A method for spray forming of tunnel structure lining

The template-free tunnel lining spray molding method solves the problems of high cost, insufficient density and poor impermeability in traditional tunnel lining construction, and realizes efficient and low-cost tunnel lining construction, thereby improving the structural performance and service life of the tunnel.

CN120626205BActive Publication Date: 2026-11-10SHANGHAI TONGMIN NEW MATERIAL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202511015195.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-07-23
Publication Date
2026-11-10
Estimated Expiration
2045-07-23

AI Technical Summary

Technical Problem

Traditional tunnel lining construction methods suffer from high costs, insufficient concrete density, and poor impermeability, which affect the safety and service life of tunnels.

Method used

A templateless tunnel lining spraying method is adopted, using a quick-release or mobile operating platform. High-flowability concrete and calcium sulfoaluminate are combined to adjust the setting time. The concrete is sprayed in layers, increasing the thickness of the side lining in one spraying and advancing the initial setting time of the top lining. Multiple layers are sprayed and finished. The thickness of the top lining layer and the setting time are determined based on the thickness of the side lining.

Benefits of technology

It reduced construction costs, improved the density and impermeability of concrete, and enhanced the durability and safety of the tunnel structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120626205B_ABST
    Figure CN120626205B_ABST
Patent Text Reader

Abstract

This disclosure provides a method for shotcreting tunnel lining, including preparing an operating platform, preparing mechanical equipment, preparing materials, and performing concrete spraying. After the reinforcement installation and acceptance, no formwork is required; concrete is sprayed in layers, with each subsequent layer completed before the initial setting of the previous layer. For the side lining, the thickness of each spraying is increased, and spraying proceeds sequentially from bottom to top. For the top lining, the concrete setting time is adjusted to advance initial setting; a dispersed spraying method is used, with multiple layers and multiple sprayings, and the surface is finished just before initial setting. The thickness of each layer of the top lining and the setting time of the top lining concrete are determined based on the thickness of the side lining. This method solves the problems of high cost, insufficient concrete density, and poor impermeability caused by the use of formwork in tunnel lining construction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of tunnel engineering technology, specifically to a method for spray forming of tunnel structure lining. Background Technology

[0002] In tunnel construction, the tunnel lining, as a key component of the tunnel structure, directly affects the tunnel's safety, stability, and service life. Traditional tunnel lining construction methods often employ formwork, a method that, while having a certain foundation in long-term engineering practice, has also revealed many problems that urgently need to be addressed.

[0003] First, formwork construction is costly. The fabrication, transportation, installation, and dismantling of formwork all require significant investment of manpower, resources, and time. This is especially true for tunnels with complex cross-sections, where the cost of custom-made formwork is prohibitively high. Furthermore, the reusability of formwork is limited; once damaged or deformed, it must be replaced, further increasing construction costs and placing a heavy financial burden on construction companies.

[0004] Secondly, insufficient concrete density. During formwork construction, the gaps at the formwork joints are difficult to seal completely, leading to grout leakage and segregation in these areas during concrete pouring. Furthermore, the rigidity and stability of the formwork supports also affect the quality of concrete pouring. If the formwork deforms or shifts during pouring, defects such as voids and honeycombing can occur within the concrete, reducing its density. Insufficient concrete density directly impacts the structural strength and durability of the tunnel lining, making it prone to cracking and spalling during long-term use, ultimately jeopardizing tunnel safety.

[0005] Furthermore, its impermeability is poor. The impermeability of the tunnel lining is crucial for preventing groundwater seepage, protecting the internal structure of the tunnel, and ensuring its normal functionality. However, tunnel linings constructed using formwork often fail to achieve ideal impermeability due to insufficient concrete density and gaps at formwork joints. Groundwater can easily seep into the tunnel through these weak points, not only eroding the concrete lining but also damaging the mechanical and electrical equipment and communication facilities within the tunnel, severely impacting its service life and operational safety.

[0006] In summary, existing formwork construction methods for tunnel linings suffer from numerous problems, including high costs, insufficient concrete density, and poor impermeability. These issues severely restrict the high-quality development of tunnel engineering, necessitating a new construction technology or method to address these technical challenges, improve the construction quality of tunnel linings, reduce construction costs, and enhance the structural performance and service life of tunnels. Summary of the Invention

[0007] In view of this, the present disclosure provides a method for spray forming of tunnel structure lining, which at least partially solves the problems existing in the prior art.

[0008] This application discloses a method for spray forming a tunnel structure lining, comprising:

[0009] Prepare an operating platform, using a quick-release or movable operating platform, ensuring that the operating surface is 1.5m to 1.8m away from the construction surface, and that the width of the operating surface is not less than 0.8m;

[0010] Prepare the machinery and equipment, including a wet concrete spraying machine, an air compressor, and concrete mixer trucks;

[0011] Prepare materials, select high-flowability concrete materials, and add calcium sulfoaluminate to adjust the setting time of the concrete.

[0012] For concrete spraying, after the steel reinforcement installation is accepted, there is no need to install formwork. Concrete is sprayed in layers, with the next layer of concrete sprayed before the previous layer has initially set.

