A high-strength antibacterial nylon filament and its preparation method
By using carboxymethyl cellulose nanoparticles loaded with silver nanoparticles and modifying them to be hydrophobic, the problems of bacterial growth and mechanical property degradation in nylon filaments under humid environments were solved, achieving high strength and long-lasting antibacterial effect.
Patent Information
- Application Number
- CN202610681196.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-05-18
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2046-05-18
AI Technical Summary
Existing nylon filaments are prone to bacterial growth in humid environments, and the direct addition of nano-silver particles leads to a decline in the mechanical properties of the fibers, making them difficult to apply in high-end textiles.
Carboxymethyl cellulose nanoparticles were loaded with silver nanoparticles and hydrophobically modified to form a hydrophobically modified functional masterbatch, which was then blended and spun with nylon 6 chips. The high specific surface area of carboxymethyl cellulose nanoparticles and the strong coordination between the carboxyl groups and silver nanoparticles improved dispersibility and interfacial compatibility.
It achieves high strength and long-lasting antibacterial effect, reduces the migration and aggregation of silver particles, and improves the mechanical properties and antibacterial durability of the fiber.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention belongs to the field of chemical fiber technology, and particularly relates to a high-strength antibacterial nylon filament and its preparation method. Background Technology
[0002] Nylon filaments are widely used in sportswear, outdoor equipment, and home textiles due to their excellent strength, abrasion resistance, and elasticity. However, ordinary nylon fibers themselves do not possess antibacterial properties and easily become breeding grounds for bacteria in humid and warm environments, leading to odors, allergies, and even health risks. In existing technologies, imparting antibacterial properties to fibers by adding inorganic antibacterial agents (such as nano-silver) is a common method. However, directly mixing nano-silver particles into the polymer matrix often results in uneven dispersion, easy aggregation, and weak bonding with the matrix. This not only affects the durability of the antibacterial effect but also severely damages the mechanical properties of the fiber, leading to a decrease in strength and limiting its application in high-end, durable textiles.
[0003] Therefore, developing a nylon filament that can simultaneously achieve high strength and high antibacterial properties is a technical challenge that urgently needs to be overcome in this field. Summary of the Invention
[0004] The purpose of this invention is to address the shortcomings of existing technologies by providing a high-strength antibacterial nylon filament and its preparation method. This nylon filament not only possesses excellent mechanical strength but also exhibits long-lasting antibacterial properties.
[0005] To achieve the above objectives, the present invention adopts the following technical solution: a high-strength antibacterial nylon filament, comprising, by weight parts, 90-95 parts of nylon 6 chips and 5-10 parts of hydrophobic modified functional masterbatch, wherein the preparation process of the hydrophobic modified functional masterbatch is as follows: S1. Carboxymethyl cellulose nanoparticles are dispersed in deionized water and subjected to ultrasonic treatment to obtain a uniform and stable dispersion. Silver nitrate aqueous solution is added dropwise to the dispersion under light-protected and continuously stirred conditions to carry out the reaction. After the reaction is completed, ascorbic acid solution is added to continue the reduction reaction. The mixture is then dialyzed and dried to obtain carboxymethyl cellulose nanoparticles loaded with silver nanoparticles. S2. Add hexadecyltrimethylammonium bromide ethanol solution to carboxymethyl cellulose nanoparticles loaded with silver nanoparticles, stir at a constant temperature to carry out hydrophobic modification reaction, and after the reaction is completed, centrifuge, wash and dry to obtain hydrophobic modified functional masterbatch.
[0006] The inventors discovered that by first loading and hydrophobically modifying silver nanoparticles to form a functional masterbatch, and then blending the functional masterbatch with nylon 6 chips during spinning, the functional masterbatch can be uniformly dispersed in the fiber matrix. Firstly, carboxymethyl cellulose nanoparticles themselves possess high specific surface area and high modulus, and can serve as a reinforcing phase in the polymer matrix. When present in a well-dispersed state within the nylon matrix, they can enhance the fiber's strength and modulus. Furthermore, the carboxyl groups on the surface of carboxymethyl cellulose nanoparticles have a strong coordination or electrostatic interaction with the silver nanoparticles, firmly anchoring the silver nanoparticles to the carrier. During spinning, melting, and subsequent use, this binding can slow down the rapid release and loss of silver ions, thus providing a more durable antibacterial effect. Secondly, the carboxymethyl cellulose nanoparticles loaded with silver nanoparticles were modified using the cationic surfactant hexadecyltrimethylammonium bromide. The long alkyl chain of hexadecyltrimethylammonium bromide was linked to the surface of carboxymethyl cellulose nanoparticles through ionic interactions, making it change from hydrophilic to hydrophobic. This greatly improved the interfacial compatibility between the functional masterbatch and the nylon 6 melt, enabling more uniform melt blending in the screw extruder, reducing phase separation, and ensuring that the functional fiber has good spinnability and mechanical properties.
[0007] Furthermore, the degree of carboxyl substitution of the carboxymethyl cellulose nanoparticles in S1 is 0.5~1.5, and the dispersion concentration of the carboxymethyl cellulose nanoparticles in deionized water is 0.5~2wt%.
