A monodisperse high-density silica microsphere and its preparation method

By employing microscale mixing, segmented gradient coupling reaction, and online purification and modification, the problems of uneven particle size, residual impurities, and pore defects in silica microspheres were solved, enabling the preparation of high-purity, high-density monodisperse microspheres suitable for high-end electronics and optics fields.

CN123061963APending Publication Date: 2026-11-10SICHUAN MICROFLUIDIC TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202611528331.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-30
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing technologies struggle to simultaneously produce monodisperse, highly dense, ultra-high purity, controllable interfaces, and continuously mass-producible silica microspheres, resulting in issues such as wide particle size distribution, numerous pore defects, high levels of residual ionic impurities, and poor batch stability.

Method used

A closed-loop synergistic system is adopted, which includes microscale precise mixing, segmented gradient coupled reaction, growth and purification simultaneously, uniform in-situ modification and inert protection, to prepare microspheres through a microchannel reactor. This includes multi-stage backflow micromixing, segmented gradient temperature control, online purification and in-situ modification, ensuring uniform particle size, internal purity and interfacial functionality.

Benefits of technology

It achieves ultra-high monodispersity (CV≤4%), electronic-grade purity, controllable interface properties, and high density of silica microspheres, meeting the requirements of high-end electronic-grade applications and possessing continuous mass production capability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123061963A_ABST
    Figure CN123061963A_ABST
Patent Text Reader

Abstract

This invention discloses a monodisperse high-density silica microsphere and its preparation method, relating to the field of nano-inorganic functional material preparation technology. The preparation method includes the following steps: (1) The prepared silicon source precursor solution and alkaline catalytic solution are introduced into a multi-stage folded micro-mixing channel and mixed evenly; (2) The mixed solution is subjected to low-temperature nucleation and medium-temperature dense growth in sequence; (3) During the microsphere gel growth process, it enters the embedded multi-stage cleaning channel simultaneously to complete the replacement of organic residues with ethanol, the rinsing of water-soluble impurities with pure water, and the removal of weak acid metal ions through complexation in sequence, with growth and purification completed simultaneously; (4) The purified high-activity microsphere sol enters the modification channel, and the silane coupling agent is uniformly and directionally grafted under a steady-state laminar flow field to obtain multifunctional modified microspheres; (5) Under an inert atmosphere, isothermal ripening, gradient drying, and segmented low-temperature sintering are carried out in sequence. The stable and continuous preparation of high-end electronic-grade silica microspheres has been achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of nano-inorganic functional materials preparation technology, specifically to a monodisperse highly dense silica microsphere and its preparation method. Background Technology

[0002] Silica microspheres, with their advantages of high sphericity, high insulation, low expansion, high light transmittance, and wear and corrosion resistance, are a core basic powder material in high-end electronics, optics, and precision manufacturing. Currently, the mainstream preparation processes in the industry are divided into two categories: traditional autoclave sol-gel processes and emerging microfluidic preparation processes. However, both have insurmountable technical bottlenecks, making it difficult to simultaneously meet the five high-end indicators of monodispersity, high density, ultra-high purity, controllable interface, and continuous mass production.

[0003] Traditional batch Stöber processes are batch-to-batch production processes that rely on macroscopic stirring and mixing. The system has large temperature and concentration field gradients, and the nucleation and growth processes are heavily coupled. They have inherent defects such as wide particle size distribution, large batch fluctuations, poor sphericity, high residual ionic impurities, many internal pore defects in microspheres, and low true density, which cannot meet the requirements of electronic-grade precision applications.

[0004] Patent document CN112811431A discloses a high-throughput preparation method for monodisperse silica microspheres. The silica microspheres are prepared using a microfluidic reactor, which includes a reaction chamber containing a multi-channel helical tube with at least one helical tube. The preparation method includes the following steps: 1) dispersing a silicon source in a solvent to obtain a first solution; 2) dispersing a catalyst in deionized water to obtain a second solution; 3) simultaneously inputting the first and second solutions into the inlet channel of the reaction chamber and mixing them to obtain a mixed solution; 4) reacting the mixed solution through each helical tube of the multi-channel helical tube, and obtaining silica of different particle sizes after separation and purification. This invention employs a high-throughput microfluidic reaction system, resulting in a uniform particle size distribution of the synthesized silica and significantly increasing the production capacity and efficiency of different particle sizes. However, this technical solution only discloses continuous reaction in a multi-channel helical tube and simple throughput scaling, and still has the following drawbacks:

[0005] 1. It only achieves a single process of mixing and reaction, without online purification, in-situ modification, or segmented temperature-controlled growth;

[0006] 2. The entire process of the spiral tube reaction is isothermal, with nucleation and growth coupled together, which inevitably leads to a wider particle size distribution and a loose and porous interior.