[0013] Specifically, for the side lining, the thickness of a single spray is increased, and the spraying is carried out sequentially from bottom to top; for the top lining, the concrete setting time is adjusted to advance the initial setting, and the concrete is sprayed in a dispersed manner, in multiple layers and multiple times, and the surface is finished when the concrete is close to the initial setting. The thickness of a single layer of the top lining and the setting time of the top lining concrete are determined based on the thickness of the side lining.

[0014] Specifically, the steps of determining the single-layer thickness of the top lining and the setting time of the top lining concrete based on the thickness of the side lining include:

[0015] Measure and record the actual thickness of the side lining, denoted as H_s;

[0016] The thickness H_t of a single layer of the top liner is calculated based on H_s, where H_t is inversely proportional to H_s;

[0017] The setting time T_c of the top lining concrete is determined based on H_s;

[0018] If H_s is greater than the design threshold, then reduce H_t and shorten T_c to accelerate initial setting.

[0019] Specifically, the step of calculating the single-layer thickness H_t of the top liner based on H_s includes:

[0020] Obtain the side liner thickness measurement value H_s;

[0021] The scaling factor α is determined based on the tunnel cross-sectional dimensions;

[0022] Calculate H_t = β / (H_s × α), where β is the reference thickness parameter;

[0023] If H_s < S_min, then set H_t = T_max; otherwise, set H_t = β / (H_s × α), where H_s represents the side liner thickness, S_min represents the minimum allowable side liner thickness, and T_max represents the maximum allowable top single-layer thickness.

[0024] Specifically, the step of determining the scaling factor α based on the tunnel cross-sectional dimensions includes:

[0025] Measure the width W and height H of the tunnel cross-section;

[0026] The cross-sectional area A = W × H is calculated based on W and H.

[0027] α is determined based on A, where α = δ / √A, and δ is the size factor;

[0028] If A > A_ref, then set α = α_min, where W represents the tunnel width, H represents the tunnel height, A represents the cross-sectional area, δ represents the size factor, A_ref represents the reference cross-sectional area, and α_min represents the minimum scaling factor.

[0029] Specifically, the step of determining α based on A includes:

[0030] Obtain the cross-sectional area A;

[0031] The δ value is determined based on material properties;

[0032] Calculate α = δ / √A;

[0033] If A ≤ A_low, then set α = α_high, where A represents the cross-sectional area, δ represents the size factor, A_low represents the low area threshold, and α_high represents the high scaling factor.

[0034] Specifically, the step of determining the δ value based on material properties includes:

[0035] Test the flowability F of concrete materials;

[0036] δ is determined based on F, where δ is positively correlated with F;

[0037] If F > F_max, then set δ = δ_max; otherwise, set δ = m × F, where F represents the flowability of concrete, δ represents the size factor, F_max represents the maximum allowable flowability, δ_max represents the maximum size factor, and m represents the flowability ratio factor.

[0038] Specifically, the step of determining δ based on F includes:

[0039] The slump S of concrete is measured as an indicator of its fluidity.

[0040] The liquidity index F = S / S_ref is calculated based on S, where S_ref is the reference collapse rate.

[0041] Based on F, δ = n × F is determined, where n is the material coefficient;

[0042] If S < S_min, then set δ = δ_default, where S represents the concrete slump, S_ref represents the reference slump, F represents the fluidity index, n represents the material coefficient, S_min represents the minimum allowable slump, and δ_default represents the default size coefficient.

[0043] Specifically, the side lining is sprayed to a thickness of 15-20cm in a single application.

[0044] Specifically, for the top liner, the initial setting time is advanced to 5-10 minutes by adjusting the amount of calcium sulfoaluminate added.

[0045] Specifically, the setting time T_c of the top lining concrete is obtained by looking up the table based on the H_s value.

[0046] This disclosure provides a method for shotcreting tunnel lining, including: preparing an operating platform (using a quick-release or movable platform, with the operating surface 5m-8m from the construction surface and a width of not less than 8m); preparing mechanical equipment, including a wet concrete spraying machine, an air compressor, and a concrete mixer truck; preparing materials, using high-flowability concrete and adding calcium sulfoaluminate to adjust the concrete's setting time; and performing concrete spraying, where, after the reinforcement installation and acceptance, no formwork is required, and concrete is sprayed in layers, with each subsequent layer completed before the initial setting of the previous layer. For the side lining, the thickness of each spraying is increased, and spraying proceeds sequentially from bottom to top. For the top lining, the concrete setting time is adjusted to advance initial setting, using a dispersed spraying method, multiple layers, and finishing the surface near initial setting. The thickness of each single layer of the top lining and the setting time of the top lining concrete are determined based on the thickness of the side lining. This method solves the problems of high cost, insufficient concrete density, and poor impermeability caused by the use of formwork in tunnel lining construction. Attached Figure Description

[0047] In the accompanying drawings, unless otherwise specified, the same reference numerals throughout the various drawings denote the same or similar parts or elements. These drawings are not necessarily drawn to scale. It should be understood that these drawings depict only some embodiments disclosed in this application and should not be construed as limiting the scope of this application.

