Preparation methods of basic composite oxides, the prepared basic composite oxides and their applications
By optimizing the preparation method of aluminum-calcium composite oxides and combining hydrothermal treatment and calcination steps, the problems of high energy consumption and insufficient strength and specific surface area were solved, and alkaline composite oxides with high strength and large specific surface area were prepared for application in the fields of catalyst support and heat-resistant filler.
Patent Information
- Application Number
- CN202510583863.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-07
- Publication Date
- 2026-11-10
AI Technical Summary
In the existing technology, the preparation process of alkaline composite oxides is energy-intensive, and the products obtained cannot have both high strength and high specific surface area.
By molding a mixture containing aluminum-calcium composite oxide, alumina precursor, calcium oxide precursor, carbon material and lanthanide oxide precursor, followed by hydrothermal treatment and calcination, the preparation conditions are optimized to obtain an alkaline composite oxide with high mechanical strength and large specific surface area.
The preparation process is simple, the raw materials are readily available, and the resulting alkaline composite oxide has a large specific surface area and high mechanical strength, making it suitable for catalyst supports and heat-resistant fillers.
Smart Images

Figure CN123059637A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of catalyst supports, specifically to a method for preparing an alkaline composite oxide, the prepared alkaline composite oxide, and its applications. Background Technology
[0002] Calcium aluminate, as a special hydraulic material, has long been known and widely used in the production of high-performance (low water content, low cement content) refractory castables.
[0003] Typically, pure calcium aluminate refractory cement is a cementitious material made by mixing industrial alumina powder and high-quality limestone in a certain proportion, crushing and grinding them, pressing them into rough blanks, calcining them at high temperatures, and then crushing and grinding them again. Its main mineral components are monocalcium aluminate (CA2), monocalcium aluminate (CA), monocalcium hexaaluminate (CA6), and α-alumina (α-Al2O3). Due to the high Al2O3 content in calcium aluminate cement, the content of calcium and impurities is correspondingly reduced, resulting in a refractoriness of over 1690℃. Refractory castables prepared with pure calcium aluminate refractory cement have excellent high-temperature performance, including high refractoriness, good thermal shock resistance, and good resistance to slag erosion. They are suitable for refractory linings and refractory furnace materials in high-temperature kilns and thermal equipment in the cement, chemical, and metallurgical industries. Compared with refractory bricks, refractory castables prepared with it have advantages such as simple manufacturing process and convenient construction, making them suitable for on-site construction in any location and shape. Large precast products can also be made to meet various application needs.
[0004] The main chemical components of calcium aluminate are α-alumina and CaO. In the CaO-Al₂O₃ binary system, C₃A and C₂O are present. 12 Five compounds, A7, CA, CA2, and CA6, are involved. Conventionally synthesized calcium aluminate materials typically contain multiple crystalline phases and have low specific surface area and strength. For example, the literature (Yang Qing. Preparation of pure calcium aluminate special cement by sintering method [J]. Cement, 1992(9):27-28) reports that the synthesized calcium aluminate special cement contains approximately 73% CA2 and 27% CA, with a specific surface area of approximately 0.6 m². 2 / g.
[0005] As mentioned above, calcium aluminate, as a special high-temperature resistant material, has been widely used and attracted attention in the cement, ceramics and metallurgical industries. In addition, it can also be used as an alkaline catalyst and support material (①Wang Sihan, Zhang Yujian. Research status of hydrogen production technology by steam reforming of natural gas[J]. Industrial Catalysis, 2016, 24(4):26-30; ②Wang Rongbin. Calcium aluminate catalytic heavy oil cracking-gasification process[J]. Acta Petrolei Sinica (Petroleum Processing), 2021, 37(2):384-390). As a catalyst support for the conversion of natural gas into syngas, calcium aluminate has been applied in industry (①Huang Zhongtao. Handbook of Industrial Catalysts[M]. Chemical Industry Press, 2004, p676; ②Shen Wenjie. Industrial application of CN-20 type catalyst[J]. Natural Gas Chemical Industry, 2002, 27(1):19-25).
[0006] For catalytic materials, the strength and specific surface area of different materials have a significant impact on their performance. Most calcium aluminate materials reported in the literature have small specific surface areas and low strength. How to synthesize calcium aluminate materials that have both high mechanical strength and high specific surface area is the problem that this invention focuses on solving. Summary of the Invention
[0007] The purpose of this invention is to overcome the problems of high energy consumption in the preparation process of alkaline composite oxides in the prior art, and the inability of the prepared products to have both high strength and high specific surface area. This invention provides a method for preparing alkaline composite oxides, the alkaline composite oxides obtained therefrom, and their applications. The raw materials for this method are readily available, the preparation steps are simple, and the alkaline composite oxides obtained have good mechanical properties and water absorption.
[0008] To achieve the above objectives, the first aspect of the present invention provides a method for preparing an alkaline composite oxide, wherein the preparation method includes the following steps:
[0009] (1) A mixture containing aluminum-calcium composite oxide, aluminum oxide precursor, calcium oxide precursor, carbon material and lanthanide oxide precursor is shaped to obtain a solid product;
[0010] (2) The solid product from step (1) is subjected to hydrothermal treatment and first calcination.
