A Mg-based hydrogen storage material, its preparation method and application
By modifying MgH2 and utilizing the carbonized derivatives of Ni-Ce bimetallic MOF materials, the hydrogen absorption and desorption performance and stability of Mg-based hydrogen storage materials were improved, solving the performance deficiencies in existing technologies.
Patent Information
- Application Number
- CN202511306488.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-09-12
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2045-09-12
AI Technical Summary
Existing Mg-based hydrogen storage materials cannot meet the practical application requirements in terms of hydrogen absorption/desorption, hydrogen storage performance, or stability, and their preparation methods are cumbersome and not suitable for large-scale promotion.
The MgH2 was modified by using the carbonized derivative of the Ni-Ce bimetallic MOF material. The hydrogen storage performance and stability were improved by physical isolation and loading of the hierarchical porous carbon framework, interface enhancement of Mg-C bond, catalytic activation of Ni nanoparticles, and grain boundary effect and oxygen vacancy regulation of Ce-based oxide.
The hydrogen absorption and desorption performance and stability of Mg-based hydrogen storage materials have been improved, achieving excellent hydrogen storage performance and strong stability.
Smart Images

Figure CN121158729B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of solid-state hydrogen storage technology, and relates to a Mg-based hydrogen storage material, and more particularly to a Mg-based hydrogen storage material and its preparation method and application. Background Technology
[0002] Due to the increasingly severe energy crisis and environmental protection requirements, the development of new energy sources that can replace fossil fuels has become an important social issue. Hydrogen energy has a wide range of sources, extremely high energy density, and its product after appropriate energy conversion is water. It can serve as a substitute for current fossil fuels and is considered the most promising new energy source at present.
[0003] Currently, to promote the efficient utilization of hydrogen energy at the technological level, it is necessary to overcome key challenges in hydrogen production, storage, transportation, and utilization. In existing technologies, the storage and transportation of hydrogen are constrained by its high volatility and flammability, making them key technological bottlenecks limiting the large-scale commercial application of hydrogen energy.
[0004] Currently, there are three main methods for storing hydrogen: high-pressure gaseous storage, cryogenic liquid storage, and room-temperature solid-state storage. Among them, metal hydride solid-state hydrogen storage technology has advantages such as high hydrogen storage density, low operating cost, good safety, and high energy density. Therefore, it is considered to be the most promising hydrogen storage method and can be used as a hydrogen source for fuel cells in transportation vehicles that require large amounts of hydrogen.
[0005] Furthermore, Mg is a commonly used metal hydrogen storage material due to its wide availability and advantages such as high hydrogen storage density (7.6% wt%), good reversibility, and environmental friendliness. However, the high thermodynamic temperature (>200℃) of the reaction between Mg and H2 and the slow hydrogen absorption / desorption kinetics, requiring high temperature and pressure, limit the widespread application of Mg-based hydrogen storage materials. Due to these drawbacks, modification of Mg-based hydrogen storage materials is necessary.
[0006] For example, CN118417573A discloses a method and apparatus for preparing graphene-reinforced titanium-based hydrogen storage alloy powder. The method involves precisely proportioning Ti, Zr, Mn, Cr, and Fe metals with graphene, followed by multiple steps including vacuum melting, belt spinning, mechanical crushing, and high-energy ball milling to obtain highly dispersed graphene-modified titanium alloy composite powder. However, the hydrogen storage performance and stability of this graphene-reinforced titanium-based hydrogen storage alloy powder still cannot meet the needs of practical applications. Furthermore, the preparation method requires specialized metal smelting equipment, involves cumbersome processing steps, and has strict processing requirements, making it unsuitable for large-scale promotion and use.
[0007] For example, CN115784147A discloses a single-atom catalytic magnesium hydride solid hydrogen storage material, its application, and preparation method. The hydrogen storage material is composed of magnesium hydride as the main material and a catalyst, wherein the catalyst is a single-atom Ni supported on TiO2. However, the hydrogen absorption and desorption performance and stability of this single-atom catalytic magnesium hydride solid hydrogen storage material cannot meet the requirements of practical applications.
[0008] However, the doping modification of the aforementioned hydrogen storage materials has improved the hydrogen absorption and desorption performance and cycle stability of the original hydrogen storage materials to some extent. However, the preparation conditions of the catalysts in the above methods are quite harsh, requiring special production equipment to maintain the catalyst preparation environment, and the process steps are complicated; in addition, the preparation methods disclosed in the above methods mostly use high-speed spherical graphite physical mixing methods to cause solid-solid mixing between metal materials, which can easily cause problems such as local element enrichment.
[0009] Existing Mg-based hydrogen storage materials all have certain drawbacks, with their hydrogen absorption / desorption performance, hydrogen storage performance, or stability failing to meet the requirements for practical applications. Therefore, it is crucial to develop and design a novel Mg-based hydrogen storage material and its preparation method. Summary of the Invention
[0010] To address the shortcomings of existing technologies, the present invention aims to provide a Mg-based hydrogen storage material, its preparation method, and its applications. This invention modifies MgH2 using a carbonized derivative of a MOF material containing carbonized Ni-Ce bimetallic MOF material, thus obtaining a Mg-based hydrogen storage material. Through the synergistic effects of physical isolation and loading of the hierarchical porous carbon framework, interface enhancement of Mg-C bonds, catalytic activation of Ni nanoparticles, and grain boundary effects and oxygen vacancy regulation of Ce-based oxides, the hydrogen storage performance of the material is effectively improved, and structural changes during cycling are suppressed. Therefore, the Mg-based hydrogen storage material exhibits excellent hydrogen storage performance and strong stability.
[0011] To achieve this objective, the present invention adopts the following technical solution:
[0012] In a first aspect, the present invention provides a Mg-based hydrogen storage material, wherein the Mg-based hydrogen storage material comprises MgH2 and a carbonized derivative of MOF material; the carbonized derivative of MOF material comprises a carbonized Ni-Ce bimetallic MOF material.
[0013] MOF materials possess unique nanoscale porous structures, excellent electronic transport properties, and efficient catalytic performance, showing significant application potential in improving the performance of magnesium-based hydrogen storage materials. Furthermore, the carbide derivatives of MOF materials not only possess the advantages of MOF materials but also exhibit a more stable framework structure. Based on this, this invention provides a Mg-based hydrogen storage material comprising MgH2 and a carbide derivative of MOF materials, used to improve the hydrogen storage performance of Mg-based hydrogen storage materials. To further enhance the hydrogen storage performance of Mg-based hydrogen storage materials, this invention uses raw materials containing Ni-Ce bimetallic MOF materials for carbide processing to prepare carbide derivatives of MOF materials, and then uses these MOF carbide derivatives to modify MgH2, thereby optimizing the performance of the Mg-based hydrogen storage material.
[0014] In this invention, the MOF material carbonization derivative in Mg-based hydrogen storage materials improves the performance of Mg-based hydrogen storage materials in the following ways:
[0015] First, the carbonized derivatives of the Ni-Ce bimetallic MOF material formed by carbonization contain a carbon framework with hierarchical pores. The hierarchical porous carbon framework can not only provide a highly dispersed loading interface for MgH2 and catalytic sites, but also suppress the growth of Mg grains caused by the hydrogen absorption-desorption cycle through the confinement effect.
[0016] Second, there is a weak Mg-C chemical bond between MgH2 and the hierarchical porous carbon framework of the MOF material carbonization derivative, which enhances the interfacial bonding force between the hierarchical porous carbon framework and MgH2, improves the stability of Mg-based hydrogen storage materials, and thus reduces the shedding of MgH2 during cycling.
[0017] Third, the carbonized derivatives of the Ni-Ce bimetallic MOF material contain Ni nanoparticles. The Ni nanoparticles are uniformly dispersed on the hierarchical porous carbon framework derived from the MOF, serving as highly efficient catalytic active sites that can promote the dissociation and adsorption of H2 molecules.
[0018] Fourth, the carbonization derivatives of MOF materials include nano Ce2O3 particles and / or nano CeO2 particles formed during the carbonization process of Ni-Ce bimetallic MOF materials. The nano Ce2O3 particles and / or nano CeO2 particles form a symbiotic structure with the grain boundaries of MgH2, which can promote the diffusion of hydrogen atoms along the grain boundaries.
[0019] Fifth, the carbonization derivatives of MOF materials include nano-Ce2O3 particles and / or nano-CeO2 particles formed during the carbonization process of Ni-Ce bimetallic MOF materials. 3+The resulting lattice distortion creates dynamic oxygen vacancy regions on the surface of nano-Ce2O3 particles and / or nano-CeO2 particles, which lowers the adsorption energy of surface H atoms and the dissociation energy barrier of Mg-H bonds. These regions can serve as “capture-release” sites for hydrogen atoms, further accelerating the diffusion and recombination of hydrogen.
[0020] Sixth, the hierarchical porous carbon framework inhibits the aggregation of Ni and Ce2O3 / CeO2 during carbonization through physical isolation, thereby improving the long-term stability of the nanocatalytic interface.
[0021] In summary, this invention modifies MgH2 with a carbonized derivative of a MOF material containing carbonized Ni-Ce bimetallic MOF material to obtain a Mg-based hydrogen storage material. Through the synergistic effects of physical isolation and loading of the hierarchical porous carbon framework, interface enhancement of Mg-C bonds, catalytic activation of Ni nanoparticles, and grain boundary effects and oxygen vacancy regulation of Ce-based oxides, the hydrogen storage performance of the material is effectively improved, and structural changes during cycling are suppressed. Therefore, the Mg-based hydrogen storage material exhibits excellent hydrogen adsorption / desorption performance, hydrogen storage performance, and strong stability.
[0022] Preferably, in the Mg-based hydrogen storage material, the mass ratio of the MOF material carbonized derivative to MgH2 is (5-20):100, for example, it can be 5:100, 6:100, 8:100, 10:100, 12:100, 14:100, 15:100, 16:100, 18:100 or 20:100, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0023] Preferably, the mass fraction of carbon material in the MOF material carbonized derivative is 65wt% to 85wt%, based on the mass percentage of the MOF material carbonized derivative. For example, it can be 65wt%, 68wt%, 70wt%, 72wt%, 75wt%, 78wt%, 80wt%, 82wt%, or 85wt%, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0024] Preferably, the molar ratio of Ni to Ce in the Mg-based hydrogen storage material is (1-3):(1-4). Typical but non-limiting combinations include 1:1, 1:2, 1:3, 1:4, 2:1, 2:2, 2:3, 2:4, 3:1, 3:2, 3:3, or 3:4, but are not limited to the listed values. Other unlisted values within this range are also applicable.
[0025] In a second aspect, the present invention provides a method for preparing the Mg-based hydrogen storage material described in the first aspect, the method comprising:
[0026] Ni-Ce bimetallic MOF material was heat-treated to obtain a carbide derivative of the MOF material; the obtained carbide derivative of the MOF material was then mixed with MgH2 to obtain a Mg-based hydrogen storage material.
[0027] The method for preparing Mg-based hydrogen storage materials proposed in this invention has a simple process, mild reaction conditions, and can be widely applied in most hydrogen storage systems.
[0028] Preferably, the method for preparing the Ni-Ce bimetallic MOF material includes: mixing Ni salt, Ce salt, solvent and ligand solution, and then carrying out a hydrothermal reaction to obtain the Ni-Ce bimetallic MOF material.
[0029] Preferably, the molar ratio of Ni salt to Ce salt in the mixture is (1-3):(1-4). Typical but non-limiting combinations include 1:1, 1:2, 1:3, 1:4, 2:1, 2:2, 2:3, 2:4, 3:1, 3:2, 3:3 or 3:4, but are not limited to the listed values. Other unlisted values within this range are also applicable.
[0030] Preferably, the Ni salt includes any one or a combination of at least two of Ni(NO3)2, Ni(CH3COO)2, NiSO4, NiCl2, Ni(NO3)2·6H2O, Ni(CH3COO)2·4H2O, NiSO4·6H2O, or NiCl2·6H2O. Typical but non-limiting combinations include the combination of Ni(NO3)2 and NiSO4, the combination of Ni(NO3)2·6H2O and Ni(CH3COO)2·4H2O, or the combination of Ni(NO3)2·6H2O, NiSO4, and NiCl2.
[0031] Preferably, the Ce salt includes any one or a combination of at least two of Ce(NO3)3, CeCl3, Ce(NO3)3·6H2O, (NH4)2Ce(NO3)6, or CeCl3·7H2O. Typical but non-limiting combinations include the combination of Ce(NO3)3 and CeCl3, the combination of (NH4)2Ce(NO3)6 and CeCl3·7H2O, or the combination of Ce(NO3)3·6H2O, (NH4)2Ce(NO3)6, and CeCl3.
