TC bearing and preparation method and application thereof
By plating nickel on the surface of the cemented carbide of TC bearings, the diffusion of copper elements is blocked and a dense composite structure is formed, which solves the problem of insufficient wear resistance and corrosion resistance of existing TC bearings, and significantly improves the service life.
Patent Information
- Application Number
- CN202510669422.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-23
- Publication Date
- 2025-08-08
AI Technical Summary
In the existing TC bearing preparation process, the diffusion and permeation of copper lead to a degradation of cemented carbide performance, insufficient wear resistance and corrosion resistance, which affects service life.
Nickel plating is performed on the surface of the cemented carbide, the copper element diffusion is blocked through the nickel layer, and mixed with the copper alloy impregnation material during the sintering process to form a dense composite structure to improve corrosion resistance and wear resistance.
It effectively avoids the diffusion of copper elements on cemented carbide, improves the wear resistance and corrosion resistance of TC bearings, and extends the service life.
Smart Images

Figure CN120443184A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of bearings, and in particular to a TC bearing and a preparation method and application thereof. Background Art
[0002] TC bearings are one of the important accessories in screw power drill tools used in oil exploration and drilling. Downhole power drill tools rely on TC bearings to withstand harsh working conditions such as impact, friction, and corrosion. Their reliability and life are crucial to ensuring smooth drilling. The quality and performance of TC bearings are directly related to the life of the entire drill tool and are the key components affecting the life of screw drill tools.
[0003] Currently, TC bearings are mostly manufactured using a high-temperature furnace sintering and infiltration process, where the impregnation material, tungsten carbide powder, and cemented carbide are sintered and fused together, followed by machining. This process ensures that the sintered layer is firmly bonded to the steel body, preventing flaking or shedding, effectively improving bearing quality. However, this process also has drawbacks: during the TC bearing sintering and infiltration process, the copper-based impregnation material remains in a liquid phase for at least one hour. Due to the prolonged sintering time, the liquid copper-based solder coats the surfaces of the cemented carbide and the steel substrate for a long time, diffusing and infiltrating with the W and Co elements in the cemented carbide and the Fe elements in the steel substrate. This severely degrades the physical properties of the cemented carbide, destroys the structure of the bonding phase on the cemented carbide surface, reduces the hardness and bending strength of the cemented carbide, and significantly reduces the alloy toughness and wear resistance of the TC bearing. Furthermore, weak links form in the areas where the copper-based solder diffuses and infiltrates, accelerating wear and shortening the service life of the TC bearing.
[0004] In addition, the TC bearings in downhole power drilling tools operate in a mud environment containing sand particles, which is extremely harsh working conditions. The drilling fluid constantly erodes and corrodes them. Cobalt, as a binder for cemented carbide, is easily oxidized and corroded, causing the cemented carbide blocks to fail, affecting the drilling process and easily wasting huge manpower and material resources.
[0005] In view of this, the present invention is proposed. Summary of the Invention
[0006] The first purpose of the present invention is to provide a method for preparing TC bearings, which is mainly used to solve the negative impact of copper diffusion and infiltration on bearing performance during the sintering and infiltration process of conventional preparation technology, or the defect of insufficient corrosion resistance of conventional bearing products.
[0007] A second object of the present invention is to provide a TC bearing that has significantly enhanced wear resistance and corrosion resistance, thereby further increasing the service life of the TC bearing.
[0008] A third object of the present invention is to provide the use of the TC bearing in oil drilling, including but not limited to a drilling tool product containing the TC bearing, or an oil drilling process performed using a drilling tool product containing the TC bearing.
[0009] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are adopted:
[0010] A method for preparing a TC bearing comprises the following steps:
[0011] The cemented carbide is nickel plated to obtain a cemented carbide with a nickel layer on the surface; and then the cemented carbide is welded to a matching mold to obtain a matching mold loaded with the cemented carbide;
[0012] Assembling the loaded cemented carbide die and the bearing base, and filling the cast tungsten carbide in an oscillating state to obtain a dense composite assembly;
[0013] Welding the supporting die of the loaded cemented carbide to the bottom of the bearing base, and performing heat preservation treatment on the welding points to obtain a composite weldment;
[0014] The composite weldment is mixed with a copper alloy impregnating material and dehydrated borax, and sintered. After sintering, the TC bearing is obtained by machining.
[0015] A TC bearing is manufactured based on the manufacturing method of the TC bearing, and the use of the TC bearing in oil drilling.
