Treatment method for eliminating large-size carbides in carburized surface layer of rare earth M50NiL steel
Through surface deformation treatment and high-temperature tempering, large-size carbides on the surface carburized layer of M50NiL steel are eliminated, stress concentration problem is solved, and the wear resistance and service life of bearing steel are improved.
Patent Information
- Application Number
- CN202510246750.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-03-04
- Publication Date
- 2025-08-05
AI Technical Summary
The prior art is difficult to effectively eliminate large-size carbides in the surface of carburizing M50NiL steel for aircraft engines, resulting in stress concentration and fatigue failure of bearing parts.
By performing surface deformation treatment after carburizing treatment, the sample surface is subjected to high-frequency impact using an ultrasonic shot peening device, combined with high-temperature tempering, quenching and deep-cold treatment, the carbide size is refined and its distribution uniformity is improved.
Significantly reduce the number density of large-size carbides on the carburized surface, improve the uniformity of carbide size distribution, enhance the wear resistance of the material, and extend the service life of bearing parts.
Smart Images

Figure CN120425274A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of microstructure optimization of M50NiL high-temperature carburized bearing steel for aircraft engines, and in particular to a treatment method for eliminating large-sized carbides in the carburized surface layer of rare earth M50NiL steel. Background Art
[0002] M50NiL steel is a second-generation surface-treated bearing steel for aircraft engine main shaft bearings. It is developed based on the existing high-temperature bearing steel M50 steel by reducing the carbon content and increasing the nickel content. The lower carbon content in M50NiL steel allows the carbides in the structure to be fine and dispersed, solving the problem of large carbides in M50 steel. At the same time, the fracture toughness is increased by more than 2 times, and after carburizing, it is "hard on the outside and tough on the inside." Compared with M50 steel, the bearing's limit DN value can be increased from 2.4×10 6 mm·r / min increased to 3.0×10 6 mm·r / min, so the application prospects are broader.
[0003] However, as a surface-treated bearing steel, the carbon content of the carburized surface of M50NiL steel after gas carburizing is often high. Due to the high content of strong carbide-forming elements such as Cr, Mo, and V in the steel, a large number of large-sized carbides are easily generated on the carburized surface, and it is still difficult to eliminate them by heat treatment. The large-sized carbides in this organization are prone to stress concentration under the action of alternating stress during service, leading to the initiation and expansion of cracks, and ultimately causing fatigue failure of bearing parts. At present, the refinement of large-sized carbides is mainly achieved through high-temperature diffusion, large plastic deformation such as forging and rolling, but these methods are not suitable for surface-treated bearing steel. Therefore, it is urgent to develop a targeted, simple and feasible method for eliminating large-sized carbides on the carburized surface to improve the wear resistance of bearing steel and extend the service life of aero-engine bearing parts. Summary of the Invention
[0004] In view of the problems existing in the prior art, the present invention aims to develop a treatment method for eliminating large-sized carbides in the carburized surface layer of rare earth M50NiL steel. Based on the idea that large-sized carbides are prone to preferential decomposition and refinement under the action of dislocation movement during plastic deformation, samples that meet the composition requirements are carburized and heat treated. Then, only surface deformation technology is used to treat the samples for a short time. This method can effectively reduce the number density of large-sized carbides in the carburized surface layer, improve the uniformity of the carbide size distribution in the carburized surface layer, and significantly improve the wear resistance of the material, meeting the performance requirements of current aircraft engine bearings.
[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0006] A treatment method for eliminating large-sized carbides in the carburized surface layer of rare-earth M50NiL steel. The chemical composition of rare-earth M50NiL steel and its mass percentage include: C 0.11wt.% - 0.15wt.%, Si 0.10wt.% - 0.25wt.%, Cr 4.00wt.% - 4.25wt.%, Mo 4.00wt.% - 4.50wt.%, V 1.13wt.% - 1.33wt.%, Ni 3.20wt.% - 3.60wt.%, Mn 0.15wt.% - 0.35wt.%, 0 < total amount of Ce and La ≤ 0.02wt.%, P ≤ 0.01wt.%, S ≤ 0.01wt.%, and the balance is Fe.
[0007] For the treatment method for eliminating large-sized carbides in the carburized surface layer of rare-earth M50NiL steel, preferably, the total amount of Ce and La is 0.003wt.% - 0.02wt.%, and the mass fraction ratio of Ce to La elements is 3:(1 - 2).