[0032] Preferably, in the mixture, the ratio of the total molar amount of the Ni salt and Ce salt to the molar amount of the ligand in the ligand solution is 1:(1.5 to 3.5), for example, it can be 1:1.5, 1:1.8, 1:2.0, 1:2.2, 1:2.5, 1:2.8, 1:3.0, 1:3.2 or 1:3.5, but it is not limited to the listed values, and other unlisted values within this range are also applicable.
[0033] Preferably, the concentration of the ligand in the ligand solution is 1 mol / L to 3 mol / L, for example, it can be 1 mol / L, 1.2 mol / L, 1.4 mol / L, 1.6 mol / L, 1.8 mol / L, 2 mol / L, 2.2 mol / L, 2.4 mol / L, 2.6 mol / L, 2.8 mol / L or 3 mol / L, but it is not limited to the listed values, and other unlisted values within this range are also applicable.
[0034] Preferably, the ligand in the ligand solution comprises any one or a combination of at least two of terephthalic acid, 1,3,5-benzenetricarboxylic acid, biphenyl terephthalic acid, or 2-aminoterephthalic acid. Typical but non-limiting combinations include a combination of terephthalic acid and 1,3,5-benzenetricarboxylic acid, a combination of biphenyl terephthalic acid and 2-aminoterephthalic acid, or a combination of terephthalic acid, biphenyl terephthalic acid, and 2-aminoterephthalic acid.
[0035] Preferably, the ligand solvent in the ligand solution includes any one or a combination of at least two of water, N,N-dimethylformamide, N,N-diethylformamide, N-methylpyrrolidone, or ethanol. Typical but non-limiting combinations include a combination of water and N,N-dimethylformamide, a combination of N-methylpyrrolidone and ethanol, or a combination of water, N,N-diethylformamide, and ethanol.
[0036] Preferably, in the mixture, the ratio of the total molar amount of Ni salt and Ce salt to the volume of the solvent is 1:(200-1000), for example, it can be 1:200, 1:300, 1:400, 1:500, 1:600, 1:700, 1:800, 1:900 or 1:1000, but it is not limited to the listed values. Other unlisted values within this range are also applicable, and the unit is mol / L.
[0037] Preferably, the solvent comprises any one or a combination of at least two of water, N,N-dimethylformamide, N,N-diethylformamide, N-methylpyrrolidone, or ethanol. Typical but non-limiting combinations include a combination of water and N,N-dimethylformamide, a combination of N-methylpyrrolidone and ethanol, or a combination of water, N,N-diethylformamide, and ethanol.
[0038] Preferably, the mixture further includes the incorporation of an auxiliary solution.
[0039] Preferably, the auxiliary solution includes any one or a combination of at least two of sodium hydroxide solution, ammonia solution, or potassium hydroxide solution. Typical but non-limiting combinations include a combination of sodium hydroxide solution and ammonia solution, a combination of ammonia solution and potassium hydroxide solution, or a combination of sodium hydroxide solution, ammonia solution, and potassium hydroxide solution.
[0040] Preferably, the concentration of the solute in the auxiliary solution is 0.2 mol / L to 4 mol / L, for example, it can be 0.2 mol / L, 0.5 mol / L, 1.0 mol / L, 1.5 mol / L, 2.0 mol / L, 2.5 mol / L, 3.0 mol / L, 3.5 mol / L or 4.0 mol / L, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0041] Preferably, the solvent in the auxiliary solution includes water.
[0042] Preferably, the mixing method includes: initially mixing Ni salt, Ce salt, solvent and auxiliary solution to obtain a mixed solution; and then further mixing the obtained mixed solution with ligand solution to obtain a mixed liquid.
[0043] Preferably, the initial mixing includes: mixing the solvent and the auxiliary solution to obtain a first mixture; then adding the Ni salt and Ce salt sequentially to the obtained first mixture to obtain a clear and homogeneous mixture.
[0044] Preferably, the first mixing method includes a first magnetic stirring, wherein the first magnetic stirring time is 10 min to 20 min and the rotation speed is 300 rpm to 1100 rpm.
[0045] In this invention, the first magnetic stirring time is 10 min to 20 min, for example, it can be 10 min, 11 min, 12 min, 13 min, 14 min, 15 min, 16 min, 17 min, 18 min, 19 min or 20 min, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0046] In this invention, the rotation speed of the first magnetic stirrer is 300 rpm to 1100 rpm, for example, it can be 300 rpm, 400 rpm, 500 rpm, 600 rpm, 700 rpm, 800 rpm, 900 rpm, 1000 rpm or 1100 rpm, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0047] Preferably, during the process of sequentially adding Ni salt and Ce salt to the obtained first mixture, a second magnetic stirring is also carried out. The second magnetic stirring time is 10 min to 30 min, and the rotation speed is 500 rpm to 1400 rpm.
[0048] In this invention, the second magnetic stirring time is 10 min to 30 min, for example, it can be 10 min, 12 min, 14 min, 16 min, 18 min, 20 min, 22 min, 24 min, 26 min, 28 min or 30 min, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0049] In this invention, the rotation speed of the second magnetic stirrer is 500 rpm to 1400 rpm, for example, it can be 500 rpm, 600 rpm, 700 rpm, 800 rpm, 900 rpm, 1000 rpm, 1100 rpm, 1200 rpm, 1300 rpm or 1400 rpm, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0050] Preferably, during the process of sequentially adding Ni salt and Ce salt to the obtained first mixture, the temperature is controlled not to exceed 60°C. For example, it can be 10°C, 20°C, 30°C, 40°C, 50°C or 60°C, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0051] Preferably, the remixing includes adding the ligand solution to the resulting mixture.
[0052] Preferably, when the ligand solution is added to the resulting mixture, a third magnetic stirring is performed simultaneously. The third magnetic stirring time is 0.5h to 1.5h, and the rotation speed is 150rpm to 800rpm.
[0053] In this invention, the third magnetic stirring time is 0.5h to 1.5h, for example, it can be 0.5h, 0.6h, 0.7h, 0.8h, 0.9h, 1.0h, 1.1h, 1.2h, 1.3h, 1.4h or 1.5h, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0054] In this invention, the rotation speed of the third magnetic stirrer is 150 rpm to 800 rpm, for example, it can be 150 rpm, 200 rpm, 250 rpm, 300 rpm, 350 rpm, 400 rpm, 450 rpm, 500 rpm, 550 rpm, 600 rpm, 650 rpm, 700 rpm, 750 rpm or 800 rpm, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0055] Preferably, the method for preparing the Ni-Ce bimetallic MOF material further includes pH adjustment between the mixing and the hydrothermal reaction.
[0056] Preferably, the pH adjuster used in the pH adjustment includes any one or a combination of at least two of sodium hydroxide solution, ammonia solution, or potassium hydroxide solution. Typical but non-limiting combinations include a combination of sodium hydroxide solution and ammonia solution, a combination of ammonia solution and potassium hydroxide solution, or a combination of sodium hydroxide solution, ammonia solution, and potassium hydroxide solution.
[0057] Preferably, the pH of the mixture is adjusted to 5-6 during pH adjustment, for example, it can be 5.0, 5.1, 5.2, 5.3, 5.4, 5.5, 5.6, 5.7, 5.8, 5.9 or 6.0, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0058] Preferably, the hydrothermal reaction is carried out at a temperature of 100℃ to 120℃ for a duration of 24h to 48h.
[0059] In this invention, the temperature of the hydrothermal reaction is 100℃ to 120℃, for example, it can be 100℃, 102℃, 104℃, 106℃, 108℃, 110℃, 112℃, 114℃, 116℃, 118℃ or 120℃, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0060] In this invention, the hydrothermal reaction time is 24h to 48h, for example, it can be 24h, 26h, 28h, 30h, 32h, 34h, 36h, 38h, 40h, 42h, 44h, 46h or 48h, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0061] Preferably, the method for preparing the Ni-Ce bimetallic MOF material further includes cooling after the hydrothermal reaction.
[0062] Preferably, the final temperature of the cooling is 10°C to 30°C, for example, it can be 10°C, 12°C, 14°C, 16°C, 18°C, 20°C, 22°C, 24°C, 26°C, 28°C or 30°C, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0063] Preferably, the method for preparing the Ni-Ce bimetallic MOF material further includes the post-treatment after cooling.
[0064] Preferably, the post-processing includes: performing primary centrifugation, three rounds of washing, final centrifugation, and drying in sequence.
[0065] Preferably, the primary centrifugation speed is 800 rpm to 1500 rpm, and the time is 3 min to 10 min.
[0066] In this invention, the rotation speed of the primary centrifuge is 800 rpm to 1500 rpm, for example, it can be 800 rpm, 900 rpm, 1000 rpm, 1100 rpm, 1200 rpm, 1300 rpm, 1400 rpm or 1500 rpm, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0067] In this invention, the initial centrifugation time is 3 min to 10 min, for example, it can be 3 min, 4 min, 5 min, 6 min, 7 min, 8 min, 9 min or 10 min, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0068] Preferably, the washing solution used in the first round of the three-round washing includes any one or a combination of at least two of DMF solution, DEF solution or NMP solution, and the temperature of the washing solution is 60℃~80℃.
[0069] In this invention, the washing solution used in the first round of washing includes any one or at least two of DMF solution, DEF solution, or NMP solution. Typical but non-limiting combinations include the combination of DMF solution and DEF solution, the combination of DEF solution and NMP solution, the combination of DMF solution and NMP solution, or the combination of DMF solution, DEF solution, and NMP solution.
[0070] In this invention, the temperature of the washing solution used in the first round of washing is 60℃~80℃, for example, it can be 60℃, 62℃, 64℃, 66℃, 68℃, 70℃, 72℃, 74℃, 76℃, 78℃ or 80℃, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0071] Preferably, the washing solution used in the second round of washing includes an anhydrous ethanol solution with added hydrochloric acid; the anhydrous ethanol solution is composed of hydrochloric acid and anhydrous ethanol, the concentration of HCl in the hydrochloric acid is 0.5 mol / L to 3 mol / L, and the volume concentration of hydrochloric acid in the anhydrous ethanol solution is 1 vol% to 2 vol%.
[0072] In this invention, the concentration of HCl in the hydrochloric acid is 0.5 mol / L to 3 mol / L.
[0073] In this invention, the volume concentration of hydrochloric acid in the anhydrous ethanol solution is 1 vol% to 2 vol%.
[0074] In this invention, the temperature of the washing solution used in the second round of washing is 10℃ to 30℃, for example, it can be 10℃, 12℃, 14℃, 16℃, 18℃, 20℃, 22℃, 24℃, 26℃, 28℃ or 30℃, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0075] Preferably, the washing solution used in the third round of washing in the three-round washing includes a mixture of methanol and diethyl ether, wherein the volume ratio of methanol to diethyl ether in the mixture is (1-3):1, and the temperature of the washing solution is 10℃-30℃.
[0076] In this invention, the volume ratio of methanol to diethyl ether in the methanol-diethyl ether mixture during the third round of washing is (1-3):1, for example, it can be 1:1, 1.2:1, 1.4:1, 1.6:1, 1.8:1, 2:1, 2.2:1, 2.4:1, 2.6:1, 2.8:1 or 3:1, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0077] In this invention, the temperature of the washing solution in the third round of washing is 10℃ to 30℃, for example, it can be 10℃, 12℃, 14℃, 16℃, 18℃, 20℃, 22℃, 24℃, 26℃, 28℃ or 30℃, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0078] Preferably, the final centrifugation speed is 2000 rpm to 2600 rpm, and the time is 5 min to 20 min.
[0079] In this invention, the rotation speed of the final centrifugation is 2000 rpm to 2600 rpm, for example, it can be 2000 rpm, 2100 rpm, 2200 rpm, 2300 rpm, 2400 rpm, 2500 rpm or 2600 rpm, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0080] In this invention, the final centrifugation time is 5 min to 20 min, for example, it can be 5 min, 6 min, 7 min, 8 min, 9 min, 10 min, 11 min, 12 min, 13 min, 14 min, 15 min, 16 min, 17 min, 18 min, 19 min or 20 min, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0081] Preferably, the drying process includes: first, vacuum drying for 12 to 24 hours in a vacuum environment with a temperature of 60℃ to 80℃ and a vacuum degree of ≤0.1MPa, and then drying for 6 to 10 hours in a mixed atmosphere with a temperature of 60℃ to 80℃ and a nitrogen to hydrogen volume ratio of (80 to 95):(5 to 20).