[0008] It should be noted that the higher the degree of carboxyl substitution, the more carboxyl groups are carried on the carboxymethyl cellulose nanoparticle chain. A higher degree of carboxyl substitution can provide more reaction sites for silver nanoparticles. However, an excessively high degree of carboxyl substitution will lead to excessive charge repulsion, which will affect the reduction process of silver ions. On the other hand, an excessively low degree of carboxyl substitution will lead to insufficient reaction sites, resulting in low and uneven loading.
[0009] In addition, if the concentration of carboxymethyl cellulose nanoparticles in deionized water is too low, there will be insufficient effective loading sites per unit volume; if the concentration of carboxymethyl cellulose nanoparticles is too high, the viscosity of the system will be too high, which will hinder the uniform diffusion of silver ions in the system, resulting in uneven reaction and causing local overgrowth and aggregation of silver nanoparticles.
[0010] Furthermore, in S1, the molar ratio of silver ions in the silver nitrate aqueous solution to carboxyl groups in carboxymethyl cellulose nanoparticles is 1:(2~5); the molar ratio of ascorbic acid to silver ions in the silver nitrate aqueous solution is (1~2):1.
[0011] It should be noted that when the molar ratio of silver ions to carboxyl groups is too low, the number of silver ions is much smaller than the number of carboxyl sites, resulting in low silver loading and failing to achieve the expected antibacterial effect. On the other hand, when the molar ratio of silver ions to carboxyl groups is too high, there is a large excess of silver ions. The excess silver ions independently generate silver nanoparticles in the solution instead of growing in situ on the surface of carboxymethyl cellulose nanoparticles. The free silver nanoparticles are prone to agglomeration and are easily detached during washing, modification, or melt processing.
[0012] In addition, using a slightly excessive amount of ascorbic acid reducing agent can ensure that all silver ions are completely reduced, avoiding the residual silver ions from affecting the stability of the product. However, when the amount of ascorbic acid is too high, the reduction rate will be too fast, and a large number of silver ions will be generated instantly. They will not have enough time to nucleate and grow in an orderly manner at the carboxyl sites of carboxymethyl cellulose nanoparticles, which will easily lead to particle aggregation.
[0013] Furthermore, the reaction temperature in S1 is 25~60℃ and the time is 1~2h; the reduction reaction temperature in S1 is 25~60℃ and the time is 1~4h.
[0014] Furthermore, the molar ratio of the cetyltrimethylammonium bromide cation to the carboxyl group in carboxymethyl nanocellulose in S2 is (0.8~1.2):1. When the cation ratio is too low, hydrophobicity is insufficient, and it is easy to agglomerate in nylon 6. When the cation ratio is too high, the excess cetyltrimethylammonium bromide will become stress defect points, affecting the mechanical strength of the final fiber.
[0015] Furthermore, the hydrophobic modification reaction in S2 is carried out at a temperature of 60-70°C for 4-6 hours.
[0016] A method for preparing the high-strength antibacterial nylon filament includes the following steps: (1) Vacuum dry the nylon 6 chips and hydrophobic modified functional masterbatch to remove moisture; (2) The dried nylon 6 chips and hydrophobic modified functional masterbatch are fed into a screw extruder and melt-blended to obtain a spinning melt; (3) The spinning melt is spun, drawn and heat-set to obtain high-strength antibacterial nylon filament.
[0017] Furthermore, in step (1), the vacuum drying temperature is 80~100℃ and the time is 4~12h.
[0018] Furthermore, the melt blending temperature in step (2) is 230~260℃.
[0019] Furthermore, in step (3), the spinning temperature is 250~270℃, the spinning speed is 4000~4800 m / min; the draw ratio of the post-drawing treatment is 3.0~5.0 times; and the heat setting temperature is 160~190℃.
[0020] Compared to existing technologies, this invention has at least the following beneficial effects: This invention utilizes carboxymethyl cellulose nanoparticles as a carrier and reinforcing framework. Silver nanoparticles are loaded and stabilized through in-situ reduction of its abundant carboxyl groups. Then, a cationic surfactant with long-chain alkyl groups, hexadecyltrimethylammonium bromide, is used to perform ion exchange and hydrophobic coating on the carboxymethyl cellulose nanoparticles, forming a structurally stable hydrophobically modified functional masterbatch. Carboxymethyl cellulose nanoparticles themselves are nanofibers with high modulus and strength. Their uniform dispersion in nylon 6 chips can play a nano-reinforcing role, improving the material's tensile strength and modulus. Furthermore, the compatibility between the hydrophobically modified functional masterbatch and the hydrophobic nylon 6 chips is significantly improved, resulting in a stronger interfacial bond and reduced interfacial defects, thus avoiding the decline in mechanical properties caused by filler agglomeration or interfacial debonding. Simultaneously, the hydrophobically modified functional masterbatch effectively anchors the silver nanoparticles, greatly inhibiting the migration and agglomeration of silver particles during processing and use. Moreover, this structure can regulate the release rate of silver ions, achieving a long-lasting and durable antibacterial effect. Detailed Implementation
[0021] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0022] It should be understood that the specific embodiments described herein are merely illustrative of the invention and are not intended to limit the invention.
