Functional polymers with cage-like conformations and their preparation methods, functional polymer coatings and their preparation methods

By preparing a triblock polymer coating with a cage-like conformation, the problems of anti-biocontamination and lubrication performance on the material surface were solved, achieving the effects of reducing pollutant adsorption and improving lubrication performance.

CN122726416BActive Publication Date: 2026-11-17EAST CHINA UNIV OF SCI & TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611200206.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-08-10
Publication Date
2026-11-17
Estimated Expiration
2046-08-10

AI Technical Summary

Technical Problem

Existing technologies are insufficient to effectively improve the resistance to biofouling and lubrication properties of material surfaces, especially in terms of the non-specific adsorption of pollutants such as proteins and bacteria.

Method used

A coating is prepared by using a triblock polymer with a cage-like conformation and forming a unique three-dimensional topological structure through multi-arm polyethylene glycol to reduce contaminant adsorption and improve lubrication performance.

Benefits of technology

It significantly reduces the adsorption of contaminants such as proteins and bacteria on the material surface, increases the stability of the material in use, and significantly improves lubrication performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122726416B_ABST
    Figure CN122726416B_ABST
Patent Text Reader

Abstract

This application belongs to the field of functional polymer materials technology, and discloses a functional polymer with a cage-like conformation and its preparation method, as well as a functional polymer coating and its preparation method. The functional polymer is a triblock polymer, and in its structural formula, n ranges from 20 to 450; x ranges from 5 to 40; y ranges from 5 to 100; and z ranges from 5 to 40. The coating prepared from the functional polymer provided in this application can improve the surface resistance to biofouling, reduce the non-specific adsorption of contaminants such as proteins and bacteria on the surface, increase the stability of the material in use, and significantly improve lubrication performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of polymer materials technology, specifically to a functional polymer with a cage-like conformation and its preparation method, as well as a functional polymer coating and its preparation method. Background Technology

[0002] In nature, the superhydrophobic surface of lotus leaves, the antifouling texture of shark skin, and the bottle-brush structure of lubricant (LUB) in mammalian synovial fluid all demonstrate the crucial role of surface chemistry in achieving efficient surface protection. Inspired by these biological systems, researchers have effectively improved the anti-protein adsorption, low friction, and long-lasting lubrication properties of material surfaces by precisely controlling surface conformation. Currently, precise design strategies of surface chemistry have shown significant application potential in many fields, including marine antifouling, energy conversion systems, drug delivery, implantable medical devices, and advanced robotic devices capable of operating in complex environments, gaining widespread attention from the academic community. However, further molecular structure design is still needed to more effectively improve the antifouling capabilities of material surfaces. Summary of the Invention

[0003] Based on this, this application provides a functional polymer with a cage-like conformation that can reduce the non-specific adsorption of contaminants such as proteins and bacteria on the material surface, improve the material surface's resistance to biofouling, increase the material's stability in use, and also significantly increase lubrication performance.

[0004] A functional polymer having a cage-like conformation, wherein the functional polymer has a structural formula of either structural formula (I) or structural formula (II):

[0005] (I)

[0006] (II) In structural formulas (I) and (II), the value of n ranges from 20 to 450. The functional polymer is a triblock polymer, with x ranging from 5 to 40, y ranging from 5 to 100, and z ranging from 5 to 40.

[0007] In the triblock polymer provided in this application, the middle block is formed into a cage-like conformation by multi-arm polyethylene glycol. The cage has a unique three-dimensional topological structure and has a cavity of a defined size inside. The size of the cavity inside the cage can be precisely controlled by adjusting the degree of polymerization n.

[0008] By preparing a coating on the surface of a substrate using the functional polymer provided in this application, the lubrication performance of the substrate surface can be significantly improved, and the adsorption of contaminants such as proteins and bacteria can be effectively reduced.

[0009] Several alternative methods are provided below, but they are not intended as additional limitations on the overall solution above. They are merely further additions or optimizations. Provided there are no technical or logical contradictions, each alternative method can be combined individually with respect to the overall solution above, or multiple alternative methods can be combined with each other.