[0011] Preferably, the aluminum-calcium composite oxide is prepared by the following method:
[0012] (a) Mix the alumina source, calcium oxide source and solvent, grind and dry;
[0013] (b) The dried product from step (a) is subjected to a second calcination.
[0014] Preferably, the alumina source is selected from at least one of hydrated alumina, transition phase alumina, and inert α-alumina, and is preferably hydrated alumina.
[0015] Preferably, the calcium oxide source is selected from at least one of calcium hydroxide, calcium oxide, and calcium carbonate, and is preferably calcium carbonate.
[0016] Preferably, the amount of alumina source used is such that the alumina content in the aluminum-calcium composite oxide is 60-72 wt%, more preferably 63-70 wt%.
[0017] Preferably, the amount of calcium oxide source used is such that the calcium oxide content in the aluminum-calcium composite oxide is 28-40 wt%, more preferably 30-37 wt%.
[0018] Preferably, the solvent is selected from at least one of water, ethanol, and acetone.
[0019] Preferably, the amount of solvent used is 0-200 wt% of the total mass of the alumina source and the calcium oxide source, and more preferably 20-100 wt%.
[0020] Preferably, in step (a), the alumina source and calcium oxide source particles are ground to a D50 ≤ 30 μm, more preferably D50 ≤ 20 μm, and even more preferably D50 ≤ 15 μm.
[0021] Preferably, in step (b), the conditions for the second calcination include: a calcination temperature of 1200-1420℃, more preferably 1250-1400℃; and a calcination time of 1-8h, more preferably 2-6h.
[0022] Preferably, in step (1), the amount of the aluminum-calcium composite oxide used is 1-10 wt% of the solid product of step (1), preferably 2-6 wt%.
[0023] Preferably, the alumina precursor is selected from at least one of hydrated alumina, transition phase alumina, and inert α-alumina, and is preferably hydrated alumina.
[0024] Preferably, the calcium oxide precursor is selected from at least one of calcium hydroxide, calcium oxide, and calcium carbonate, and is preferably calcium carbonate.
[0025] Preferably, the amount of the calcium oxide precursor used is 8-20 wt% of the solid product of step (1), more preferably 10-15 wt%.
[0026] Preferably, the amount of the alumina precursor used is 78-90 wt% of the solid product of step (1), more preferably 80-86 wt%.
[0027] Preferably, the carbon material is selected from at least one of starch, graphite, coke, stearic acid and stearate, more preferably from at least one of stearate, graphite and coke, and even more preferably from graphite.
[0028] Preferably, the amount of carbon material used is 0.3-10 wt% of the solid product of step (1), more preferably 0.5-6 wt%, and more preferably 0.8-5 wt%.
[0029] Preferably, the lanthanide oxide precursor is selected from at least one of lanthanide metal hydroxides, oxides, and carbonates.
[0030] Preferably, the lanthanide metal is selected from at least one of lanthanum, cerium, praseodymium, neodymium, samarium, and dysprosium.
[0031] Preferably, the lanthanide oxide precursor is selected from at least one of lanthanum hydroxide, lanthanum oxide, lanthanum carbonate, cerium hydroxide, cerium oxide, cerium carbonate, praseodymium hydroxide, and praseodymium oxide.
[0032] Preferably, the amount of the lanthanide oxide precursor used is 0.5-5 wt% of the solid product of step (1), and more preferably 0.8-4 wt%.
[0033] Preferably, the conditions for the hydrothermal treatment include: a hydrothermal temperature of 160-240℃, more preferably 180-230℃; and a hydrothermal time of 2-40h, more preferably 6-30h.
[0034] Preferably, the first calcination conditions include: under an oxygen-containing atmosphere, a calcination temperature of 1250-1500℃, more preferably 1280-1450℃; and a calcination time of 1-8h, more preferably 2-6h.
[0035] Preferably, the heating rate of the first calcination is 50-200℃ / h, and more preferably 80-170℃ / h.
[0036] The second aspect of this invention provides an alkaline composite oxide prepared by the preparation method described in the first aspect.
[0037] The third aspect of this invention provides the application of the alkaline composite oxide prepared by the preparation method described in the first aspect or the alkaline composite oxide described in the second aspect in the field of catalyst support or heat-resistant filler.
[0038] The beneficial effects achieved through the above technical solution are as follows:
[0039] In this invention, the preparation method of alkaline composite oxide is simple, the raw materials are easy to obtain, the preparation conditions are controllable, and the obtained alkaline composite oxide has a large specific surface area and high mechanical strength. Attached Figure Description
[0040] Figure 1 This is the XRD diffraction pattern of the basic composite oxide of Example 1;
[0041] Figure 2This is the XRD diffraction pattern of the basic composite oxide in Example 2;
[0042] Figure 3 This is the XRD diffraction pattern of the basic composite oxide in Comparative Example 2. Detailed Implementation
[0043] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
[0044] The first aspect of this invention provides a method for preparing an alkaline composite oxide, wherein the preparation method includes the following steps:
[0045] (1) A mixture containing aluminum-calcium composite oxide, aluminum oxide precursor, calcium oxide precursor, carbon material and lanthanide oxide precursor is shaped to obtain a solid product;
[0046] (2) The solid product from step (1) is subjected to hydrothermal treatment and first calcination.