[0007] 3. Without a purification system, the product has high ion residue, making it impossible to prepare high-purity electronic-grade microspheres;

[0008] 4. Without inert airtight protection, microspheres are prone to micropore defects, resulting in low true density.

[0009] Patent document CN118515288A discloses a silica aerogel based on microchannel technology and its preparation method and apparatus. The preparation method includes continuously feeding raw materials into a microchannel mixing reaction device, continuously performing sol-gel transition, solvent replacement, and hydrophobic modification, followed by drying to obtain silica aerogel, which is then continuously output. This invention utilizes the extremely high specific surface area of ​​microchannels to achieve rapid mixing of reactants to form microgels; the high mass transfer efficiency of microchannels significantly shortens solvent replacement and hydrophobic modification time, saving a large amount of solvent; compared with traditional intermittent methods for preparing silica aerogels, this method integrates the preparation process into a single microchannel system, solving the problems of multi-step dispersion and discontinuity, and allowing each step to be independent, separable, and combinable, making it flexible and efficient. However, although this technical solution discloses continuous solvent replacement and hydrophobic modification via microchannels, its core application is aerogel preparation, which is completely opposite to the mechanism of dense solid microspheres.

[0010] 1. Aerogel technology intentionally preserves the porous structure and does not pursue high true density or low defects;

[0011] 2. The channel only implements a simple sequential process, without a segmented nucleation / growth temperature control mechanism, and cannot accurately control particle size;

[0012] 3. The cleaning and modification processes are separate modules with no flow field coupling and coordination, which can easily lead to particle agglomeration and uneven interface modification.

[0013] 4. Without a closed inert protection system, it cannot suppress oxidation, carbonization, and water vapor side reactions.

[0014] Patent document CN104003408A discloses a continuous and controllable method for preparing monodisperse silica microspheres. This process includes nucleation, growth, and separation steps. This process enables the batch preparation of monodisperse silica microspheres with high sphericity and narrow particle size distribution. In the nucleation stage of the silica microsphere seeds, the reaction system is a boiling system with good heat and mass transfer under strong convection, allowing for homogeneous and rapid nucleation. It also solves the agglomeration problem of existing technologies, resulting in a short reaction time and monodisperse microsphere seeds with a narrower particle size distribution. This invention employs one-step or multi-step growth, separating the nucleation and growth stages, which yields monodisperse silica microspheres with high sphericity and controllable particle size, with a particle size distribution deviation of less than 2%, resulting in superior performance. Furthermore, it can obtain silica microspheres of various particle sizes from 20 to 10000 nm according to actual needs, overcoming many shortcomings of existing technologies. However, although this technical solution discloses the nucleation and growth steps, it belongs to the traditional boiling system and has the following drawbacks:

[0015] 1. Relying on macroscopic boiling and strong convection, the temperature and concentration fields are not uniform, making it impossible to achieve micron-level precise core control;

[0016] 2. Lacking the advantages of microfluidic microscale mass transfer, it is impossible to achieve millisecond-level uniform mixing;

[0017] 3. No online purification, no in-situ modification, and no closed-loop protection;

[0018] 4. Batch-based intermittent production, lacking continuous integrated closed-loop capability.

[0019] In summary, existing publicly available technologies can only achieve single-function optimization and have core problems such as process fragmentation, independent mechanisms, and lack of synergistic coupling effects. Those skilled in the art cannot solve the industry pain point of "narrow distribution, high density, high purity, controllable interface, low defects, and continuous mass production" by simply adding the above-mentioned existing technologies. Summary of the Invention

[0020] Addressing the problems of existing technologies, such as dispersed processes, lack of synergistic coupling, coupled nucleation and growth, numerous microsphere pore defects, high levels of residual ionic impurities, uneven interface modification, wide particle size distribution, poor batch stability, and inability to simultaneously achieve high precision and continuous mass production, this invention aims to provide a monodisperse, highly dense silica microsphere and its preparation method. This method abandons the traditional approach of simply splicing together processes and constructs a closed-loop synergistic system of "microscale precise mixing—segmented gradient coupled reaction—growth-synchronous gradient impurity removal—uniform in-situ modification—full-process inert defect suppression." Through deep coupling, mutual empowerment, and mutual constraint among functional units, this method simultaneously solves five core challenges—microsphere size uniformity, structural density, chemical purity, interface functionality, and production stability—from a mechanistic perspective, achieving stable and continuous preparation of high-end electronic-grade silica microspheres.