[0048] Figure 1 This is a flowchart of a method for spray molding tunnel structure linings;

[0049] Figure 2 This is a flowchart for determining the single-layer thickness of the top lining and the setting time of the top lining concrete based on the thickness of the side lining.

[0050] Figure 3 This is a flowchart for calculating the single-layer thickness H_t of the top liner based on H_s;

[0051] Figure 4 This is a flowchart for determining the scaling factor α based on the tunnel cross-section dimensions;

[0052] Figure 5 This is a flowchart for determining α based on A;

[0053] Figure 6 This is a flowchart for determining the δ value based on material properties;

[0054] Figure 7 This is a flowchart for determining δ based on F. Detailed Implementation

[0055] The embodiments of this disclosure will now be described in detail with reference to the accompanying drawings.

[0056] The following specific examples illustrate the implementation of this disclosure. Those skilled in the art can easily understand other advantages and effects of this disclosure from the content disclosed in this specification. Obviously, the described embodiments are only a part of the embodiments of this disclosure, and not all of them. This disclosure can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed based on different viewpoints and applications without departing from the spirit of this disclosure. It should be noted that, in the absence of conflict, the following embodiments and features in the embodiments can be combined with each other. Based on the embodiments in this disclosure, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this disclosure.

[0057] It should be noted that various aspects of embodiments within the scope of the appended claims are described below. It will be apparent that the aspects described herein can be embodied in a wide variety of forms, and any particular structure and / or function described herein is merely illustrative. Based on this disclosure, those skilled in the art will understand that one aspect described herein can be implemented independently of any other aspect, and two or more of these aspects can be combined in various ways. For example, any number of aspects set forth herein can be used to implement the device and / or practice the method. Additionally, this device and / or method can be implemented using structures and / or functionalities other than one or more of the aspects set forth herein.

[0058] It should also be noted that the illustrations provided in the following embodiments are only schematic representations of the basic concept of this disclosure. The drawings only show the components related to this disclosure and are not drawn according to the number, shape and size of the components in actual implementation. In actual implementation, the form, quantity and proportion of each component can be arbitrarily changed, and the layout of the components may also be more complex.

[0059] Furthermore, specific details are provided in the following description to facilitate a thorough understanding of the examples. However, those skilled in the art will understand that the described aspects can be practiced without these specific details.

[0060] Next, refer to Figure 1 This describes the various steps of a tunnel structure lining spray forming method according to the present invention.

[0061] S101: Prepare the operating platform. Use a quick-release or mobile operating platform, ensuring the operating surface is 1.5m to 1.8m away from the construction surface, and the operating surface width is not less than 0.8m. In specific operations, use a quick-release or mobile operating platform to ensure easy assembly and disassembly to reduce construction interruptions. When setting up the platform, the distance between the operating surface and the tunnel construction surface should be controlled between 1.5m and 1.8m to provide a safe and efficient operating space. At the same time, the operating surface width should not be less than 0.8m to ensure sufficient movement area for workers and equipment. This is achieved by adjusting the height and position of the platform support, avoiding the time-consuming and costly problems associated with traditional scaffolding.

[0062] S102: Prepare the mechanical equipment, including a wet concrete spraying machine, an air compressor, and a concrete mixer truck. Specific operations involve checking the equipment's operating status, such as connecting the wet spraying machine and the air compressor to provide stable air pressure, and scheduling the concrete mixer truck to supply the mixture in a timely manner to ensure continuous spraying. Specifically, in one embodiment, for urban subway tunnel construction, a high-performance wet spraying machine is used in conjunction with a variable frequency air compressor, with the pressure controlled at 0.7-0.8 MPa. The concrete mixer truck delivers fresh material every 30 minutes to avoid material waste caused by interruption of spraying.

[0063] S103: Prepare materials, select high-flowability concrete materials, and add calcium sulfoaluminate to adjust the setting time of the concrete. For example, select high-flowability concrete materials (such as slump controlled at 180-220mm), and add calcium sulfoaluminate as a setting accelerator during the mixing stage. The dosage is adjusted according to the design requirements (e.g., add 2-3kg per cubic meter of concrete) to accurately control the setting time. During operation, the materials are mixed evenly at the mixing plant and then transported by tanker truck to ensure that the concrete remains fluid before spraying, avoiding the impact on construction quality due to setting too fast or too slow.

[0064] In a more specific embodiment, the step includes mixing cement, aggregate, and water in proportion, with calcium sulfoaluminate added at 1-2% of the cement weight to precisely control the initial setting time to 10-20 minutes; for example, in one embodiment, for hydraulic tunnel engineering, the concrete mix design is a water-cement ratio of 0.4, with 1.5% calcium sulfoaluminate added to ensure rapid solidification after spraying, improve impermeability, and reduce material loss.

[0065] S104: For shotcreting, after the reinforcement installation and acceptance, no formwork is required. Concrete is shotcreted in layers, with each subsequent layer completed before the initial setting of the previous layer. Specifically, initial setting refers to the stage from when concrete is mixed with water until it gradually loses its plasticity and begins to harden but has not yet completely lost its workability. Furthermore, the term final setting refers to the critical point from when concrete is mixed with water until it completely loses its plasticity, enters the hardening stage, and begins to develop strength.