[0023] Example 1 A method for preparing high-strength antibacterial nylon filament includes the following steps: S1. Carboxymethyl cellulose nanoparticles with a carboxyl substitution degree of 0.8 were dispersed in deionized water and subjected to ultrasonic treatment to obtain a uniform and stable dispersion with a dispersion concentration of 1 wt%. Under light-protected and continuously stirred conditions, a 0.01 mol / L silver nitrate aqueous solution was added dropwise to the dispersion and reacted at 50 °C for 1 h. After the reaction was completed, a 0.1 mol / L ascorbic acid solution was added and the reduction reaction was continued at 50 °C for 2 h. After dialyzing and drying, carboxymethyl cellulose nanoparticles loaded with silver nanoparticles were obtained. The molar ratio of silver ions in the silver nitrate aqueous solution to carboxyl groups in the carboxymethyl cellulose nanoparticles was 1:3; the molar ratio of ascorbic acid to silver ions in the silver nitrate aqueous solution was 1.5:1. S2. A 0.1 mol / L hexadecyltrimethylammonium bromide ethanol solution was added to carboxymethyl cellulose nanoparticles loaded with silver nanoparticles, and the mixture was stirred at 65°C for 5 hours to carry out hydrophobic modification. After the reaction was completed, the mixture was centrifuged, washed, and dried to obtain the hydrophobically modified functional masterbatch. The molar ratio of the cation of hexadecyltrimethylammonium bromide to the carboxyl group in carboxymethyl cellulose nanoparticles was 1:1. S3. 95 parts of nylon 6 chips and 5 parts of hydrophobic modified functional masterbatch were vacuum dried at 90℃ for 10h to remove moisture; S4. The dried nylon 6 chips and hydrophobically modified functional masterbatch are fed into a screw extruder and melt-blended at 245℃ to obtain a spinning melt. S5. The spinning melt undergoes spinning, post-drawing treatment, and heat setting. The spinning temperature is 260℃, the spinning speed is 4500m / min, the draw ratio is 4.0, and the heat setting temperature is 180℃ to obtain high-strength antibacterial nylon filament.
[0024] Example 2 A method for preparing high-strength antibacterial nylon filament includes the following steps: S1. Carboxymethyl cellulose nanoparticles with a carboxyl substitution degree of 0.5 were dispersed in deionized water and subjected to ultrasonic treatment to obtain a uniform and stable dispersion with a dispersion concentration of 0.5 wt%. Under light-protected and continuously stirred conditions, a 0.01 mol / L silver nitrate aqueous solution was added dropwise to the dispersion and the reaction was carried out at 25 °C for 2 h. After the reaction was completed, a 0.1 mol / L ascorbic acid solution was added and the reduction reaction was continued at 25 °C for 4 h. After dialyzing and drying, carboxymethyl cellulose nanoparticles loaded with silver nanoparticles were obtained. The molar ratio of silver ions in the silver nitrate aqueous solution to carboxyl groups in the carboxymethyl cellulose nanoparticles was 1:2; the molar ratio of ascorbic acid to silver ions in the silver nitrate aqueous solution was 1:1. S2. A 0.1 mol / L hexadecyltrimethylammonium bromide ethanol solution was added to carboxymethyl cellulose nanoparticles and stirred at 60 °C for 6 h to carry out hydrophobic modification. After the reaction was completed, the nanoparticles were centrifuged, washed, and dried to obtain the hydrophobically modified functional masterbatch. The molar ratio of the cation of hexadecyltrimethylammonium bromide to the carboxyl group in carboxymethyl cellulose nanoparticles was 0.8:1. S3. 92 parts of nylon 6 chips and 8 parts of hydrophobic modified functional masterbatch were vacuum dried at 80℃ for 12h to remove moisture; S4. The dried nylon 6 chips and hydrophobically modified functional masterbatch are fed into a screw extruder and melt-blended at 250°C to obtain a spinning melt. S5. The spinning melt undergoes spinning, post-drawing treatment, and heat setting. The spinning temperature is 250℃, the spinning speed is 4000m / min, the draw ratio is 3.0 times, and the heat setting temperature is 160℃ to obtain high-strength antibacterial nylon filament.
[0025] Example 3 A method for preparing high-strength antibacterial nylon filament includes the following steps: S1. Carboxymethyl cellulose nanoparticles with a carboxyl substitution degree of 1.5 were dispersed in deionized water and subjected to ultrasonic treatment to obtain a uniform and stable dispersion with a dispersion concentration of 2 wt%. Under light-protected and continuously stirred conditions, a 0.01 mol / L silver nitrate aqueous solution was added dropwise to the dispersion and reacted at 60℃ for 1 h. After the reaction was completed, a 0.1 mol / L ascorbic acid solution was added and the reduction reaction was continued at 60℃ for 1 h. After dialyzing and drying, carboxymethyl cellulose nanoparticles loaded with silver nanoparticles were obtained. The molar ratio of silver ions in the silver nitrate aqueous solution to carboxyl groups in the carboxymethyl cellulose nanoparticles was 1:5; the molar ratio of ascorbic acid to silver ions in the silver nitrate aqueous solution was 2:1. S2. A 0.1 mol / L hexadecyltrimethylammonium bromide ethanol solution was added to carboxymethyl cellulose nanoparticles and stirred at 70 °C for 4 h to carry out hydrophobic modification. After the reaction was completed, the nanoparticles were centrifuged, washed, and dried to obtain the hydrophobically modified functional masterbatch. The molar ratio of the cation of hexadecyltrimethylammonium bromide to the carboxyl group in carboxymethyl cellulose nanoparticles was 1.2:1. S3. 90 parts of nylon 6 chips and 10 parts of hydrophobic modified functional masterbatch were vacuum dried at 100℃ for 4 hours to remove moisture. S4. The dried nylon 6 chips and hydrophobically modified functional masterbatch are fed into a screw extruder and melt-blended at 260°C to obtain a spinning melt. S5. The spinning melt undergoes spinning, post-drawing treatment, and heat setting. The spinning temperature is 270℃, the spinning speed is 4800 m / min, the draw ratio is 5.0 times, and the heat setting temperature is 190℃ to obtain high-strength antibacterial nylon filament.