[0010] Optionally, in structural formulas (I) and (II), the value of n ranges from 100 to 250. The value of x ranges from 5 to 20, the value of y ranges from 5 to 50, and the value of z ranges from 5 to 20.

[0011] This application also provides a method for preparing the aforementioned functional polymer with a cage-like conformation, comprising: Step 1: Using dichloromethane as solvent, N,N'-dicyclohexylcarbodiimide as condensing agent, and 4-dimethylaminopyridine as catalyst, an externally-5-norbornene carboxylic acid and multi-arm terminal hydroxyl polyethylene glycol are reacted to prepare terminally functionalized macromonomers. The multi-arm terminal hydroxyl polyethylene glycol is 3-arm-PEG-OH or 4-arm-PEG-OH. Step 2: Under the catalysis of Grubbs third-generation catalyst, anchored monomer blocks with a degree of polymerization x are prepared using anchored monomers. Step 3: Add the terminal-functionalized macromonomer to the product of Step 2, and connect the terminal-functionalized macromonomer block with a degree of polymerization of y to the anchoring monomer block with a degree of polymerization of x. Step 4: Add the anchoring monomer to the product of step 3 to quaternize the reaction product and obtain the functional polymer. The structural formula of the anchoring monomer is as follows: .

[0012] For the functional polymer with structural formula (Ⅰ), the reaction equation for step 1 is as follows:

[0013] For the functional polymer with structural formula (Ⅱ), the reaction equation for step 1 is as follows:

[0014] In step 1, the molar ratio of exo-5-norborneolene carboxylic acid to the hydroxyl groups of multi-arm terminal hydroxyl polyethylene glycol is 2~5:1.

[0015] In step 1, the ratio of exo-5-norborneolene carboxylic acid, N,N'-dicyclohexylcarbodiimide, 4-dimethylaminopyridine, and dichloromethane is 1 mmol: 1~2 mmol: 0.05~0.15 mmol: 70~90 mL.

[0016] Step 1 is carried out under a nitrogen atmosphere at room temperature for 8–16 hours. In Step 1, exo-5-norbornenic acid, multi-arm terminal hydroxyl polyethylene glycol, 4-dimethylaminopyridine, and dichloromethane are stirred and mixed evenly in an ice-water bath. N,N'-dicyclohexylcarbodiimide is dissolved in a small amount of dichloromethane and slowly added dropwise to the reaction system.

[0017] In steps 2 and 4, anchoring monomers are introduced respectively. The anchoring monomer introduced in step 2 forms an anchoring monomer block with a degree of polymerization of x, and the anchoring monomer introduced in step 4 forms an anchoring monomer block with a degree of polymerization of z.

[0018] In steps 2 and 4, the amount of anchored monomer is A mmol each. In step 3, the amount of terminal-functionalized macromonomer is B mmol. The ratio of A to B ranges from 1:1 to 2.5.

[0019] Optionally, in step 2, the amount of Grubbs third-generation catalyst used is C mmol, and the A:C ratio ranges from 5 to 40:1. More preferably, the A:C ratio ranges from 5 to 20:1.

[0020] Steps 2 through 4 are all carried out in a nitrogen atmosphere at room temperature. The reaction time for step 2 is 1 to 3 hours, the reaction time for step 3 is 3 to 5 hours, and the reaction time for step 4 is 1 to 3 hours.

[0021] In steps 2, 3, and 4, dichloromethane was used as the solvent, with an amount of dichloromethane of D mL. The ratio of A to D ranged from 0.035 mmol to 100-130 mL.

[0022] Optionally, the quaternization includes reacting the reaction product with bromoethane.

[0023] The quaternization process mainly causes the anchoring monomer to form quaternary ammonium cations, which generate electrostatic interactions with the substrate surface and bind more stably to the substrate surface.