[0008] For the treatment method for eliminating large-sized carbides in the carburized surface layer of rare-earth M50NiL steel, the as-cast billet of rare-earth M50NiL steel is made by a double-vacuum smelting method of vacuum induction + vacuum consumable.
[0009] The treatment method for eliminating large-sized carbides in the carburized surface layer of rare-earth M50NiL steel includes surface carburization, high-temperature tempering, quenching, cryogenic treatment, tempering, machining, and surface deformation treatment processes. The specific steps are as follows:
[0010] (1) Surface carburization: The sample is subjected to gas carburization treatment for 20h - 40h under the carburizing atmosphere created by an RX gas generator. The carburization temperature is 930 ± 20°C, and after carburization, it is cooled to room temperature with the furnace.
[0011] (2) High-temperature tempering: After surface carburization treatment, high-temperature tempering is carried out. The tempering temperature is 750 ± 20°C, the holding time is 4h - 6h, then it is cooled to 550 ± 20°C in the furnace, and then taken out of the furnace and air-cooled to room temperature.
[0012] (3) Quenching: After high-temperature tempering, it is first heated to 650 ± 20°C at a heating rate of 100°C - 300°C / h for 0.5h - 1h for preheating and holding, then heated to 850 ± 20°C at a heating rate of 100°C - 300°C / h for 0.5h - 1h for preheating and holding, and then heated to the quenching temperature of 1100 ± 20°C at a heating rate of 100°C - 300°C / h, with a holding time of 0.5h - 1h, and then oil-cooled to room temperature.
[0013] (4) Cryogenic treatment: After quenching, the steel is rapidly cryogenically treated within 1 hour, cooling to -196°C to -40°C at a cooling rate of 25°C to 100°C / h, and then kept at this temperature for 2h to 4h, and then heated to room temperature at the same heating rate;
[0014] (5) Tempering: After cryogenic treatment, tempering treatment is carried out, heating to 280±20℃ at a heating rate of 100℃~300℃ / h, preheating and holding for 0.5h~1h, then heating to a heating temperature of 500℃~580℃ at a heating rate of 100℃~300℃ / h, holding time for 1h~3h, and then air cooling to room temperature. This process is repeated 2~4 times;
[0015] (6) Machining: Grind the heat-treated sample using a grinder to ensure surface quality, with a machining volume of 0.1 mm to 0.5 mm;
[0016] (7) Surface deformation: An ultrasonic shot peening device was used. The operating frequency of the ultrasonic generator was set to 20 ± 1 kHz, the amplitude was 30 μm to 50 μm, and tungsten steel shots with a diameter of 0.5 mm to 3.0 mm were selected. The sample surface was repeatedly subjected to high-frequency impact treatment in a closed chamber for 0 min to 10 min.
[0017] In the treatment method for eliminating large-sized carbides in the carburized surface layer of rare earth M50NiL steel, high-temperature tempering, quenching and tempering processes are all carried out in a vacuum heat treatment furnace to prevent surface decarburization.
[0018] The design concept of the present invention is:
[0019] During the surface deformation process, the carburized surface structure will undergo severe plastic deformation dominated by dislocation movement under the impact of high-energy projectiles. Due to the poor plastic deformation ability of carbides and the lack of coordination with the plastic deformation of the matrix, dislocations tend to proliferate and accumulate at the carbide boundaries, resulting in carbide interface stresses much higher than the structural stress. When the shear stress acting on the slip plane along the slip direction reaches a critical value, slip begins to occur within the carbide, causing decomposition and refinement. Under the same conditions, the size of the carbide determines the degree of plastic deformation and refinement. Generally, the larger the carbide size, the more frequent the dislocation movement, which makes decomposition and refinement more likely to occur.
[0020] The advantages and beneficial effects of the present invention are:
[0021] 1. This invention adds a small amount of rare earth elements to existing M50NiL steel. By modifying inclusions with rare earth elements, it effectively mitigates the harmful effects of inclusions in the steel. Furthermore, through surface deformation treatment, large carbides in the carburized surface layer are specifically eliminated, effectively increasing the uniformity of carbide size distribution within the structure. This invention helps reduce sources of failure in bearing components during service, improves the overall performance of bearing steel, and meets the performance requirements of current aircraft engine bearings.