[0082] In this invention, the temperature for vacuum drying in a vacuum environment is 60℃~80℃, for example, it can be 60℃, 62℃, 64℃, 66℃, 68℃, 70℃, 72℃, 74℃, 76℃, 78℃ or 80℃, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0083] In this invention, during the drying process, the vacuum level of the vacuum environment is ≤0.1MPa, for example, it can be 0.01MPa, 0.02MPa, 0.03MPa, 0.04MPa, 0.05MPa, 0.06MPa, 0.07MPa, 0.08MPa, 0.09MPa or 0.1MPa, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0084] In this invention, the drying process is carried out in a vacuum environment for 12 to 24 hours, for example, 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, 20h, 21h, 22h, 23h or 24h, but is not limited to the listed values. Other unlisted values within this range are also applicable.
[0085] In this invention, the drying process is carried out in a mixed atmosphere containing nitrogen and hydrogen at a temperature of 60°C to 80°C. For example, the temperature can be 60°C, 62°C, 64°C, 66°C, 68°C, 70°C, 72°C, 74°C, 76°C, 78°C, or 80°C, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0086] In this invention, the drying process is carried out in a mixed atmosphere of nitrogen and hydrogen with a volume ratio of (80-95):(5-20), for example, 80:20, 82:18, 85:15, 88:12, 90:10, 92:8 or 95:5, but is not limited to the listed values. Other unlisted values within this range are also applicable.
[0087] In this invention, the drying process is carried out in a mixed atmosphere of nitrogen and hydrogen for 6 to 10 hours. For example, it can be 6 hours, 6.5 hours, 7 hours, 7.5 hours, 8 hours, 8.5 hours, 9 hours, 9.5 hours, or 10 hours, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0088] Preferably, the heat treatment includes a first heating, a second heating, and a holding period performed sequentially, wherein a reducing gas mixture comprising a protective gas and a reducing gas is introduced during the first heating, the second heating, and the holding period.
[0089] In this invention, during the first heating process, the ligands of the Ni-Ce bimetallic MOF material undergo pyrolysis, followed by carbonization; during the second heating process, the crystal phase is reconstructed, and the reconstructed crystal phase is amorphous CeO. x The conversion to Ce2O3 / CeO2 significantly increases the oxygen vacancy concentration, Ni 0 Nanoparticles are dispersed on a carbon matrix. Ni / Ce2O3 / CeO2 particles act as nucleation sites, pinning carbon grain boundaries and inhibiting high-temperature graphitization shrinkage. Meanwhile, the carbon matrix constrains the abnormal growth of metal grains, ultimately forming a stable composite structure of "metal-oxide-carbon" three-way interlocking. The third heating process is a stabilization process, in which Ni grains complete grain boundary migration and reorganization, forming a thin carbon shell (0.5nm~1nm) on the surface. The abnormal grain growth is inhibited by Ni-C chemical bonding. The Ce2O3 / CeO2 lattice undergoes ordered shear distortion. The oxygen vacancy channels of Ce2O3 / CeO2 enhance the charge transfer at the Ni-C interface. The carbon matrix can buffer the thermal expansion difference of Ni / CeO2 through lattice shear stress matching, ultimately forming a stable high-temperature sintered three-dimensional interlocking architecture.
[0090] Preferably, the volume fraction of reducing gas in the reducing mixture introduced during the first heating is higher than the volume fraction of reducing gas in the reducing mixture introduced during the second heating and holding.
[0091] Preferably, during the first heating process, a reducing mixture of protective gas and reducing gas with a volume ratio of (85-93):(7-15) is introduced. For example, it can be 85:15, 86:14, 87:13, 88:12, 89:11, 90:10, 91:9, 92:8 or 93:7, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0092] Preferably, during the second heating process, a reducing mixture of protective gas and reducing gas with a volume ratio of (93-97):(3-7) is introduced. For example, it can be 93:7, 94:6, 95:5, 96:4 or 97:3, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0093] Preferably, during the heat preservation process, a reducing mixture of protective gas and reducing gas with a volume ratio of (93-97):(3-7) is introduced. For example, it can be 93:7, 94:6, 95:5, 96:4 or 97:3, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0094] Preferably, the flow rate of the reducing gas mixture introduced during the first heating is lower than the flow rate of the reducing gas mixture introduced during the second heating and holding periods.
[0095] Preferably, the rate at which the reducing gas mixture is introduced during the first heating process is 100 mL / min to 140 mL / min, for example, it can be 100 mL / min, 105 mL / min, 110 mL / min, 115 mL / min, 120 mL / min, 125 mL / min, 130 mL / min, 135 mL / min or 140 mL / min, but it is not limited to the listed values, and other unlisted values within this range are also applicable.
[0096] Preferably, the rate at which the reducing gas mixture is introduced during the second heating process is 140 mL / min to 200 mL / min, for example, it can be 140 mL / min, 145 mL / min, 150 mL / min, 155 mL / min, 160 mL / min, 165 mL / min, 170 mL / min, 175 mL / min, 180 mL / min, 185 mL / min, 190 mL / min, 195 mL / min or 200 mL / min, but is not limited to the listed values, other unlisted values within this range are also applicable.
[0097] Preferably, the rate at which the reducing gas mixture is introduced during the heat preservation process is 140 mL / min to 200 mL / min, for example, it can be 140 mL / min, 145 mL / min, 150 mL / min, 155 mL / min, 160 mL / min, 165 mL / min, 170 mL / min, 175 mL / min, 180 mL / min, 185 mL / min, 190 mL / min, 195 mL / min or 200 mL / min, but is not limited to the listed values, other unlisted values within this range are also applicable.
[0098] Preferably, the heating rate in the first heating process is higher than the heating rate in the second heating process.
[0099] Preferably, the heating rate of the first heating is 4℃ / min to 8℃ / min, and the final temperature is 400℃ to 600℃.
[0100] In this invention, the heating rate of the first heating is 4℃ / min to 8℃ / min, for example, it can be 4℃ / min, 4.5℃ / min, 5℃ / min, 5.5℃ / min, 6℃ / min, 6.5℃ / min, 7℃ / min, 7.5℃ / min or 8℃ / min, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0101] In this invention, the endpoint temperature of the first heating is 400℃ to 600℃, for example, it can be 400℃, 420℃, 440℃, 460℃, 480℃, 500℃, 520℃, 540℃, 560℃, 580℃ or 600℃, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0102] Preferably, the heating rate of the second heating is 2℃ / min to 4℃ / min, and the final temperature is 700℃ to 900℃.
[0103] In this invention, the heating rate of the second heating is 2℃ / min to 4℃ / min, for example, it can be 2℃ / min, 2.2℃ / min, 2.4℃ / min, 2.6℃ / min, 2.8℃ / min, 3℃ / min, 3.2℃ / min, 3.4℃ / min, 3.6℃ / min, 3.8℃ / min or 4℃ / min, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0104] In this invention, the endpoint temperature of the second heating is 700℃ to 900℃, for example, it can be 700℃, 720℃, 740℃, 760℃, 780℃, 800℃, 820℃, 840℃, 860℃, 880℃ or 900℃, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0105] Preferably, the temperature for heat preservation is the endpoint temperature of the second heating, and the heat preservation time is 0.5h to 1.5h, for example, it can be 0.5h, 0.6h, 0.7h, 0.8h, 0.9h, 1.0h, 1.1h, 1.2h, 1.3h, 1.4h or 1.5h, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0106] Preferably, pre-drying is included before the first heating.
[0107] Preferably, the pre-drying includes: heating to 180°C to 220°C at a heating rate of 3°C / min to 6°C / min and then maintaining the temperature at that temperature for 0.5h to 2h.
[0108] In this invention, during the pre-drying process, the temperature is increased at a rate of 3°C / min to 6°C / min, for example, 3°C / min, 3.5°C / min, 4°C / min, 4.5°C / min, 5°C / min, 5.5°C / min or 6°C / min, but is not limited to the listed values. Other unlisted values within this range are also applicable.
[0109] In this invention, during the pre-drying process, the temperature is raised to 180℃~220℃ and then kept constant. The temperature for constant temperature holding can be, for example, 180℃, 185℃, 190℃, 195℃, 200℃, 205℃, 210℃, 215℃ or 220℃, but is not limited to the listed values. Other unlisted values within this range are also applicable.
[0110] In this invention, the pre-drying process is carried out at a constant temperature for 0.5h to 2h, for example, it can be 0.5h, 0.8h, 1.0h, 1.2h, 1.5h, 1.8h or 2.0h, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0111] Preferably, during the pre-drying process, a protective gas is introduced at a rate of 180 mL / min to 250 mL / min. The rate of introduction of the protective gas can be, for example, 180 mL / min, 190 mL / min, 200 mL / min, 210 mL / min, 220 mL / min, 230 mL / min, 240 mL / min or 250 mL / min, but is not limited to the listed values. Other unlisted values within this range are also applicable.
[0112] Preferably, the process after heat preservation includes cooling, wherein a reducing gas mixture comprising a protective gas and a reducing gas is introduced during the cooling process, and the volume fraction of the reducing gas in the reducing gas mixture introduced during cooling is higher than the volume fraction of the reducing gas in the reducing gas mixture introduced during the first heating.
[0113] Preferably, during the cooling process, a reducing gas mixture comprising a protective gas and a reducing gas in a volume ratio of (80-92):(8-20) is introduced. The volume ratio of the protective gas to the reducing gas in the reducing gas mixture introduced during the cooling process can be, for example, 80:20, 82:18, 84:16, 86:14, 88:12, 90:10, or 92:8, but is not limited to the listed values. Other unlisted values within this range are also applicable.
[0114] Preferably, the rate at which the reducing gas mixture is introduced during the cooling process is 50 mL / min to 100 mL / min, for example, it can be 50 mL / min, 55 mL / min, 60 mL / min, 65 mL / min, 70 mL / min, 75 mL / min, 80 mL / min, 85 mL / min, 90 mL / min, 95 mL / min or 100 mL / min, but it is not limited to the listed values, and other unlisted values within this range are also applicable.
[0115] Preferably, the cooling method includes furnace cooling, with an endpoint temperature of 10℃ to 30℃, for example, 10℃, 12℃, 14℃, 16℃, 18℃, 20℃, 22℃, 24℃, 26℃, 28℃ or 30℃, but not limited to the listed values, other unlisted values within this range are also applicable.
[0116] Preferably, the protective gas includes any one or a combination of at least two of nitrogen, argon, helium or neon. Typical but non-limiting combinations include combinations of nitrogen and argon, helium and neon, argon and helium, or nitrogen, argon and helium.
[0117] Preferably, the reducing gas includes hydrogen and / or carbon monoxide.
[0118] Preferably, the preparation method further includes a first pre-ball milling of the MOF material carbonized derivative between the heat treatment and the mixing.
[0119] Preferably, the first pre-ball milling is carried out in a protective atmosphere, with a ball-to-material ratio of (8-12):1, a rotation speed of 200 rpm to 600 rpm, and a time of 0.5 h to 3 h.
[0120] In this invention, the ball-to-material ratio of the first pre-ball mill is (8-12):1, for example, it can be 8:1, 8.5:1, 9:1, 9.5:1, 10:1, 10.5:1, 11:1, 11.5:1 or 12:1, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0121] In this invention, the rotation speed of the first pre-ball mill is 200 rpm to 600 rpm, for example, it can be 200 rpm, 250 rpm, 300 rpm, 350 rpm, 400 rpm, 450 rpm, 500 rpm, 550 rpm or 600 rpm, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0122] In this invention, the first pre-ball milling time is 0.5h to 3h, for example, it can be 0.5h, 0.8h, 1.0h, 1.2h, 1.5h, 1.8h, 2.0h, 2.2h, 2.5h, 2.8h or 3.0h, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0123] Preferably, the preparation method further includes pretreatment of MgH2 before mixing, the pretreatment including drying MgH2 and then performing a second pre-ball milling.
[0124] Preferably, the drying in the pretreatment includes vacuum drying at 50°C to 70°C for 18 to 36 hours.
[0125] In this invention, the vacuum drying in the pretreatment is carried out at 50°C to 70°C, for example, 50°C, 52°C, 54°C, 56°C, 58°C, 60°C, 62°C, 64°C, 66°C, 68°C or 70°C, but is not limited to the listed values. Other unlisted values within this range are also applicable.