[0016] Compared with existing technologies, the present invention offers the following advantages: It specifically provides a process for preparing TC bearings. By innovatively plating the cemented carbide surface with nickel, it effectively prevents copper from penetrating into the carbide layer in subsequent high-temperature environments, thereby improving the wear resistance of the TC bearings. Furthermore, the penetration of nickel during the sintering process enhances the corrosion resistance of the carbide, further extending the service life of the TC bearings. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] In order to more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the specific embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0018] Figure 1 A schematic diagram of copper diffusion in the preparation method of the present invention is provided. DETAILED DESCRIPTION
[0019] The technical solution of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments. However, it will be understood by those skilled in the art that the following embodiments are only some embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially. In addition, the terms "first", "second" and "third" are only used for descriptive purposes and are not to be construed as indicating or implying relative importance.
[0020] The present invention provides a method for preparing a TC bearing, a TC bearing product obtained using the method, and the use of the TC bearing product in oil drilling. The following describes the specific implementation of the method.
[0021] The preparation method of the TC bearing mainly includes the following steps: (1) nickel-plating the cemented carbide to obtain a cemented carbide with a nickel layer on the surface; then welding the cemented carbide to a matching mold to obtain a matching mold for loading cemented carbide; (2) assembling the matching mold for loading cemented carbide with a bearing base, filling cast tungsten carbide under an oscillating state, and obtaining a dense composite assembly component; (3) welding the matching mold for loading cemented carbide and the bottom of the bearing base, and heat-insulating the welding point to obtain a composite weldment; (4) mixing the composite weldment with a copper alloy impregnation material and dehydrated borax, and sintering the composite weldment. After sintering, the composite weldment is machined to obtain a TC bearing.
[0022] As a preferred embodiment, the cemented carbide adopts tungsten-cobalt cemented carbide, and its cobalt content is 3% to 30%, including but not limited to any one of 3%, 5%, 8%, 10%, 12%, 15%, 18%, 20%, 22%, 25%, 28%, 30% or a numerical range composed of any two, and is further preferably 6wt.% to 14wt.%; in some more preferred embodiments, the cemented carbide includes at least one of YG6, YG8, YG12 or YG14.
[0023] As a preferred embodiment, the shape of the cemented carbide includes but is not limited to a cylinder, a cuboid or a prism, etc. In some more preferred embodiments, when the cemented carbide adopts tungsten-cobalt cemented carbide, the grain size of the tungsten carbide therein is 1μm to 30μm.
[0024] As a preferred embodiment, the cemented carbide can be purchased directly through commercial channels or prepared by conventional powder metallurgy processes; when the latter is adopted, those skilled in the art can adaptively adjust the metal powder ratio, molding and high-temperature densification conditions according to the composition of the cemented carbide to obtain the cemented carbide that meets the requirements.
[0025] As a preferred embodiment, the thickness of the nickel layer obtained after the nickel plating treatment is 0.01mm to 0.3mm, including but not limited to any one of 0.01, 0.02, 0.05, 0.08, 0.1, 0.12, 0.15, 0.18, 0.2, 0.22, 0.25, 0.28, 0.3 (mm) or a numerical range composed of any two of them.
[0026] It should also be emphasized that the nickel layer is plated on all outer surfaces of the cemented carbide; for example, when the cemented carbide is a rectangular parallelepiped, the nickel layer is plated on all six outer surfaces; and for example, when the cemented carbide is a cylinder, the nickel layer is plated on the upper and lower bottom surfaces and curved side surfaces.
[0027] As a preferred embodiment, the nickel plating process includes the following steps: firstly performing chemical plating on the surface of the cemented carbide, and then performing electroplating to obtain an inner chemical plating layer and an outer electroplating layer, which together serve as the nickel layer.
[0028] As a more preferred embodiment, the chemical plating includes the following steps: immersing the surface cemented carbide in a nickel solution, adjusting the pH to 4 to 6, conducting a chemical reaction for 1 hour to 10 hours, and then separating to obtain a cemented carbide coated with a chemical plating layer; wherein, in some optional embodiments, the nickel solution includes nickel sulfate, sodium citrate, sodium hypophosphite and water. As some reference characteristics, in the nickel solution, the concentration of nickel sulfate is 100g / L to 250g / L, the concentration of sodium citrate is 6g / L to 18g / L, and the concentration of sodium hypophosphite is 0.15mol / L to 0.35mol / L.