[0066] Furthermore, in this application, for the side lining, the thickness of a single spraying is increased to 15-20 cm during operation, and spraying is performed sequentially from bottom to top, utilizing gravity to reduce material loss. In traditional tunnel structure lining spraying, when lining plates (such as wooden backing plates, steel supports, etc.) are installed, the thickness of the side lining is usually consistent with the height of the steel support profile (e.g., the thickness of the sprayed concrete is designed to match the height of the steel support profile, with a strength grade of C15~C20). In addition, the thickness of the wooden backing plate can be 30~50 mm, while the thickness of the filling layer (such as coarse sand or cement mortar) is preferably 30 mm. At this time, if the filling layer is too thick, it may lead to material waste, and under high ground stress, simply increasing the thickness or increasing the concrete grade cannot significantly improve the stress state (i.e., the material far from the inner edge of the lining is not fully utilized). If it is too thin, it may not meet the bearing capacity requirements of the initial support (the initial support needs to withstand more than 25%~50% of the frozen wall load, and in special cases, even the entire load), leading to structural safety risks. In contrast, in this application, the thickness of the side liner is significantly increased, specifically, the thickness is sprayed to 15-20 cm in a single application.

[0067] For the top lining, the initial setting time is advanced to 5-10 minutes by adjusting the amount of calcium sulfoaluminate added. The concrete is sprayed in a dispersed manner (nozzles oscillating in a fan shape), in multiple layers (each layer 3-5 cm thick), and compacted with a trowel when it is nearing initial setting. It should be understood that, in this application, the single spray thickness for the side linings is greater than that for the top lining. Furthermore, adjusting the concrete setting time to advance the initial setting refers to the top lining having an earlier initial setting time than the side linings.

[0068] In one specific embodiment, during mine tunnel construction, the side lining is sprayed with a 12 cm thick layer in a single pass, progressing from the base upwards. Workers check the flatness after each section is sprayed, significantly accelerating the forming speed. For the top lining, the concrete setting time is adjusted to advance the initial setting, using a dispersed spraying method, applying multiple layers, and finishing the surface just before the concrete reaches initial setting. Specifically, this involves increasing the calcium sulfoaluminate content to 2% to shorten the initial setting time to 8-12 minutes, using a fan-shaped nozzle to disperse the concrete during spraying, applying 3-4 thin layers, and finishing the surface 2 minutes before initial setting. In one embodiment, for example, when used for the top of a subsea tunnel, the setting time is adjusted to 10 minutes for initial setting, spraying in 4 layers of 4 cm each, and finishing with a trowel just before initial setting to reduce the risk of sagging. Furthermore, this application also includes scraping and smoothing excess concrete; specifically, this involves immediately removing protrusions with a scraper after spraying, and then smoothing the surface with a trowel to ensure a smooth lining; for example, in one embodiment, applied to the arch of a highway tunnel, workers use an aluminum alloy scraper to remove excess material, and then an electric trowel to finish the surface, improving impermeability and appearance quality. Additionally, the method of this application also includes water curing starting before and after the final setting of the concrete, with a curing time of not less than 14 days; specifically, this involves starting an automatic sprinkler system within 2 hours after final setting to keep the surface moist, watering 3-4 times daily; specifically, in one embodiment, for hydroelectric tunnel projects, immediately after final setting, wet burlap sacks are covered and water is sprinkled, with curing lasting more than 14 days to ensure strength development and durability.

[0069] In this application, the thickness of the top lining layer and the setting time of the top lining concrete are determined based on the thickness of the side lining. Specifically, the required structural support for the top is calculated by estimating the side thickness (e.g., 20cm): if the side thickness is large, the top single-layer thickness can be reduced (e.g., reduced to 3cm) and the setting time further shortened (e.g., 5 minutes) to prevent sagging and ensure compactness; conversely, it is appropriately increased. That is, the greater the side thickness, the smaller the top single-layer thickness and the shorter the setting time; conversely, the smaller the side thickness, the greater the top single-layer thickness and the longer the setting time. This solves the problems of high cost, insufficient concrete compactness, and poor impermeability caused by the use of formwork. For example, formwork-free construction reduces material waste and labor, and layered spraying combined with setting control improves compactness and impermeability.

[0070] For example, in one embodiment, applied to the construction of an urban subway tunnel, specifically, the tunnel diameter is 8m, the side lining thickness is designed to be 20cm, the operating platform uses a quick-release bracket, is 1.6m away from the construction surface, and is 0.9m wide; the mechanical equipment used is a wet spraying machine with rated power and an air compressor output pressure of 0.6MPa; 2.5kg / m³ of calcium sulfoaluminate is added to the concrete to make the setting time adjustable; based on the 20cm side thickness, the thickness of the top single layer is determined to be 4cm (calculation shows that a thin layer is needed to resist gravity), and the setting time is advanced to 6 minutes; during spraying, two layers (10cm each) are sprayed from bottom to top on the sides, and five layers (4cm each) are sprayed on the top, and the surface is finished before initial setting. As a result, the cost is reduced by 30%, the density test meets the standard, and the impermeability grade is improved to P10.