[0126] In this invention, the vacuum drying time in the pretreatment is 18h to 36h, for example, it can be 18h, 20h, 22h, 24h, 26h, 28h, 30h, 32h, 34h or 36h, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0127] Preferably, the second pre-ball milling is carried out in a protective atmosphere, with a ball-to-material ratio of (10-15):1, a rotation speed of 300-500 rpm, and a time of 0.5-1.5 h.
[0128] In this invention, the ball-to-material ratio of the second pre-ball mill is (10-15):1, for example, it can be 10:1, 11:1, 12:1, 13:1, 14:1 or 15:1, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0129] In this invention, the rotation speed of the second pre-ball mill is 300 rpm to 500 rpm, for example, it can be 300 rpm, 325 rpm, 350 rpm, 375 rpm, 400 rpm, 425 rpm, 450 rpm, 475 rpm or 500 rpm, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0130] In this invention, the second pre-ball milling time is 0.5h to 1.5h, for example, it can be 0.5h, 0.6h, 0.7h, 0.8h, 0.9h, 1.0h, 1.1h, 1.2h, 1.3h, 1.4h or 1.5h, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0131] Preferably, the mixing includes sequentially performing a first ball milling, a second ball milling, and a third ball milling.
[0132] In this invention, the staged ball milling process of mixing the carbonized derivatives of MOF materials with MgH2 facilitates the formation of a multi-level nanocomposite structure, thereby improving the adsorption performance and stability of the Mg-based hydrogen storage material.
[0133] Preferably, the rotational speed of the second ball mill is greater than that of the first ball mill and the third ball mill.
[0134] Preferably, the rotation speed of the first ball mill is 200 rpm to 400 rpm, and the time is 2 h to 4 h.
[0135] In this invention, the rotational speed of the first ball mill is 200 rpm to 400 rpm, for example, it can be 200 rpm, 220 rpm, 240 rpm, 260 rpm, 280 rpm, 300 rpm, 320 rpm, 340 rpm, 360 rpm, 380 rpm or 400 rpm, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0136] In this invention, the first ball milling time is 2h to 4h, for example, it can be 2h, 2.2h, 2.4h, 2.6h, 2.8h, 3h, 3.2h, 3.4h, 3.6h, 3.8h or 4h, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0137] Preferably, the second ball mill rotates at 500 rpm to 600 rpm for 4 hours to 6 hours, and during the second ball milling process, it cools for 10 minutes to 30 minutes every 1 hour to 1.5 hours.
[0138] In this invention, the rotational speed of the second ball mill is 500 rpm to 600 rpm, for example, it can be 500 rpm, 510 rpm, 520 rpm, 530 rpm, 540 rpm, 550 rpm, 560 rpm, 570 rpm, 580 rpm, 590 rpm or 600 rpm, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0139] In this invention, the second ball milling time is 4h to 6h, for example, it can be 4h, 4.2h, 4.4h, 4.6h, 4.8h, 5h, 5.2h, 5.4h, 5.6h, 5.8h or 6h, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0140] In this invention, during the second ball milling process, the cooling time is 10 min to 30 min every 1 h to 1.5 h of ball milling. For example, it can be 10 min every 1 h, 15 min every 1.2 h, 20 min every 1.3 h, or 30 min every 1.5 h, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0141] In this invention, the second ball milling time is 4h to 6h, for example, it can be 4h, 4.2h, 4.4h, 4.6h, 4.8h, 5h, 5.2h, 5.4h, 5.6h, 5.8h or 6h, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0142] Preferably, the rotation speed of the third ball mill is 350 rpm to 450 rpm, and the time is 1 h to 2 h.
[0143] In this invention, the rotational speed of the third ball mill is 350 rpm to 450 rpm, for example, it can be 350 rpm, 360 rpm, 370 rpm, 380 rpm, 390 rpm, 400 rpm, 410 rpm, 420 rpm, 430 rpm, 440 rpm or 450 rpm, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0144] In this invention, the third ball milling time is 1h to 2h, for example, it can be 1h, 1.1h, 1.2h, 1.3h, 1.4h, 1.5h, 1.6h, 1.7h, 1.8h, 1.9h or 2h, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0145] Preferably, the first, second, and third ball millings are each carried out independently in a protective atmosphere with a pressure of 1 bar to 2 bar. The pressure of the protective atmosphere can be, for example, 1.0 bar, 1.1 bar, 1.2 bar, 1.3 bar, 1.4 bar, 1.5 bar, 1.6 bar, 1.7 bar, 1.8 bar, 1.9 bar, or 2.0 bar, but is not limited to the listed values. Other unlisted values within this range are also applicable.
[0146] Preferably, the protective atmosphere includes any one or a combination of at least two of nitrogen, argon, helium or neon. Typical but non-limiting combinations include a combination of nitrogen and argon, a combination of helium and neon, a combination of argon and helium, or a combination of nitrogen, argon and helium.
[0147] As a preferred embodiment of the preparation method of the present invention, the preparation method includes:
[0148] (1) The solvent and an auxiliary solution with a solute concentration of 0.2 mol / L to 4 mol / L were mixed for 10 min to 20 min by stirring at a speed of 300 rpm to 1100 rpm to obtain a first mixture; Ni salt and Ce salt were then added to the first mixture in sequence at a temperature not higher than 60℃, while stirring at a speed of 500 rpm to 1400 rpm for 10 min to 30 min to obtain a clear and homogeneous mixture; a ligand solution with a ligand concentration of 1 mol / L to 3 mol / L was then added to the mixture while stirring at a speed of 150 rpm to 800 rpm for 0.5 h to 1.5 h to obtain a mixed liquid.
[0149] The ratio of the total molar amount of the Ni salt and Ce salt to the volume of the solvent (excluding the solvent in the auxiliary solution and the ligand solvent in the ligand solution) is 1:(200-1000), in mol / L; the molar ratio of the Ni salt to the Ce salt is (1-3):(1-4); the ratio of the total molar amount of the Ni salt and Ce salt to the molar amount of the ligand in the ligand solution is 1:(1.5-3.5).
[0150] (2) Adjust the pH of the mixture obtained in step (1) to 5-6 with at least one of sodium hydroxide solution, ammonia solution, or potassium hydroxide solution. Then, perform hydrothermal treatment at 100℃-120℃ for 24-48 hours, cool to 10℃-30℃, centrifuge at 800rpm-1500rpm for 3-10 minutes, wash with a washing solution at 60℃-80℃, wash again with anhydrous ethanol solution containing hydrochloric acid at 10℃-30℃, and then wash again with a solution containing hydrochloric acid at 10℃-30℃. The mixture of methanol and diethyl ether in a volume ratio of (1-3):1 was washed and then centrifuged at 2000-2600 rpm for 5-20 minutes. The solid obtained after centrifugation was then vacuum dried in a vacuum environment at 60-80℃ and a vacuum degree ≤0.1MPa for 12-24 hours, and then dried in a mixed atmosphere at 60-80℃ and a nitrogen to hydrogen volume ratio of (80-95):(5-20) for 6-10 hours to obtain Ni-Ce bimetallic MOF material.
[0151] (3) After pre-drying the Ni-Ce bimetallic MOF material obtained in step (2), the first heating, the second heating, the heat preservation and the cooling are performed in sequence to obtain the MOF material carbonized derivative.
[0152] The pre-drying process includes: heating to 180℃~220℃ at a heating rate of 3℃ / min~6℃ / min and then maintaining the temperature at a constant temperature for 0.5h~2h, during which a protective gas is introduced at a rate of 180mL / min~250mL / min.
[0153] The first heating includes: heating to 400℃ to 600℃ at a heating rate of 4℃ / min to 8℃ / min, and during the first heating process, introducing a reducing gas mixture comprising a protective gas and a reducing gas in a volume ratio of (85 to 93):(7 to 15) at a rate of 100mL / min to 140mL / min.
[0154] The second heating includes heating to 700℃ to 900℃ at a heating rate of 2℃ / min to 4℃ / min, during which a reducing mixture of protective gas and reducing gas with a volume ratio of (93 to 97):(3 to 7) is introduced at a rate of 140mL / min to 200mL / min.
[0155] The heat preservation includes: heat preservation at 700℃~900℃ for 0.5h~1.5h, during which a reducing gas mixture comprising a protective gas and a reducing gas in a volume ratio of (93~97):(3~7) is introduced at a rate of 140mL / min~200mL / min.
[0156] The cooling process includes: cooling the furnace to 10°C to 30°C, during which a reducing mixture of protective gas and reducing gas with a volume ratio of (80 to 92):(8 to 20) is introduced at a rate of 50 mL / min to 100 mL / min.
[0157] The volume fraction of reducing gas in the reducing mixture introduced during the first heating is higher than the volume fraction of reducing gas in the reducing mixture introduced during the second heating and holding.
[0158] The flow rate of the reducing gas mixture introduced during the first heating is lower than the flow rate of the reducing gas mixture introduced during the second heating and holding periods.
[0159] The heating rate in the first heating process is higher than the heating rate in the second heating process;
[0160] The volume fraction of reducing gas in the reducing mixture introduced during cooling is higher than the volume fraction of reducing gas in the reducing mixture introduced during the first heating.
[0161] (4) In a protective atmosphere, the MOF material carbonized derivative obtained in step (3) is subjected to a first pre-ball milling. The ball-to-material ratio of the first pre-ball milling is (8-12):1, the rotation speed is 200 rpm to 600 rpm, and the time is 0.5 h to 3 h, to obtain the MOF material carbonized derivative after ball milling.
[0162] After vacuum drying of MgH2 at 50℃~70℃ for 18h~36h, a second pre-ball milling is carried out in a protective atmosphere. The ball-to-material ratio of the second pre-ball milling is (10~15):1, the rotation speed is 300rpm~500rpm, and the time is 0.5h~1.5h to obtain ball-milled MgH2.
[0163] (5) In a protective atmosphere with a pressure of 1 bar to 2 bar, the carbonized derivative of the MOF material obtained in step (4) and the MgH2 obtained after ball milling are first mixed by a first ball milling at a speed of 200 rpm to 400 rpm for 2 h to 4 h to obtain a first mixture; then the first mixture is ball milled at a speed of 500 rpm to 600 rpm for 4 h to 6 h. During the second ball milling, the mixture is cooled for 10 min to 30 min every 1 h to 1.5 h of ball milling. After the second ball milling, a second mixture is obtained; then the second mixture is ball milled at a speed of 350 rpm to 450 rpm for 1 h to 2 h to obtain a Mg-based hydrogen storage material.
[0164] Thirdly, the present invention provides an application of the Mg-based hydrogen storage material described in the first aspect, wherein the Mg-based hydrogen storage material is used in metal hydride solid-state hydrogen storage technology.
[0165] The numerical range described in this invention includes not only the point values listed above, but also any point values within the numerical ranges not listed above. Due to space limitations and for the sake of brevity, this invention will not exhaustively list all the specific point values included in the range.
[0166] Compared with the prior art, the present invention has the following beneficial effects:
[0167] (1) The carbonized derivative of the Ni-Ce bimetallic MOF material formed by carbonization contains a carbon skeleton with hierarchical pores. The hierarchical pore carbon skeleton can not only provide a highly dispersed loading interface for MgH2 and catalytic sites, but also suppress the growth of Mg grains caused by the hydrogen absorption-desorption cycle through the confinement effect.
[0168] (2) There is a weak Mg-C chemical bond between MgH2 and the hierarchical porous carbon framework of the MOF material carbonization derivative, which enhances the interfacial bonding force between the hierarchical porous carbon framework and MgH2, improves the stability of Mg-based hydrogen storage materials, and thus reduces the shedding of MgH2 during cycling.
[0169] (3) The carbonized derivative of the Ni-Ce bimetallic MOF material formed by carbonization contains Ni nanoparticles. The Ni nanoparticles are uniformly dispersed on the hierarchical porous carbon framework derived from MOF, serving as highly efficient catalytic active sites that can promote the dissociation and adsorption of H2 molecules.
[0170] (4) The carbonization derivatives of MOF materials include nano Ce2O3 particles and / or nano CeO2 particles formed during the carbonization process of Ni-Ce bimetallic MOF materials. The nano Ce2O3 particles and / or nano CeO2 particles form a symbiotic structure with the grain boundaries of MgH2, which can promote the diffusion of hydrogen atoms along the grain boundaries.