[0024] The quaternization process uses tetrahydrofuran as a solvent, and the ratio of the reaction product of the anchoring monomer and the terminal-functionalized macromonomer, bromoethane, and tetrahydrofuran is 20 mg: 0.01~0.10 mmol: 3~10 mL.

[0025] During the quaternization process, the mixing of the reaction product with bromoethane is carried out in an ice-water bath, and the reaction is conducted at room temperature for 8 to 24 hours.

[0026] The reaction equation for preparing triblock functionalized polymers from end-functionalized macromonomers obtained from 3-arm-PEG-OH is as follows:

[0027] The reaction equation for preparing triblock functionalized polymers from end-functionalized macromonomers obtained from 4-arm-PEG-OH is as follows:

[0028] Optionally, the method for preparing the anchoring monomer includes: preparing the anchoring monomer by reacting cis-5-norbornene-extrin-2,3-dicarboxylic anhydride and N,N-dimethylethylenediamine. The reaction equation is as follows:

[0029] The molar ratio of cis-5-norbornene-exo-2,3-dicarboxylic anhydride and N,N-dimethylethylenediamine is 1:1.3~1.6.

[0030] The anchoring monomer was obtained by mixing and stirring cis-5-norbornene-ex-2,3-dicarboxylic anhydride, N,N-dimethylethylenediamine, and toluene until homogeneous, and then refluxing at 120-150°C for 5-8 hours. The ratio of cis-5-norbornene-ex-2,3-dicarboxylic anhydride to toluene was 1 mmol: 4-6 mL.

[0031] This application also provides a method for preparing a functional polymer coating, comprising the following steps: (1) Dissolve the functional polymer with the cage conformation in tetrahydrofuran to obtain a functional polymer solution; (2) Immerse the substrate in the functional polymer solution for 0.3 to 1 hour to form the functional polymer coating on the substrate surface.

[0032] This application also provides a functional polymer coating, which is prepared using the method described above.

[0033] The coating prepared by the functional polymer provided in this application can improve the resistance of material surface to biofouling, reduce the non-specific adsorption of pollutants such as proteins and bacteria on the material surface, increase the stability of the material in use, and also significantly increase lubrication performance. Attached Figure Description

[0034] Figure 1 It is the anchoring monomer in Embodiment 1 of this application. 1 H NMR spectrum; Figure 2 It is the terminal-functionalized macromonomer NB-3arm-PEG in Example 1 of this application. 1 H NMR spectrum; Figure 3 It is DM-cage3-GPEG in Example 1 of this application. 1 H NMR spectrum; Figure 4 It is the DM-line-GPEG in Comparative Example 1 of this application. 1 H NMR spectrum; Figure 5 It is the DM-loop-GPEG in Comparative Example 2 of this application. 1 H NMR spectrum; Figure 6 It is DM-cage4-GPEG in Example 3 of this application. 1 H NMR spectrum; Figure 7 These are AFM spectra of polymer coatings prepared in different application examples of this application, where (a) is the functional polymer coating prepared in application example 2, (b) is the functional polymer coating prepared in application example 3, (c) is the functional polymer coating prepared in application example 1, (d) is the functional polymer coating prepared in application example 4, (e) is the functional polymer coating prepared in application example 5, and (f) is the functional polymer coating prepared in application example 6. Figure 8 This is a comparison diagram of the water contact angles of polymer coatings prepared in different application examples of this application; Figure 9 This is a comparison chart of the friction coefficients of polymer coatings prepared in different application examples of this application; Figure 10 These are the anti-bovine serum albumin QCM-D curves of polymer coatings prepared in different application examples of this application. Detailed Implementation

[0035] The technical solution of this application will be described in detail below with reference to specific embodiments.