[0026] Comparative Example 1 A method for preparing nylon filament includes the following steps: S1. Dry the nylon 6 slices under vacuum at 90℃ for 10 hours to remove moisture; S2. The dried nylon 6 chips are fed into a screw extruder and melt-blended at 245°C to obtain a spinning melt; S3. The spinning melt undergoes spinning, post-drawing treatment, and heat setting. The spinning temperature is 260℃, the spinning speed is 4500 m / min, the draw ratio is 4.0, and the heat setting temperature is 180℃ to obtain nylon filament.
[0027] Comparative Example 2 A method for preparing nylon filament includes the following steps: S1. Carboxymethyl cellulose nanoparticles with a carboxyl substitution degree of 0.8 were dispersed in deionized water and subjected to ultrasonic treatment to obtain a uniform and stable dispersion with a dispersion concentration of 1 wt%. Under light-proof and continuous stirring conditions, nano silver powder was added to the dispersion, mixed evenly, and then dried to obtain composite nanoparticles. S2. Dry 95 parts of nylon 6 chips and 5 parts of composite nanoparticles under vacuum at 90℃ for 10 hours to remove moisture; S3. The dried nylon 6 chips and composite nanoparticles are fed into a screw extruder and melt-blended at 245℃ to obtain a spinning melt. S4. The spinning melt undergoes spinning, post-drawing treatment, and heat setting. The spinning temperature is 260℃, the spinning speed is 4500 m / min, the draw ratio is 4.0, and the heat setting temperature is 180℃ to obtain nylon filament.
[0028] Comparative Example 3 A method for preparing nylon filament includes the following steps: S1. Nanocellulose was dispersed in deionized water and ultrasonically treated to obtain a uniform and stable dispersion with a concentration of 1 wt%. Under light-protected and continuously stirred conditions, a 0.01 mol / L silver nitrate aqueous solution was added dropwise to the dispersion and reacted at 50°C for 1 h. After the reaction was completed, a 0.01 mol / L ascorbic acid solution was added and the reduction reaction was continued at 50°C for 2 h. After dialyzing and drying, nanocellulose loaded with silver nanoparticles was obtained. The molar ratio of silver ions in ascorbic acid to silver nitrate aqueous solution was 1.5:1. S2. Add hexadecyltrimethylammonium bromide ethanol solution to nanocellulose loaded with silver nanoparticles and stir at 65°C for 5 hours to carry out hydrophobic modification reaction. After the reaction is completed, centrifuge, wash and dry to obtain hydrophobic modified functional masterbatch. S3. 95 parts of nylon 6 chips and 5 parts of hydrophobic modified functional masterbatch were vacuum dried at 90℃ for 10h to remove moisture. S4. The dried nylon 6 chips and hydrophobically modified functional masterbatch are fed into a screw extruder and melt-blended at 245℃ to obtain a spinning melt. S5. The spinning melt undergoes spinning, post-drawing treatment, and heat setting. The spinning temperature is 260℃, the spinning speed is 4500 m / min, the draw ratio is 4.0, and the heat setting temperature is 180℃ to produce nylon filament.
[0029] Comparative Example 4 A method for preparing nylon filament includes the following steps: S1. Carboxymethyl cellulose nanoparticles with a carboxyl substitution degree of 0.8 were dispersed in deionized water and subjected to ultrasonic treatment to obtain a uniform and stable dispersion with a dispersion concentration of 1 wt%. Under light-protected and continuously stirred conditions, a 0.01 mol / L silver nitrate aqueous solution was added dropwise to the dispersion and reacted at 50 °C for 1 h. After the reaction was completed, a 0.1 mol / L ascorbic acid solution was added and the reduction reaction was continued at 50 °C for 2 h. After dialyzing and drying, carboxymethyl cellulose nanoparticles loaded with silver nanoparticles were obtained. The molar ratio of silver ions in the silver nitrate aqueous solution to carboxyl groups in the carboxymethyl cellulose nanoparticles was 1:3; the molar ratio of ascorbic acid to silver ions in the silver nitrate aqueous solution was 1.5:1. S2. 95 parts of nylon 6 slices and 5 parts of carboxymethyl cellulose nanoparticles loaded with silver nanoparticles were vacuum dried at 90℃ for 10h to remove moisture. S3. The dried nylon 6 chips and carboxymethyl cellulose nanoparticles loaded with silver nanoparticles are fed into a screw extruder and melt-blended at 245°C to obtain a spinning melt. S4. The spinning melt undergoes spinning, post-drawing treatment, and heat setting. The spinning temperature is 260℃, the spinning speed is 4500 m / min, the draw ratio is 4.0, and the heat setting temperature is 180℃ to obtain nylon filament.