[0171] (5) Carbonized derivatives of MOF materials include nano-Ce2O3 particles and / or nano-CeO2 particles formed during the carbonization process of Ni-Ce bimetallic MOF materials. 3+ The resulting lattice distortion creates dynamic oxygen vacancy regions on the surface of nano-Ce2O3 particles and / or nano-CeO2 particles, which lowers the adsorption energy of surface H atoms and the dissociation energy barrier of Mg-H bonds. These regions can serve as “capture-release” sites for hydrogen atoms, further accelerating the diffusion and recombination of hydrogen.
[0172] (6) The hierarchical porous carbon framework inhibits the aggregation of Ni and Ce2O3 / CeO2 during carbonization through physical isolation effect, thereby improving the long-term stability of the nanocatalytic interface.
[0173] (7) The present invention modifies MgH2 with a carbonized derivative of MOF material containing carbonized Ni-Ce bimetallic MOF material to obtain Mg-based hydrogen storage material. Through the synergistic effects of physical isolation and loading of hierarchical porous carbon framework, interface enhancement of Mg-C bond, catalytic activation of Ni nanoparticles, and grain boundary effect and oxygen vacancy regulation of Ce-based oxide, the hydrogen storage performance of the material is effectively improved and structural changes during cycling are suppressed. Therefore, the Mg-based hydrogen storage material has excellent hydrogen storage performance and strong stability. Attached Figure Description
[0174] Figure 1 The curves show the changes in hydrogen content of the Mg-based hydrogen storage material provided in Example 4 at 423K, 523K, 573K, 623K, and 673K as a function of hydrogen storage time. Detailed Implementation
[0175] The technical solution of the present invention will be further illustrated below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely illustrative of the present invention and should not be construed as limiting the invention in any way.
[0176] Example 1
[0177] This embodiment provides a Mg-based hydrogen storage material, which includes MgH2 and a carbonized derivative of MOF material; the carbonized derivative of MOF material includes a carbonized Ni-Ce bimetallic MOF material.
[0178] In the Mg-based hydrogen storage material, the mass ratio of the MOF material carbonized derivative to MgH2 is 5:100;
[0179] Based on the mass percentage of the MOF material carbonized derivative, the mass fraction of carbon material in the MOF material carbonized derivative is 70 wt%.
[0180] The molar ratio of Ni to Ce in the Mg-based hydrogen storage material is 1:3;
[0181] The preparation method of the Mg-based hydrogen storage material includes:
[0182] (1) N,N-dimethylformamide solvent and sodium hydroxide solution with a solute concentration of 2 mol / L were mixed for 15 min by magnetic stirring at a speed of 700 rpm to obtain a first mixture; then Ni(NO3)2·6H2O and Ce(NO3)3·6H2O were added to the first mixture in sequence at 25℃, and stirred at a speed of 600 rpm for 20 min during the addition process to obtain a clear and homogeneous mixture; then terephthalic acid solution with a ligand concentration of 2 mol / L was added to the mixture, and stirred at a speed of 500 rpm for 1 h during the addition process to obtain a mixed liquid;
[0183] The volume ratio of the sodium hydroxide solution to the N,N-dimethylformamide solvent is 30:200; the ratio of the total molar amount of Ni(NO3)2·6H2O and Ce(NO3)3·6H2O to the volume of the N,N-dimethylformamide solvent is 1:500 (mol / L); the molar ratio of Ni(NO3)2·6H2O to Ce(NO3)3·6H2O is 1:3; the ratio of the total molar amount of Ni(NO3)2·6H2O and Ce(NO3)3·6H2O to the molar amount of the ligand in the ligand solution is 1:2.5.
[0184] (2) Adjust the pH of the mixture obtained in step (1) to 5.5 with ammonia water, perform hydrothermal treatment at 100℃ for 36 hours, cool to 25℃, centrifuge at 800 rpm for 7 minutes, wash the solid obtained by centrifugation with DMF solution at 60℃, wash with anhydrous ethanol solution with added hydrochloric acid at 25℃, wash with a mixture of methanol and diethyl ether at 25℃ (volume ratio 3:1), centrifuge at 2300 rpm for 10 minutes, vacuum dry the solid obtained by centrifugation in a vacuum environment at 70℃ and vacuum degree ≤0.1MPa for 12 hours, and then dry in a mixed atmosphere at 70℃ and nitrogen and hydrogen at a volume ratio of 90:10 for 8 hours to obtain Ni-Ce bimetallic MOF material.
[0185] (3) After pre-drying the Ni-Ce bimetallic MOF material obtained in step (2), the first heating, the second heating, the heat preservation and the cooling are performed in sequence to obtain the MOF material carbonized derivative.
[0186] The pre-drying process includes: heating to 200°C at a heating rate of 5°C / min and maintaining the temperature at 200 mL / min during the process.
[0187] The first heating includes: heating to 500°C at a heating rate of 5°C / min, and then introducing a reducing mixture of helium and hydrogen with a volume ratio of 92:8 at a rate of 120 mL / min during the first heating process.
[0188] The second heating includes heating to 800°C at a heating rate of 3°C / min, during which a reducing mixture of helium and hydrogen with a volume ratio of 95:5 is introduced at a rate of 150 mL / min.
[0189] The heat preservation includes: heat preservation at 800℃ for 1 hour, during which a reducing mixture of helium and hydrogen with a volume ratio of 95:5 is introduced at a rate of 150 mL / min.
[0190] The cooling process includes: cooling the furnace to 25°C while introducing a reducing mixture of helium and hydrogen at a volume ratio of 90:10 at a rate of 80 mL / min.
[0191] (4) In an argon atmosphere, the MOF material carbonized derivative obtained in step (3) is subjected to a first pre-ball milling. The ball-to-material ratio of the first pre-ball milling is 10:1, the rotation speed is 300 rpm, and the time is 0.5 h, so as to obtain the MOF material carbonized derivative after ball milling.
[0192] After vacuum drying of MgH2 at 60℃ for 24h, a second pre-ball milling was carried out in an argon atmosphere. The ball-to-material ratio of the second pre-ball milling was 12:1, the rotation speed was 400rpm, and the time was 1h, to obtain ball-milled MgH2.
[0193] (5) In an argon atmosphere with a pressure of 1.2 bar, the carbonized derivative of the MOF material obtained in step (4) and the MgH2 obtained after ball milling are first mixed by ball milling at a speed of 400 rpm for 2 hours to obtain a first mixture; then the first mixture is ball milled at a speed of 500 rpm for 5 hours. During the second ball milling, the mixture is cooled for 10 minutes every 1 hour of ball milling (the time of the second ball milling does not include the cooling time). The second mixture is obtained after the second ball milling; then the second mixture is ball milled at a speed of 350 rpm for 1 hour to obtain a Mg-based hydrogen storage material.
[0194] Example 2
[0195] This embodiment provides a Mg-based hydrogen storage material, except that the molar ratio of Ni to Ce in the Mg-based hydrogen storage material is 1.5:2.5;
[0196] In step (1) of the preparation method of the Mg-based hydrogen storage material, the molar ratio of Ni(NO3)2·6H2O to Ce(NO3)3·6H2O is 1.5:2.5, and the total molar amount of Ni(NO3)2·6H2O and Ce(NO3)3·6H2O added remains unchanged. All other steps are the same as in Example 1.
[0197] Example 3
[0198] This embodiment provides a Mg-based hydrogen storage material, except that the molar ratio of Ni to Ce in the Mg-based hydrogen storage material is 2:2;
[0199] In step (1) of the preparation method of the Mg-based hydrogen storage material, the molar ratio of Ni(NO3)2·6H2O to Ce(NO3)3·6H2O is 2:2, and the total molar amount of Ni(NO3)2·6H2O and Ce(NO3)3·6H2O added remains unchanged. All other steps are the same as in Example 1.
[0200] Example 4
[0201] This embodiment provides a Mg-based hydrogen storage material, except that the molar ratio of Ni to Ce in the Mg-based hydrogen storage material is 2.5:1.5;
[0202] In step (1) of the preparation method of the Mg-based hydrogen storage material, the molar ratio of Ni(NO3)2·6H2O to Ce(NO3)3·6H2O is 2.5:1.5, and the total molar amount of Ni(NO3)2·6H2O and Ce(NO3)3·6H2O added remains unchanged. All other steps are the same as in Example 1.
[0203] Example 5
[0204] This embodiment provides a Mg-based hydrogen storage material, except that the molar ratio of Ni to Ce in the Mg-based hydrogen storage material is 3:1;
[0205] In step (1) of the preparation method of the Mg-based hydrogen storage material, the molar ratio of Ni(NO3)2·6H2O to Ce(NO3)3·6H2O is 3:1, and the total molar amount of Ni(NO3)2·6H2O and Ce(NO3)3·6H2O added remains unchanged. All other steps are the same as in Example 1.
[0206] Example 6
[0207] This embodiment provides a Mg-based hydrogen storage material, which includes MgH2 and a carbonized derivative of MOF material; the carbonized derivative of MOF material includes a carbonized Ni-Ce bimetallic MOF material.
[0208] In the Mg-based hydrogen storage material, the mass ratio of the MOF material carbonized derivative to MgH2 is 5:100;
[0209] Based on the mass percentage of the MOF material carbonized derivative, the mass fraction of carbon material in the MOF material carbonized derivative is 65 wt%.
[0210] The molar ratio of Ni to Ce in the Mg-based hydrogen storage material is 3:1;
[0211] The preparation method of the Mg-based hydrogen storage material includes:
[0212] (1) N-methylpyrrolidone solvent and potassium hydroxide solution with a solute concentration of 0.2 mol / L were mixed for 20 min by magnetic stirring at a speed of 300 rpm to obtain a first mixture; then NiSO4 and CeCl3 were added to the first mixture in sequence at 55℃, and the addition was accompanied by stirring at a speed of 1400 rpm for 10 min to obtain a clear and homogeneous mixture; then biphenyl dicarboxylic acid solution with a ligand concentration of 1 mol / L was added to the mixture, and the addition was accompanied by stirring at a speed of 150 rpm for 1.5 h to obtain a mixed liquid.
[0213] The volume ratio of the potassium hydroxide solution to the N-methylpyrrolidone solvent is 30:200; the ratio of the total molar amount of NiSO4 and CeCl3 to the volume of the N-methylpyrrolidone solvent is 1:200 (in mol / L); the molar ratio of NiSO4 to CeCl3 is 3:1; the ratio of the total molar amount of NiSO4 and CeCl3 to the molar amount of 1,3,5-benzenetricarboxylic acid in the 1,3,5-benzenetricarboxylic acid solution is 1:1.5.
[0214] (2) The pH of the mixture obtained in step (1) was adjusted to 5 with potassium hydroxide solution, and then subjected to hydrothermal treatment at 120°C for 24 hours. After cooling to 30°C, it was centrifuged at 1500 rpm for 3 minutes, washed with a washing solution at 80°C, washed with anhydrous ethanol solution containing hydrochloric acid at 30°C, washed with a mixture of methanol and diethyl ether at a volume ratio of 1:1 at 30°C, and then centrifuged at 2000 rpm for 20 minutes. The solid obtained after centrifugation was first vacuum dried in a vacuum environment at 80°C and a vacuum degree ≤0.1MPa for 12 hours, and then dried in a mixed atmosphere at 80°C and a nitrogen to hydrogen volume ratio of 80:20 for 6 hours to obtain Ni-Ce bimetallic MOF material.
[0215] (3) After pre-drying the Ni-Ce bimetallic MOF material obtained in step (2), the first heating, the second heating, the heat preservation and the cooling are performed in sequence to obtain the MOF material carbonized derivative.
[0216] The pre-drying process includes: heating to 180°C at a heating rate of 3°C / min and maintaining the temperature at 180°C for 2 hours, during which nitrogen gas is introduced at a rate of 180 mL / min.
[0217] The first heating includes: heating to 400°C at a heating rate of 4°C / min, and during the first heating process, introducing a reducing gas mixture of nitrogen and hydrogen with a volume ratio of 85:15 at a rate of 100 mL / min.
[0218] The second heating includes heating to 700°C at a heating rate of 2°C / min, during which a reducing mixture of nitrogen and hydrogen with a volume ratio of 93:7 is introduced at a rate of 140 mL / min.
[0219] The heat preservation includes: heat preservation at 700℃ for 1.5h, during which a reducing mixture of nitrogen and hydrogen with a volume ratio of 93:7 is introduced at a rate of 140mL / min.
[0220] The cooling process includes: cooling the furnace to 10°C while introducing a reducing mixture of nitrogen and hydrogen in a volume ratio of 80:20 at a rate of 50 mL / min.