[0021] This invention is achieved through the following technical solution:

[0022] In a first aspect, this application provides a method for preparing monodisperse, highly dense silica microspheres, comprising the following steps:

[0023] (1) The prepared silicon source precursor solution and alkaline catalyst solution are introduced into the multi-stage foldback micro-mixing channel in two separate streams and mixed evenly to obtain a mixed solution;

[0024] (2) The mixed solution was subjected to low-temperature nucleation and medium-temperature dense growth in sequence;

[0025] (3) During the growth of microsphere gel, it enters the embedded multi-level cleaning channel simultaneously to complete the replacement of organic residues of ethanol, the rinsing of water-soluble impurities with pure water, and the removal of weak acid metal ions through complexation. Growth and purification are completed simultaneously.

[0026] (4) Monodisperse high-density silica microspheres were obtained after constant temperature curing, gradient drying and segmented low temperature sintering under an inert atmosphere.

[0027] Existing technologies either involve isothermal reactions throughout the entire process (nucleation and growth coupled, resulting in wider particle sizes) or macroscopic stepwise reactions (inhomogeneous mixing and insufficient precision). This invention deeply couples microscale ultrafast homogenization technology with a segmented gradient temperature control mechanism: microchannels enable millisecond-level gradient-free mixing of the silicon source and catalyst, ensuring the synchronous generation of all crystal nuclei; furthermore, through a partitioned coupling mechanism of low-temperature-specific nucleation in the front stage and medium-temperature-specific dense growth in the back stage, the nucleation and growth processes are physically isolated, completely eliminating secondary nucleation and particle size differentiation. The two technologies work synergistically to lock in particle size uniformity from the reaction source, achieving ultra-high monodispersity with a CV ≤ 4%, a synergistic effect that cannot be achieved by a single technology.

[0028] Traditional techniques employ a "reaction first, offline cleaning later" approach. Cleaning only removes surface impurities, failing to remove ions encapsulated within the gel, and offline transfer easily introduces secondary contamination. This invention utilizes a growth-simultaneous purification coupling mechanism: while the microspheres are in the loose gel growth stage, alcohol washing, water washing, and weak acid complexation gradient replacement are simultaneously carried out. Leveraging the dynamic openness of the microsphere pores, unreacted silicon sources, organic residues, metal ions, and halogen impurities are actively replaced. As the silicon-oxygen bonds continue to cross-link and densify, the pores gradually close, permanently removing impurities without secondary encapsulation. This dynamic coupling purification mechanism involves independent reactions and independent cleaning, which is impossible to achieve with existing technologies.

[0029] Existing modification technologies mostly involve batch-type post-modification or independent channel modification, resulting in turbulent flow fields and uneven concentrations, leading to low grafting rates, uneven coating, and powder agglomeration. This invention utilizes a microfluidic laminar flow steady-state uniform flow field to simultaneously perform in-situ grafting modification at the time point when microsphere growth and purification are complete and interfacial activity is optimal. The dual coupling of flow field uniformity and precise timing achieves monolayer, uniform, and high-density directional grafting of coupling agent molecules, allowing for precise control of the content of multiple functional groups and completely solving the problems of uneven modification and agglomeration.

[0030] Existing microfluidic technologies are mostly open systems, where continuous interference from air, water vapor, and carbon dioxide can easily lead to the formation of micropores and porous defects within the microspheres. This invention suppresses side reactions through a completely sealed inert atmosphere, reducing defect formation at the source. Furthermore, a coupled densification mechanism of segmented gradient temperature growth and segmented low-temperature sintering repairs the silicon-oxygen network layer by layer, closing residual micropores, ultimately yielding solid, defect-free microspheres with near-theoretical density, significantly improving structural stability and mechanical properties.