[0036] Example 1 A method for preparing a functional polymer with a cage-like conformation includes the following steps: (1) Synthetic anchoring monomer Add cis-5-norbornene-extrin-2,3-dicarboxylic anhydride (1.59 g, 9.9 mmol), N,N-dimethylethylenediamine (1.28 g, 14.5 mmol), and toluene (50 mL) to a 100 mL round-bottom flask with a pre-stirred rod. Then, install a Dean-Stark water separator and a spherical condenser on the flask, ensuring the apparatus is airtight. Slowly heat the round-bottom flask to 130 °C and reflux for 6 hours. After the reaction is complete, remove the heating element and allow it to cool to room temperature. Concentrate the reaction solution by rotary evaporation to remove the solvent. Dissolve the remaining solid in ethyl acetate (50 mL). Transfer the organic phase to a separatory funnel and wash twice with 50 mL of saturated sodium bicarbonate aqueous solution. Add anhydrous magnesium sulfate to the collected organic phase until the anhydrous magnesium sulfate is loose and does not clump. Dry overnight. The solid was removed by filtration, and the filtrate was concentrated by rotary evaporation to obtain 1.8 g of colorless oily product, namely the anchoring monomer (NB-N(Me)2) (7.7 mmol), with a yield of 77.8%. The anchoring monomer... 1 See the H NMR spectrum. Figure 1 As shown.

[0037] (2) Synthesis of terminal-functionalized macromonomers Under a nitrogen atmosphere, exo-5-norbornene carboxylic acid (0.33 g, 2.4 mmol), 3-arm-PEG-OH (Mn, SEC = 5000 g / mol, 1 g, 0.2 mmol, 0.6 mmol hydroxyl group), 4-dimethylaminopyridine (DMAP, 29.32 mg, 0.24 mmol), and 200 mL of ultra-dry dichloromethane were added to a 250 mL three-necked flask with a pre-stirred stir bar (prepared by vacuum heating twice before use). The reaction flask was placed in an ice-water bath to cool and stirred for 30 minutes to mix thoroughly. A small amount of N,N'-dicyclohexylcarbodiimide (DCC, 742.8 mg, 3.6 mmol) dissolved in DCM was added to a constant pressure dropping funnel using a syringe. The mixture was stirred in an ice-water bath for 1 h, and then stirred at room temperature for 12 h after removing the ice-water bath. The solution was filtered, the filtrate was concentrated by rotary evaporation, precipitated three times in diethyl ether cooled in an ice-salt bath, and dried to constant weight in a vacuum oven to give 1.2 g of a white solid product, namely the terminal-functionalized macromonomer NB-3arm-PEG. Its NMR spectrum is shown below. Figure 2 As shown.

[0038] (3) Synthetic functional polymers In a glove box under a nitrogen atmosphere, add the anchoring monomer (NB-N(Me)2) (8.3 mg, 0.035 mmol) to a 250 mL round-bottom flask with a pre-stirred piece. Add 20 mL of ultra-dry dichloromethane (DCM) using a syringe and stir at room temperature. Dissolve the Grubbs third-generation catalyst (3 mg, 0.0034 mmol) in 1 mL of ultra-dry DCM and slowly add it dropwise to the round-bottom flask. Stir at room temperature for 2 hours. Add NB-3arm-PEG5000 (180 mg, 0.035 mmol) and 100 mL of ultra-dry DCM to the resulting mixture and stir at room temperature for 4 hours.

[0039] To the reaction mixture, the anchoring monomer (NB-N(Me)2) (8.3 mg, 0.035 mmol) and 20 mL of ultra-dry DCM were added, and the mixture was stirred at room temperature for 2 hours. The reaction was quenched by adding 5 mL of vinyl ether, and the reaction solution was concentrated by rotary evaporation. Precipitation was performed three times in ether cooled in an ice-salt bath, and the product was dried to constant weight in a vacuum oven to obtain 152 mg of solid product DM-cage3-GPEG. The NMR characterization spectrum is shown below. Figure 3 As shown.