[0071] Through the above steps, the template-free design of this method reduces the cost of mold making and removal; layered spraying combined with setting control (such as rapid setting of the top thin layer) ensures that the concrete fills the voids densely and avoids voids; at the same time, the finishing operation and flowable materials enhance the impermeable layer, improving the overall durability.

[0072] The above only describes the relationship between the thickness of the side lining, the thickness of a single layer of the top lining, and the setting time of the top lining concrete. Next, refer to... Figure 2 The present invention specifically describes the steps of determining the single-layer thickness of the top lining and the setting time of the top lining concrete based on the thickness of the side lining.

[0073] S201: Measure and record the actual thickness of the side lining, denoted as H_s; this step obtains the thickness value of the tunnel side lining through on-site instruments, which serves as the basis for subsequent calculations.

[0074] S202: Calculate the thickness H_t of the top lining single layer based on H_s, where H_t is inversely proportional to H_s. The specific formula is H_t = k / H_s, where k is a proportionality constant in mm². This formula ensures that when the thicker side provides sufficient support, the top layer is thinned to reduce the risk of gravity sagging. The value of k is set according to experiments to optimize the flowability and bond strength of the concrete.

[0075] S203: Determine the setting time T_c of the top lining concrete based on H_s; this step involves looking up or calculating T_c based on the H_s value, with a range of 5-60 minutes to accommodate the initial setting requirements of different thicknesses and prevent voids. Specifically, when obtaining T_c by looking up a table, the table can be obtained from historical data.

[0076] S204: If H_s is greater than the design threshold (e.g., 150mm), then reduce H_t and shorten T_c to accelerate initial setting. This logic improves density through dynamic adjustment, avoiding cracks caused by concrete sagging. For example, in a tunnel construction embodiment, H_s is measured to be 200mm (greater than the threshold), H_t is calculated to be 50mm (k=10000), and T_c is determined to be 25 minutes; subsequently, H_t is reduced to 40mm and T_c is shortened to 20 minutes to ensure rapid initial setting of the shotcrete, good bonding with the sides, and improved impermeability.

[0077] Next, refer to Figure 3 This describes the steps of calculating the single-layer thickness H_t of the top liner based on H_s according to an embodiment of the present invention.

[0078] S301: Obtain the side lining thickness measurement value H_s. This step involves collecting the actual thickness value of the side lining in real time during tunnel shotcreting construction using sensors or manual measurement.

[0079] S302: Determine the scaling factor α based on the tunnel cross-sectional dimensions. This factor is calculated from the tunnel diameter or shape parameters and is used to reflect the influence of cross-sectional geometry on thickness distribution.

[0080] S303: Calculate the initial H_t = β / (H_s × α), where β is the reference thickness parameter, representing the ideal lining thickness reference; this formula adjusts the top thickness through an inverse proportional relationship to ensure the uniform distribution of concrete in the tunnel arch and sidewalls.

[0081] S304: If H_s < S_min, then set H_t = T_max, where S_min represents the minimum allowable side lining thickness and T_max represents the maximum allowable top single-layer thickness; otherwise, set H_t = β / (H_s × α). This judgment handles abnormal situations. When H_s is too small, H_t is fixed at T_max to prevent structural instability; when H_s is normal, the concrete dosage is optimized using an inverse formula.

[0082] For example, in one embodiment, the tunnel cross-section diameter is 8 meters, and α is determined to be 0.9. Specifically, the measured value of H_s is 210 mm (assuming S_min is 220 mm). Since H_s < S_min, H_t = T_max = 100 mm is set. Conversely, if H_s is 240 mm, then H_t = β / (H_s × α) is calculated. For example, if γ is 19200 mm², H_t = 89 mm. It should be understood that the value of γ can be obtained from historical experimental data, and when the calculated H_t is greater than T_max, H_t = T_max is set.

[0083] For the formula parameters, β is the baseline thickness parameter, which can be set based on the concrete compressive strength, and the greater the compressive strength, the larger the β value; α is based on the tunnel size, ranging from 0.8 to 1.0; S_min is the safety threshold, ranging from 200 to 250 mm; T_max is the structural upper limit. The formula is set up in this way because the inverse proportional relationship (H_t ∝ 1 / H_s) compensates for the load difference between the sidewall and the arch, and the condition judgment handles the risk of thin sidewalls, maintaining the overall stability and resource efficiency of the tunnel.

[0084] Next, refer to Figure 4 The present invention describes the steps for determining the scaling factor α based on the tunnel cross-section size.

[0085] S401: Measure the width W and height H of the tunnel cross section. This step obtains the basic geometric dimensions of the tunnel, providing input for subsequent calculations.

[0086] S402: Calculate the cross-sectional area A = W × H based on W and H. This means that the cross-sectional shape of the tunnel is simplified by a rectangle, and the cross-sectional area A is obtained to represent the size.

[0087] S403: α is determined based on A, where α = δ / √A, and δ is a size factor. In the formula, δ represents an empirical size factor, usually ranging from 8 to 10. The optimal value needs to be determined experimentally based on the characteristics of the sprayed material (such as the fluidity of concrete). For example, δ=9 is a common value. A is the area (in m²), and its range depends on the actual tunnel size (such as 10-200 m²). This formula means that α is inversely proportional to √A, ensuring that α decreases as the area increases, in order to adapt to the calculation of lining thickness under different tunnel sizes. This setting is to make α reflect the size scaling effect and avoid the excessively large scaling factor leading to uneven spraying.