[0022] 2. The present invention can be operated on the basis of existing production processes. By simply applying a simple deformation treatment to the original sample surface, it can quickly and effectively eliminate large-sized carbides on the carburized surface, achieving low cost and high performance, and has a very broad application prospect. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a scanning electron microscope (SEM) image of the carbide distribution on the carburized surface without surface deformation treatment;
[0024] Figure 2 This is the SEM image of carbide distribution on the carburized surface after 5 minutes of surface deformation treatment;
[0025] Figure 3 This is the SEM image of carbide distribution on the carburized surface after 10 minutes of surface deformation treatment;
[0026] Figure 4 The following is a comparison chart of the wear rates of three example samples (Untreated: no surface deformation treatment applied, Treated-5: surface deformation treatment applied for 5 minutes, Treated-10: surface deformation treatment applied for 10 minutes) after reciprocating sliding for 0.5 hours under oil lubrication conditions with a load of 120N, a stroke of 10mm, and a frequency of 4Hz. DETAILED DESCRIPTION
[0027] In the specific implementation process, the present invention proposes a treatment method for eliminating large-sized carbides in the carburized surface layer of rare-earth M50NiL steel. The chemical composition of rare-earth M50NiL steel and its mass percentage include: C 0.11wt.% - 0.15wt.%, Si 0.10wt.% - 0.25wt.%, Cr 4.00wt.% - 4.25wt.%, Mo 4.00wt.% - 4.50wt.%, V 1.13wt.% - 1.33wt.%, Ni 3.20wt.% - 3.60wt.%, Mn 0.15wt.% - 0.35wt.%, 0 < total amount of Ce and La ≤ 0.02wt.%, P ≤ 0.01wt.%, S ≤ 0.01wt.%, and the balance is Fe. Among them, 0 < total amount of Ce and La ≤ 0.02wt.%, and the as-cast billet is made by double-vacuum smelting method of vacuum induction + vacuum consumable.
[0028] The described treatment method for eliminating large-sized carbides in the carburized surface layer of rare-earth M50NiL steel includes surface carburization, high-temperature tempering, quenching, cryogenic treatment, tempering, machining and surface deformation treatment processes. The specific steps are as follows:
[0029] (1) Surface carburization: The sample is subjected to gas carburization treatment for 20h - 40h in the carburizing atmosphere created by an RX gas generator. The carburizing temperature is 930 ± 20°C, and after carburization, it is cooled to room temperature with the furnace.
[0030] (2) High-temperature tempering: After surface carburization treatment, high-temperature tempering is carried out. The tempering temperature is 750 ± 20°C, the holding time is 4h - 6h, then it is cooled in the furnace to 550 ± 20°C, and then taken out of the furnace and air-cooled to room temperature.
[0031] (3) Quenching: After high-temperature tempering, it is first heated to 650 ± 20°C at a heating rate of 100°C - 300°C / h for 0.5h - 1h of preheating and holding, then heated to 850 ± 20°C at a heating rate of 100°C - 300°C / h for 0.5h - 1h of preheating and holding, and then heated to the quenching temperature of 1100 ± 20°C at a heating rate of 100°C - 300°C / h. The holding time is 0.5h - 1h, and then it is oil-cooled to room temperature.
[0032] (4) Cryogenic treatment: After quenching, cryogenic treatment is quickly carried out within 1h. It is cooled to -196°C - -40°C at a cooling rate of 25°C - 100°C / h, and held at this temperature for 2h - 4h, and then heated to room temperature at the same heating rate.
[0033] (5) Tempering: After deep cooling, tempering treatment is carried out, heating to 280±20℃ at a heating rate of 100℃~300℃ / h, preheating and holding for 0.5h~1h, then heating to a heating temperature of 500℃~580℃ at a heating rate of 100℃~300℃ / h, holding time for 1h~3h, and then air cooling to room temperature. This process is repeated 2~4 times;
[0034] (6) Machining: Grind the heat-treated sample using a grinder to ensure surface quality, with a machining volume of 0.1 mm to 0.5 mm;
[0035] (7) Surface deformation: An ultrasonic shot peening device was used. The operating frequency of the ultrasonic generator was set to 20 ± 1 kHz, the amplitude was 30 μm to 50 μm, and tungsten steel shots with a diameter of 0.5 mm to 3.0 mm were selected. The sample surface was repeatedly subjected to high-frequency impact treatment in a closed chamber for 0 min to 10 min.
[0036] Among them, high-temperature tempering, quenching and tempering processes are all carried out in a vacuum heat treatment furnace to prevent surface decarburization.
