A one-way easy-tear film, its preparation process and its application in labels

The unidirectional easy-tear film prepared by the three-layer co-extrusion casting process solves the problems of uncontrollable tear direction and poor printability of traditional films, and achieves controllable unidirectional easy tear and good adhesive performance, making it suitable for label applications.

CN122684103BActive Publication Date: 2026-11-10SHANTOU JINGSU PACKAGING MATERIAL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611203696.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-08-10
Publication Date
2026-11-10
Estimated Expiration
2046-08-10

AI Technical Summary

Technical Problem

Traditional polyolefin films have uncontrollable tearing direction, are prone to skewed tearing, and physical perforation damages mechanical integrity. The low surface polarity of longitudinally stretched polyethylene films results in poor printability and difficulty in applying adhesive backing, and the tape is prone to breakage during high-speed labeling.

Method used

A three-layer co-extrusion casting process is used to prepare a unidirectional easy-tear film, which includes a printed composite layer, an impact-resistant molding layer, and an adhesive base layer. The impact-resistant molding layer has a micro-nano-scale fiber structure, the outer surface of the printed composite layer has a micro-nano-uneven structure, and the adhesive base layer has a smooth surface. The melt stretching is controlled by the co-extrusion die and cooling system, and the controllable unidirectional easy-tear film is achieved by combining corona treatment.

Benefits of technology

While ensuring the overall tensile strength and interlayer bonding of the film, controllable unidirectional straight tearing is achieved, improving printability and adhesive performance, and avoiding longitudinal tape breakage during high-speed labeling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

This invention relates to the field of polymer film materials and their molding processes, specifically to a unidirectional easy-tear film, its preparation process, and its application in labels. The preparation process includes raw material pretreatment, three-layer co-extrusion, casting, traction and secondary orientation, surface activation, and winding steps. The process combines the synergistic effect of the three-layer co-extrusion structure and the multiphase blend system in the impact-resistant molding layer. Its core is to utilize the shear stress of the co-extrusion die to stretch and deform the cyclic olefin copolymer, followed by rapid cooling and in-situ longitudinal traction to construct a longitudinally aligned micro / nano-scale fiber structure, while simultaneously imprinting a micro / nano frosted surface onto the outer surface. This invention overcomes the shortcomings of traditional films, such as uncontrollable tear direction, low polarity, and easy breakage during high-speed traction. By utilizing the fiber-guiding and surface morphology control mechanism of the impact-resistant molding layer, controllable unidirectional linear easy tearing of the film is achieved without sacrificing overall mechanical strength and interlayer bonding, while also ensuring excellent printing and coating performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of polymer film materials and their molding processes, specifically to a one-way easy-tear film, its preparation process, and its application in labels. Background Technology

[0002] In the modern packaging and label manufacturing industry, film substrates need to withstand the strong friction and traction of high-speed labeling machines, while also meeting the convenience of consumers manually tearing them open in end applications; traditional polyolefin films are uncontrollable in direction when torn, tending to produce oblique tears that damage the label content; to improve the tearability of films, existing technologies mostly use physical perforation or unidirectional stretching of single-layer films. However, physical perforation will damage the mechanical integrity of the label; although longitudinally stretched polyethylene is easy to tear, its high crystal orientation results in low surface polarity, poor printability, and difficulty in directly coating the backing with adhesive. Under the traction of a high-speed labeling machine, it tends to break longitudinally. Therefore, how to achieve controllable unidirectional linear easy tearing without sacrificing the overall tensile strength and interlayer bonding of the film, while also taking into account the multifunctionality of printing and coating, is a technical problem that needs to be solved in this field. Summary of the Invention