[0047] In this invention, the preparation method of alkaline composite oxide is simple, the raw materials are easy to obtain, the preparation conditions are controllable, and the obtained alkaline composite oxide has a large specific surface area and high mechanical strength.
[0048] According to the present invention, preferably, the aluminum-calcium composite oxide is prepared by the following method:
[0049] (a) Mix the alumina source, calcium oxide source and optionally a solvent, grind and dry;
[0050] (b) The dried product from step (a) is subjected to a second calcination.
[0051] According to the present invention, the type of alumina source is not particularly limited, and any material that has been conventionally calcined to obtain alumina is acceptable. Preferably, the alumina source is selected from at least one of hydrated alumina, transition phase alumina, and inert α-alumina, and is preferably hydrated alumina.
[0052] According to the present invention, the type of calcium oxide source is not particularly limited, and any substance that yields calcium oxide after calcination is conventional in the art. Preferably, the calcium oxide source is selected from at least one of calcium hydroxide, calcium oxide, and calcium carbonate, and is preferably calcium carbonate.
[0053] According to the present invention, preferably, the amount of alumina source added is such that the mass percentage of alumina in the aluminum-calcium composite oxide is 60-72 wt%, for example 60 wt%, 61 wt%, 62 wt%, 63 wt%, 64 wt%, 65 wt%, 66 wt%, 67 wt%, 68 wt%, 69 wt%, 70 wt%, 72 wt%, or any range between the two, preferably 63-70 wt%.
[0054] According to the present invention, preferably, the amount of calcium oxide source added is such that the mass percentage of calcium oxide in the aluminum-calcium composite oxide is 28-40 wt%, for example, 28 wt%, 29 wt%, 30 wt%, 31 wt%, 32 wt%, 33 wt%, 34 wt%, 35 wt%, 36 wt%, 37 wt%, 38 wt%, 39 wt%, 40 wt%, or any range between the two, preferably 30-37 wt%.
[0055] According to the present invention, the type of solvent is not particularly limited, and those skilled in the art can choose conventional organic and / or inorganic solvents. Preferably, the solvent is selected from at least one of water, ethanol and acetone.
[0056] According to the present invention, preferably, the amount of solvent added is 0-200 wt% of the total mass of the alumina source and the calcium oxide source, more preferably 20-100 wt%. In the present invention, adding solvent according to the above-mentioned mass can improve grinding efficiency and save energy and reduce consumption. In the present invention, unless otherwise specified, "optionally" means containing or not containing, adding or not adding, using or not using. Specifically, step (a) of the present invention may or may not involve adding solvent.
[0057] According to the present invention, preferably, in step (a), the grinding is carried out until the D50 of the alumina source and calcium oxide source particles is ≤20μm, and more preferably D50 is ≤15μm. In the present invention, the grinding method and grinding conditions in step (a) are not particularly limited, as long as the grinding product meets the above-mentioned particle size limitation. At least one of ball mills, colloid mills, and sand mills can be used, with ball milling being preferred as it simplifies operation.
[0058] In this invention, the drying method and drying conditions are not particularly limited. Those skilled in the art can choose conventional drying methods and drying conditions. Preferably, in step (a), the drying conditions include: a drying temperature of 50-110℃ and a drying time of 4-12h.
[0059] According to the present invention, preferably, in step (b), the conditions for the second calcination include: a calcination temperature of 1200-1420℃, more preferably 1250-1400℃; and a calcination time of 1-8h, more preferably 2-6h.
[0060] In this invention, preferably, in step (b), the second roasted product is crushed and ground until it can pass through a 200-mesh sieve, more preferably a 400-mesh sieve. In this invention, the term "mesh" has a conventional meaning in the art, referring to the number of openings per square inch of the sieve mesh; for example, 200 mesh means there are 200 openings per square inch of sieve mesh.
[0061] According to the present invention, preferably, in step (1), the amount of aluminum-calcium composite oxide added is 1-10 wt% of the solid product of step (1), preferably 2-6 wt%.
[0062] According to the present invention, the type of alumina precursor is not particularly limited, and it may be the same as or different from the alumina source. Preferably, the alumina precursor is selected from at least one of hydrated alumina, transition phase alumina, and inert α-alumina, and is preferably hydrated alumina.
[0063] According to the present invention, the type of calcium oxide precursor is not particularly limited, and it may be the same as or different from the calcium oxide source. Preferably, the calcium oxide precursor is selected from at least one of calcium hydroxide, calcium oxide, and calcium carbonate, and is preferably calcium carbonate.
[0064] According to the present invention, preferably, the amount of calcium oxide precursor added is 8-20 wt% of the solid product of step (1), more preferably 10-15 wt%.
[0065] According to the present invention, preferably, the amount of the alumina precursor added is 78-90 wt% of the solid product of step (1), more preferably 80-86 wt%.
[0066] According to the present invention, the type of carbon material is not particularly limited and can be any conventional carbon material in the art. Preferably, the carbon material is selected from at least one of starch, graphite, coke, stearic acid, and stearate, more preferably from at least one of stearate, graphite, and coke, and even more preferably from graphite. In the present invention, the addition of the above-mentioned carbon material can act as a release agent, and the removal of the carbon material after the first calcination does not affect the composition of the final product.