[0088] S404: If A > A_ref, then set α = α_min; in the formula, A_ref represents the reference cross-sectional area (range 50-150 m², optimal value 100 m² based on standard tunnel design), and α_min is the minimum scaling factor; the meaning of this formula is that when A is too large, α_min is fixed to control the calculation stability (avoid numerical problems caused by α being too small), otherwise α is negatively correlated with A to ensure that the lining thickness H_t calculation is suitable for small-sized tunnels; this setting is to maintain the minimum spraying ratio in large tunnels and achieve dynamic adjustment in small tunnels.

[0089] Specifically, in an embodiment of a tunnel lining shotcreting method, for example in a tunnel project, the measured width W = 10 meters and height H = 8 meters, then A = 10 × 8 = 80 m². The size factor δ is taken as a common value of 9, √A ≈ 8.94, therefore, the initial α = 9 / 8.94 ≈ 1.0067. The reference area A_ref is set to 100 m² (optimal value). Since A = 80 < A_ref, α = 1.0067 is set. This α is used for subsequent shotcreting thickness calculations to ensure that the lining is suitable for this medium-sized tunnel.

[0090] It is understood that in this application, the parameter δ can be obtained from historical experimental data, and other methods can also be used to determine α based on A.

[0091] Next, refer to Figure 5 This describes the steps of determining α based on A in one embodiment of the present invention.

[0092] S501: Obtain the cross-sectional area A, which is the cross-sectional area of ​​the tunnel lining, used to reflect the lining size.

[0093] S502: The δ value is determined based on the material properties. δ represents the size factor, which is determined by the strength or density characteristics of materials such as concrete.

[0094] S503: Calculate α = δ / √A, where A is the cross-sectional area; δ is determined based on material experiments and ranges from 8 to 10. This formula makes α inversely proportional to √A because the scaling factor α decreases as the area increases, thus optimizing the spray thickness control and avoiding excessive material waste.

[0095] S504: If A ≤ A_low, then set α = α_high. A_low is the low area threshold, such as 50 square meters; α_high is the high scaling factor, such as 1.0. The reason for this setting is that when A is too small (such as in a narrow tunnel section), α_high enhances the adjustment effect to ensure the minimum spray thickness; otherwise, α is inversely proportional to A to precisely control the thickness distribution.

[0096] In one embodiment, specifically for shotcreting of tunnel lining, for example using concrete, A = 40 square meters is initially obtained; based on material properties, δ is determined to be 10. The initial α is calculated as 10 / √40 ≈ 1.58. If A_low = 50 square meters, since A = 40 ≤ 50, α = α_high = 1.0 is set to enhance the adjustment effect in small areas and prevent the lining from being too thin. Conversely, if A = 150 square meters, then α = δ / √A = 10 / √150 ≈ 0.81, optimizing the scaling factor to match larger cross-sections and achieving uniform shotcrete thickness control.

[0097] It should be understood that in actual regulation, if the α calculated according to α = δ / √A exceeds α_high, then α is directly set to α_high to avoid abnormal regulation.

[0098] Next, refer to Figure 6 This describes the steps of determining the δ value based on material properties according to one embodiment of the present invention.

[0099] S601: Test the flowability F of the concrete material. This step measures the flowability of the concrete using standard tests (such as slump test), in millimeters (mm), as a key input.

[0100] S602: δ is determined based on F, where δ is positively correlated with F. This means that the size factor δ increases with increasing flowability to ensure that the liner thickness adapts to the material flow characteristics during spray molding, avoiding uneven molding.

[0101] S603: If F > F_max, then set δ = δ_max; otherwise, set δ = m × F. This step means controlling the adjustment range of δ. When the fluidity is too high, use the maximum δ_max to prevent splashing or deformation caused by excessive spraying; otherwise, maintain a positive correlation through a linear relationship to optimize molding quality.

[0102] For the formulas δ = m × F (when F ≤ F_max) and δ = δ_max (when F > F_max), the parameters have the following meanings: F represents the flowability of concrete, typically ranging from 100 to 200 mm; δ represents the size factor, ranging from 8 to 10; F_max represents the maximum allowable flowability, ranging from 140 to 160 mm, with an optimal value of 150 mm to prevent runaway flow; δ_max represents the maximum size factor, which can be set to 12 for example; m represents the flowability ratio factor, ranging from 0.05 to 0.1, with an optimal value of 0.07 to maintain linear correlation. The formulas mean that when F is too high, δ_max provides an upper limit protection; otherwise, m × F ensures a positive correlation between δ and F, guaranteeing that the size factor dynamically matches the material properties. This setting is intended to balance adaptability (e.g., avoiding lining cracking) and stability (e.g., controlling spraying pressure) in tunnel shotcreting, preventing material waste or structural defects.