[0003] The purpose of this invention is to provide a unidirectional easy-tear film, its preparation process, and its application in labels. This invention aims to solve the problems of uncontrollable tearing direction and easy skewed tearing in traditional polyolefin films, physical perforation damaging mechanical integrity, and the low surface polarity of longitudinally stretched polyethylene films leading to poor printability, difficulty in applying adhesive, and a tendency for longitudinal tape breakage during high-speed labeling. Specifically, the technical solution of this invention is as follows: A one-way easy-tear film, wherein the one-way easy-tear film comprises, in sequence along the thickness direction, a printed composite layer, an impact-resistant molding layer, and an adhesive base layer; the raw materials of the printed composite layer include: 60-75 parts of a first polyethylene base resin, 22-30 parts of metallocene polyethylene, and 1-3 parts of erucamide. The raw materials for the impact-resistant molding layer include: 60-70 parts of polypropylene base resin, 15-25 parts of cyclic olefin copolymer, and 10-15 parts of polyolefin elastomer; the raw materials for the adhesive base layer include: 70-80 parts of second polyethylene base resin and 20-30 parts of maleic anhydride grafted polyolefin; the impact-resistant molding layer has a micro / nano-scale fiber structure arranged along the longitudinal orientation of the film; the micro / nano-scale fiber structure is a continuous fibrous structure formed by the cyclic olefin copolymer as a rigid dispersed phase distributed in the polypropylene base resin matrix; the outer surface of the printed composite layer is a frosted surface with a micro / nano-scale uneven structure; the outer surface of the adhesive base layer is a smooth surface.

[0004] Preferably, the diameter of the micro-nano-scale fiber-forming structure is 100-500 nm.

[0005] Another object of the present invention is to provide a preparation process for the above-mentioned unidirectional easy-tear film, comprising the following steps: Raw material pretreatment: The raw materials for the printed composite layer, the impact-resistant molding layer and the adhesive base layer are respectively fed into a high-speed mixer for high-speed mixing; Three-layer co-extrusion: The three layers of raw materials are heated and melted independently, combined by a distributor, and then sent to the co-extrusion die. They are extruded under the shear stress of the flow channel of the co-extrusion die. After air gap stretching at a melt stretch ratio of 15-25, they enter a pressure cooling system composed of a mirror casting roller and a silicone roller with micro-nano structures on its surface for rapid cooling and shaping. The printed composite layer is in contact with the silicone roller with micro-nano structures, and the adhesive base layer is in contact with the mirror casting roller. Traction and secondary orientation: After rapid cooling and shaping, the film enters the traction roller group and is longitudinally tractioned under a traction tension of 25-45 N / m; Surface activation and winding: The surface of the printed composite layer is subjected to corona treatment, and after edge trimming, thickness measurement feedback adjustment, and winding, a unidirectional easy-tear film is obtained.

[0006] Preferably, in the raw material pretreatment step, the high-speed mixing temperature is 90-100℃, the rotation speed is 700-800 r / min, and the time is 12-15 min.

[0007] Preferably, in the three-layer co-extrusion step, the heating and melting extrusion temperature of the printing composite layer raw material is 225-230℃, the heating and melting extrusion temperature of the impact-resistant molding layer raw material is 230-235℃, and the heating and melting extrusion temperature of the adhesive base layer raw material is 225-230℃.

[0008] Preferably, cooling water at 20-25°C is introduced into the pressure cooling system to reduce the melt temperature below the glass transition temperature of the cyclic olefin copolymer.

[0009] Preferably, in the surface activation and winding steps, the voltage of the corona treatment is 10-30kV.

[0010] Another object of the present invention is to provide an application of a one-way easy-tear film in labels, wherein the one-way easy-tear film is used to prepare anti-counterfeiting labels, express waybills or food easy-tear labels.

[0011] The beneficial effects of this invention are as follows: This invention produces a unidirectional easy-tear film comprising a printed composite layer, an impact-resistant molding layer, and an adhesive base layer through a co-extrusion casting process; by utilizing the micro-nano-scale fiber-forming structure inside the impact-resistant molding layer, controllable unidirectional linear easy tearing of the film is achieved; at the same time, the printed composite layer has a frosted surface with a micro-nano-uneven structure, and the adhesive base layer is a smooth mirror surface, which improves the printing adaptability and coating performance of the film while ensuring the overall mechanical strength and interlayer bonding force, and overcomes the defect of longitudinal tape breakage during high-speed labeling. Attached Figure Description