[0067] According to the present invention, preferably, the amount of carbon material added is 0.3-10 wt% of the solid product of step (1), more preferably 0.5-6 wt%, and more preferably 0.8-5 wt%.
[0068] According to the present invention, preferably, the lanthanide oxide precursor is selected from at least one of lanthanide metal hydroxides, oxides and carbonates.
[0069] According to the present invention, the type of lanthanide metal is not particularly limited, and is a conventional lanthanide metal element in the art. Preferably, the lanthanide metal is selected from at least one of lanthanum, cerium, praseodymium, neodymium, samarium, and dysprosium, and more preferably lanthanum.
[0070] More preferably, the lanthanide oxide precursor is selected from at least one of lanthanum hydroxide, lanthanum oxide, lanthanum carbonate, cerium hydroxide, cerium oxide, cerium carbonate, praseodymium hydroxide, and praseodymium oxide. In this invention, using the above-mentioned lanthanide oxide precursors to prepare basic composite oxides can improve the structural stability and crystal phase structure of the composite oxides.
[0071] According to the present invention, preferably, the amount of the lanthanide oxide precursor used is 0.5-5 wt% of the solid product of step (1), for example, 0.5 wt%, 0.6 wt%, 0.8 wt%, 1 wt%, 1.2 wt%, 1.5 wt%, 1.8 wt%, 2 wt%, 2.2 wt%, 2.5 wt%, 2.7 wt%, 3 wt%, 3.2 wt%, 3.5 wt%, 3.7 wt%, 4 wt%, 4.5 wt%, 5 wt%, or any range between the two, preferably 0.8-4 wt%.
[0072] In this invention, preferably, step (1) further includes a grinding step of the mixed product. The mixing and grinding conditions in step (1) are not particularly limited; it is sufficient to mix the components in step (1) until they are homogeneous. Preferably, the grinding is performed until the particle size distribution (D50) of the mixed product is ≤30 μm, and more preferably, D50 is ≤20 μm. D50 has a conventional interpretation in the art, referring to the particle size corresponding to a cumulative particle size distribution percentage of 50% of the sample, measured by a laser particle size analyzer.
[0073] In this invention, preferably, step (1) further includes a process of dry pressing and crushing the ground product before molding. Preferably, dry granulation is used, and the resulting product passes through a 16-mesh sieve, more preferably through a 20-200 mesh sieve. Using the above method can reduce manufacturing costs and improve production efficiency.
[0074] In this invention, the molding method is not particularly limited, and those skilled in the art can adapt it accordingly. Preferably, sheet forming is used, and the molded shape is not limited, selected from at least one of cylindrical, Raschig ring, honeycomb cylindrical, and four-hole cylindrical shapes. The diameter of the molded product is 5-30 mm, and the length is 4-20 mm.
[0075] According to the present invention, preferably, the conditions for the hydrothermal treatment include: a hydrothermal temperature of 160-240℃, for example 160℃, 170℃, 180℃, 190℃, 200℃, 210℃, 220℃, 230℃, 240℃, or any range between the two, preferably 180-230℃; and a hydrothermal time of 2-40h, for example 2h, 4h, 6h, 9h, 12h, 15h, 18h, 20h, 25h, 30h, 35h, 40h, or any range between the two, preferably 6-30h.
[0076] In this invention, the equipment used for hydrothermal treatment is not particularly limited; those skilled in the art can choose conventional hydrothermal treatment equipment, preferably performed in a hydrothermal reactor. In this invention, it is preferable to open the hydrothermal reactor after the hydrothermal treatment is completed, allowing it to cool down (preferably to room temperature). This preferred embodiment avoids the safety hazards that may arise when opening the reactor due to the self-generated pressure inside the reactor caused by hydrothermal treatment at high temperatures.
[0077] According to a preferred embodiment of the present invention, the hydrothermal treatment is carried out in a hydrothermal reactor. A certain amount of water is filled into the hydrothermal reactor, a stainless steel mesh is placed above the water surface, the sample is placed on the mesh (the sample does not contact the water), the lid of the hydrothermal reactor is tightened, and the hydrothermal treatment is carried out.
[0078] In this invention, preferably, the hydrothermal reaction product is dried before undergoing a first calcination. The drying conditions are not particularly limited, but are preferably 60-120℃ for 1-10 hours.
[0079] According to the present invention, preferably, the first calcination conditions include: calcination temperature of 1250-1500℃, preferably 1280-1450℃, under an air atmosphere; and calcination time of 1-8h, preferably 2-6h.
[0080] According to the present invention, preferably, the heating rate of the first calcination is 50-200℃ / h, more preferably 80-170℃ / h. In the present invention, performing the first calcination under the above conditions can reduce energy consumption, further improve the mechanical strength of the obtained alkaline composite oxide, and increase the water absorption rate and specific surface area of the alkaline composite oxide.
[0081] In this invention, the equipment for the first and second roasting is not particularly limited. Preferably, the first and second roasting can be carried out in a muffle furnace and / or a high-temperature electric furnace.
[0082] The second aspect of this invention provides an alkaline composite oxide prepared by the preparation method described in the first aspect.