[0037] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is further described below in conjunction with embodiments and drawings, so as to make a clearer and more definite definition of the protection scope of the present invention.
[0038] Example 1
[0039] In this embodiment (numbered Untreated), a treatment method for eliminating large-sized carbides in the carburized surface layer of rare earth M50NiL steel is determined, wherein:
[0040] The chemical composition and mass percentage of rare earth M50NiL steel include: C 0.12wt.%, Si 0.23wt.%, Cr 4.14wt.%, Mo 4.31wt.%, V 1.25wt.%, Ni 3.39wt.%, Mn 0.23wt.%, the total amount of Ce and La is 0.005wt.% (the mass fraction ratio of Ce to La is 3:2), P 0.01wt.%, S 0.0014wt.%, and the balance is Fe, totaling 100wt.%.
[0041] The samples that meet the chemical composition requirements are gas carburized for 25 hours in the carburizing atmosphere created by the RX gas generator, with the carburizing temperature at 930℃. After carburizing, they are cooled to room temperature with the furnace; in a vacuum heat treatment furnace, they are subjected to high-temperature tempering at a tempering temperature of 750℃ for 5 hours, then the furnace is cooled to 550℃, and then taken out of the furnace and air-cooled to room temperature; in a vacuum heat treatment furnace, they are first heated to 650℃ at a heating rate of 200℃ / h for 0.5h preheating and heat preservation, then heated to 850℃ at a heating rate of 200℃ / h for 0.5h preheating and heat preservation, and then heated to quenching temperature of 1100℃ at a heating rate of 200℃ / h for 0.5h preheating and heat preservation. The time is 0.5h, and then oil-cooled to room temperature; deep cryogenic treatment is performed immediately after quenching, cooling to -80℃ at a cooling rate of 50℃ / h, and keeping warm at this temperature for 2h, and then heating to room temperature at the same heating rate; tempering treatment is performed in a vacuum heat treatment furnace, heating to 280℃ at a heating rate of 250℃ / h, preheating and keeping warm for 0.5h, and then heating to the tempering temperature of 540℃ at a heating rate of 250℃ / h, keeping warm for 2h, and then air-cooling to room temperature. This process is repeated three times; the heat-treated sample is ground using a grinder, the processing amount is 0.5mm, and the surface quality is guaranteed; this embodiment does not perform surface deformation treatment.
[0042] Example 2
[0043] In this embodiment (No. Treated-5), a treatment method for eliminating large-sized carbides in the carburized surface layer of rare earth M50NiL steel is determined, wherein:
[0044] The chemical composition and mass percentage of rare earth M50NiL steel include: C 0.12wt.%, Si 0.23wt.%, Cr 4.14wt.%, Mo 4.31wt.%, V 1.25wt.%, Ni 3.39wt.%, Mn 0.23wt.%, the total amount of Ce and La is 0.005wt.% (the mass fraction ratio of Ce to La is 3:2), P 0.01wt.%, S 0.0014wt.%, and the balance is Fe, totaling 100wt.%.
[0045] The samples that meet the chemical composition requirements are gas carburized for 25 hours in a carburizing atmosphere created by an RX gas generator, with a carburizing temperature of 930°C. After carburizing, they are cooled to room temperature with the furnace; in a vacuum heat treatment furnace, they are subjected to high-temperature tempering, with a tempering temperature of 750°C and a holding time of 5 hours, then the furnace is cooled to 550°C, and then taken out of the furnace and air-cooled to room temperature; in a vacuum heat treatment furnace, they are first heated to 650°C at a heating rate of 200°C / h for 0.5h preheating and holding, then heated to 850°C at a heating rate of 200°C / h for 0.5h preheating and holding, then heated to quenching temperature of 1100°C at a heating rate of 200°C / h for 0.5h preheating and holding, and then oil-cooled to room temperature; deep freezing treatment is immediately performed after quenching, and the temperature is cooled at a cooling rate of 50°C / h To -80℃, and keep it at this temperature for 2h, and then heat it to room temperature at the same heating rate; in a vacuum heat treatment furnace, carry out tempering treatment, heat it to 280℃ at a heating rate of 250℃ / h, preheat and keep it for 0.5h, and then heat it to the tempering temperature of 540℃ at a heating rate of 250℃ / h, keep it warm for 2h, and then air cool it to room temperature. This process is repeated three times; the heat-treated sample is ground using a grinder with a processing volume of 0.5mm and the surface quality is guaranteed; surface deformation treatment is carried out using an ultrasonic shot peening device, the ultrasonic generator operating frequency is set to 20kHz, the amplitude is 40μm, and YG8 tungsten steel shot with a diameter of 2mm is selected. The sample surface is repeatedly subjected to high-frequency impact treatment in a closed chamber for 5min.