[0012] The above and other objects, features and advantages of the present invention will become clearer from the following description of embodiments of the invention with reference to the accompanying drawings, in which: Figure 1 The SEM image is from Example 1; Figure 2 The SEM image is from Example 2; Figure 3 The SEM image is from Example 3; Figure 4 The SEM image is from Example 4; Figure 5 The SEM image is shown in Comparative Example 1. Figure 6 The SEM image is shown in Comparative Example 2. Figure 7 The SEM image is shown in Comparative Example 3; Figure 8 The SEM image is shown in Comparative Example 4. Figure 9 This is the SEM image of Comparative Example 5. Detailed Implementation

[0013] The technical solutions in the embodiments of the present invention will be clearly and completely described below; the described embodiments are only some embodiments of the present invention, and not all embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.

[0014] In this invention, the first polyethylene base resin and the second polyethylene base resin are independent of each other and are selected from one or more combinations of linear low-density polyethylene, low-density polyethylene, or high-density polyethylene; the cyclic olefin copolymer is selected from ethylene-norbornene copolymer; the polyolefin elastomer is selected from ethylene-octene copolymer elastomer; and the maleic anhydride-grafted polyolefin is selected from maleic anhydride-grafted polyethylene, wherein the molecular formula of the grafting monomer maleic anhydride is C4H2O3.

[0015] Example 1

[0016] This embodiment provides a unidirectional easy-tear three-layer co-extruded film with a microfiber structure, a total thickness of 60 μm, and the thicknesses of the three layers are 10 μm, 40 μm and 10 μm, respectively; Raw material composition: The printing composite layer raw materials include: 70 parts of linear low-density polyethylene as the first polyethylene base resin, 28 parts of metallocene polyethylene, and 2 parts of erucamide; the impact-resistant molding layer raw materials include: 65 parts of homopolymer polypropylene, 20 parts of cyclic olefin copolymer, and 15 parts of polyolefin elastomer; the glass transition temperature of the cyclic olefin copolymer is 138℃; the adhesive base layer raw materials include: 75 parts of low-density polyethylene as the second polyethylene base resin and 25 parts of maleic anhydride grafted polyolefin. Raw material pretreatment: The printing composite layer raw material is added to a high-speed mixer and mixed for 15 minutes at 95℃ and 750r / min; the impact-resistant molding layer raw material is added to a high-speed mixer and mixed for 15 minutes at 95℃ and 750r / min; the adhesive base layer raw material is added to a high-speed mixer and mixed for 15 minutes at 95℃ and 750r / min. After this step, the cyclic olefin copolymer and polyolefin elastomer in the impact-resistant molding layer form a macroscopically uniform mixture in the polypropylene matrix. Three-layer co-extrusion: The three sets of mixed raw materials are fed into three extruders for melting and plasticizing. The extrusion temperature of the printed composite layer is set at 228℃, the extrusion temperature of the impact-resistant molding layer is set at 235℃, and the extrusion temperature of the adhesive base layer is set at 228℃. The three melts are combined by a distributor according to their thickness ratio and then sent to the co-extrusion die. The melt of the impact-resistant molding layer is subjected to shearing in the die channel, and the cyclic olefin copolymer dispersed phase undergoes tensile deformation along the extrusion direction. Casting: After the combined three-layer melt is extruded from the die, it enters the pressure cooling system through a 10-50mm air gap under the condition that the melt stretch ratio is controlled at 20. The pressure cooling system consists of a mirror-finish casting roller and a nano-silicone roller with a surface roughness of 1.25μm. Cooling water at 22℃ is circulated inside the cooling roller. During the cooling process, the stretched cyclic olefin copolymer dispersed phase in the impact-resistant molding layer is rapidly solidified, inhibiting shrinkage. The outer surface of the printed composite layer forms a uniform frosted microstructure under the action of the nano-silicone roller. The outer surface of the adhesive base layer contacts the mirror roller to form a smooth mirror surface. Traction and secondary orientation: After cooling, the film enters the traction roller group and is longitudinally tractioned under the action of 35 N / m traction tension. The solidified fibrous dispersed phase in the impact-resistant forming layer continues to be refined and extended longitudinally to form an oriented fiber structure, thus obtaining a secondary orientation film intermediate. Surface activation and winding: The surface of the printed composite layer of the secondary orientation film intermediate is subjected to corona treatment with a corona voltage of 25kV; after edge trimming and online thickness adjustment, it is wound up to obtain a unidirectional easy-tear film.