[0029] As a more preferred embodiment, the electroplating includes the following steps: using nickel as the anode and the cemented carbide coated with the chemical plating layer as the cathode, adjusting the pH of the electroplating solution to 4-6 and then electroplating to obtain the cemented carbide with the nickel layer on the surface; wherein, in some optional embodiments, the electroplating solution includes nickel sulfate, boric acid, sodium chloride, sodium dodecyl sulfate and water. As some reference characteristics, in the electroplating solution, the concentration of nickel sulfate is 100g / L~300g / L, the concentration of boric acid is 20g / L~40g / L, the concentration of sodium chloride is 6g / L~20g / L, and the concentration of sodium dodecyl sulfate is 0.1g / L; in other optional embodiments, the voltage of the electroplating operation is 2V~4V, the current is 0.5A~3A, and the time of the electroplating operation is 1h~120h.
[0030] As a preferred embodiment, before the first welding (i.e., before the welding of step (1)), the following pretreatment step is also included: the cemented carbide with a nickel-plated surface, the matching mold and the bearing substrate are placed in boiling borax for purification to improve the bonding strength between the bearing steel substrate and the cemented carbide.
[0031] As a preferred embodiment, welding the nickel-plated cemented carbide to the matching mold includes the following steps: according to the size of the substrate and the preset distribution of the cemented carbide on the substrate, a PET plate tooling mold with a corresponding structure is prepared, and the nickel-plated cemented carbide is arranged and bonded to the surface of the tape with small holes through the PET plate tooling mold, and the position of the small hole is the same as the position of the nickel-plated cemented carbide; then the nickel-plated cemented carbide at the position of the small hole is fixed to the matching mold by spot welding.
[0032] The present invention obtains cemented carbides with corresponding position distribution through a PET plate tooling mold with a specific structure, and fixes them with a tape with small holes, which is conducive to fixing these cemented carbides with specific position distribution on the surface of the mold in the subsequent steps; through the specific angles, spacing and other arrangement characteristics of the cemented carbides, it can effectively withstand harsh working conditions such as mud scouring and quartz sand wear, and at the same time simply achieves precise correspondence between the cemented carbides and the grooves, steps and other structures of the bearing base introduced in the subsequent steps.
[0033] As a preferred embodiment, the bearing base is a steel base, and the material of the steel base includes but is not limited to 4140, 4340, 4145H Mod, 4330V, 17-4PH, etc.
[0034] As a preferred embodiment, the particle size of the cast tungsten carbide ranges from 50 μm to 200 μm.
[0035] It is understandable that in the art, after the matching mold of the loaded cemented carbide and the bearing matrix are assembled, the cast tungsten carbide is filled into the gaps of the assembled composite parts; on the one hand, the cast tungsten carbide is used to achieve the embedding between the cemented carbide particles, and on the other hand, the cast tungsten carbide is used to ensure the densification of the bearing matrix. Based on the filling of the cast tungsten carbide, high wear resistance, high impact resistance and high thermal stability are achieved, thereby overall improving the service life of the TC bearing.
[0036] As a preferred embodiment, those skilled in the art can measure the amount of cast tungsten carbide by measuring the volume of the assembly gap between the die for loading the cemented carbide and the bearing base; in some optional embodiments, the filling height of the cast tungsten carbide is 10 mm to 20 mm higher than the cemented carbide loaded on the die.
[0037] As a preferred embodiment, the oscillation state is implemented by an oscillator, the amplitude of the oscillation state is 0.1 mm to 2 mm, and the vibration frequency of the oscillation state is 100 Hz to 5000 Hz.
[0038] As a preferred embodiment, in the oscillation state, it also includes: rotating and tapping the matching mold and bearing base of the loaded cemented carbide; in some more preferred embodiments, the frequency of the rotation is 0.5rpm~10rpm, that is, it is preferably carried out by manual rotation; the granularity of the tapping is 10N~200N, and the frequency of the tapping is 20~200 times / min.
[0039] As a preferred embodiment, welding the loaded cemented carbide die and the bottom of the bearing base means that: the loaded cemented carbide die and the bearing base are welded in the contact area at the bottom; the welding methods described here include but are not limited to arc welding, carbon dioxide gas shielded welding, laser welding, argon arc welding, etc. As long as a tight welding can be achieved, there is no strict restriction on the welding process.
[0040] As a preferred embodiment, the insulation treatment includes the following steps: covering and protecting the welding points with insulation materials to maintain the temperature at the welding points from dropping too quickly, thereby enhancing the firmness of the welding; in some more preferred embodiments, the insulation materials include but are not limited to insulation cotton, ceramic fiber felt, silicate composite felt, aerogel composite cloth, composite insulation sleeves, etc.
