Phase-stable anti-CMAS corrosion material and preparation method thereof
By using solid solution ceramic materials doped with Hf and Ta, the problem of phase transformation instability of thermal barrier coatings in CMAS corrosion has been solved, and the phase stability and corrosion resistance of the materials at high temperatures have been improved, making them suitable for components such as turbine blades of aero-engines.
Patent Information
- Application Number
- CN202610119329.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-01-28
- Publication Date
- 2026-05-01
AI Technical Summary
Existing thermal barrier coating materials are susceptible to CMAS corrosion in aero engines, which leads to the destruction of coating integrity, affects working efficiency and shortens service life. Furthermore, ZrO2-based materials are unstable in phase transformation at high temperatures and have insufficient resistance to CMAS corrosion.
The solid solution ceramic (Zr1-x-yHfx)TayO2+0.5y is used. By doping with Hf and Ta, the high-temperature phase transformation of ZrO2 is suppressed, thereby improving the high-temperature stability and resistance to CMAS corrosion of the material. The preparation method includes wet ball milling, pressing and sintering processes.
The material maintains tetragonal phase stability at high temperatures, has an extremely high melting point and excellent resistance to molten salt corrosion, and can withstand complex environments above 1250 ℃ for a long time, thus extending the service life of aero-engine components.
Smart Images

Figure CN121948963A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a thermal barrier coating material, specifically, to a phase-stable CMAS corrosion-resistant material and its preparation method. Background Technology
[0002] Thermal barrier coatings are indeed key materials in aerospace, gas turbine, and other fields. However, in the actual operating environment of aero engines, they inevitably come into contact with dust, gravel, ash, and other contaminants in the air. These deposits accumulate on the high-pressure areas and roots of turbine blades, forming molten calcium magnesium aluminum silicate (CMAS) at high temperatures. This damages the integrity of the coating, severely limiting the operating efficiency of aero engines and significantly shortening their service life. 7-8 wt.% Y₂O₃ stabilized zirconia (YSZ) is currently the most widely used thermal barrier coating material in industrial and aerospace applications. However, its uncontrollable phase transformation and insufficient resistance to CMAS corrosion limit its long-term effective protection in high-temperature environments. Therefore, the industry urgently needs to develop novel oxide ceramic systems with excellent resistance to CMAS corrosion. The mechanisms affecting the improvement of CMAS corrosion resistance have long remained unresolved, seriously hindering the rational design of new thermal barrier coating materials.
[0003] In order to solve the above problems, people have been seeking an ideal technological solution. Summary of the Invention
[0004] The purpose of this invention is to address the shortcomings of existing technologies by providing a phase-stable CMAS corrosion-resistant material and its preparation method.
[0005] To achieve the above objectives, the technical solution adopted by the present invention is as follows: A phase-stable CMAS corrosion-resistant material, wherein the CMAS corrosion-resistant material is a solid solution ceramic, and the molecular formula of the solid solution ceramic is (Zr... 1-x-y Hf x )Ta y O 2+0.5y , where 0.4 > x > 0.1, 0.4 > y > 0.1.
[0006] A method for preparing the phase-stabilized CMAS corrosion-resistant material includes the following steps: Weigh out ZrO2, HfO2 and Ta2O5 according to their molecular formulas, and mix the weighed raw materials evenly. The uniformly mixed powder is pressed into a green compact using a tablet press. The green blank is placed in a sintering furnace and sintered to form a ceramic.
[0007] The sintering process is as follows: the ceramic is fired in an air atmosphere at a heating rate of 3-10 ℃ / min, a firing temperature of 1500-1800 ℃, and a holding time of 6-12 h. After sintering, the ceramic is cooled to room temperature in the furnace to obtain a solid solution ceramic.
[0008] The pressing process is as follows: pressure is 10-20 MPa, and holding time is 10-60 min.
[0009] The weighed raw materials were mixed evenly using wet ball milling; the ball milling medium was anhydrous ethanol, the ball-to-material ratio was 3:1, the ball milling speed was 300 r / min, and the ball milling time was 18-24 h.
[0010] After wet ball milling, the powder is dried at 70-80 ℃ for 6-24 h to obtain a uniformly mixed powder, which is then pressed.