[0017] Example 2

[0018] The total thickness of the film provided in this embodiment is 60 μm, and the thicknesses of the three layers are 12 μm, 36 μm and 12 μm, respectively. Raw material composition: The printing composite layer raw materials include: 60 parts of high-density polyethylene as the first polyethylene base resin, 30 parts of metallocene polyethylene, and 1 part of erucamide; the impact-resistant molding layer raw materials include: 70 parts of polypropylene base resin, 15 parts of cyclic olefin copolymer, and 15 parts of polyolefin elastomer; the glass transition temperature of the cyclic olefin copolymer is 130℃; the adhesive base layer raw materials include: 80 parts of the second polyethylene base resin and 20 parts of maleic anhydride grafted polyolefin. Raw material pretreatment: The three layers of raw materials were mixed at 90℃ and 700r / min for 12 minutes respectively; Three-layer co-extrusion: the printing composite layer is extruded at a temperature of 225℃, the impact-resistant molding layer is extruded at a temperature of 230℃, and the adhesive base layer is extruded at a temperature of 225℃. Casting: A pressure cooling system consisting of a mirror-finish casting roller and a micro-nano structured silicone roller with a surface roughness of 1.21μm is used, with a cooling water temperature of 25℃; and the melt stretching ratio is controlled at 15. Traction and secondary orientation: The cooled film is introduced into the traction roller group and longitudinally traction is performed under a traction tension of 25 N / m; Surface activation and winding: Corona voltage is 10kV, followed by winding.

[0019] Example 3

[0020] The total thickness of the film provided in this embodiment is 65 μm, and the thicknesses of the three layers are 11 μm, 43 μm and 11 μm, respectively. Raw material composition: In the printing composite layer raw material, there are 68 parts of linear low-density polyethylene, 29 parts of metallocene polyethylene, and 3 parts of erucamide as the first polyethylene base resin; in the impact-resistant molding layer raw material, there are 60 parts of polypropylene base resin, 25 parts of cyclic olefin copolymer, and 15 parts of polyolefin elastomer; the glass transition temperature of the cyclic olefin copolymer is 145℃; in the adhesive base layer raw material, there are 72 parts of low-density polyethylene and 28 parts of maleic anhydride grafted polyolefin as the second polyethylene base resin. Raw material pretreatment: The three layers of raw materials were mixed at 100℃ and 800r / min for 12 minutes respectively; Three-layer co-extrusion: the printing composite layer is extruded at 230℃, the impact-resistant molding layer is extruded at 233℃, and the adhesive base layer is extruded at 230℃. Casting: A pressure cooling system consisting of a mirror-finish casting roller and a micro-nano structured silicone roller with a surface roughness of 1.28μm is used, with a cooling water temperature of 20℃; and the melt stretching ratio is controlled at 25. Traction and secondary orientation: The cooled film is introduced into the traction roller group and longitudinally traction is performed under a traction tension of 45 N / m; Surface activation and winding: Corona voltage is 30kV, followed by winding.

[0021] Example 4

[0022] The total thickness of the film provided in this embodiment is 55 μm, and the thicknesses of the three layers are 9 μm, 37 μm and 9 μm, respectively. Raw material composition: In the printing composite layer raw material, there are 75 parts of the first polyethylene base resin, 22 parts of metallocene polyethylene, and 3 parts of erucamide; in the impact-resistant molding layer raw material, there are 64 parts of polypropylene base resin, 22 parts of cyclic olefin copolymer, and 14 parts of polyolefin elastomer; the glass transition temperature of the cyclic olefin copolymer is 150℃; in the adhesive base layer raw material, there are 70 parts of the second polyethylene base resin and 30 parts of maleic anhydride grafted polyolefin. Raw material pretreatment: The three layers of raw materials were mixed at 98℃ and 780r / min for 14 minutes respectively; Three-layer co-extrusion: the printing composite layer is extruded at a temperature of 227°C, the impact-resistant molding layer is extruded at a temperature of 234°C, and the adhesive base layer is extruded at a temperature of 227°C. Casting: A pressure cooling system consisting of a mirror-finish casting roller and a micro-nano structured silicone roller with a surface roughness of 1.22μm is used, with a cooling water temperature of 23℃; and the melt stretching ratio is controlled at 18. Traction and secondary orientation: The cooled film is introduced into the traction roller group and longitudinally traction is performed under the action of traction tension of 30 N / m; Surface activation and winding: Corona voltage is 20kV, followed by winding.