[0221] (4) In a nitrogen atmosphere, the MOF material carbonized derivative obtained in step (3) is subjected to a first pre-ball milling. The ball-to-material ratio of the first pre-ball milling is 8:1, the rotation speed is 200 rpm, and the time is 3 h, so as to obtain the MOF material carbonized derivative after ball milling.
[0222] After vacuum drying of MgH2 at 70℃ for 18h, a second pre-ball milling was carried out in a nitrogen atmosphere. The ball-to-material ratio of the second pre-ball milling was 15:1, the rotation speed was 500rpm, and the time was 0.5h, to obtain ball-milled MgH2.
[0223] (5) In a nitrogen atmosphere with a pressure of 1 bar, the carbonized derivative of the MOF material obtained in step (4) and the MgH2 obtained after ball milling are first mixed by ball milling at a speed of 200 rpm for 4 hours to obtain a first mixture; then the first mixture is ball milled at a speed of 600 rpm for 4 hours. During the second ball milling, the mixture is cooled for 10 minutes every 1 hour of ball milling (the time of the second ball milling does not include the cooling time). After the second ball milling, a second mixture is obtained; then the second mixture is ball milled at a speed of 450 rpm for 1 hour to obtain a Mg-based hydrogen storage material.
[0224] Example 7
[0225] This embodiment provides a Mg-based hydrogen storage material, which includes MgH2 and a carbonized derivative of MOF material; the carbonized derivative of MOF material includes a carbonized Ni-Ce bimetallic MOF material.
[0226] In the Mg-based hydrogen storage material, the mass ratio of the MOF material carbonized derivative to MgH2 is 20:100;
[0227] Based on the mass percentage of the MOF material carbonized derivative, the mass fraction of carbon material in the MOF material carbonized derivative is 85 wt%.
[0228] The molar ratio of Ni to Ce in the Mg-based hydrogen storage material is 1:4;
[0229] The preparation method of the Mg-based hydrogen storage material includes:
[0230] (1) N-methylpyrrolidone solvent and sodium hydroxide solution with a solute concentration of 4 mol / L were mixed for 10 min by magnetic stirring at a speed of 300 rpm to 1100 rpm to obtain a first mixture; then Ni(CH3COO)2·4H2O and CeCl3·7H2O were added to the first mixture in sequence at a temperature of 20℃, while stirring at a speed of 500 rpm for 30 min during the addition process to obtain a clear and homogeneous mixture; then biphenyl dicarboxylic acid solution with a ligand concentration of 3 mol / L was added to the mixture while stirring at a speed of 800 rpm for 0.5 h during the addition process to obtain a mixed liquid;
[0231] The volume ratio of the sodium hydroxide solution to the N-methylpyrrolidone solvent is 30:200; the ratio of the total molar amount of Ni(CH3COO)2·4H2O and CeCl3·7H2O to the volume of the N-methylpyrrolidone solvent is 1:1000 (mol / L); the molar ratio of Ni(CH3COO)2·4H2O to CeCl3·7H2O is 1:4; the ratio of the total molar amount of Ni(CH3COO)2·4H2O and CeCl3·7H2O to the molar amount of biphenylcarboxylic acid in the biphenylcarboxylic acid solution is 1:3.5.
[0232] (2) The pH of the mixture obtained in step (1) was adjusted to 6 with sodium hydroxide solution, and then subjected to hydrothermal treatment at 100°C for 48 hours. After cooling to 10°C, it was centrifuged at 800 rpm for 10 minutes, washed with a washing solution at 60°C, washed with anhydrous ethanol solution containing hydrochloric acid at 10°C, washed with a mixture of methanol and diethyl ether at a volume ratio of 3:1 at 10°C, and then centrifuged at 2600 rpm for 5 minutes. The solid obtained after centrifugation was first vacuum dried in a vacuum environment at 60°C and a vacuum degree ≤0.1MPa for 24 hours, and then dried in a mixed atmosphere at 60°C and a nitrogen to hydrogen volume ratio of 95:5 for 10 hours to obtain Ni-Ce bimetallic MOF material.
[0233] (3) After pre-drying the Ni-Ce bimetallic MOF material obtained in step (2), the first heating, the second heating, the heat preservation and the cooling are performed in sequence to obtain the MOF material carbonized derivative.
[0234] The pre-drying process includes: heating to 220°C at a heating rate of 6°C / min and holding at that temperature for 0.5 hours, during which argon gas is introduced at a rate of 250 mL / min.
[0235] The first heating includes: heating to 600°C at a heating rate of 8°C / min, and then introducing a reducing mixture of argon and hydrogen with a volume ratio of 93:7 at a rate of 140 mL / min during the first heating process.
[0236] The second heating includes heating to 900°C at a heating rate of 4°C / min, during which a reducing mixture of argon and hydrogen with a volume ratio of 97:3 is introduced at a rate of 200 mL / min.
[0237] The heat preservation includes: heat preservation at 900℃ for 0.5h, during which a reducing mixture of argon and hydrogen with a volume ratio of 97:3 is introduced at a rate of 200mL / min.
[0238] The cooling process includes: cooling the furnace to 30°C while introducing a reducing mixture of argon and hydrogen at a volume ratio of 92:8 at a rate of 100 mL / min.
[0239] (4) In an argon atmosphere, the MOF material carbonized derivative obtained in step (3) is subjected to a first pre-ball milling. The ball-to-material ratio of the first pre-ball milling is 12:1, the rotation speed is 600 rpm, and the time is 0.5 h, so as to obtain the MOF material carbonized derivative after ball milling.
[0240] After vacuum drying of MgH2 at 50℃ for 36h, a second pre-ball milling was carried out in an argon atmosphere. The ball-to-material ratio of the second pre-ball milling was 10:1, the rotation speed was 300rpm, and the time was 1.5h, to obtain ball-milled MgH2.
[0241] (5) In an argon atmosphere with a pressure of 2 bar, the carbonized derivative of the MOF material obtained in step (4) and the MgH2 obtained after ball milling are first mixed by ball milling at a speed of 400 rpm for 2 hours to obtain a first mixture; then the first mixture is ball milled at a speed of 500 rpm for 6 hours (the time of the second ball milling does not include the cooling time). During the second ball milling process, the mixture is cooled for 30 minutes every 1.5 hours of ball milling. After the second ball milling, a second mixture is obtained; then the second mixture is ball milled at a speed of 350 rpm for 2 hours to obtain a Mg-based hydrogen storage material.
[0242] Example 8
[0243] This embodiment provides a Mg-based hydrogen storage material, wherein the mass ratio of the MgH2 to the carbide derivative of the MOF material is 2:100.
[0244] Except for step (5) of the preparation method of the Mg-based hydrogen storage material, in which the mass ratio of the carbonized derivative of the MOF material after ball milling to the MgH2 after ball milling is 2:100, all other steps are the same as in Example 1.
[0245] Example 9
[0246] This embodiment provides a Mg-based hydrogen storage material, except that the mass ratio of the carbide derivative of the MOF material to MgH2 is 30:100;
[0247] Except for step (5) of the preparation method of the Mg-based hydrogen storage material, in which the mass ratio of the carbonized derivative of the MOF material after ball milling to the MgH2 after ball milling is 30:100, all other steps are the same as in Example 1.
[0248] Example 10
[0249] This embodiment provides a Mg-based hydrogen storage material, wherein the mass fraction of carbon material in the MOF material carbonized derivative is 50 wt%.
[0250] Except for the ratio of the total molar amount of Ni(NO3)2·6H2O and Ce(NO3)3·6H2O to the molar amount of ligand in the ligand solution in step (1) of the preparation method of the Mg-based hydrogen storage material, which is 1.6:1, all other steps are the same as in Example 1.
[0251] Example 11
[0252] This embodiment provides a Mg-based hydrogen storage material, wherein the mass fraction of carbon material in the MOF material carbonized derivative is 95 wt%.
[0253] Except for the ratio of the total molar amount of Ni(NO3)2·6H2O and Ce(NO3)3·6H2O to the molar amount of ligand in the ligand solution in step (1) of the preparation method of the Mg-based hydrogen storage material, which is 0.085:1, all other steps are the same as in Example 1.
[0254] Example 12
[0255] This embodiment provides a Mg-based hydrogen storage material. Except for step (3) of the preparation method of the Mg-based hydrogen storage material, in which a reducing mixture of protective gas and reducing gas with a volume ratio of 95:5 is introduced during the first heating, the rest is the same as in Example 1.
[0256] Example 13
[0257] This embodiment provides a Mg-based hydrogen storage material. Except for step (3) of the preparation method of the Mg-based hydrogen storage material, in which a reducing mixture of protective gas and reducing gas with a volume ratio of 97:3 is introduced during the first heating, the rest is the same as in Example 1.
[0258] Example 14
[0259] This embodiment provides a Mg-based hydrogen storage material. Except for step (3) of the preparation method of the Mg-based hydrogen storage material, in which a reducing mixture including a protective gas and a reducing gas is introduced at a rate of 150 mL / min during the first heating process, the rest is the same as in Example 1.
[0260] Example 15
[0261] This embodiment provides a Mg-based hydrogen storage material. Except for step (3) of the preparation method of the Mg-based hydrogen storage material, in which a reducing mixture including a protective gas and a reducing gas is introduced at a rate of 200 mL / min during the first heating process, the rest is the same as in Example 1.
[0262] Example 16
[0263] This embodiment provides a Mg-based hydrogen storage material. Except for step (5) of the preparation method of the Mg-based hydrogen storage material, in which the rotation speed of the second ball mill is 400 rpm, the rest is the same as in Example 1.
[0264] Example 17
[0265] This embodiment provides a Mg-based hydrogen storage material. Except for step (5) of the preparation method of the Mg-based hydrogen storage material, in which the rotation speed of the second ball mill is 350 rpm, the rest is the same as in Example 1.
[0266] Comparative Example 1
[0267] This comparative example provides a Mg-based hydrogen storage material, except that the carbonized derivative of the MOF material is a carbonized Ni-MOF material;
[0268] In step (1) of the preparation method of the Mg-based hydrogen storage material, the addition of Ce(NO3)3·6H2O is omitted, and the molar amount of Ni(NO3)2·6H2O added is the same as the total molar amount of Ni(NO3)2·6H2O and Ce(NO3)3·6H2O added in the original Example 1.
[0269] Comparative Example 2
[0270] This comparative example provides a Mg-based hydrogen storage material, except that the carbonized derivative of the MOF material is a carbonized Ni-MOF material;
[0271] In step (1) of the preparation method of the Mg-based hydrogen storage material, the addition of Ni(NO3)2·6H2O is omitted, and the molar amount of Ce(NO3)3·6H2O added is the same as the total molar amount of Ni(NO3)2·6H2O and Ce(NO3)3·6H2O added in the original Example 1.
[0272] Comparative Example 3
[0273] This comparative example provides a Mg-based hydrogen storage material, except that the MOF material carbonized derivative is replaced with conductive carbon black;
[0274] In the Mg-based hydrogen storage material, the mass ratio of MgH2 to conductive carbon black is 5:100;
[0275] That is, steps (1) and (2) of the preparation method of Mg-based hydrogen storage material are omitted, and except that the Ni-Ce bimetallic MOF material in step (3) is replaced with conductive carbon black, the rest is the same as in Example 1.
[0276] The hydrogen absorption activation energy of the Mg-based hydrogen storage materials provided in the above embodiments and comparative examples was tested. The test method was as follows: 0.1g of Mg-based hydrogen storage material was placed in a hydrogen storage instrument and degassed for 2h at 350℃ and vacuum degree ≤1Pa. Then, the change curves of time and hydrogen absorption were obtained at different temperatures (50-300℃, 50℃ interval) with an initial hydrogen pressure of 3MPa. The slope was fitted using the commonly used JMAK (Johnson-Mehl-Avrami-Kolmogorov) model and the final calculated data of hydrogen absorption activation energy are shown in Table 1.
[0277] The Mg-based hydrogen storage materials provided in the above embodiments and comparative examples were tested for hydrogen storage content over 1 hour. The test method was as follows: 0.5 g of Mg-based hydrogen storage material was placed in a high-pressure reactor and subjected to vacuum degassing treatment (temperature 300℃, vacuum degree ≤1 Pa, time 1 hour). Then, a hydrogen atmosphere with a purity of 99.999% was introduced. The initial hydrogen pressure was set to 3 MPa and the reaction temperature to 150℃. Subsequently, the weight gain of the Mg-based hydrogen storage material was measured by gravimetric method. The hydrogen storage content of the Mg-based hydrogen storage material at 673 K for 1 hour is shown in Table 1. Among them, the curves of hydrogen content change of the Mg-based hydrogen storage material provided in Example 4 with hydrogen storage time at 423 K, 523 K, 573 K, 623 K and 673 K are shown in Table 1. Figure 1 As shown.