[0011] This invention has significant substantive features and remarkable progress compared to existing technologies. Specifically, this invention provides a phase-stable CMAS corrosion-resistant material by doping with Hf and Ta to suppress the high-temperature phase transition of ZrO2 and enhance the (Zr) phase stability. 1-x- y Hf x )Ta y O 2+0.5y The high-temperature stability of the material is improved, while the melting point and resistance to CMAS corrosion are also enhanced. After corrosion, the main crystalline phase of the resulting solid solution ceramic remains tetragonal zirconium dioxide, with no monoclinic phase generated. The material also exhibits an extremely high melting point (approximately 3006℃) and excellent resistance to molten salt corrosion, enabling it to withstand complex molten salt environments above 1250℃ for extended periods. This makes it a promising candidate for applications in cutting-edge fields such as aero-engine turbine blades. Attached Figure Description
[0012] Figure 1 The solid solution (Zr) obtained in Example 1 0.35 Hf 0.35 )Ta 0.3 O 2.15 XRD patterns of ZrO2 ceramic samples and comparison samples.
[0013] Figure 2 SEM images of the ZrO2 cross-section of the sample were used for comparison.
[0014] Figure 3 The solid solution (Zr) obtained in Example 1 0.35 Hf 0.35 )Ta 0.3 O 2.15 SEM image of the cross section.
[0015] Figure 4To compare the SEM images of the cross-section of the ZrO2 sample after molten salt corrosion.
[0016] Figure 5 The solid solution (Zr) obtained in Example 1 0.35 Hf 0.35 )Ta 0.3 O 2.15 SEM image of the cross-section after molten salt corrosion. Detailed Implementation
[0017] The technical solution of the present invention will be further described in detail below through specific embodiments. Example 1
[0018] This embodiment provides a phase-stable CMAS corrosion-resistant material, which is a solid solution ceramic with the molecular formula (Zr) 0.35 Hf 0.35 )Ta 0.3 O 2.15 .
[0019] This embodiment also provides a method for preparing the solid solution ceramic, which includes the following steps: (1) Weigh out ZrO2, HfO2 and Ta2O5 according to the ratio of Zr, Hf and Ta in the molecular formula; (2) The weighed raw materials are mixed by wet ball milling; the wet ball milling process is as follows: the ball milling medium is anhydrous ethanol, the ball-to-material ratio is 3:1, the ball milling speed is 300 r / min, and the ball milling time is 24 hours. (3) The slurry obtained by wet ball milling is dried to obtain a uniformly mixed powder; the drying process is as follows: drying at 80 ℃ for 12 hours to obtain a uniformly mixed powder; (4) The uniformly mixed powder is pressed into a green compact using a tablet press; the pressing process is as follows: pressure is 10 MPa, holding time is 60 min; (5) The green body is placed in a sintering furnace and sintered to obtain a solid solution ceramic. The sintering process is as follows: the green body is fired in an air atmosphere, the heating rate is 3 ℃ / min, the firing temperature is 1600 ℃, the holding time is 8 hours, and after sintering, it is cooled to room temperature with the furnace to obtain a solid solution ceramic. Example 2
[0020] This embodiment provides a phase-stable CMAS corrosion-resistant material, which is a solid solution ceramic with the molecular formula (Zr) 0.4 Hf 0.3 )Ta 0.3 O 2.15 .
[0021] This embodiment also provides a method for preparing the solid solution ceramic, which includes the following steps: (1) Weigh out ZrO2, HfO2 and Ta2O5 according to the ratio of Zr, Hf and Ta in the molecular formula; (2) The weighed raw materials are mixed by wet ball milling; the wet ball milling process is as follows: the ball milling medium is anhydrous ethanol, the ball-to-material ratio is 3:1, the ball milling speed is 300 r / min, and the ball milling time is 18 hours. (3) The slurry obtained by wet ball milling is dried to obtain a uniformly mixed powder; the drying process is as follows: drying at 80 ℃ for 16 hours to obtain a uniformly mixed powder; (4) The uniformly mixed powder is pressed into a green body using a tablet press; the pressing process is as follows: pressure is 20 MPa, holding time is 100 min; (5) The green body is placed in a sintering furnace and sintered to obtain a solid solution ceramic. The sintering process is as follows: the green body is fired in an air atmosphere, the heating rate is 5℃ / min, the firing temperature is 1700℃, the holding time is 6 hours, and the green body is cooled to room temperature with the furnace after sintering to obtain a solid solution ceramic. Example 3
[0022] This embodiment provides a phase-stable CMAS corrosion-resistant material, which is a solid solution ceramic with the molecular formula (Zr) 0.5 Hf 0.2 )Ta 0.3 O 2.15 .