[0083] According to the present invention, preferably, the specific surface area of the alkaline composite oxide is 1-6 m². 2 / g, for example, 1m 2 / g, 1.5m 2 / g, 1.8m 2 / g、2m 2 / g, 2.5m 2 / g、3m 2 / g, 3.5m 2 / g、4m 2 / g, 4.5m 2 / g、5m 2 / g, 5.5m 2 / g、6m 2 / g, or any range between the two, preferably 1.5-5m 2 / g, more preferably 2-4m 2 / g. In this invention, the method for determining the specific surface area of the alkaline composite oxide is as follows: the sample is pre-degassed under vacuum at 200℃ for 3 hours to remove adsorbed moisture and impurity gases. Then, the N2 adsorption-desorption isotherm of the sample is measured using a Micromeritics ASAP2460 physical adsorption instrument, and the specific surface area of the sample is calculated according to the BET equation.
[0084] According to the present invention, preferably, the lateral crushing strength of the alkaline composite oxide is 20-45 N / mm, for example, 20 N / mm, 22 N / mm, 24 N / mm, 26 N / mm, 28 N / mm, 30 N / mm, 32 N / mm, 35 N / mm, 37 N / mm, 40 N / mm, 43 N / mm, 45 N / mm, or any range between the two, preferably 25-40 N / mm. The method for determining the lateral crushing strength is as follows: select 20 samples, measure the thickness (in mm) of each sample, and then use a DLⅢ type intelligent particle strength meter to measure the lateral crushing strength of the sample. Divide the obtained strength value by the thickness and take the average value.
[0085] According to the present invention, preferably, the water absorption rate of the alkaline composite oxide is greater than or equal to 25%, for example 25%, 27%, 30%, 32%, 34%, 36%, 38%, 40%, or any range between the two, preferably 27-40%.
[0086] In this invention, the method for determining the water absorption rate is as follows: Weigh 2-5g of sample (sample mass denoted as m1) and place it in a 50mL beaker. Then add 50mL of deionized water to the beaker, place it on a digital display magnetic stirring hot plate, and maintain the temperature at 70℃ for 30min. Drain off excess water, weigh the mass of the wet sample using a balance (denoted as m2), and calculate the water absorption rate of the carrier according to the following formula: Water absorption rate = (m2-m1) / m1×100%.
[0087] In this invention, the XRD diffraction pattern of the prepared composite basic oxide was measured using Cu target Kα rays, with a measurement range of 10°-80° and a scanning step size of 2° / min. The XRD diffraction pattern showed diffraction peaks at 2θ of 25.4°, 34.1°, 36.2°, and 57.5°. The peak at 25.4° corresponds to calcium dialuminate, and the peaks at 34.1° and 36.2° correspond to calcium hexaaluminate. This indicates that the composite basic oxide mainly consists of calcium dialuminate and calcium hexaaluminate, as well as a small amount of α-alumina (57.5°).
[0088] In this invention, preferably, the alkaline composite oxide has a large specific surface area, high mechanical strength, and high water absorption rate.
[0089] The third aspect of this invention provides the application of the alkaline composite oxide prepared by the preparation method described in the first aspect or the alkaline composite oxide described in the second aspect in the field of catalyst support or heat-resistant filler.
[0090] According to the present invention, preferably, the alkaline composite oxide is used in the fields of catalyst support for hydrocarbon catalytic conversion, heavy oil pyrolysis-gasification coupled hydrogen production, and transesterification reactions, as well as in the field of heat-resistant packing materials. Preferably, the hydrocarbon catalytic conversion includes natural gas steam catalytic conversion, natural gas carbon dioxide dry gas catalytic conversion, natural gas partial oxidation conversion, and steam-carbon dioxide co-conversion.
[0091] The present invention will be described in detail below through examples and comparative examples. Unless otherwise specified, all reagents used in the following examples and comparative examples are commercially available.
[0092] Example 1
[0093] (a) Weigh 100 parts by weight of α-gibbsite, 49 parts of calcium carbonate powder passing through 80 mesh, and 100 parts of water. After mixing thoroughly, add the mixture to a ball mill jar and grind it until D50 = 10 μm. The resulting slurry is placed in an enamel tray and dried in an oven at 80°C for 6 hours.
[0094] (b) The product from step (a) was calcined in a muffle furnace at 1320°C for 3 hours, then crushed and passed through a 200-mesh sieve to obtain aluminum-calcium composite oxide.
[0095] (1) Weigh 100 parts of α-alumina trihydrate passing through 100 mesh, 15 parts of calcium carbonate passing through 150 mesh, 3 parts of aluminum-calcium composite oxide, and 1 part of lanthanum oxide passing through 200 mesh, ball mill them until the particle size D50 is 18 μm, and pass them through a 150 mesh sieve.
[0096] The obtained powder is dry-pressed and crushed, sieved to 20-100 mesh, and 2.5 parts of graphite powder are added to every 100 parts and mixed. The mixture is then pressed into Raschig rings with a diameter of 17mm × 12mm × 5mm to obtain a solid product.
[0097] (2) Place the product from step (1) in a mesh basket above the water surface in a hydrothermal reactor and treat it at 200°C using the self-generated pressure of steam for 12 hours. The hydrothermal product is first dried at 80°C for 3 hours, then gradually heated to 1300°C within 12 hours and calcined for 4 hours. After natural cooling, alkaline composite oxide A is obtained.