[0023] Comparative Example 1: The difference between this comparative example and Example 1 is that no cyclic olefin copolymer is added to the impact-resistant molding layer, and 20 parts of cyclic olefin copolymer in Example 1 are replaced with 20 parts of polypropylene base resin, so that the impact-resistant molding layer formulation is 85 parts of polypropylene base resin and 15 parts of polyolefin elastomer; other operating steps and process parameters are exactly the same as in Example 1.

[0024] Comparative Example 2: The difference between this comparative example and Example 1 is that the cooling water temperature in the casting process is changed from 22°C to 60°C; the other operating steps and process parameters are exactly the same as in Example 1.

[0025] Comparative Example 3: The difference between this comparative example and Example 1 is that in the casting process, the micro-nano structured silicone roller is replaced with a smooth steel roller with a surface roughness of 0.15 μm; the other operating steps and process parameters are exactly the same as in Example 1.

[0026] Comparative Example 4: The difference between this comparative example and Example 1 is that the melt stretching ratio in the casting process is changed from 20 to 8; the other operating steps and process parameters are exactly the same as in Example 1.

[0027] Comparative Example 5: The difference between this comparative example and Example 1 is that maleic anhydride-grafted polyolefin is not added to the adhesive base layer, and 25 parts of maleic anhydride-grafted polyolefin in Example 1 are replaced with 25 parts of polyolefin elastomer; other operating steps and process parameters are exactly the same as in Example 1.

[0028] Performance Testing and Datasheets The test methods are briefly described as follows: Tear strength was tested according to ASTM D1922, measuring both longitudinal and transverse tear strengths and recording the tear deflection angle; tensile strength was tested according to ASTM D882, and interlaminar peel strength was tested according to ASTM D903; surface tension was measured using the dyne pen method, and the coefficient of dynamic friction was measured according to GB / T10006; glass transition temperature was tested using differential scanning calorimetry according to GB / T19466; surface roughness was tested using a surface roughness measuring instrument according to GB / T1031; the diameter of the micro / nano-scale fiber structure was obtained by averaging 100 randomly selected fibers using scanning electron microscopy images and image analysis software; the micromorphology of the impact-resistant molding layer was observed using a scanning electron microscope after light etching with xylene. The SEM images of each embodiment and comparative example are shown below. Figures 1 to 9 As shown; Table 1. Performance test results of each embodiment and comparative example.

[0029]

[0030]

[0031]

[0032]

[0033]

[0034]

