 1: After preparing boron nitride slurry and silicon nitride slurry, defoaming treatment is performed separately to obtain boron nitride casting slurry and silicon nitride casting slurry; Step 2: Boron nitride casting slurry, silicon nitride casting slurry, and boron nitride casting slurry are cast sequentially from roll to roll to obtain green ceramic tape; Step 3: Post-processing: After debinding and sintering treatment, the green ceramic tape is used to obtain a ready-to-fire silicon nitride ceramic substrate.
2. The method for preparing a ready-to-fire silicon nitride ceramic substrate according to claim 1, characterized in that, When preparing boron nitride slurry, mix 60-65% boron nitride powder, 5-10% binder I, 1-5% dispersant I, 1-5% defoamer, and 25-35% anhydrous ethanol by mass percentage and ball mill for 10-20 hours.
3. The method for preparing a ready-to-fire silicon nitride ceramic substrate according to claim 2, characterized in that, The boron nitride powder has a purity >99.8%, an average particle size D50 of 15-25 μm, and a specific surface area of 5-10 m² / g; the binder I is one of polyvinyl butyral, methylcellulose, ethylcellulose, and polyacrylic acid; the dispersant I is one of polyacrylate, polyacrylamide, ammonium polyelectrolyte, and trioleic acid glyceride; and the defoamer is one of polypropylene glycol, polysiloxane, isooctyl alcohol, and diethylhexanol.
4. The method for preparing a ready-to-fire silicon nitride ceramic substrate according to claim 2, characterized in that, When preparing silicon nitride slurry, 55-60% silicon nitride powder, 5-10% sintering aid, 0.5-1.5% dispersant II, and 15-20% organic solvent are placed in a ball mill by mass percentage and the dispersion slurry is obtained after one ball milling. 5-10% binder II and 1-5% plasticizer are placed in the dispersion slurry and the silicon nitride slurry is obtained after a second ball milling.
5. The method for preparing a ready-to-fire silicon nitride ceramic substrate according to claim 4, characterized in that, The silicon nitride powder has a purity >99.8%, an average particle size D50 of 0.4–0.8 μm, and a specific surface area of 10–15 m² / g; the sintering aid is a mixture of magnesium oxide and yttrium oxide, with average particle sizes D50 of 0.1–0.5 μm and 1.0–1.5 μm, respectively; the dispersant II is one of herring oil, sesame oil, and triethanolamine; the binder II is polyvinyl butyral; the plasticizer is at least one of dibutyl phthalate and polyethylene glycol; and the organic solvent is at least two of toluene, isopropanol, anhydrous ethanol, and xylene.
6. The method for preparing a ready-to-fire silicon nitride ceramic substrate according to claim 4, characterized in that, Silicon nitride magnetic balls are added into the ball mill, the volume of which occupies 1 / 3 of the internal volume of the ball mill. The rotation speed is 100-200 r / min, the first ball milling time is 10-20 h, and the second ball milling time is 20-30 h.
7. The method for preparing a ready-to-fire silicon nitride ceramic substrate according to claim 4, characterized in that, The viscosity of the boron nitride casting slurry is 1000-2000 cps, and the viscosity of the silicon nitride casting slurry is 5000-10000 cps.
8. The method for preparing a ready-to-fire silicon nitride ceramic substrate according to claim 4, characterized in that, The casting speed of the boron nitride casting slurry is 0.5–2 m / min, and the casting speed of the silicon nitride casting slurry is 0.1–2 m / min; the green ceramic tape has a three-layer structure of boron nitride / silicon nitride / boron nitride, with a total thickness of 0.44–1.2 mm, a single layer of boron nitride with a thickness of 0.02–0.1 mm, and a silicon nitride with a thickness of 0.4–1.0 mm.
9. The method for preparing a ready-to-fire silicon nitride ceramic substrate according to claim 4, characterized in that, During the debinding process, the temperature is 450–600℃, the heating rate is 0.5–2℃ / min, and the holding time is 5–10h; during sintering, the sintering temperature is 1700–1900℃, the heating rate is 1–5℃ / min, and the holding time is 1–5h.
10. A ready-to-fire silicon nitride ceramic substrate, characterized in that, The silicon nitride ceramic substrate is prepared by any one of the following methods: a sinterable silicon nitride ceramic substrate, wherein the warpage of the silicon nitride ceramic substrate is <3 / 1000, the flexural strength is >800 MPa, and the thermal conductivity is >80 W / (m·K).
Citation Information
Patent Citations
Low-temperature co-fired ceramic raw material belt and preparation method thereof
CN111484336A
Method for preparing ceramic substrate isolating layer by using boron nitride ultrathin cast film tape
CN115196972A