[0023] This embodiment also provides a method for preparing the solid solution ceramic, which includes the following steps: (1) Weigh out ZrO2, HfO2 and Ta2O5 according to the ratio of Zr, Hf and Ta in the molecular formula; (2) The weighed raw materials are mixed by wet ball milling; the wet ball milling process is as follows: the ball milling medium is anhydrous ethanol, the ball-to-material ratio is 3:1, the ball milling speed is 300 r / min, and the ball milling time is 20 hours. (3) The slurry obtained by wet ball milling is dried to obtain a uniformly mixed powder; the drying process is as follows: drying at 70 ℃ for 20 hours to obtain a uniformly mixed powder; (4) The uniformly mixed powder is pressed into a green compact using a tablet press; the pressing process is as follows: pressure is 15 MPa, holding time is 30 min; (5) The green body is placed in a sintering furnace and sintered to obtain a solid solution ceramic. The sintering process is as follows: the green body is fired in an air atmosphere, the heating rate is 8 ℃ / min, the firing temperature is 1600 ℃, the holding time is 12 hours, and after sintering, it is cooled to room temperature with the furnace to obtain a solid solution ceramic.
[0024] Comparative Example 1 Comparative Example 1 is basically the same as Example 1, except that the raw material of Comparative Example 1 is zirconium oxide, and the ceramic obtained is zirconium oxide ceramic.
[0025] Comparative Test The ceramics prepared in Comparative Example 1 and Example 1 were tested. They were prepared according to the molecular formula 33CaO-9MgO-13AlO. 1.5 -45SiO2 was used to prepare a corrosion molten salt to simulate real high-temperature corrosion. CaO, MgO, Al2O3, and SiO2 were weighed and mixed using a wet ball mill. Anhydrous ethanol was used as the milling medium, the ball-to-material ratio was 3:1, the milling speed was 300 r / min, and the milling time was 24 hours. The slurry obtained from the wet ball milling was uniformly coated onto the ceramic surface to achieve a loading of 30 mg / cm³. 2 The coated and dried block was dried at 80 ℃ for 2 hours. It was then heated in air at a heating rate of 5 ℃ / min, a firing temperature of 1250 ℃, and a holding time of 5 hours. After sintering, it was cooled to room temperature in the furnace to obtain the etched block.
[0026] X-ray diffraction was used to analyze the phase composition of the ceramic matrix and the corroded cross-section to confirm the formation of the solid solution and the phase composition of the corroded cross-section. Scanning electron microscopy was used to characterize the morphology of the solid solution ceramic surface and the corroded cross-section. The test results are shown below. Figure 1-5 ,Depend on Figure 1-5 It can be seen that the corrosion layer thickness of ZrO2 ceramics after molten salt corrosion is much greater than that of the solid solution (ZrO2). 0.35 Hf 0.35 )Ta 0.3 O 2.15 Ceramics, solid solution (Zr 0.35 Hf 0.35 )Ta 0.3 O 2.15 Ceramics exhibit excellent phase stability during molten salt corrosion, resulting in a significant reduction in the corrosion layer.
[0027] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and not to limit them; although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications can still be made to the specific implementation of the present invention or equivalent substitutions can be made to some technical features without departing from the spirit of the technical solutions of the present invention, and all such modifications and substitutions should be covered within the scope of the technical solutions claimed in the present invention.
Claims
1. A phase-stable CMAS corrosion-resistant material, characterized in that: The CMAS corrosion-resistant material is a solid solution ceramic, and the molecular formula of the solid solution ceramic is (Zr... 1-x-y Hf x )Ta y O 2+0.5y , where 0.4 > x > 0.1, 0.4 > y > 0.
1.
2. A method for preparing the phase-stabilized CMAS corrosion-resistant material according to claim 1, comprising the following steps: Weigh out ZrO2, HfO2 and Ta2O5 according to their molecular formulas, and mix the weighed raw materials evenly. The uniformly mixed powder is pressed into a green compact using a tablet press. The green blank is placed in a sintering furnace and sintered to form a ceramic.
3. The preparation method according to claim 2, characterized in that: The sintering process is as follows: the ceramic is fired in an air atmosphere at a heating rate of 3-10 ℃ / min, a firing temperature of 1500-1800 ℃, and a holding time of 6-12 h. After sintering, the ceramic is cooled to room temperature in the furnace to obtain a solid solution ceramic.
4. The preparation method according to claim 2, characterized in that: The pressing process is as follows: pressure is 10-20 MPa, and holding time is 10-60 min.
5. The preparation method according to claim 2, characterized in that: The weighed raw materials were mixed evenly using wet ball milling; the ball milling medium was anhydrous ethanol, the ball-to-material ratio was 3:1, the ball milling speed was 300 r / min, and the ball milling time was 18-24 h.
6. The preparation method according to claim 5, characterized in that: After wet ball milling, the powder is dried at 70-80 ℃ for 6-24 h to obtain a uniformly mixed powder, which is then pressed.