[0041] As a preferred embodiment, the effective ingredients of the copper alloy impregnating material include copper, nickel, zinc and manganese, and the mass ratio of the copper element in the copper alloy impregnating material is 40wt.% to 72wt.%, including but not limited to any one of 42, 45, 48, 50, 52, 55, 58, 60, 62, 65, 68, 70, 72 (wt.%) or a numerical range consisting of any two of them.
[0042] As a more preferred embodiment, the effective components of the copper alloy impregnating material include: Cu 47wt.% to 57wt.%, Ni 14wt.% to 16wt.%, Zn 7wt.% to 9wt.%, and Mn 23wt.% to 25wt.%.
[0043] As a preferred embodiment, the mass ratio of the copper alloy impregnating material to the cast tungsten carbide is (0.7-1.5):1, including but not limited to any one of 0.7:1, 0.8:1, 0.9:1, 1:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1, and 1.5:1, or a ratio range consisting of any two of the above.
[0044] As a preferred embodiment, the mass ratio of the dehydrated borax to the cast tungsten carbide is 1:(50-400), including but not limited to any one of 1:50, 1:80, 1:100, 1:150, 1:200, 1:250, 1:300, 1:350, 1:375, 1:400 or a ratio interval consisting of any two of them.
[0045] As a preferred embodiment, the sintering treatment temperature is 850°C to 1250°C, including but not limited to any one of 850, 900, 950, 1000, 1050, 1100, 1150, 1200, 1250 (°C) or a numerical range consisting of any two of them; the sintering treatment time is 50min to 80min, including but not limited to any one of 50, 55, 60, 65, 70, 80 (min) or a numerical range consisting of any two of them.
[0046] As a preferred embodiment, after the sintering treatment, when the bearing precursor is cooled to 300°C to 400°C, it is kept warm for 0.1h to 24h; during the cooling process, necessary insulation measures can be taken according to the temperature and material.
[0047] As a preferred embodiment, the machining primarily involves performing necessary finishing operations to improve the dimensional accuracy, shape tolerance, and surface quality of the TC bearing. The specific process methods are not specifically limited in this disclosure. It is worth noting that the machining also involves lathing and grinding the mating die. Specifically, the mating die serves to create a gap with the bearing base for filling the infiltration material, but it does not constitute a component of the TC bearing.
[0048] like Figure 1 FIG. 1 shows a schematic diagram of copper diffusion during the sintering process of the present invention. Figure 1 The main body of the material includes a cemented carbide region uninfiltrated by copper (corresponding to the blank area in the center of the figure), followed by a cemented carbide region diffusely infiltrated by copper (corresponding to the Cu diffusion zone in the figure), a nickel layer coated on the outside of the cemented carbide (corresponding to the nickel layer in the figure), and a pile of added copper alloy impregnation material and dehydrated borax (corresponding to the infiltration layer in the figure). During the preparation process, as the sintering temperature increases, the copper alloy impregnation material melts under the action of the borax flux. Driven by gravity, the molten copper alloy impregnation material gradually infiltrates and fills the gaps between the cast tungsten carbide particles, forming a composite structure with cast tungsten carbide as the skeleton material and copper alloy as the matrix binder phase, achieving a metallurgical bond between the cast tungsten carbide, cemented carbide, and the die assembly. Under comparable conditions without the nickel-plated cemented carbide of the present invention, the Cu element in the copper alloy significantly interdiffused with the W and Co elements in the cemented carbide matrix. However, when the nickel-plated cemented carbide of the present invention is used, the nickel coating on its surface effectively blocks the diffusion pathways, resulting in only trace amounts of Cu diffusing into the cemented carbide matrix, accompanied by limited interdiffusion of Ni with W and Co. Due to the improved compatibility of Ni with the cemented carbide matrix, its diffusion significantly reduces the negative impact on key performance indicators such as the wear resistance of the cemented carbide compared to Cu diffusion, effectively maintaining the wear resistance of the cemented carbide matrix and ensuring the overall performance stability of the TC bearing product.
[0049] Example 1
[0050] (1) Prepare a cemented carbide (YG8) with a cobalt content of 8% and a rectangular parallelepiped shape (length 12 mm * width 5 mm * height 3 mm).