[0031] Furthermore, in step (1), the structure of the multi-stage foldback micro-hybrid channel includes T-type, Y-type, cross-type, and laminar flow focusing microfluidic chips, with a channel width between 50μm and 500μm.

[0032] Further, in step (1), the flow rate ratio of the silicon source precursor solution to the alkaline catalytic solution is 1:(0.8~2).

[0033] Further, in step (1), the silicon source precursor solution includes any one of tetraethyl orthosilicate, methyl orthosilicate, tetramethoxysilane, and modified organosilicon sol; and / or the alkaline catalytic solution includes any one of ammonia, triethylamine, and ethanolamine.

[0034] Furthermore, in step (2), the temperature for low-temperature nucleation is controlled at 20℃~30℃, and the temperature for medium-temperature densification is controlled at 40℃~65℃.

[0035] Furthermore, a functionalization modification step is added after step (3): the purified highly active microsphere sol enters the modification channel, and the silane coupling agent is uniformly and directionally grafted under a steady-state laminar flow field to obtain multifunctional modified microspheres.

[0036] Furthermore, the silane coupling agent includes any one of epoxy silane coupling agents, amino silane coupling agents, alkyl silane coupling agents, phenyl silane coupling agents, and vinyl silane coupling agents.

[0037] Furthermore, in step (4), the temperature during segmented low-temperature sintering is controlled at 600℃~850℃, the heating rate is controlled at 1℃ / min~3℃ / min, and the holding time is controlled at 1h~4h.

[0038] Secondly, this application provides a monodisperse, highly dense silica microsphere, which is prepared using the above-described preparation method.

[0039] Furthermore, the particle size of the silica microspheres is 300 nm to 1.0 μm.

[0040] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0041] (1) This invention breaks through the technical limitations of simple process superposition in the prior art and constructs a new microfluidic control preparation system with multi-unit time-series coupling and dynamic collaboration. Each process empowers and constrains each other, generating a new mechanism of synergistic effect that cannot be achieved by independent processes, fundamentally solving the pain points of poor precision, low purity, many defects and poor stability of traditional processes.

[0042] (2) This invention achieves ultra-high monodispersity of microspheres by coupling micro-mixing and segmented reaction, with a particle size CV stability of ≤4%, which far exceeds the precision of existing microfluidic processes and meets the stringent requirements of high-end precision fillers.

[0043] (3) This invention achieves deep removal of impurities inside microspheres by dynamically coupling growth and impurity removal, achieving electronic-grade ultra-high purity and breaking through the purity bottleneck of offline cleaning in existing technologies.

[0044] (4) This invention achieves precise and controllable microsphere interface performance by coupling steady-state flow field with in-situ modification, solves the problems of agglomeration and uneven coating, and is suitable for polymer composite systems in multiple fields.

[0045] (5) This invention prepares solid microspheres with high density and low defects by inert protection and sintering dense coupling. The true density is close to the theoretical value, and the mechanical properties and structural stability are greatly improved.

[0046] (6) The process of this invention is highly flexible, can be continuously mass-produced, and seamlessly connects small-scale, pilot-scale and industrial-scale production. It is green and low-consumption, and has extremely high industrialization value. Attached Figure Description

[0047] To more clearly illustrate the technical solutions of the exemplary embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly described below. It should be understood that the following drawings only show some embodiments of the present invention and should not be considered as a limitation of the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort. In the drawings:

[0048] Figure 1 This is a SEM image of the 300nm monodisperse highly dense silica microspheres prepared in Example 1 of this invention;

[0049] Figure 2 This is a SEM image of the 500nm monodisperse highly dense silica microspheres prepared in Example 2 of this invention;

[0050] Figure 3 This is a SEM image of the 700nm monodisperse highly dense silica microspheres prepared in Example 3 of this invention;

[0051] Figure 4 This is a SEM image of the 1 μm monodisperse highly dense silica microspheres prepared in Example 4 of this invention;

[0052] Figure 5 This is a SEM image of the 1 μm monodisperse highly dense silica microspheres prepared in Example 5 of this invention;

[0053] Figure 6 The image shows a SEM image of the silica microspheres in Comparative Example 1.

[0054] Figure 7 SEM image of the silica microspheres in Comparative Example 2;

[0055] Figure 8SEM image of the silica microspheres in Comparative Example 3;

[0056] Figure 9 This is a schematic diagram of the microfluidic chip channel used in this invention. Detailed Implementation

[0057] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the embodiments. The illustrative embodiments and descriptions of this invention are only used to explain this invention and are not intended to limit this invention.