[0103] In one embodiment, specifically during tunnel lining shotcreting, the test concrete is F = 180 mm. Assuming F_max = 150 mm, δ_max = 12, and m = 0.07, since F > F_max, δ = δ_max = 12 is set to limit the spraying amount to prevent splashing. For example, if F = 120 mm (lower than F_max), then δ = m × F = 0.07 × 120 = 8.4, increasing the spraying size to accommodate flowability and ensure uniform lining formation.

[0104] Next, refer to Figure 7 The present invention describes the steps for determining δ based on F. The steps include: S701, measuring the concrete slump S as a flowability indicator;

[0105] S702, the liquidity index F = S / S_ref is calculated based on S, where S_ref is the reference collapse rate;

[0106] S703, based on F, δ = n × F is determined, where n is the material coefficient;

[0107] S704, if S < S_min, then set δ = δ_default.

[0108] Step S701 assesses the flowability of concrete through slump testing to ensure its suitability for shotcreting. Step S702 standardizes the slump to F to eliminate the influence of units and facilitates comparison of flowability. Step S703 calculates δ using F and n, ensuring that δ is positively correlated with flowability to optimize the shotcreting effect. Step S704 guarantees basic performance through conditional judgment: when the slump is too low, the default δ_default is used to prevent shotcreting defects.

[0109] For the formula, firstly, F = S / S_ref: S is the measured slump (range 50-150mm), S_ref is a reference value, for example, 1mm, and F is dimensionless (range 50-150mm). This formula normalizes the fluidity index, making it easier to calculate δ. Secondly, δ = n × F, n is the material coefficient (range 0.08-0.12, depending on the cement type), and δ is the size coefficient (affecting the spraying thickness). The formula is set so that δ changes linearly with F, ensuring that δ increases when fluidity is enhanced to improve the lining density. Finally, the conditional formula δ = δ_default (if S < S_min), S_min is the minimum slump (range 40-60mm, optimal value 50mm), and δ_default is the default coefficient (e.g., 8). The meaning of the formula is that when S is insufficient, δ_default is used to ensure that the spraying does not fail; otherwise, δ is proportional to S to dynamically adapt to fluidity and avoid lining cracking or rebound.

[0110] For example, in one embodiment, during the shotcreting of the tunnel structure lining, S_ref=1mm, n=0.12, S_min=50mm, and δ_default=8 are set. Specifically, if the measured slump S=40mm (less than S_min), then δ=δ_default=8 is set to ensure stable shotcrete thickness under low fluidity conditions and prevent tunnel lining detachment. If S=80mm (greater than S_min), first calculate F=80 / 1=80, then δ=0.12×80=9.6.

[0111] The present invention provides a method for shotcreting tunnel lining, comprising: First, preparing an operating platform, employing a quick-release or movable operating platform, ensuring the operating surface is within 1.5m to 1.8m of the construction surface, and the operating surface width is not less than 0.8m, to provide a stable and efficient working environment. Second, preparing mechanical equipment, including a wet concrete spraying machine, an air compressor, and a concrete mixer truck, which work together to ensure the continuity of concrete delivery and spraying. Next, preparing materials, selecting high-flowability concrete materials, and adding calcium sulfoaluminate as an admixture to precisely adjust the concrete's setting time, thereby optimizing its workability. Then, after the reinforcement installation and acceptance are completed, without installing any formwork, directly carrying out concrete spraying construction, using a layered spraying method to ensure that the subsequent layer of concrete is completed before the initial setting of the previous layer, to enhance the overall bonding strength and density of the concrete. During the specific spraying process, for the side lining, the thickness of a single spray is increased (e.g., by 20%-30% based on the design thickness), and spraying is carried out sequentially from bottom to top to reduce the impact of gravity and improve construction efficiency; for the top lining, the initial setting time is advanced by adjusting the amount of calcium sulfoaluminate added (e.g., shortened to 50%-70% of ordinary concrete), and a dispersed spraying method is adopted, with multiple layers sprayed in multiple times (e.g., each layer thickness is controlled at 5-10cm), and a finishing operation is carried out when the concrete is close to initial setting to form a smooth and dense surface.

[0112] The core innovation of this method lies in determining the single-layer thickness of the top lining and the setting time of the top lining concrete based on the thickness of the side lining, thereby effectively solving the problems of high cost, insufficient concrete density, and poor impermeability caused by the use of formwork in tunnel lining construction. Specifically, the thickness of the side lining (e.g., designed as 30cm-50cm) is used as a key parameter, and through engineering calculations and experimental verification, it is directly linked to the setting of the single-layer thickness of the top lining (e.g., adjusting the single-layer thickness of the top lining to 1 / 2-2 / 3 of the side lining thickness), and simultaneously optimizing the setting time (e.g., shortening the initial setting time according to the increase in side lining thickness). This correlated design eliminates the need for formwork, avoiding the high costs of formwork installation and removal (saving approximately 30% of construction costs). At the same time, by layered spraying and completing subsequent layers before initial setting, it ensures that the concrete can achieve high density (porosity reduced to below 5%) even without formwork, thereby improving impermeability (permeability coefficient reduced to the 10^{-12} cm / s level). Furthermore, the dispersed spraying and early setting strategy of the top lining prevents concrete collapse or segregation, further enhancing the uniformity and durability of the overall structure, ultimately achieving efficient and low-cost tunnel lining construction. The overall process is simple and efficient, suitable for various tunnel engineering environments.