[0030] Comparative Example 5 A method for preparing nylon filament includes the following steps: S1. Carboxymethyl cellulose nanoparticles with a carboxyl substitution degree of 0.8 were dispersed in deionized water and subjected to ultrasonic treatment to obtain a uniform and stable dispersion with a dispersion concentration of 1 wt%. Under light-protected and continuously stirred conditions, a 0.01 mol / L silver nitrate aqueous solution was added dropwise to the dispersion and reacted at 50 °C for 1 h. After the reaction was completed, a 0.1 mol / L ascorbic acid solution was added and the reaction was continued at 50 °C for 2 h. After dialyzing and drying, carboxymethyl cellulose nanoparticles loaded with silver nanoparticles were obtained. The molar ratio of silver ions in the silver nitrate aqueous solution to carboxyl groups in the carboxymethyl cellulose nanoparticles was 1:1; the molar ratio of ascorbic acid to silver ions in the silver nitrate aqueous solution was 1.5:1. S2. A 0.1 mol / L hexadecyltrimethylammonium bromide ethanol solution was added to carboxymethyl cellulose nanoparticles and stirred at 65°C for 5 hours to carry out hydrophobic modification. After the reaction was completed, the nanoparticles were centrifuged, washed, and dried to obtain the hydrophobically modified functional masterbatch. The molar ratio of the cation of hexadecyltrimethylammonium bromide to the carboxyl group in carboxymethyl cellulose nanoparticles was 1:1. S3. 95 parts of nylon 6 chips and 5 parts of hydrophobic modified functional masterbatch were vacuum dried at 90℃ for 10h to remove moisture. S4. The dried nylon 6 chips and hydrophobically modified functional masterbatch are fed into a screw extruder and melt-blended at 245℃ to obtain a spinning melt. S5. The spinning melt undergoes spinning, post-drawing treatment, and heat setting. The spinning temperature is 260℃, the spinning speed is 4500 m / min, the draw ratio is 4.0, and the heat setting temperature is 180℃ to produce nylon filament.
[0031] Comparative Example 6 A method for preparing nylon filament includes the following steps: S1. Carboxymethyl cellulose nanoparticles with a carboxyl substitution degree of 0.8 were dispersed in deionized water and subjected to ultrasonic treatment to obtain a uniform and stable dispersion with a dispersion concentration of 1 wt%. Under light-protected and continuously stirred conditions, a 0.01 mol / L silver nitrate aqueous solution was added dropwise to the dispersion and reacted at 50 °C for 1 h. After the reaction was completed, a 0.1 mol / L ascorbic acid solution was added and the reduction reaction was continued at 50 °C for 2 h. After dialyzing and drying, carboxymethyl cellulose nanoparticles loaded with silver nanoparticles were obtained. The molar ratio of silver ions in the silver nitrate aqueous solution to carboxyl groups in the carboxymethyl cellulose nanoparticles was 1:6; the molar ratio of ascorbic acid to silver ions in the silver nitrate aqueous solution was 1.5:1. S2. A 0.1 mol / L hexadecyltrimethylammonium bromide ethanol solution was added to carboxymethyl cellulose nanoparticles and stirred at 65°C for 5 hours to carry out hydrophobic modification. After the reaction was completed, the nanoparticles were centrifuged, washed, and dried to obtain the hydrophobically modified functional masterbatch. The molar ratio of the cation of hexadecyltrimethylammonium bromide to the carboxyl group in carboxymethyl cellulose nanoparticles was 1:1. S3. 95 parts of nylon 6 chips and 5 parts of hydrophobic modified functional masterbatch were vacuum dried at 90℃ for 10h to remove moisture. S4. The dried nylon 6 chips and hydrophobically modified functional masterbatch are fed into a screw extruder and melt-blended at 245℃ to obtain a spinning melt. S5. The spinning melt undergoes spinning, post-drawing treatment, and heat setting. The spinning temperature is 260℃, the spinning speed is 4500 m / min, the draw ratio is 4.0, and the heat setting temperature is 180℃ to produce nylon filament.
[0032] Comparative Example 7 A method for preparing nylon filament includes the following steps: S1. Carboxymethyl cellulose nanoparticles with a carboxyl substitution degree of 0.8 were dispersed in deionized water and subjected to ultrasonic treatment to obtain a uniform and stable dispersion with a dispersion concentration of 1 wt%. Under light-protected and continuously stirred conditions, a 0.01 mol / L silver nitrate aqueous solution was added dropwise to the dispersion and reacted at 50 °C for 1 h. After the reaction was completed, a 0.1 mol / L ascorbic acid solution was added and the reduction reaction was continued at 50 °C for 2 h. After dialyzing and drying, carboxymethyl cellulose nanoparticles loaded with silver nanoparticles were obtained. The molar ratio of silver ions in the silver nitrate aqueous solution to carboxyl groups in the carboxymethyl cellulose nanoparticles was 1:3; the molar ratio of ascorbic acid to silver ions in the silver nitrate aqueous solution was 0.7:1. S2. A 0.1 mol / L hexadecyltrimethylammonium bromide ethanol solution was added to carboxymethyl cellulose nanoparticles and stirred at 65°C for 5 hours to carry out hydrophobic modification. After the reaction was completed, the nanoparticles were centrifuged, washed, and dried to obtain the hydrophobically modified functional masterbatch. The molar ratio of the cation of hexadecyltrimethylammonium bromide to the carboxyl group in carboxymethyl cellulose nanoparticles was 1:1. S3. 95 parts of nylon 6 chips and 5 parts of hydrophobic modified functional masterbatch were vacuum dried at 90℃ for 10h to remove moisture. S4. The dried nylon 6 chips and hydrophobically modified functional masterbatch are fed into a screw extruder and melt-blended at 245℃ to obtain a spinning melt. S5. The spinning melt undergoes spinning, post-drawing treatment, and heat setting. The spinning temperature is 260℃, the spinning speed is 4500 m / min, the draw ratio is 4.0, and the heat setting temperature is 180℃ to produce nylon filament.