[0098] Figure 1 The XRD diffraction pattern of the composite basic oxide A prepared in Example 1 is shown below. Figure 1 As can be seen, diffraction peaks were observed at 2θ of 25.4°, 34.1°, 36.2°, and 57.5°. The peak at 25.4° is calcium dialuminate, the peaks at 34.1° and 36.2° are calcium hexaaluminate, and a small amount of α-alumina (at 2θ of 57.5°) is present. In the example, the diffraction peaks of calcium aluminate (CaAl2O4) were basically undetectable.
[0099] Example 2
[0100] (a) Weigh 100 parts by weight of gibbsite, 54 parts by weight of calcium carbonate powder passing through 80 mesh, and 120 parts by weight of water. Mix them thoroughly and add them to a ball mill jar. Grind until D50 = 10 μm. The resulting slurry is placed in an enamel tray and dried overnight in an oven at 80°C.
[0101] (b) The product of step (a) was calcined in a muffle furnace at 1340°C for 4 hours, then crushed and passed through a 200-mesh sieve to obtain aluminum-calcium composite oxide.
[0102] (1) Weigh 100 parts of 100-mesh alumina, 18 parts of 100-mesh calcium carbonate, 4 parts of aluminum-calcium composite oxide, and 1.6 parts of 100-mesh lanthanum oxide, ball mill them until the particle size D50 is 16 μm, and pass them through a 100-mesh sieve.
[0103] The obtained powder is crushed after dry pressing and sieved to 20-100 mesh. 3 parts of graphite powder are added to every 100 parts, and the mixture is pressed into a Raschig ring with a diameter of 17mm × 12mm × 5mm (inner diameter).
[0104] (2) Place the product from step (1) in a mesh basket above the water surface in a hydrothermal reactor and treat it at 190°C using the self-generated pressure of steam for 22 hours. The hydrothermal product is first dried at 80°C for 6 hours, and then gradually heated to 1280°C within 20 hours, calcined for 4 hours, and then cooled naturally to obtain alkaline composite oxide B.
[0105] Figure 2The XRD diffraction pattern of the basic composite oxide in Example 2 is shown below. Figure 2 As can be seen, diffraction peaks were observed at 2θ of 25.4°, 34.1°, 36.2°, and 57.5°. The peak at 25.4° is calcium dialuminate, the peaks at 34.1° and 36.2° are calcium hexaaluminate, and a small amount of α-alumina (at 2θ of 57.5°) is present. In the example, the diffraction peaks of calcium aluminate (CaAl2O4) were basically undetectable.
[0106] Example 3
[0107] (a) Weigh 100 parts by weight of α-gibbsite, 66 parts of calcium carbonate powder passing through 100 mesh, and 120 parts of water. After mixing thoroughly, add the mixture to a ball mill jar and grind it until D50 = 12 μm. The resulting slurry is placed in an enamel tray and dried in an oven at 80°C for 6 hours.
[0108] (b) The product from step (a) was calcined in a muffle furnace at 1380°C for 3 hours, then crushed and passed through a 200-mesh sieve to obtain aluminum-calcium composite oxide.
[0109] (1) Weigh 100 parts of α-alumina trihydrate passing through 100 mesh, 12 parts of calcium carbonate passing through 200 mesh, 5 parts of aluminum-calcium composite oxide, and 3 parts of praseodymium oxide passing through 100 mesh, ball mill them until the particle size D50 is 15 μm, and pass them through a 100 mesh sieve.
[0110] The obtained powder is dry-pressed and crushed, sieved to 20-100 mesh, and 4 parts of graphite powder are added to every 100 parts and mixed; the powder is pressed into Raschig rings with a diameter of 17mm × 12mm × 5mm (inner diameter);
[0111] (2) Place the product from step (1) in a mesh basket above the water surface in a hydrothermal reactor and treat it at 210°C using the self-generated pressure of steam for 16 hours. The hydrothermal product is first dried at 80°C for 3 hours, then gradually heated to 1360°C within 10 hours, calcined for 4 hours, and then naturally cooled to obtain alkaline composite oxide C.
[0112] Example 4
[0113] Aluminum-calcium composite oxide X was prepared according to steps (a) and (b) in Example 1. Then:
[0114] (1) Weigh 100 parts of α-alumina trihydrate (passed through 100 mesh), 14 parts of calcium carbonate (passed through 200 mesh), 5 parts of composite oxide X, and 2 parts of lanthanum oxide (passed through 100 mesh), ball mill them until the particle size D50 is 8.5 μm, and pass them through a 100-mesh sieve.
[0115] The obtained powder is dry-pressed and crushed, sieved to 20-100 mesh, and mixed with 2.5 parts of graphite powder per 100 parts; it is then pressed into Raschig rings with a diameter of 17mm × 12mm × 5mm (inner diameter);
[0116] (2) Place the product from step (1) in a mesh basket above the water surface in a hydrothermal reactor and treat it at 220°C using the self-generated pressure of steam for 15 hours. The hydrothermal product is first dried at 80°C for 3 hours, then gradually heated to 1300°C within 16 hours, calcined for 4 hours, and then cooled naturally to obtain alkaline composite oxide D.