[0278] The Mg-based hydrogen storage materials provided in the above embodiments and comparative examples were subjected to 30 hydrogen absorption and desorption cycles (each hydrogen absorption and desorption cycle was performed as follows: 0.50 g of dry hydrogen storage material powder was placed in a stainless steel reactor and sealed; the first step was pre-activation: the reactor was evacuated to 10... -4 Pa, the temperature is increased to 500℃ at 5℃ / min and held for 1 hour, then naturally cooled to 300℃; the second step is the hydrogen absorption stage: high-purity H2 is introduced into the reactor to a pressure of 3MPa, and the temperature is kept constant at 300℃ for 1 hour, and the average hydrogen absorption within 1 hour is calculated (using the pressure-volume-temperature equation); the third step is the hydrogen release stage: the temperature is increased to 340℃ at 10℃ / min, and a vacuum is drawn (back pressure ≤10-3Pa) and maintained for 30 minutes. When the dehydrogenation rate is ≤0.01wt% / min by online monitoring using a mass spectrometer, complete hydrogen release is determined; the fourth Step 1 is cycle reset: Cool the reactor to 300℃, evacuate for 10 minutes to remove residual hydrogen, and then enter the hydrogen absorption stage to start a new cycle. The hydrogen storage content of the Mg-based hydrogen storage material in each hydrogen absorption and desorption cycle can be obtained by testing. The initial 1-hour hydrogen storage content (A0) of the first cycle and the 1-hour hydrogen storage content of the Mg-based hydrogen storage material after 30 hydrogen absorption and desorption cycles (A1) are selected. The hydrogen storage content retention rate after 30 cycles is calculated as shown in Table 1; Hydrogen storage content retention rate = |A1-A0| / A0×100%.
[0279] Table 1
[0280]
[0281] From Table 1, we can obtain:
[0282] (1) The Mg-based hydrogen storage materials provided in Examples 1 to 7 have low hydrogen absorption activation energy, high 1h hydrogen storage content, and high stability.
[0283] (2) By comparing Example 1 with Examples 8 and 9, it can be seen that in this invention, the mass ratio of MgH2 to the carbide derivative of MOF material affects the performance of Mg-based hydrogen storage material. When the mass ratio of the carbide derivative of MOF material to MgH2 is (5~20):100, the Mg-based hydrogen storage material has better comprehensive performance. This is because when the mass ratio of the carbide derivative of MOF material to MgH2 is in this range, the carbide derivative of MOF material can be fully dispersed between MgH2, which can play a catalytic role, improve the stability of the material system, and inhibit the aggregation of MgH2 caused by multiple hydrogen absorption and desorption processes.
[0284] (3) By comparing Example 1 with Examples 10 and 11, it can be seen that in the present invention, the mass fraction of carbon material in the MOF material carbonization derivative affects the performance of the Mg-based hydrogen storage material; when the mass fraction of carbon material is 65wt% to 85wt%, the Mg-based hydrogen storage material has better comprehensive performance. This is because the carbon material plays the role of Ni / Ce metal atom carrier in the MOF material carbonization derivative. The appropriate mass fraction of carbon material content can make the metal atoms uniformly modified on the carbon material. The carbon material can provide more catalytic active sites and avoid the agglomeration of catalytic particles.
[0285] (4) By comparing Example 1 with Examples 12 and 13, it can be seen that in the preparation method of Mg-based hydrogen storage material in the present invention, the volume fraction of reducing gas in the reducing mixed gas introduced during the first heating in the heat treatment is higher than the volume fraction of reducing gas in the reducing mixed gas introduced during the second heating and heat preservation. This is beneficial to improving the performance of Mg-based hydrogen storage material. This is because during the first heating process in the heat treatment, the Ni-Ce bimetallic MOF material will undergo preliminary pyrolysis. Under high temperature conditions, oxygen will be gradually released from the material. On the one hand, the higher content of reducing gas can fully react with the released oxygen and carry the oxygen out of the Ni-Ce bimetallic MOF material; on the other hand, the higher content of reducing gas environment can maintain the structural stability of carbon material under high temperature conditions and prevent the carbon skeleton from being oxidized.
[0286] (5) By comparing Example 1 with Examples 14 and 15, it can be seen that in the preparation method of Mg-based hydrogen storage material in this invention, the flow rate of the reducing mixed gas introduced during the first heating in the heat treatment is lower than the flow rate of the reducing mixed gas introduced during the second heating and holding. This is beneficial to improving the performance of Mg-based hydrogen storage material. This is because during the first heating in the heat treatment, the material undergoes initial pyrolysis. It is necessary to increase the flow rate of the reducing mixed gas to treat the oxygen element contained in the heat treatment environment, fully remove the oxygen element in the heat treatment environment, and allow some of the oxidized Ce to be removed. 4+ Converted to Ce 3+ This results in lattice distortion, enhancing the system's hydrogen atom transport capacity;
[0287] (6) By comparing Example 1 with Examples 16 and 17, it can be seen that in this invention, the rotation speed of the second ball mill is greater than that of the first ball mill and the third ball mill, which is beneficial to improving the performance of Mg-based hydrogen storage materials. This is because the higher ball milling speed used in the second ball mill can fully break up the large pieces of hydrogen storage materials remaining in the powder after the first ball milling, and achieve the mechanical force to mix the carbon materials and MOF material carbonized derivatives, generate enough Mg-C weak chemical bonds, enhance the interfacial bonding force between the hierarchical porous carbon skeleton and MgH2, thereby fully improving the stability of the mixed system.
[0288] (6) As can be seen from Examples 1-5 and Comparative Examples 1-3, from Example 1 to Example 5, the Ni content gradually increases and the Ce content gradually decreases; Ni atoms provide catalytic active sites in the hydrogen storage material system, which can catalytically decompose H2 molecules into 2 H atoms. The H atoms are small enough to penetrate from the material surface into the material interior. During this process, Ce... 3+ The resulting lattice distortion forms dynamic oxygen vacancy regions on the Ce2O3 / CeO2 surface, which act as "capture-release sites" for hydrogen atoms and play the role of "hydrogen pumps". This promotes the transport of hydrogen atoms into the material interior and accelerates the bonding process between hydrogen and magnesium.
[0289] Therefore, as the Ni content gradually increases, the catalytic decomposition of H2 molecules increases. In Examples 3 and 4, the Ce content is relatively sufficient, which promotes the transport and combination of hydrogen atoms to Mg, resulting in higher hydrogen storage capacity in Examples 3 and 4. However, in Example 5, the Ce content decreases, leading to a weakening of the transport effect, and the final hydrogen storage capacity decreases to some extent. From the perspective of hydrogen storage mechanism, Ni and Ce need to cooperate and promote each other in the hydrogen storage process. Therefore, Ni and Ce alone have limitations in promoting the hydrogen storage process.
[0290] In addition, in Comparative Example 1, the Ni content was the highest. Ni has a stronger catalytic effect on the decomposition of hydrogen atoms in the material system. However, the lack of Ce limited the further penetration of H atoms into the interior, so the total hydrogen storage capacity only increased slightly. Combined with the data on hydrogen absorption activation energy in Table 1, it can be seen that the activation energy decreases with the increase of Ni content, but the degree of decrease is gradually decreasing. This indicates that the addition of Ni can reduce the energy required for the hydrogen storage material to begin absorbing hydrogen to a certain extent, making the material more likely to undergo hydrogen absorption reaction.
[0291] (7) By comparing Example 1 with Comparative Examples 1 to 3, it can be seen that in the present invention, the carbonized derivative of the Ni-Ce bimetallic MOF material formed by carbonization contains a carbon skeleton with hierarchical pores. The hierarchical pore carbon skeleton can not only provide a highly dispersed loading interface for MgH2 and catalytic sites, but also suppress the growth of Mg grains caused by the absorption-desorption hydrogen cycle through the confinement effect.
[0292] In this invention, there is a weak Mg-C chemical bond between MgH2 and the hierarchical porous carbon framework of the MOF material carbonization derivative, which enhances the interfacial bonding force between the hierarchical porous carbon framework and MgH2, improves the stability of Mg-based hydrogen storage materials, and thus reduces the shedding of MgH2 during cycling.
[0293] In this invention, the carbonized derivative of the Ni-Ce bimetallic MOF material contains Ni nanoparticles. The Ni nanoparticles are uniformly dispersed on the hierarchical porous carbon framework derived from the MOF, serving as highly efficient catalytic active sites that can promote the dissociation and adsorption of H2 molecules.
[0294] In this invention, the carbonized derivatives of MOF materials include nano-Ce2O3 particles and / or nano-CeO2 particles formed during the carbonization process of Ni-Ce bimetallic MOF materials. The nano-Ce2O3 particles and / or nano-CeO2 particles form a symbiotic structure with the grain boundaries of MgH2, which can promote the diffusion of hydrogen atoms along the grain boundaries.
[0295] In this invention, the carbonized derivatives of MOF materials include nano-Ce2O3 particles and / or nano-CeO2 particles formed during the carbonization process of Ni-Ce bimetallic MOF materials. 3+ The resulting lattice distortion creates dynamic oxygen vacancy regions on the surface of nano-Ce2O3 particles and / or nano-CeO2 particles, which lowers the adsorption energy of surface H atoms and the dissociation energy barrier of Mg-H bonds. These regions can serve as “capture-release” sites for hydrogen atoms, further accelerating the diffusion and recombination of hydrogen.
[0296] In this invention, the hierarchical porous carbon framework inhibits the aggregation of Ni and Ce2O3 / CeO2 during carbonization through physical isolation effect, thereby improving the long-term stability of the nanocatalytic interface.
[0297] In summary, this invention modifies MgH2 with a carbonized derivative of a MOF material containing carbonized Ni-Ce bimetallic MOF material to obtain a Mg-based hydrogen storage material. Through the synergistic effects of physical isolation and loading of the hierarchical porous carbon framework, interface enhancement of Mg-C bonds, catalytic activation of Ni nanoparticles, and grain boundary effects and oxygen vacancy regulation of Ce-based oxides, the hydrogen storage performance of the material is effectively improved, and structural changes during cycling are suppressed. Therefore, the Mg-based hydrogen storage material exhibits excellent hydrogen storage performance and strong stability.
[0298] The above description is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention fall within the protection and disclosure scope of the present invention.
Claims
1. A Mg-based hydrogen storage material, characterized in that, The Mg-based hydrogen storage material includes MgH2 and a carbonized derivative of MOF material; the carbonized derivative of MOF material includes a carbonized Ni-Ce bimetallic MOF material, and the MOF material carbonized derivative formed by the carbonized Ni-Ce bimetallic MOF material contains a carbon skeleton with hierarchical pores. 2.The Mg-based hydrogen storage material of claim 1, wherein, In the Mg-based hydrogen storage material, the mass ratio of the MOF material carbonized derivative to MgH2 is (5~20):
100. 3.The Mg-based hydrogen storage material of claim 1, wherein, Based on the mass percentage of the MOF material carbonized derivative, the mass fraction of carbon material in the MOF material carbonized derivative is 65wt%~85wt%.
4. The Mg-based hydrogen storage material according to claim 1, characterized in that, The molar ratio of Ni to Ce in the Mg-based hydrogen storage material is (1~3):(1~4).
5. A method for preparing the Mg-based hydrogen storage material according to any one of claims 1 to 4, characterized in that, The preparation method includes: Ni-Ce bimetallic MOF material was heat-treated to obtain a carbide derivative of the MOF material; the obtained carbide derivative of the MOF material was then mixed with MgH2 to obtain a Mg-based hydrogen storage material.
6. The preparation method according to claim 5, characterized in that, The method for preparing the Ni-Ce bimetallic MOF material includes: mixing Ni salt, Ce salt, solvent and ligand solution, and then carrying out a hydrothermal reaction to obtain Ni-Ce bimetallic MOF material.
7. The preparation method according to claim 6, characterized in that, The molar ratio of Ni salt to Ce salt in the mixture is (1~3):(1~4).
8. The preparation method according to claim 6, characterized in that, In the mixture, the ratio of the total molar amount of the Ni salt and Ce salt to the molar amount of the ligand in the ligand solution is 1:(1.5~3.5).