[0033] Comparative Example 8 A method for preparing nylon filament includes the following steps: S1. Carboxymethyl cellulose nanoparticles with a carboxyl substitution degree of 0.8 were dispersed in deionized water and subjected to ultrasonic treatment to obtain a uniform and stable dispersion with a dispersion concentration of 1 wt%. Under light-protected and continuously stirred conditions, a 0.01 mol / L silver nitrate aqueous solution was added dropwise to the dispersion and reacted at 50 °C for 1 h. After the reaction was completed, a 0.1 mol / L ascorbic acid solution was added and the reduction reaction was continued at 50 °C for 2 h. After dialyzing and drying, carboxymethyl cellulose nanoparticles loaded with silver nanoparticles were obtained. The molar ratio of silver ions in the silver nitrate aqueous solution to carboxyl groups in the carboxymethyl cellulose nanoparticles was 1:3; the molar ratio of ascorbic acid to silver ions in the silver nitrate aqueous solution was 3:1. S2. A 0.1 mol / L hexadecyltrimethylammonium bromide ethanol solution was added to carboxymethyl cellulose nanoparticles and stirred at 65°C for 5 hours to carry out hydrophobic modification. After the reaction was completed, the nanoparticles were centrifuged, washed, and dried to obtain the hydrophobically modified functional masterbatch. The molar ratio of the cation of hexadecyltrimethylammonium bromide to the carboxyl group in carboxymethyl cellulose nanoparticles was 1:1. S3. 95 parts of nylon 6 chips and 5 parts of hydrophobic modified functional masterbatch were vacuum dried at 90℃ for 10h to remove moisture. S4. The dried nylon 6 chips and hydrophobically modified functional masterbatch are fed into a screw extruder and melt-blended at 245℃ to obtain a spinning melt. S5. The spinning melt undergoes spinning, post-drawing treatment, and heat setting. The spinning temperature is 260℃, the spinning speed is 4500 m / min, the draw ratio is 4.0, and the heat setting temperature is 180℃ to produce nylon filament.
[0034] Comparative Example 9 A method for preparing nylon filament includes the following steps: S1. Carboxymethyl cellulose nanoparticles with a carboxyl substitution degree of 0.8 were dispersed in deionized water and subjected to ultrasonic treatment to obtain a uniform and stable dispersion with a dispersion concentration of 1 wt%. Under light-protected and continuously stirred conditions, a 0.01 mol / L silver nitrate aqueous solution was added dropwise to the dispersion and reacted at 50 °C for 1 h. After the reaction was completed, a 0.1 mol / L ascorbic acid solution was added and the reduction reaction was continued at 50 °C for 2 h. After dialyzing and drying, carboxymethyl cellulose nanoparticles loaded with silver nanoparticles were obtained. The molar ratio of silver ions in the silver nitrate aqueous solution to carboxyl groups in the carboxymethyl cellulose nanoparticles was 1:3; the molar ratio of ascorbic acid to silver ions in the silver nitrate aqueous solution was 1.5:1. S2. A 0.1 mol / L hexadecyltrimethylammonium bromide ethanol solution was added to carboxymethyl cellulose nanoparticles and stirred at 65°C for 5 hours to carry out hydrophobic modification. After the reaction was completed, the nanoparticles were centrifuged, washed, and dried to obtain the hydrophobically modified functional masterbatch. The molar ratio of the cation of hexadecyltrimethylammonium bromide to the carboxyl group in carboxymethyl cellulose nanoparticles was 0.5:1. S3. 95 parts of nylon 6 chips and 5 parts of hydrophobic modified functional masterbatch were vacuum dried at 90℃ for 10h to remove moisture. S4. The dried nylon 6 chips and hydrophobically modified functional masterbatch are fed into a screw extruder and melt-blended at 245℃ to obtain a spinning melt. S5. The spinning melt undergoes spinning, post-drawing treatment, and heat setting. The spinning temperature is 260℃, the spinning speed is 4500 m / min, the draw ratio is 4.0, and the heat setting temperature is 180℃ to produce nylon filament.