[0051] (2) Nickel plating of cemented carbide:
[0052] (2.1) The cemented carbide was placed in a mixture containing 180 g / L nickel sulfate, 12 g / L sodium citrate, and 0.22 mol / L sodium hypophosphite. The pH value of the solution was adjusted to 4.5 with phosphoric acid. The solution was allowed to react for 2 h and then washed. The solution was then placed in a vacuum furnace and heated to 400°C. The temperature was kept constant for 2 h and then cooled to 200°C for use.
[0053] (2.2) A mixed solution containing 150 g / L nickel sulfate, 35 g / L boric acid, 15 g / L sodium chloride, and 0.1 g / L sodium dodecyl sulfate was prepared as an electroplating solution, and the pH value of the solution was adjusted to 4.5. Then, nickel was used as the anode and the chemically nickel-plated cemented carbide was used as the cathode. The electroplating was started with a current of 2 A, a voltage of 3 V, and an electroplating time of 24 hours. The solution was then washed and dried to obtain a nickel-plated cemented carbide composite material with a total nickel plating thickness of 0.05 mm.
[0054] (3) The nickel-plated carbide, the machined substrate (made of 4140 steel), and the matching mold (45# steel) were placed in boiling borax for purification.
[0055] (4) According to the preset inner and outer sleeve dimensions of the TC bearing, the nickel-plated carbide is arranged and designed, and a corresponding PET plate tooling mold (hereinafter referred to as the "mold") is carved; the nickel-plated carbide is arranged and bonded to a tape with small holes through the mold, and then the alloy is fixed to the mold using a spot welder, and the working voltage of the spot welder is set to 10V and the current is set to 100A.
[0056] (5) The die welded with nickel-plated cemented carbide is matched with the steel substrate, and a layer of cast tungsten carbide powder is pre-placed in the gap between the substrate and the die, and the powder stacking height is controlled to be 15±0.5mm above the cemented carbide; a total of 2156 grams of cast tungsten carbide is filled into the gap, so that the cast tungsten carbide powder is 15mm higher than the cemented carbide block. The filling process should always be carried out on the oscillator, with an oscillation amplitude of 0.5mm and a frequency of 1000Hz, and it should be knocked while rotating, with a rotation frequency of 3rpm, a knocking force of 50N, and a knocking frequency of 100 times / min.
[0057] (6) Use argon arc welding to weld the bearing base and the bottom of the matching mold. Set the welding parameters as follows: welding current 150A, argon gas flow 8L / min, and the distance between the nozzle and the workpiece is about 10mm. After welding, the welding point is insulated with thermal insulation cotton and kept warm for 1 hour.
[0058] (7) After the insulation is completed, 1830g of copper alloy impregnation material (54.2wt.% copper, 14.5wt.% nickel, 7.2wt.% zinc, 23.9% manganese, and the remainder is impurities) is added to the cast tungsten carbide powder layer, and then 12g of dehydrated borax is added.
[0059] (8) After the sintering furnace is raised to 1180°C, the bearing precursor and the mixed material are placed in the sintering furnace for sintering. After 60 minutes, they are taken out and cooled. After the temperature reaches 350°C, they are placed in a heat preservation furnace and kept warm for 6 hours, and then slowly cooled to room temperature.
[0060] (9) The sintered bearing is machined to the finished size to obtain the TC bearing of this embodiment.
[0061] Example 2
[0062] The method is basically the same as Example 1, except that the electroplating time in step (2.2) is extended until a nickel-plated cemented carbide composite material with a total nickel plating layer thickness of 0.15 mm is obtained.
[0063] Example 3
[0064] The method is basically the same as Example 1, except that the electroplating time in step (2.2) is extended until a nickel-plated cemented carbide composite material with a total nickel plating layer thickness of 0.25 mm is obtained.
[0065] Example 4
[0066] The method is basically the same as Example 1, with the only difference being that the cemented carbide raw material in step (1) is replaced with YG11 (with a cobalt content of 11%), with a size of 13 mm*5 mm*2.5 mm.
[0067] Example 5
[0068] The process is basically the same as Example 1, except that the amount of copper alloy impregnating material in step (7) is replaced with 3234 g.
[0069] Example 6
[0070] The process is basically the same as Example 1, except that the sintering time of the sintering furnace in step (8) is replaced with 120 min.
[0071] Comparative Example
[0072] It is basically the same as Example 1, except that step (2) is cancelled, and the "nickel-plated cemented carbide" in the subsequent steps is replaced by the cemented carbide raw material in step (1).