[0117] Example 5
[0118] The basic composite oxide was prepared according to the method of Example 4, except that the hydrothermal treatment conditions in step (2) were: treatment at 190°C using the self-generated pressure of water vapor for 22 hours, and the calcination conditions were: gradually increasing the temperature to 1290°C within 16 hours, with a calcination time of 4 hours. Other conditions were the same as in Example 4. After natural cooling, the basic composite oxide E was obtained.
[0119] Example 6
[0120] The alkaline composite oxide was prepared according to the method of Example 1, except that (1) 100 parts of α-alumina trihydrate passing through 100 mesh, 15 parts of calcium carbonate passing through 150 mesh, 3 parts of aluminum-calcium composite oxide, and 7 parts of lanthanum oxide passing through 200 mesh were weighed, ball-milled to a particle size D50 of 18 μm, and passed through a 150 mesh sieve. Other conditions were the same as in Example 1 to obtain alkaline composite oxide F.
[0121] Example 7
[0122] The alkaline composite oxide was prepared according to the method of Example 1, except that (1) 100 parts of α-alumina trihydrate passing through 100 mesh, 15 parts of calcium carbonate passing through 150 mesh, 3 parts of aluminum-calcium composite oxide, and 4 parts of cerium oxide passing through 200 mesh were weighed, ball-milled to a particle size D50 of 18 μm, and passed through a 150 mesh sieve. Other conditions were the same as in Example 1 to obtain alkaline composite oxide G.
[0123] Example 8
[0124] The basic composite oxide was prepared according to the method of Example 1, except that the second calcination temperature was 1000℃, and other conditions were the same as in Example 1, to obtain basic composite oxide H.
[0125] Comparative Example 1
[0126] (1) Weigh 100 parts of α-alumina trihydrate passing through 100 mesh, 15 parts of calcium carbonate passing through 150 mesh, 1 part of lanthanum oxide, and 100 parts of water, and ball mill them to a particle size D50 = 19 μm. The resulting slurry is placed in an enamel tray and dried overnight in an oven at 80°C.
[0127] The obtained powder is dry-pressed and crushed, sieved to 20-100 mesh, and 3 parts of graphite powder are added for every 100 parts and mixed thoroughly; the powder is pressed into Raschig rings with a diameter of 17mm × 12mm × 5mm (inner diameter);
[0128] (2) The product from step (1) was gradually heated to 1300℃ over 10 hours, calcined for 4 hours, and then cooled naturally to obtain the alkaline composite oxide DB1.
[0129] Comparative Example 2
[0130] (1) Weigh 100 parts of α-alumina trihydrate that passes through 100 mesh, 16 parts of calcium carbonate that passes through 150 mesh, and 2.5 parts of graphite powder, mix them thoroughly, and compress them into Raschig rings with a diameter of 17mm × 12mm × 5mm.
[0131] (2) The product from step (1) was gradually heated to 1340℃ within 10 hours, calcined for 4 hours, and then cooled naturally to obtain the alkaline composite oxide DB2.
[0132] Figure 3 The XRD diffraction pattern of the basic composite oxide in Comparative Example 2 is shown below. Figure 3 As can be seen from the data, the basic composite oxide sample of Comparative Example 2 is mainly composed of α-alumina (2θ = 57.5°) and calcium aluminate (CaAl4O7) (2θ = 24.4°), with a small amount of calcium aluminate (CaAl2O4, 2θ = 30.1°) detectable.
[0133] Comparative Example 3
[0134] (1) Weigh 100 parts of α-alumina trihydrate (passed through 100 mesh), 17 parts of calcium carbonate (passed through 150 mesh), 1.7 parts of lanthanum oxide (passed through 100 mesh), and 3.5 parts of graphite powder, and mix them thoroughly; compress them into Raschig rings with a diameter of Φ17mm × 12mm × 5mm (inner diameter);
[0135] (2) The product from step (1) was gradually heated to 1330℃ over 9 hours, calcined for 4 hours, and then cooled naturally to obtain the alkaline composite oxide DB3.
[0136] Comparative Example 4
[0137] The alkaline composite oxide was prepared according to the method of Example 4, except that step (2) was not hydrothermal treatment, but directly calcined. The rest was the same as in Example 4, and the alkaline composite oxide DB4 was obtained.
[0138] Test case
[0139] The lateral compressive strength, water absorption rate, and specific surface area of the prepared alkaline composite oxide were tested, and the results are shown in Table 1.
[0140] Table 1
[0141] sample Lateral compressive strength (N / mm) Water absorption rate (%) <![CDATA[Specific surface area (m 2 / g)]]> A 32.2 29.0 3.00 B 31.0 30.2 3.20 C 30.2 27.0 2.90 D 34.0 29.2 3.02 E 33.6 30.0 3.10 F 23.1 29.6 3.04 G 20.0 28.5 2.78 H 13.2 37.7 12.0 DB1 12.2 31.9 3.22 DB2 8.0 33.2 2.65 DB3 9.4 33.4 2.90 DB4 12.6 31.4 3.31
[0142] As can be seen from the results in Table 1, the alkaline composite oxides prepared by the method of the present invention significantly improve the lateral compressive strength while maintaining the water absorption rate and specific surface area. The lateral compressive strength of the alkaline composite oxides in Comparative Examples 1-4 is significantly lower.