[0035] As can be seen from the comparison of the test results of Example 1 and Comparative Example 1 in Table 1, after omitting the cyclic olefin copolymer, the longitudinal tear strength increased from 0.42 N / mm to 8.6 N / mm, the transverse tear strength decreased to 9.4 N / mm, and the tear deflection angle increased to 23 degrees. The underlying mechanism is that the impact-resistant molding layer lacks components that can form a rigid fiber phase under shear and traction conditions. The polypropylene and polyolefin elastomer system only forms a conventional two-phase dispersion structure and cannot form a long-distance continuous orientation interface. When the crack propagates, there is a lack of longitudinal low-resistance propagation channels, which leads to a significant increase in longitudinal tearing resistance. There is also a lack of fiber blocking effect in the transverse direction, which leads to a decrease in transverse tear resistance. The film exhibits an approximately isotropic tearing behavior. As can be seen from the comparison of the test results of Example 1 and Comparative Example 2 in Table 1, after the cooling water temperature was increased from 22℃ to 60℃, the longitudinal tear strength increased to 3.9 N / mm, the transverse tear strength decreased to 11.1 N / mm, and the tear deflection angle increased to 14 degrees. The underlying mechanism is that, as the cooling rate decreases, the stretched dispersed phase formed by the die shearing cannot be fixed before the dispersed phase molecular chains undergo stress relaxation and shrinkage. The cyclic olefin copolymer, due to not being rapidly cooled below its glass transition temperature in time, shrinks under the action of interfacial tension, and the dispersed phase that could originally form fibers partially transforms into short rod-shaped or ellipsoidal structures. As the number of continuous orientation interfaces in the impact-resistant molding layer decreases, the longitudinal crack guiding effect weakens, leading to an increase in the longitudinal tear strength value. At the same time, the transverse crack-blocking structure is also incomplete, thus reducing the stability of the tear direction and significantly increasing the tear deflection angle. As can be seen from the comparison of the test results of Example 1 and Comparative Example 3 in Table 1, after replacing the micro-nano structured silicone roller with a smooth steel roller, the fluctuation of longitudinal and transverse tear data is within the allowable range of ±5% measurement error, but the dynamic friction coefficient increases from 0.18 to 0.31. The underlying mechanism is that the change does not alter the fiber formation process of the impact-resistant molding layer, so the tear and tensile properties change little; however, the outer surface of the printed composite layer lacks micro-nano imprinting structures, and the low-friction layer formed after the migration of erucic acid amide is difficult to coordinate with the surface rough structure for stability, resulting in an increase in the surface contact area and an increase in the sliding resistance of the film when it contacts the roller surface and guide, thus significantly increasing the dynamic friction coefficient. As can be seen from the comparison of the test results of Example 1 and Comparative Example 4 in Table 1, after the melt stretching ratio in the casting process was reduced from 20 to 8, the longitudinal tear strength increased to 1.75 N / mm, the transverse tear strength decreased to 14.0 N / mm, and the longitudinal tensile strength decreased to 41 MPa. The underlying mechanism is that when the traction tension is insufficient, the primary fibers retained after rapid cooling cannot continue to extend and refine sufficiently, and the fiber length and aspect ratio in the impact-resistant molding layer decrease, as does the longitudinal alignment. When the crack propagates longitudinally, the interface connection is discontinuous, and the crack propagation resistance increases. Therefore, the longitudinal tearability of the film deteriorates, leading to an increase in the longitudinal tear strength. At the same time, the orientation reinforcement effect is insufficient, causing the longitudinal tensile strength to decrease synchronously. As can be seen from the comparison of the test results of Example 1 and Comparative Example 5 in Table 1, after omitting maleic anhydride-grafted polyolefin, the interlayer peel strength decreased from 3.8 N / 15 mm to 1.1 N / 15 mm, the surface tension decreased from 44 dyn / cm to 36 dyn / cm, while the tear data changed little. The underlying mechanism is that maleic anhydride-grafted polyolefin provides polar groups on the surface of the adhesive base layer and improves the segment diffusion and interfacial bonding ability between the adhesive base layer and adjacent layers. After replacing it with a non-polar polyolefin elastomer, the surface polarity of the adhesive base layer decreases, the interaction with the subsequent adhesive is weakened, and the interfacial bonding force decreases. Therefore, the main manifestations are a significant decrease in peel strength and surface tension. Since the fiber structure of the impact-resistant molding layer is not changed, the tear directionality is basically retained. The test results of Examples 1 to 4 show that a stable unidirectional tearable structure can be formed within the component range and process range defined by the present invention. Example 2 uses a lower cyclic olefin copolymer content and a lower draw ratio, and still obtains a good longitudinal tearable effect, but the fiber continuity is slightly lower, so the longitudinal tear strength is slightly higher than that of Example 1. Example 3 uses a higher content of cyclic olefin copolymers, a lower cooling water temperature and a higher draw ratio, resulting in finer and denser fibers in the impact-resistant molding layer. Therefore, the longitudinal tear strength and surface friction coefficient are both kept at a low level. Example 4 increases the proportion of maleic anhydride-grafted polyolefins in the adhesive base layer, resulting in higher interlayer peel strength while maintaining good tear directionality and processing stability. The above results indicate that there is a clear synergistic relationship between the three-layer structure, the fiber-forming formulation of the impact-resistant molding layer, the rapid cooling and shaping, and the traction orientation, which together determine the unidirectional tear resistance, interlayer bonding performance, and surface processing performance of the film.