[0046] Example 3
[0047] In this embodiment (No. Treated-10), a treatment method for eliminating large-sized carbides in the carburized surface layer of rare earth M50NiL steel is determined, wherein:
[0048] The chemical composition and mass percentage of rare earth M50NiL steel include: C 0.12wt.%, Si 0.23wt.%, Cr 4.14wt.%, Mo 4.31wt.%, V 1.25wt.%, Ni 3.39wt.%, Mn 0.23wt.%, the total amount of Ce and La is 0.005wt.% (the mass fraction ratio of Ce to La is 3:2), P 0.01wt.%, S 0.0014wt.%, and the balance is Fe, totaling 100wt.%.
[0049] The samples that meet the chemical composition requirements are gas carburized for 25 hours in a carburizing atmosphere created by an RX gas generator, with a carburizing temperature of 930°C. After carburizing, they are cooled to room temperature with the furnace; in a vacuum heat treatment furnace, they are subjected to high-temperature tempering, with a tempering temperature of 750°C and a holding time of 5 hours, then the furnace is cooled to 550°C, and then taken out of the furnace and air-cooled to room temperature; in a vacuum heat treatment furnace, they are first heated to 650°C at a heating rate of 200°C / h for 0.5h preheating and holding, then heated to 850°C at a heating rate of 200°C / h for 0.5h preheating and holding, then heated to quenching temperature of 1100°C at a heating rate of 200°C / h for 0.5h preheating and holding, and then oil-cooled to room temperature; deep freezing treatment is immediately performed after quenching, and the temperature is cooled at a cooling rate of 50°C / h To -80℃, and keep it at this temperature for 2h, and then heat it to room temperature at the same heating rate; in a vacuum heat treatment furnace, carry out tempering treatment, heat it to 280℃ at a heating rate of 250℃ / h, preheat and keep it for 0.5h, and then heat it to the tempering temperature of 540℃ at a heating rate of 250℃ / h, keep it warm for 2h, and then air cool it to room temperature. This process is repeated three times; the heat-treated sample is ground using a grinder with a processing volume of 0.5mm and the surface quality is guaranteed; surface deformation treatment is carried out using an ultrasonic shot peening device, the ultrasonic generator operating frequency is set to 20kHz, the amplitude is 40μm, and YG8 tungsten steel shot with a diameter of 2mm is selected. The sample surface is repeatedly subjected to high-frequency impact treatment in a closed chamber for 10min.
[0050] like Figure 1 As shown in the SEM image of the carbide distribution in the carburized surface without surface deformation treatment, it can be seen that in addition to small circular carbides, there are also a large number of large rod-shaped carbides in the structure, which increases the difference in size and shape between the carbides in the carburized surface. These large carbides are very likely to cause stress concentration under the action of alternating stress during service, leading to the initiation and propagation of cracks, and ultimately causing fatigue failure of bearing parts.
[0051] like Figure 2-Figure 3 As shown in Figure 2, SEM images of the carbide distribution in the carburized surface after 5 and 10 minutes of surface deformation treatment show that the carburized surface structure has undergone significant plastic deformation. Due to the influence of dislocation movement, the number density of large carbides in this area has been significantly reduced, and the uniformity of carbide size has been significantly improved. In addition, the longer the treatment time, the more significant the improvement of carbides.
[0052] like Figure 4As shown in the comparison of the wear rates of the three examples under the conditions of oil lubrication, a load of 120N, a stroke of 10mm, and a frequency of 4Hz, which are reciprocating for 0.5h, it can be seen that the wear rates of Untreated, Treated-5, and Treated-10 are 3.266×10 -9 mm 3 / N·m, 2.208×10 -9 mm 3 / N·m and 1.507×10 -9 mm 3 / N·m, indicating that the wear rate of the sample increased by 32.4% and 53.9% after treatment for 5min and 10min, respectively.
[0053] Comparing the test results of the above embodiments, it can be shown that the surface deformation treatment can effectively eliminate large-sized carbides in the carburized surface layer of rare earth M50NiL steel, reduce the number density of large-sized carbides, improve the uniformity of carbide size distribution in the organization, significantly improve the wear resistance of the material, and meet the performance requirements of current aircraft engine bearings.