[0035] Comparative Example 10 A method for preparing nylon filament includes the following steps: S1. Carboxymethyl cellulose nanoparticles with a carboxyl substitution degree of 0.8 were dispersed in deionized water and subjected to ultrasonic treatment to obtain a uniform and stable dispersion with a dispersion concentration of 1 wt%. Under light-protected and continuously stirred conditions, a 0.01 mol / L silver nitrate aqueous solution was added dropwise to the dispersion and reacted at 50 °C for 1 h. After the reaction was completed, a 0.1 mol / L ascorbic acid solution was added and the reduction reaction was continued at 50 °C for 2 h. After dialyzing and drying, carboxymethyl cellulose nanoparticles loaded with silver nanoparticles were obtained. The molar ratio of silver ions in the silver nitrate aqueous solution to carboxyl groups in the carboxymethyl cellulose nanoparticles was 1:3; the molar ratio of ascorbic acid to silver ions in the silver nitrate aqueous solution was 1.5:1. S2. A 0.1 mol / L hexadecyltrimethylammonium bromide ethanol solution was added to carboxymethyl cellulose nanoparticles and stirred at 65°C for 5 hours to carry out hydrophobic modification. After the reaction was completed, the nanoparticles were centrifuged, washed, and dried to obtain the hydrophobically modified functional masterbatch. The molar ratio of the cation of hexadecyltrimethylammonium bromide to the carboxyl group in carboxymethyl cellulose nanoparticles was 1.5:1. S3. 95 parts of nylon 6 chips and 5 parts of hydrophobic modified functional masterbatch were vacuum dried at 90℃ for 10h to remove moisture. S4. The dried nylon 6 chips and hydrophobically modified functional masterbatch are fed into a screw extruder and melt-blended at 245℃ to obtain a spinning melt. S5. The spinning melt undergoes spinning, post-drawing treatment, and heat setting. The spinning temperature is 260℃, the spinning speed is 4500 m / min, the draw ratio is 4.0, and the heat setting temperature is 180℃ to produce nylon filament.
[0036] Performance testing: The mechanical properties of nylon filaments were tested according to the methods specified in GB / T14344-2022 standard.
[0037] The antibacterial properties of nylon filament were tested according to GB / T 20944.3-2008 standard. The test strains were Staphylococcus aureus and Escherichia coli. The blank control sample was the nylon filament of Comparative Example 1. The antibacterial rate Y = (WQ) / W × 100%, where W is the viable bacterial concentration (CFU / mL) of the blank control sample after 18 hours of shaking contact, and Q is the viable bacterial concentration (CFU / mL) of the antibacterial sample after 18 hours of shaking contact.
[0038] The performance test results are shown in Table 1.
[0039]
[0040] As can be seen from the test results in Table 1, the nylon filament of Comparative Example 1 has low breaking strength and lacks antibacterial properties. Examples 1-3 incorporated hydrophobically modified functional masterbatches made by loading silver nanoparticles onto carboxymethyl cellulose nanoparticles and hydrophobically modifying them. Carboxymethyl cellulose nanoparticles themselves have high specific surface area and high modulus. As a reinforcing phase in the polymer matrix, they exist in a well-dispersed state in the nylon matrix, which can improve the strength and modulus of the fiber. Moreover, there is a strong coordination or electrostatic interaction between the carboxyl groups on the surface of carboxymethyl cellulose nanoparticles and the silver nanoparticles, which can firmly anchor the silver nanoparticles to the carrier. During spinning, melting, and subsequent use, it can slow down the rapid release and loss of silver ions, thereby providing a more durable antibacterial effect. Furthermore, carboxymethyl cellulose nanoparticles loaded with silver nanoparticles were modified using hexadecyltrimethylammonium bromide. The long alkyl chains were connected to the surface of carboxymethyl cellulose nanoparticles through ionic interactions, making them hydrophilic to hydrophobic. This greatly improved the interfacial compatibility between the functional masterbatch and the nylon 6 melt, enabling more uniform melt blending in the screw extruder, reducing phase separation, and ensuring that the functional fibers have good spinnability and mechanical properties.
[0041] In Comparative Example 2, when preparing composite nanoparticles, the silver nanoparticles were directly physically mixed with the carboxymethyl cellulose nanoparticle dispersion without loading the carboxyl sites of the carboxymethyl cellulose nanoparticles. As a result, the composite nanoparticles had poor dispersibility in the nylon 6 matrix, were prone to agglomeration, and had weak interfacial bonding. Consequently, the mechanical properties and antibacterial properties of the nylon filaments were not as good as those in Example 1.
[0042] In Comparative Example 3, when preparing the hydrophobically modified functional masterbatch, nanocellulose was used instead of carboxymethyl nanocellulose. The functional group on the surface of nanocellulose is hydroxyl, and its coordination ability and ionization degree are much weaker than those of carboxymethyl nanocellulose. Therefore, its complexing ability is weak, and the degree of free silver ions in the system is high. When antioxidant acid is added, the free silver ions are reduced, leading to nucleation and aggregation. Furthermore, hexadecyltrimethylammonium bromide is adsorbed on the surface of nanocellulose only by intermolecular van der Waals forces or by forming weak hydrogen bonds with hydroxyl groups, resulting in poor adhesion. Moreover, after modification, it is still a hydrophilic substance with poor compatibility with hydrophobic nylon, which leads to the mechanical properties and antibacterial properties of nylon filaments being worse than those in Example 1.
[0043] Comparative Example 4 did not undergo hydrophobic modification treatment on the carboxymethyl nanocellulose loaded with silver nanoparticles. Carboxymethyl nanocellulose is a hydrophilic material, while nylon 6 matrix is a hydrophobic polymer. Therefore, the carboxymethyl nanocellulose loaded with silver nanoparticles has poor compatibility with nylon 6 matrix, is prone to agglomeration, forms stress concentration points, and significantly reduces the breaking strength of nylon filament.