[0073] Test example
[0074] (1) The diffusion depth of copper alloy into cemented carbide was calculated by SEM backscattered electron imaging and EDS energy spectrometer line scanning.
[0075] (2) The chemical composition of the copper diffusion area in the cemented carbide was analyzed by EDS energy spectrometer, and the mass content of copper elements in the diffusion area was calculated.
[0076] (3) The wear resistance of the TC bearings in each embodiment and comparative example was measured. The alloys sintered and infiltrated in step 8 were subjected to a grinding test. A grinding test was performed on a grinder and polisher with the speed of the grinder set at 500 rpm. After grinding for 10 minutes, the weight loss of the alloys was weighed and recorded.
[0077] Table 1 provides the results of the above experiments (1) to (3).
[0078] Table 1
[0079]
[0080] As can be seen from Table 1, the present invention forms a metal barrier layer by nickel plating the cemented carbide. The nickel-based barrier blocks the migration of copper elements to the hard phase lattice during the infiltration process and maintains the integrity of the tungsten carbide skeleton, which can significantly improve the wear resistance of the cemented carbide after infiltration, thereby increasing the service life of the bearing.
[0081] Although the present invention has been illustrated and described using specific embodiments, it should be appreciated that the above embodiments are merely intended to illustrate the technical solutions of the present invention rather than to limit them. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents, without departing from the spirit and scope of the present invention. However, these modifications or replacements do not deviate from the essence of the corresponding technical solutions within the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.
Claims
1. A method for preparing a TC bearing, characterized in that: The steps include: The cemented carbide is nickel plated to obtain a cemented carbide with a nickel layer on the surface; and then the cemented carbide is welded to a matching mold to obtain a matching mold loaded with the cemented carbide; Assembling the loaded cemented carbide die and the bearing base, and filling the cast tungsten carbide under oscillation to obtain a dense composite assembly; Welding the loaded cemented carbide die to the bottom of the bearing base, and performing heat preservation treatment on the welding points to obtain a composite weldment; The composite weldment is mixed with a copper alloy impregnating material and dehydrated borax, and sintered. After sintering, the TC bearing is obtained by machining.
2. The preparation method according to claim 1, characterized in that The cemented carbide comprises a tungsten-cobalt cemented carbide, and the cobalt content in the cemented carbide is 3wt.% to 30wt.%; Preferably, the cobalt content in the cemented carbide is 6 wt.% to 14 wt.%.
3. The preparation method according to claim 1, characterized in that The nickel layer obtained by the nickel plating treatment has a thickness of 0.01 mm to 0.3 mm; Preferably, the nickel plating treatment comprises the following steps: firstly performing chemical plating on the surface of the cemented carbide, and then performing electroplating to obtain the cemented carbide with a nickel layer plated on the surface.
4. The preparation method according to claim 1, characterized in that The steps of welding the nickel-plated hard alloy to the die include: Preparing a PET plate tooling mold; arranging and bonding the nickel-plated hard alloy to the surface of the tape with small holes through the PET plate tooling mold, wherein the positions of the small holes are the same as the positions of the nickel-plated hard alloy; Then the hard alloy with nickel coating on the surface is fixed on the matching mold by spot welding.
5. The preparation method according to claim 1, characterized in that The particle size of the cast tungsten carbide ranges from 50 μm to 200 μm.
6. The preparation method according to claim 1, characterized in that The amplitude of the oscillation state is 0.1 mm to 2 mm, and the vibration frequency of the oscillation state is 100 Hz to 5000 Hz; Preferably, while in the oscillating state, the method further comprises: rotating and striking the matching die and the bearing base of the loaded cemented carbide; The rotation frequency is 0.5 rpm to 10 rpm, the knocking force is 10 N to 200 N, and the knocking frequency is 20 to 200 times / min.
7. The preparation method according to claim 1, characterized in that The copper alloy impregnation material comprises copper, nickel, zinc and manganese, and the mass ratio of the copper element in the copper alloy impregnation material is 40wt.% to 72wt.%; Preferably, the mass ratio of the copper alloy impregnating material to the cast tungsten carbide is (0.7-1.5):1; Preferably, the mass ratio of the dehydrated borax to the cast tungsten carbide is 1:(50-400).
8. The preparation method according to claim 1, characterized in that The sintering temperature is 850° C. to 1250° C., and the sintering time is 50 min to 80 min.
9. A TC bearing produced by the method for producing a TC bearing according to any one of claims 1 to 8.
10. Use of the TC bearing according to claim 9 in oil drilling.