[0054] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the field can easily think of various equivalent modifications or replacements within the technical scope disclosed by the present invention, and these modifications or replacements should all be covered by the protection scope of the present invention.
Claims
1. A method for eliminating large-sized carbides in the carburized surface layer of rare earth M50NiL steel, characterized in that: The chemical composition and mass percentage of rare earth M50NiL steel include: C 0.11wt.% - 0.15wt.%, Si 0.10wt.% - 0.25wt.%, Cr 4.00wt.% - 4.25wt.%, Mo 4.00wt.% - 4.50wt.%, V 1.13wt.% - 1.33wt.%, Ni 3.20wt.% - 3.60wt.%, Mn 0.15wt.% - 0.35wt.%, 0 < total amount of Ce and La ≤ 0.02wt.%, P ≤ 0.01wt.%, S ≤ 0.01wt.%, and the balance is Fe.
2. A method for eliminating large-sized carbides in the carburized surface layer of rare earth M50NiL steel according to claim 1, characterized in that: Preferably, the total amount of Ce and La is 0.003wt.% - 0.02wt.%, and the mass fraction ratio of Ce to La elements is 3:(1 - 2).
3. A method for eliminating large-sized carbides in the carburized surface layer of rare earth M50NiL steel according to claim 1, characterized in that: The as-cast billet of rare earth M50NiL steel is made by a double-vacuum smelting method of vacuum induction + vacuum consumable.
4. A method for eliminating large-sized carbides in the carburized surface layer of rare earth M50NiL steel according to any one of claims 1 to 3, characterized in that: It includes processes such as surface carburizing, high-temperature tempering, quenching, cryogenic treatment, tempering, machining, and surface deformation treatment. The specific steps are as follows: (1) Surface carburizing: The sample is subjected to gas carburizing treatment for 20h - 40h in the carburizing atmosphere created by an RX gas generator. The carburizing temperature is 930 ± 20°C, and after carburizing, it is cooled to room temperature with the furnace. (2) High-temperature tempering: After surface carburizing treatment, high-temperature tempering is carried out. The tempering temperature is 750 ± 20°C, the holding time is 4h - 6h, then it is cooled in the furnace to 550 ± 20°C, and then taken out of the furnace and air-cooled to room temperature. (3) Quenching: After high-temperature tempering, it is first heated to 650 ± 20°C at a heating rate of 100°C - 300°C / h for 0.5h - 1h for preheating and holding, then heated to 850 ± 20°C at a heating rate of 100°C - 300°C / h for 0.5h - 1h for preheating and holding, and then heated to the quenching temperature of 1100 ± 20°C at a heating rate of 100°C - 300°C / h. The holding time is 0.5h - 1h, and then it is oil-cooled to room temperature. (4) Cryogenic treatment: After quenching, cryogenic treatment is carried out quickly within 1h. The cooling rate is 25°C - 100°C / h to cool down to -196°C - -40°C, and it is held at this temperature for 2h - 4h, and then heated to room temperature at the same heating rate. (5) Tempering: After cryogenic treatment, tempering treatment is carried out. It is heated to 280 ± 20°C at a heating rate of 100°C - 300°C / h for 0.5h - 1h for preheating and holding, then heated to the heating temperature of 500°C - 580°C at a heating rate of 100°C - 300°C / h. The holding time is 1h - 3h, and then air-cooled to room temperature. This process is repeated 2 - 4 times. (6) Machining: The heat-treated sample is ground by a grinding machine to ensure the surface quality, and the machining amount is 0.1mm - 0.5mm. (7) Surface deformation: An ultrasonic shot peening device was used. The operating frequency of the ultrasonic generator was set to 20 ± 1 kHz, the amplitude was 30 μm to 50 μm, and tungsten steel shots with a diameter of 0.5 mm to 3.0 mm were selected. The sample surface was repeatedly subjected to high-frequency impact treatment in a closed chamber for 0 min to 10 min.
5. A method for eliminating large-sized carbides in the carburized surface layer of rare earth M50NiL steel according to claim 4, characterized in that: High temperature tempering, quenching and tempering processes are all carried out in a vacuum heat treatment furnace to prevent surface decarburization.
Citation Information
Cited By
High-temperature carburizing bearing steel and preparation method thereof
CN121109855A