[0040] (4) Quaternization process Add 20 mg of the solid product and 5 mL of tetrahydrofuran to a 25 mL round-bottom flask with a pre-stirred paddle, and stir in an ice-water bath for 30 minutes until fully dissolved. Add 2.92 mg of bromoethane (0.027 mmol) to the reaction solution using a syringe, stir in an ice-water bath for 30 minutes, then remove the ice-water bath and stir overnight at room temperature. Concentrate the reaction solution by rotary evaporation, precipitate three times in diethyl ether cooled in an ice-salt bath, and dry to constant weight in a vacuum oven to obtain 15 mg of the solid product, namely the functional polymer cage3-GPEG5000.

[0041] Examples 2-4 Examples 2-4 were prepared using the same method as Example 1, except that the type of multi-armed hydroxyl-terminated polyethylene glycol was different. The multi-armed hydroxyl-terminated polyethylene glycol was fed in equimolar amounts as in Example 1, while the other substances and their amounts were the same as in Example 1.

[0042] Comparative Examples 1 and 2 Comparative Examples 1 and 2 were prepared using the same method as Example 1, except that the type of multi-armed hydroxyl-terminated polyethylene glycol was different. The multi-armed hydroxyl-terminated polyethylene glycol was fed in equimolar amounts as in Example 1, while the other substances and their amounts were the same as in Example 1.

[0043] Comparative Examples 1, 2, and 3: The products of the synthesized functional polymers, but not yet subjected to quaternization, were named DM-line-GPEG, DM-loop-GPEG, and DM-cage4-GPEG, respectively. Their NMR spectra are shown in [reference needed]. Figures 4-6 As shown.

[0044] Table 1

[0045] Application Example 1 A method for preparing a functional polymer coating includes the following steps: (1) The silicon wafer was cleaned with piranha solution and treated with plasma; (2) The functional polymer cage3-GPEG5000 prepared in Example 1 was dissolved in tetrahydrofuran (THF) to prepare a functional polymer solution of 100 µg / mL; (3) Soak the silicon wafer from step (1) in the functional polymer solution for 20 minutes, and clean it with a large amount of ethanol to obtain a functional polymer coating on the surface of the silicon wafer.

[0046] Application Examples 2-6 The functional polymers prepared in Comparative Examples 1 and 2, and Examples 2-4 were used to prepare functional polymer coatings in the same way as in Application Example 1.

[0047] The correspondence between application examples and implementation examples is shown in Table 2.

[0048] Table 2

[0049] Performance Characterization As in Example 1 ( Figure 3 Comparative Example 1 Figure 4 Comparative Example 2 Figure 5 Example 3 Figure 6 The NMR spectrum of the PEG showed that the characteristic peaks of the hydrogen atoms in the norbornene double bond at δ=6.60 and 6.13 ppm completely disappeared. At the same time, two characteristic peaks of vinylidene after the ring opening of the norbornene double bond appeared at δ=5.05-6.10 ppm. This indicates that the block polymer has completely reacted during the polymerization time. The peak at δ=4.25 ppm is attributed to the signal peak of the methylene group connected to the two ester groups in the PEG structure, further proving that the functional polymer was successfully prepared.

[0050] See Figure 7 As shown in the AFM morphology diagram, the surface of each functional polymer coating is relatively continuous overall, and no obvious large-scale agglomeration or phase separation phenomenon was observed, indicating that the polymer can cover the substrate surface relatively uniformly.

[0051] See Figure 8 As shown, with the increase of the number of arms and the degree of polymerization n in multi-arm terminal hydroxyl polyethylene glycol, the water contact angle gradually decreases, and the surface modified by the functional polymer has good wetting properties.

[0052] See Figure 9 As shown, with the increase of the number of arms and the degree of polymerization n in multi-arm terminal hydroxyl polyethylene glycol, the coefficient of friction gradually decreases, and the surface modified by the functional polymer has good lubrication properties.