[0036] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention in any other way. Any person skilled in the art can make changes based on the above-disclosed technical content, or modify it into an equivalent embodiment and apply it to other fields. However, any conventional modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the technical solution of the present invention shall still fall within the protection scope of the technical solution of the present invention.

Claims

1. A unidirectional easy-tear film, characterized in that, The unidirectional easy-tear film comprises, in sequence along its thickness direction, a printed composite layer, an impact-resistant molding layer, and an adhesive base layer; the raw materials of the printed composite layer include: 60-75 parts of first polyethylene base resin, 22-30 parts of metallocene polyethylene, and 1-3 parts of erucamide. The raw materials for the impact-resistant molding layer include: 60-70 parts of polypropylene base resin, 15-25 parts of cyclic olefin copolymer, and 10-15 parts of polyolefin elastomer; the raw materials for the adhesive base layer include: 70-80 parts of second polyethylene base resin and 20-30 parts of maleic anhydride-grafted polyolefin; the impact-resistant molding layer has a micro / nano-scale fiber structure arranged along the longitudinal direction of the film; the micro / nano-scale fiber structure is a continuous fibrous structure formed by the cyclic olefin copolymer as a rigid dispersed phase distributed in the polypropylene base resin matrix; the outer surface of the printed composite layer is a frosted surface with a micro / nano-uneven structure; the outer surface of the adhesive base layer is a smooth surface. The diameter of the micro-nano-scale fiber-forming structure is 100-500 nm; The unidirectional easy-tear film is a longitudinally easy-tear film; The preparation process of the unidirectional easy-tear film includes the following steps: Raw material pretreatment: The raw materials for the printed composite layer, the impact-resistant molding layer and the adhesive base layer are respectively fed into a high-speed mixer for high-speed mixing; Three-layer co-extrusion: The three layers of raw materials are heated and melted independently, combined by a distributor, and then sent to the co-extrusion die. They are extruded under the shear stress of the flow channel of the co-extrusion die. After air gap stretching at a melt stretch ratio of 15-25, they enter a pressure cooling system composed of a mirror casting roller and a silicone roller with micro-nano structures on its surface for rapid cooling and shaping. The printed composite layer is in contact with the silicone roller with micro-nano structures, and the adhesive base layer is in contact with the mirror casting roller. Traction and secondary orientation: After rapid cooling and shaping, the film enters the traction roller group and is longitudinally tractioned under a traction tension of 25-45 N / m; Surface activation and winding: The surface of the printed composite layer is subjected to corona treatment, and after edge trimming, thickness measurement feedback adjustment, it is wound up to obtain a unidirectional easy-tear film; Cooling water at 20-25°C is introduced into the pressure cooling system to reduce the melt temperature below the glass transition temperature of the cyclic olefin copolymer.

2. The unidirectional easy-tear film according to claim 1, characterized in that, In the raw material pretreatment step, the high-speed mixing temperature is 90-100℃, the rotation speed is 700-800 r / min, and the time is 12-15 min.

3. The unidirectional easy-tear film according to claim 1, characterized in that, In the three-layer co-extrusion step, the heating and melting extrusion temperature of the printing composite layer material is 225-230℃, the heating and melting extrusion temperature of the impact-resistant molding layer material is 230-235℃, and the heating and melting extrusion temperature of the adhesive base layer material is 225-230℃.

4. The unidirectional easy-tear film according to claim 1, characterized in that, In the surface activation and winding steps, the voltage of the corona treatment is 10-30kV.

5. The application of the unidirectional easy-tear film as described in claim 1 in a label, characterized in that, The one-way easy-tear film is used to prepare anti-counterfeiting labels, express delivery waybills, or easy-tear food labels.

Citation Information

Patent Citations

  • Longitudinal oriented film for tearing and laminate thereof

    CN119300982A

  • Fluid substance packaging sheet and preparation method thereof

    CN120735440A