9. The preparation method according to claim 6, characterized in that, In the mixture, the ratio of the total molar amount of Ni salt and Ce salt to the volume of the solvent is 1:(200~1000), with units of mol / L.
10. The preparation method according to claim 6, characterized in that, The mixture also includes the incorporation of an auxiliary solution.
11. The preparation method according to claim 6, characterized in that, The mixing method includes: initially mixing Ni salt, Ce salt, solvent and auxiliary solution to obtain a mixture; then further mixing the obtained mixture with ligand solution to obtain a mixed liquid.
12. The preparation method according to claim 11, characterized in that, The initial mixing includes: mixing the solvent and the auxiliary solution to obtain a first mixture; then adding the Ni salt and Ce salt to the first mixture in sequence to obtain a clear and homogeneous mixture.
13. The preparation method according to claim 11, characterized in that, The remixing includes adding the ligand solution to the resulting mixture.
14. The preparation method according to claim 6, characterized in that, The method for preparing the Ni-Ce bimetallic MOF material further includes pH adjustment between the mixture and the hydrothermal reaction.
15. The preparation method according to claim 14, characterized in that, The pH adjustment process involves setting the pH of the mixture to 5-6.
16. The preparation method according to claim 6, characterized in that, The hydrothermal reaction is carried out at a temperature of 100℃~120℃ for a duration of 24h~48h.
17. The preparation method according to claim 5, characterized in that, The heat treatment includes a first heating, a second heating, and a holding period, all performed sequentially. A reducing mixture consisting of a protective gas and a reducing gas is introduced during each of the first heating, the second heating, and the holding period.
18. The preparation method according to claim 17, characterized in that, The volume fraction of reducing gas in the reducing mixture introduced during the first heating is higher than the volume fraction of reducing gas in the reducing mixture introduced during the second heating and holding.
19. The preparation method according to claim 17, characterized in that, During the first heating process, a reducing mixture of protective gas and reducing gas with a volume ratio of (85~93):(7~15) is introduced.
20. The preparation method according to claim 17, characterized in that, During the second heating process, a reducing mixture of protective gas and reducing gas with a volume ratio of (93~97):(3~7) is introduced.
21. The preparation method according to claim 17, characterized in that, During the heat preservation process, a reducing mixture of protective gas and reducing gas with a volume ratio of (93~97):(3~7) is introduced.
22. The preparation method according to claim 17, characterized in that, The flow rate of the reducing gas mixture introduced during the first heating is lower than the flow rate of the reducing gas mixture introduced during the second heating and holding periods.
23. The preparation method according to claim 17, characterized in that, During the first heating process, the rate at which the reducing gas mixture is introduced is 100 mL / min to 140 mL / min.
24. The preparation method according to claim 17, characterized in that, During the second heating process, the rate at which the reducing mixed gas is introduced is 140 mL / min to 200 mL / min.
25. The preparation method according to claim 17, characterized in that, During the heat preservation process, the rate at which the reducing mixed gas is introduced is 140 mL / min to 200 mL / min.
26. The preparation method according to claim 17, characterized in that, The heating rate in the first heating process is higher than the heating rate in the second heating process.
27. The preparation method according to claim 17, characterized in that, The heating rate of the first heating is 4℃ / min to 8℃ / min, and the final temperature is 400℃ to 600℃.
28. The preparation method according to claim 17, characterized in that, The second heating rate is 2℃ / min to 4℃ / min, and the final temperature is 700℃ to 900℃.
29. The preparation method according to claim 17, characterized in that, The temperature at which the heat is maintained is the final temperature of the second heating, and the heat maintenance time is 0.5h to 1.5h.
30. The preparation method according to claim 17, characterized in that, Pre-drying is also included before the first heating.
31. The preparation method according to claim 30, characterized in that, The pre-drying process includes: heating to 180℃~220℃ at a heating rate of 3℃ / min~6℃ / min and then maintaining the temperature at that temperature for 0.5h~2h.
32. The preparation method according to claim 30, characterized in that, During the pre-drying process, a protective gas is introduced at a rate of 180 mL / min to 250 mL / min.
33. The preparation method according to claim 17, characterized in that, The process of heat preservation is followed by cooling. During the cooling process, a reducing gas mixture including a protective gas and a reducing gas is introduced. The volume fraction of the reducing gas in the reducing gas mixture introduced during cooling is higher than the volume fraction of the reducing gas in the reducing gas mixture introduced during the first heating.
34. The preparation method according to claim 33, characterized in that, During the cooling process, a reducing mixture of protective gas and reducing gas with a volume ratio of (80~92):(8~20) is introduced.
35. The preparation method according to claim 33, characterized in that, The rate at which the reducing gas mixture is introduced during the cooling process is 50 mL / min to 100 mL / min.
36. The preparation method according to claim 5, characterized in that, The preparation method further includes a first pre-ball milling of the MOF material carbonized derivative between the heat treatment and the mixing.
37. The preparation method according to claim 36, characterized in that, The first pre-ball milling was carried out in a protective atmosphere, with a ball-to-material ratio of (8~12):1, a rotation speed of 200rpm~600rpm, and a time of 0.5h~3h.
38. The preparation method according to claim 5, characterized in that, The preparation method further includes pretreatment of MgH2 before mixing, the pretreatment including drying MgH2 and then performing a second pre-ball milling.
39. The preparation method according to claim 38, characterized in that, The second pre-ball milling is carried out in a protective atmosphere, with a ball-to-material ratio of (10~15):1, a rotation speed of 300rpm~500rpm, and a time of 0.5h~1.5h.
40. The preparation method according to claim 5, characterized in that, The mixing process includes sequentially performing a first ball mill, a second ball mill, and a third ball mill.
41. The preparation method according to claim 40, characterized in that, The rotational speed of the second ball mill is greater than that of the first and third ball mills.
42. The preparation method according to claim 40, characterized in that, The first ball mill operates at a speed of 200 rpm to 400 rpm for 2 hours to 4 hours.
43. The preparation method according to claim 40, characterized in that, The second ball mill operates at a speed of 500 rpm to 600 rpm for 4 hours to 6 hours, and during the second ball milling process, a cooling period of 10 minutes to 30 minutes is applied every 1 hour to 1.5 hours of milling.
44. The preparation method according to claim 40, characterized in that, The third ball mill operates at a speed of 350 rpm to 450 rpm for 1 to 2 hours.
45. The preparation method according to claim 40, characterized in that, The first, second, and third ball milling processes were each carried out independently in a protective atmosphere with a pressure of 1 bar to 2 bar.
46. The preparation method according to claim 45, characterized in that, The protective atmosphere includes any one or a combination of at least two of nitrogen, argon, helium, or neon.
47. The preparation method according to claim 5, characterized in that, The preparation method includes: (1) The solvent and an auxiliary solution with a solute concentration of 0.2 mol / L to 4 mol / L were mixed for 10 min to 20 min by stirring at a speed of 300 rpm to 1100 rpm to obtain a first mixture; Ni salt and Ce salt were added to the first mixture in sequence at a temperature not higher than 60℃, while stirring at a speed of 500 rpm to 1400 rpm for 10 min to 30 min to obtain a clear and homogeneous mixture; a ligand solution with a ligand concentration of 1 mol / L to 3 mol / L was added to the mixture while stirring at a speed of 150 rpm to 800 rpm for 0.5 h to 1.5 h to obtain a mixed liquid. The ratio of the total molar amount of Ni salt and Ce salt to the volume of the solvent is 1:(200~1000), in mol / L; the molar ratio of Ni salt to Ce salt is (1~3):(1~4); the ratio of the total molar amount of Ni salt and Ce salt to the molar amount of ligand in the ligand solution is 1:(1.5~3.5). (2) Adjust the pH of the mixture obtained in step (1) to 5-6 with at least one of sodium hydroxide solution, ammonia solution, or potassium hydroxide solution, then perform hydrothermal treatment at 100℃-120℃ for 24-48 hours, cool to 10℃-30℃, then centrifuge at 800rpm-1500rpm for 3-10 minutes, wash with a washing solution at 60℃-80℃, then wash with anhydrous ethanol solution containing hydrochloric acid at 10℃-30℃, and then wash with a solution containing hydrochloric acid at 10℃-30℃. The mixture of methanol and diethyl ether in a volume ratio of (1~3):1 was washed and then centrifuged at 2000 rpm~2600 rpm for 5 min~20 min. The solid obtained after centrifugation was then vacuum dried in a vacuum environment at a temperature of 60℃~80℃ and a vacuum degree ≤0.1MPa for 12~24 h, and then dried in a mixed atmosphere at a temperature of 60℃~80℃ and a nitrogen to hydrogen volume ratio of (80~95):(5~20) for 6 h~10 h to obtain Ni-Ce bimetallic MOF material. (3) After pre-drying the Ni-Ce bimetallic MOF material obtained in step (2), the first heating, the second heating, the heat preservation and the cooling are carried out in sequence to obtain the MOF material carbonized derivative. The pre-drying process includes: heating to 180℃~220℃ at a heating rate of 3℃ / min~6℃ / min and then holding the temperature at a constant temperature for 0.5h~2h, during which a protective gas is introduced at a rate of 180mL / min~250mL / min. The first heating includes: heating to 400℃~600℃ at a heating rate of 4℃ / min~8℃ / min, and during the first heating process, introducing a reducing gas mixture comprising a protective gas and a reducing gas in a volume ratio of (85~93):(7~15) at a rate of 100mL / min~140mL / min. The second heating includes heating to 700℃~900℃ at a heating rate of 2℃ / min~4℃ / min, during the first heating process, a reducing gas mixture comprising a protective gas and a reducing gas in a volume ratio of (93~97):(3~7) is introduced at a rate of 140mL / min~200mL / min. The heat preservation includes: heat preservation at 700℃~900℃ for 0.5h~1.5h, during which a reducing gas mixture comprising a protective gas and a reducing gas in a volume ratio of (93~97):(3~7) is introduced at a rate of 140mL / min~200mL / min. The cooling process includes: cooling the furnace to 10°C to 30°C, during which a reducing mixture of protective gas and reducing gas with a volume ratio of (80 to 92): (8 to 20) is introduced at a rate of 50 mL / min to 100 mL / min. The volume fraction of reducing gas in the reducing mixture introduced during the first heating is higher than the volume fraction of reducing gas in the reducing mixture introduced during the second heating and holding. The flow rate of the reducing gas mixture introduced during the first heating is lower than the flow rate of the reducing gas mixture introduced during the second heating and holding periods. The heating rate in the first heating process is higher than the heating rate in the second heating process; The volume fraction of reducing gas in the reducing mixture introduced during cooling is higher than the volume fraction of reducing gas in the reducing mixture introduced during the first heating. (4) In a protective atmosphere, the MOF material carbonized derivative obtained in step (3) is subjected to a first pre-ball milling. The ball-to-material ratio of the first pre-ball milling is (8~12):1, the rotation speed is 200rpm~600rpm, and the time is 0.5h~3h, to obtain the MOF material carbonized derivative after ball milling. After vacuum drying of MgH2 at 50℃~70℃ for 18h~36h, a second pre-ball milling is carried out in a protective atmosphere. The ball-to-material ratio of the second pre-ball milling is (10~15):1, the rotation speed is 300rpm~500rpm, and the time is 0.5h~1.5h to obtain ball-milled MgH2. (5) In a protective atmosphere with a pressure of 1 bar to 2 bar, the carbonized derivative of the MOF material obtained in step (4) and the MgH2 obtained after ball milling are first mixed by a first ball milling at a speed of 200 rpm to 400 rpm for 2 h to 4 h to obtain a first mixture; then the first mixture is ball milled at a speed of 500 rpm to 600 rpm for 4 h to 6 h. During the second ball milling, the mixture is cooled for 10 min to 30 min every 1 h to 1.5 h of ball milling. After the second ball milling, a second mixture is obtained; then the second mixture is ball milled at a speed of 350 rpm to 450 rpm for 1 h to 2 h to obtain a Mg-based hydrogen storage material.
48. The application of the Mg-based hydrogen storage material according to any one of claims 1 to 4, characterized in that, The Mg-based hydrogen storage material is used in metal hydride solid-state hydrogen storage technology.
Citation Information
Patent Citations
Monoatomic catalyzed magnesium hydride solid hydrogen storage material, application and preparation method
CN115784147A
Preparation method of graphene reinforced titanium-based hydrogen storage alloy powder and hydrogen storage device
CN118417573A