[0053] The QCM-D frequency variation curves of the different functional polymer coatings prepared in Examples 1-6 in 30 mg / mL BSA (bovine serum albumin) solution are shown in the figure. Figure 10 As shown, the frequency of the blank silica substrate decreased significantly after BSA adsorption, indicating that BSA readily undergoes non-specific adsorption on the unmodified silicon wafer surface. In contrast, the surface frequency change amplitude was significantly reduced after functional polymer modification, indicating that the functional polymer coating can effectively reduce the direct contact between BSA and the substrate, thereby reducing protein adsorption.

[0054] It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of this application, and these all fall within the scope of protection of this application. Therefore, the scope of protection of this patent application shall be determined by the appended claims.

Claims

1. A functional polymer having a cage-like conformation, wherein the functional polymer has a structural formula of either structural formula (I) or structural formula (II): (Ⅰ) (Ⅱ) In structural formulas (I) and (II), the value of n ranges from 20 to 450. The functional polymer is a triblock polymer, with x ranging from 5 to 40, y ranging from 5 to 100, and z ranging from 5 to 40.

2. A method for preparing a functional polymer with a cage-like conformation as described in claim 1, characterized in that, include: Step 1: Using dichloromethane as solvent, N,N'-dicyclohexylcarbodiimide as condensing agent, and 4-dimethylaminopyridine as catalyst, an externally-5-norbornene carboxylic acid and multi-arm terminal hydroxyl polyethylene glycol are reacted to prepare terminally functionalized macromonomers. The multi-arm terminal hydroxyl polyethylene glycol is 3-arm-PEG-OH or 4-arm-PEG-OH. Step 2: Under the catalysis of Grubbs third-generation catalyst, anchored monomer blocks with a degree of polymerization x are prepared by anchoring monomers. Step 3: Add the terminal-functionalized macromonomer to the product of Step 2, and connect the terminal-functionalized macromonomer block with a degree of polymerization of y to the anchoring monomer block with a degree of polymerization of x. Step 4: Add the anchoring monomer to the product of Step 3 to quaternize the reaction product and obtain the functional polymer. The structural formula of the anchoring monomer is as follows: 。 3. The method for preparing the functional polymer with a cage-like conformation as described in claim 2, characterized in that, In step 1, the molar ratio of exo-5-norborneolene carboxylic acid to the hydroxyl groups of multi-arm terminal hydroxyl polyethylene glycol is 2~5:

1.

4. The method for preparing the functional polymer with a cage-like conformation as described in claim 2, characterized in that, Step 1 involves reacting under a nitrogen atmosphere at room temperature for 8-16 hours.

5. The method for preparing the functional polymer with a cage-like conformation as described in claim 2, characterized in that, In steps 2 and 4, the amount of anchored monomer is A mmol each. In step 3, the amount of terminal-functionalized macromonomer is B mmol. The ratio of A to B ranges from 1:1 to 2.

5.

6. The method for preparing the functional polymer with a cage-like conformation as described in claim 5, characterized in that, In step 2, the amount of Grubbs third-generation catalyst used is C mmol, and the A:C ratio ranges from 5 to 40:

1.

7. The method for preparing the functional polymer with a cage-like conformation as described in claim 2, characterized in that, The quaternization includes reacting the reaction product with bromoethane.

8. The method for preparing the functional polymer with a cage-like conformation as described in claim 3, characterized in that, The reactions in steps 2 through 4 were all carried out under a nitrogen atmosphere at room temperature. The reaction time for step 2 was 1 to 3 hours, the reaction time for step 3 was 3 to 5 hours, and the reaction time for step 4 was 1 to 3 hours.

9. A method for preparing a functional polymer coating, characterized in that, Includes the following steps: (1) Dissolve the functional polymer with cage conformation as described in claim 1 in tetrahydrofuran to obtain a functional polymer solution; (2) Immerse the substrate in the functional polymer solution for 0.3 to 1 hour to form the functional polymer coating on the substrate surface.

10. A functional polymer coating, characterized in that, It was prepared using the method for preparing the functional polymer coating as described in claim 9.

Citation Information

Patent Citations

  • Surface modification method for reducing protein nonspecific adsorption on micro-nano particle surface

    CN106947105A