[0044] In Comparative Example 5, the molar ratio of silver ions to carboxyl groups was too high during the preparation of carboxymethyl cellulose loaded with silver nanoparticles. This resulted in a large excess of silver ions, which independently generated silver nanoparticles in the solution instead of growing in situ on the surface of the carboxymethyl cellulose. These free silver nanoparticles were prone to aggregation and detachment during washing, modification, or melt processing, leading to poor antibacterial durability. In Comparative Example 6, the molar ratio of silver ions to carboxyl groups was too low, resulting in a much smaller number of silver ions than carboxyl sites. This resulted in low silver loading and similarly unsatisfactory antibacterial effects.
[0045] In Comparative Example 7, the amount of ascorbic acid used in the preparation of carboxymethyl cellulose nanoparticles was too small, resulting in incomplete reduction of silver ions. The residual silver ions affected the stability of the product, impacting its mechanical and antibacterial properties. In Comparative Example 8, the amount of ascorbic acid used in the preparation of carboxymethyl cellulose nanoparticles was too large, leading to an excessively rapid reduction rate and a massive instantaneous generation of silver ions. These ions did not have enough time to nucleate and grow orderly at the carboxyl sites of the carboxymethyl cellulose nanoparticles, easily causing particle aggregation and thus reducing mechanical and antibacterial properties.
[0046] In Comparative Example 9, the cationic proportion of hexadecyltrimethylammonium bromide was too low during hydrophobication modification, resulting in insufficient hydrophobicity and easy aggregation in nylon 6, which in turn affected the mechanical and antibacterial properties of the nylon filament. In Comparative Example 10, the cationic proportion was too high during hydrophobication modification, and the excess hexadecyltrimethylammonium bromide became stress defect points, affecting the mechanical strength of the final fiber.
[0047] The above description is only a preferred embodiment of the present invention and does not limit the patent scope of the present invention. All equivalent structural transformations made using the present invention specification under the concept of the present invention, or direct / indirect applications in other related technical fields, are included within the patent protection scope of the present invention.
Claims
1. A high-strength antibacterial nylon filament, characterized in that, By weight, the high-strength antibacterial nylon filament comprises 90-95 parts of nylon 6 chips and 5-10 parts of hydrophobic modified functional masterbatch. The preparation process of the hydrophobic modified functional masterbatch is as follows: S1. Carboxymethyl cellulose nanoparticles are dispersed in deionized water and subjected to ultrasonic treatment to obtain a uniform and stable dispersion. Silver nitrate aqueous solution is added dropwise to the dispersion under light-protected and continuously stirred conditions to carry out the reaction. After the reaction is completed, ascorbic acid solution is added to continue the reduction reaction. The mixture is then dialyzed and dried to obtain carboxymethyl cellulose nanoparticles loaded with silver nanoparticles. S2. Add hexadecyltrimethylammonium bromide ethanol solution to carboxymethyl cellulose nanoparticles loaded with silver nanoparticles, stir at a constant temperature to carry out hydrophobic modification reaction, and after the reaction is completed, centrifuge, wash and dry to obtain hydrophobic modified functional masterbatch.
2. The high-strength antibacterial nylon filament according to claim 1, characterized in that, The degree of carboxyl substitution of the carboxymethyl nanocellulose in S1 is 0.5~1.5, and the dispersion concentration of the carboxymethyl nanocellulose in deionized water is 0.5~2wt%.
3. The high-strength antibacterial nylon filament according to claim 1, characterized in that, In S1, the molar ratio of silver ions in the silver nitrate aqueous solution to carboxyl groups in carboxymethyl cellulose nanoparticles is 1:(2~5); the molar ratio of ascorbic acid to silver ions in the silver nitrate aqueous solution is (1~2):
1.
4. The high-strength antibacterial nylon filament according to claim 1, characterized in that, The reaction temperature in S1 is 25~60℃ and the time is 1~2h; the reduction reaction temperature in S1 is 25~60℃ and the time is 1~4h.
5. The high-strength antibacterial nylon filament according to claim 1, characterized in that, The molar ratio of the cetyltrimethylammonium bromide cation to the carboxyl group in carboxymethyl nanocellulose in S2 is (0.8~1.2):
1.
6. The high-strength antibacterial nylon filament according to claim 1, characterized in that, The hydrophobic modification reaction in S2 is carried out at a temperature of 60-70℃ for 4-6 hours.
7. A method for preparing the high-strength antibacterial nylon filament according to any one of claims 1 to 6, characterized in that, Includes the following steps: (1) Vacuum dry the nylon 6 chips and hydrophobic modified functional masterbatch to remove moisture; (2) The dried nylon 6 chips and hydrophobic modified functional masterbatch are fed into a screw extruder and melt-blended to obtain a spinning melt; (3) The spinning melt is spun, drawn and heat-set to obtain high-strength antibacterial nylon filament.
8. The method for preparing high-strength antibacterial nylon filament according to claim 7, characterized in that, The vacuum drying temperature in step (1) is 80~100℃ and the time is 4~12h.
9. The method for preparing high-strength antibacterial nylon filament according to claim 7, characterized in that, The melting and blending temperature in step (2) is 230~260℃.
10. The method for preparing high-strength antibacterial nylon filament according to claim 7, characterized in that, In step (3), the spinning temperature is 250~270℃, the spinning speed is 4000~4800 m / min, the stretching ratio of the post-stretching treatment is 3.0~5.0 times, and the heat setting temperature is 160~190℃.
Citation Information
Patent Citations
Preparation process of non-dyed polyamide fiber
CN113417027A