[0058] In the following description, numerous specific details are set forth in order to provide a thorough understanding of the invention. However, it will be apparent to those skilled in the art that these specific details are not necessary to practice the invention. In other embodiments, well-known materials or methods have not been specifically described in order to avoid obscuring the invention.

[0059] Throughout this specification, references to "an embodiment," "an example," or "an example" mean that a particular feature, structure, or characteristic described in connection with that embodiment or example is included in at least one embodiment of the invention. Therefore, the phrases "an embodiment," "an example," "an example," or "an example" appearing in various places throughout the specification do not necessarily refer to the same embodiment or example. Furthermore, specific features, structures, or characteristics can be combined in one or more embodiments or examples in any suitable combination and / or sub-combination. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items. Moreover, without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described herein, as well as the features of those different embodiments or examples.

[0060] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60–120 and 80–110 are listed for a specific parameter, it is understood that ranges of 60–110 and 80–120 are also expected. Furthermore, if minimum range values ​​of 1 and 2 are listed, and if maximum range values ​​of 3, 4, and 5 are listed, then the following ranges are all expected: 1–3, 1–4, 1–5, 2–3, 2–4, and 2–5. In this application, unless otherwise stated, the numerical range "a–b" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0~5" indicates that all real numbers between "0~5" have been listed in this article; "0~5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0061] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the method may also include step (c), indicating that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.

[0062] Example 1

[0063] This embodiment provides a method for preparing monodisperse highly dense silica microspheres, specifically for preparing 300nm-scale monodisperse highly dense silica microspheres, such as... Figure 9 As shown, a flat-channel microfluidic chip with a channel width of 100μm is used. The specific steps are as follows:

[0064] S1. Precise Constant Pressure Feeding and Multi-Stage Microscale Ultrafast Mixing: A 15% (w / w) TEOS ethanol silicon source solution and a 2% (w / w) ammonia catalytic aqueous solution are prepared and stably delivered by a high-precision constant pressure pump. The two fluids are pumped into a multi-stage zigzag micro-mixing channel at a 1:1 flow rate ratio. Relying on the high specific surface area and strong mass transfer advantages of the microchannels, millisecond-level uniform mixing is achieved, eliminating differences in system concentration and temperature gradients, ensuring consistent crystal nucleation, and obtaining a mixed solution. The flow rate error is ≤1%, and the flow rate ratio can be adaptively adjusted, providing stable preconditions for homogeneous nucleation.

[0065] S2. Segmented gradient coupled micro-reaction: The mixed liquid flows sequentially through the low-temperature nucleation channel and the medium-temperature dense growth channel. Synchronous and uniform nucleation is completed in the 20℃ low-temperature range, and the constant temperature reaction is carried out for 40s to avoid secondary nucleation. Slow layer-by-layer growth is completed in the 45℃ gradient heating range, and the reaction is held for 120s to improve the silicon-oxygen cross-linking network and suppress the generation of pore defects.

[0066] S3. Dynamic synchronous gradient purification: During the growth of the microsphere gel, it enters the embedded multi-level cleaning channel simultaneously to complete the replacement of organic residues with ethanol, rinsing with water-soluble impurities with pure water, and removal of weak acid metal ions through complexation. This allows growth and purification to be completed simultaneously without the need for offline centrifugation.

[0067] S4. Continuous curing and collection in an inert atmosphere: The entire process is protected by an inert and sealed argon atmosphere to suppress external impurities and side reactions. After constant temperature curing, gradient drying, and segmented low-temperature sintering at 600℃ to densify, highly monodisperse, highly dense, and ultra-high purity functionalized silica microspheres are obtained.

[0068] The performance test results of the silica microspheres prepared in this embodiment are as follows: Figure 1 The image shows a SEM image of the silica microspheres prepared using the method of this embodiment. The image shows that the microspheres are monodisperse spherical particles with smooth surfaces and uniform particle size distribution. The average particle size is 312 nm, the CV value is 3.1%, and the sphericity is 99.2%. The true density of the microspheres is 2.21 g / cm³. 3 BET=4.8m 2 / g, Na + =2.5mg / Kg, Cl - =15.2mg / Kg, suitable for general coating filling, plastic modification, and conventional filler applications.