[0143] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.
Claims
1. A method for preparing a basic composite oxide, characterized in that, The preparation method includes the following steps: (1) A mixture containing aluminum-calcium composite oxide, aluminum oxide precursor, calcium oxide precursor, carbon material and lanthanide oxide precursor is shaped to obtain a solid product; (2) The solid product from step (1) is subjected to hydrothermal treatment and first calcination.
2. The preparation method according to claim 1, wherein, The aluminum-calcium composite oxide was prepared by the following method: (a) Mix the alumina source, calcium oxide source and solvent, grind and dry; (b) The dried product from step (a) is subjected to a second calcination; Preferably, the alumina source is selected from at least one of hydrated alumina, transition phase alumina, and inert α-alumina, and is preferably hydrated alumina; Preferably, the calcium oxide source is selected from at least one of calcium hydroxide, calcium oxide, and calcium carbonate, and is preferably calcium carbonate.
3. The preparation method according to claim 2, wherein, The amount of alumina source used results in an alumina content of 60-72 wt% in the aluminum-calcium composite oxide, preferably 63-70 wt%. Preferably, the amount of calcium oxide source used is such that the calcium oxide content in the aluminum-calcium composite oxide is 28-40 wt%, more preferably 30-37 wt%. Preferably, the solvent is selected from at least one of water, ethanol, and acetone; Preferably, the amount of solvent used is 0-200 wt% of the total mass of the alumina source and the calcium oxide source, and more preferably 20-100 wt%.
4. The preparation method according to claim 2 or 3, wherein, In step (a), the particles of alumina source and calcium oxide source are ground until the D50 is ≤30μm, preferably D50 ≤20μm, and more preferably D50 ≤15μm. Preferably, in step (b), the conditions for the second calcination include: a calcination temperature of 1200-1420℃, more preferably 1250-1400℃; and a calcination time of 1-8h, more preferably 2-6h.
5. The preparation method according to any one of claims 1-4, wherein, In step (1), the amount of aluminum-calcium composite oxide used is 1-10 wt% of the solid product in step (1), preferably 2-6 wt%. Preferably, the alumina precursor is selected from at least one of hydrated alumina, transition phase alumina, and inert α-alumina, and is preferably hydrated alumina; Preferably, the calcium oxide precursor is selected from at least one of calcium hydroxide, calcium oxide, and calcium carbonate, and is preferably calcium carbonate; Preferably, the amount of the calcium oxide precursor used is 8-20 wt% of the solid product of step (1), preferably 10-15 wt%. Preferably, the amount of the alumina precursor used is 78-90 wt% of the solid product of step (1), more preferably 80-86 wt%.
6. The preparation method according to any one of claims 1-5, wherein, The carbon material is selected from at least one of starch, graphite, coke, stearic acid and stearate, preferably from at least one of stearate, graphite and coke, and more preferably from graphite; Preferably, the amount of carbon material used is 0.3-10 wt% of the solid product of step (1), more preferably 0.5-6 wt%, and more preferably 0.8-5 wt%. Preferably, the lanthanide oxide precursor is selected from at least one of lanthanide metal hydroxides, oxides, and carbonates; Preferably, the lanthanide metal is selected from at least one of lanthanum, cerium, praseodymium, neodymium, samarium, and dysprosium; Preferably, the lanthanide oxide precursor is selected from at least one of lanthanum hydroxide, lanthanum oxide, lanthanum carbonate, cerium hydroxide, cerium oxide, cerium carbonate, praseodymium hydroxide, and praseodymium oxide; Preferably, the amount of the lanthanide oxide precursor used is 0.5-5 wt% of the solid product of step (1), and more preferably 0.8-4 wt%.
7. The preparation method according to any one of claims 1-6, wherein, The conditions for the hydrothermal treatment include: a hydrothermal temperature of 160-240℃, preferably 180-230℃; and a hydrothermal time of 2-40h, preferably 6-30h. Preferably, the first calcination conditions include: under an oxygen-containing atmosphere, a calcination temperature of 1250-1500℃, more preferably 1280-1450℃; and a calcination time of 1-8h, more preferably 2-6h. Preferably, the heating rate of the first calcination is 50-200℃ / h, and more preferably 80-170℃ / h.
8. The alkaline composite oxide prepared by the preparation method according to any one of claims 1-7.
9. The alkaline composite oxide according to claim 8, wherein, The specific surface area of the alkaline composite oxide is 1-6 m². 2 / g, preferably 1.5-5m 2 / g, more preferably 2-4m 2 / g; Preferably, the lateral compressive strength of the alkaline composite oxide is 20-45 N / mm, more preferably 25-40 N / mm; Preferably, the water absorption rate of the alkaline composite oxide is greater than or equal to 25%, and more preferably 27-40%.
10. The application of the alkaline composite oxide prepared by the preparation method according to any one of claims 1-7 or the alkaline composite oxide according to claim 8 or 9 in the field of catalyst support or heat-resistant filler; Preferably, the alkaline composite oxide is used as a catalyst support and heat-resistant filler in hydrocarbon catalytic conversion, heavy oil pyrolysis-gasification coupled hydrogen production, and transesterification reactions.