[0113] The specific embodiments described above further illustrate the purpose, technical solutions, and beneficial effects of the embodiments of this disclosure. It should be understood that the above descriptions are merely specific embodiments of the embodiments of this disclosure and are not intended to limit the scope of protection of the embodiments of this disclosure. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the embodiments of this disclosure should be included within the scope of protection of the embodiments of this disclosure.

Claims

1. A method for spray forming a tunnel structure lining, characterized in that, include: Prepare an operating platform, using a quick-release or movable operating platform, ensuring that the operating surface is 1.5m to 1.8m away from the construction surface, and that the width of the operating surface is not less than 0.8m; Prepare the machinery and equipment, including a wet concrete spraying machine, an air compressor, and concrete mixer trucks; Prepare materials, select high-flowability concrete materials, and add calcium sulfoaluminate to adjust the setting time of the concrete. For concrete spraying, after the steel reinforcement installation is accepted, there is no need to install formwork. Concrete is sprayed in layers, with the next layer of concrete sprayed before the previous layer has initially set. Specifically, for the side lining, the thickness of a single spray is increased, and the spraying is carried out sequentially from bottom to top; for the top lining, the concrete setting time is adjusted to advance the initial setting, and the concrete is sprayed in a dispersed manner, in multiple layers and multiple times, and the surface is finished when the concrete is close to the initial setting. The thickness of a single layer of the top lining and the concrete setting time of the top lining are determined based on the thickness of the side lining. The steps of determining the single-layer thickness of the top lining and the setting time of the top lining concrete based on the thickness of the side lining include: Measure and record the actual thickness of the side lining, denoted as H_s; The thickness H_t of a single layer of the top liner is calculated based on H_s, where H_t is inversely proportional to H_s; The setting time T_c of the top lining concrete is determined based on H_s; If H_s is greater than the design threshold, then reduce H_t and shorten T_c to advance the initial setting time; Furthermore, the step of calculating the single-layer thickness H_t of the top liner based on H_s includes: Obtain the side liner thickness measurement value H_s; The scaling factor α is determined based on the tunnel cross-sectional dimensions; Calculate H_t = β / (H_s × α), where β is the reference thickness parameter; If H_s < S_min, then set H_t = T_max; otherwise, set H_t = β / (H_s × α), where H_s represents the side liner thickness, S_min represents the minimum allowable side liner thickness, and T_max represents the maximum allowable top single-layer thickness.

2. The method for spray forming of a tunnel structure lining according to claim 1, characterized in that, The step of determining the scaling factor α based on the tunnel cross-sectional dimensions includes: Measure the width W and height H of the tunnel cross-section; The cross-sectional area A = W × H is calculated based on W and H. α is determined based on A, where α = δ / √A, and δ is the size factor; If A > A_ref, then set α = α_min, where W represents the tunnel width, H represents the tunnel height, A represents the cross-sectional area, δ represents the size factor, A_ref represents the reference cross-sectional area, and α_min represents the minimum scaling factor.

3. The method for spray forming of a tunnel structure lining according to claim 2, characterized in that, The step of determining α based on A includes: Obtain the cross-sectional area A; The δ value is determined based on material properties; Calculate α = δ / √A; If A ≤ A_low, then set α = α_high, where A represents the cross-sectional area, δ represents the size factor, A_low represents the low area threshold, and α_high represents the high scaling factor.

4. The method for spray forming of a tunnel structure lining according to claim 3, characterized in that, The step of determining the δ value based on material properties includes: Test the flowability F of concrete materials; δ is determined based on F, where δ is positively correlated with F; If F > F_max, then set δ = δ_max; otherwise, set δ = m × F, where F represents the flowability of concrete, δ represents the size factor, F_max represents the maximum allowable flowability, δ_max represents the maximum size factor, and m represents the flowability ratio factor.

5. The method for spray forming of a tunnel structure lining according to claim 4, characterized in that, The steps for determining δ based on F include: The slump S of concrete is measured as an indicator of its fluidity. The liquidity index F = S / S_ref is calculated based on S, where S_ref is the reference collapse rate. Based on F, δ = n × F is determined, where n is the material coefficient; If S < S_min, then set δ = δ_default, where S represents the concrete slump, S_ref represents the reference slump, F represents the fluidity index, n represents the material coefficient, S_min represents the minimum allowable slump, and δ_default represents the default size coefficient.

6. The method for spray forming of a tunnel structure lining according to claim 1, characterized in that, The side lining is sprayed to a thickness of 15-20cm in a single application.

7. The method for spray forming of a tunnel structure lining according to claim 1, characterized in that, For the top liner, the initial setting time can be advanced to 5-10 minutes by adjusting the amount of calcium sulfoaluminate added.

8. The method for spray forming of a tunnel structure lining according to claim 1, characterized in that, The setting time T_c of the top lining concrete is obtained by looking up the table based on the H_s value.

Citation Information

Patent Citations

  • Two-layer primary support construction method based on small-distance tunnel

    CN110847932A

  • Railway tunnel lining construction method based on medium and high fluidity concrete

    CN110966022A