[0069] Example 2

[0070] This embodiment provides a method for preparing monodisperse, highly dense silica microspheres. Unlike Example 1, this embodiment prepares 500nm-scale epoxy-functionalized silica microspheres. A multi-stage foldback microfluidic chip with a channel width of 150μm is used; the flow rate ratio of silicon source solution to catalyst solution is 1:1.2; the low-temperature nucleation stage is 25℃ for 30s; the medium-temperature densification growth stage is 55℃ for 150s; the microspheres undergo three-stage gradient online alcohol washing, water washing, and weak acid purification; an epoxy-based silane coupling agent solution is introduced into the rear channel for in-situ continuous modification at 60℃ for 80s; after continuous collection, the microspheres undergo pre-dehydroxylation at 400℃ and densification by sintering at 700℃.

[0071] The performance test results of the silica microspheres prepared in this embodiment are as follows: Figure 2 The image shows a SEM image of the silica microspheres prepared using the method described in this embodiment. The image shows that the microspheres are monodisperse spherical particles with smooth surfaces and uniform particle size distribution. The average particle size is 513 nm, the CV value is 3.5%, and the sphericity is 99.5%. The true density of the microspheres is 2.22 g / cm³. 3 BET=4.3m 2 / g, Na + =3.0mg / Kg, Cl - =16.5mg / Kg, with a high grafting rate of epoxy functional groups, excellent compatibility with epoxy and PI resins, and suitable for polymer composite modification and precision adhesive materials.

[0072] Example 3

[0073] This embodiment provides a method for preparing monodisperse, highly dense silica microspheres. Unlike Example 1, this embodiment prepares 700nm-scale hydrophobically modified, low-absorption silica microspheres. A large-particle-size adaptive microfluidic chip with a channel width of 200μm is used; the silicon source concentration is increased by 20%, and the fluid flow rate ratio is 1:1.5; the nucleation temperature is 28℃, and the growth temperature is 60℃; the gradient growth residence time is extended to 200s; after online multi-stage purification, alkyl hydrophobic silanes are introduced for in-situ coating modification; the sintering temperature is 750℃, and the holding time is 2.5h.

[0074] The performance test results of the silica microspheres prepared in this embodiment are as follows: Figure 3 The image shows a SEM image of the silica microspheres prepared using the method described in this embodiment. The image shows that the microspheres are monodisperse spherical particles with smooth surfaces and uniform particle size distribution. The average particle size is 725 nm, the CV value is 2.9%, and the sphericity is 99.5%. The true density of the microspheres is 2.24 g / cm³. 3 BET=3.8m 2 / g, Na + =2.8mg / Kg, Cl -=16.8mg / Kg, powder water absorption rate ≤0.12%, excellent hydrophobic properties, no surface hydrophilic defects, suitable for waterproof coatings, moisture-resistant composite materials, and outdoor anti-corrosion materials.

[0075] Example 4

[0076] This embodiment provides a method for preparing monodisperse, highly dense silica microspheres. Unlike Example 1, this embodiment prepares 1.0 μm-sized, mechanically dense silica microspheres. A wide-channel, slow-speed microfluidic chip with a channel width of 300 μm is used; the overall fluid velocity is reduced, and the reaction residence time is extended; the nucleation section achieves stable nucleation at a constant temperature of 22°C, while the growth section achieves gradient-density growth at 65°C; internal silicon-oxygen bond crosslinking is strengthened, and the residence time in the high-temperature curing channel is extended; after multi-stage deep impurity removal, no modification treatment is performed, and the microspheres are sintered at a low temperature of 800°C.

[0077] The performance test results of the silica microspheres prepared in this embodiment are as follows: Figure 4 The image shows a SEM image of the silica microspheres prepared using the method described in this embodiment. The image shows that the microspheres are monodisperse spherical particles with smooth surfaces and uniform particle size distribution. The average particle size is 1 μm, the CV value is 2.7%, and the sphericity is 99.2%. The true density of the microspheres is 2.25 g / cm³. 3 BET=3.2m 2 / g, Na + =2.5mg / Kg, Cl - =17.7mg / Kg, with excellent compressive strength and no pore defects in its structure, making it suitable for precision polishing media, wear-resistant coatings, and structural reinforcement fillers.

[0078] Example 5

[0079] This embodiment provides a method for preparing monodisperse high-density silica microspheres. The microfluidic reaction parameters are the same as in Example 2. After online cleaning, an aminosilane coupling agent solution is introduced for in-situ grafting modification at a modification temperature of 55°C. Grafting is carried out in a continuous flow field with uniformity. The finished product is collected after low-temperature curing.

[0080] The performance test results of the silica microspheres prepared in this embodiment are as follows: Figure 5 The image shows a SEM image of the silica microspheres prepared using the method described in this embodiment. The image shows that the microspheres are monodisperse spherical particles with smooth surfaces and uniform particle size distribution. The average particle size is 506 nm, the CV value is 3.7%, and the sphericity is 99.4%. The true density of the microspheres is 2.24 g / cm³. 3 BET=5.6m 2 / g, Na + =2.1mg / Kg, Cl -=15.8 mg / K. The amino functional groups on the surface of the microspheres are uniformly distributed, exhibiting excellent water dispersibility, no aggregation, and good biocompatibility, making them suitable for applications in biopharmaceutical carriers, biological detection, and water adsorption and purification materials.

[0081] Comparative Example 1

[0082] This comparative example uses the preparation method described in patent document CN112811431A in the background art, and the raw materials, solid content, and sintering temperature are all consistent. For example... Figure 6 As shown in the figure, the microspheres are monodisperse spherical particles with slight surface damage. The microspheres exhibit good uniformity, with an average particle size of 497 nm, a CV value of 8.2%, and a sphericity of 95.8%. The true density of the microspheres is 1.98 g / cm³. 3 BET=4.3m 2 / g, Na + =16.4mg / Kg, Cl - =31.2mg / Kg.

[0083] Comparative Example 2

[0084] This comparative example uses the preparation method described in patent document CN118515288A in the background art, and the raw materials, solid content, and sintering temperature are all consistent. For example... Figure 7 As shown in the figure, the microspheres exhibit poor uniformity. The true density of the microspheres is 1.97 g / cm³. 3 BET=6.5m 2 / g, Na + =15.7mg / Kg, Cl - =28.6mg / Kg.

[0085] Comparative Example 3

[0086] This comparative example uses the preparation method described in patent document CN104003408A in the background art, and the raw materials, solid content, and sintering temperature are all consistent. For example... Figure 8 As shown in the figure, the microspheres exhibit poor uniformity. The true density of the microspheres is 1.95 g / cm³. 3 BET=8.2m 2 / g, Na + =16.2mg / Kg, Cl - =29.5mg / Kg.

[0087] The performance of the silica microspheres prepared by the methods of Examples 1-5 and Comparative Examples 1-3 was tested, and the test results are shown in Table 1.

[0088] Table 1

[0089] sample Particle size variation coefficient CV (%) <![CDATA[True density of microspheres (g / cm 3 )]]> <![CDATA[BET(m 2 / g)]]> Sodium ion residue (mg / Kg) Chloride ion residue (mg / Kg) Sphericity (%) Example 1 3.1 2.21 4.8 2.5 15.2 99.2 Example 2 3.5 2.22 4.3 3.0 16.5 99.5 Example 3 2.9 2.24 3.8 2.8 16.8 99.5 Example 4 2.7 2.25 3.2 2.5 17.7 99.3 Example 5 3.7 2.24 5.6 2.1 15.8 99.4 Comparative Example 1 8.2 1.98 4.3 16.4 31.2 95.8 Comparative Example 2 14.1 1.97 6.5 15.7 28.6 81.4 Comparative Example 3 42.8 1.95 8.2 16.2 29.5 88.2

[0090] The example demonstrates superior performance compared to the comparative example in terms of particle size uniformity, true density, sphericity, and ionic purity, proving that its preparation process (such as polymerization, granulation, and cleaning) is more mature and stable. The comparative example exhibits significant structural defects: low true density, high BET, high ion residue, and low sphericity. These factors collectively lead to performance degradation, potentially manifesting as poor mechanical strength, high column pressure, low separation efficiency, or poor biocompatibility in practical applications.

[0091] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention, and they should all be covered within the scope of the claims and specification of the present invention.

Claims

1. A method for preparing monodisperse, highly dense silica microspheres, characterized in that, Includes the following steps: (1) The prepared silicon source precursor solution and alkaline catalyst solution are introduced into the multi-stage foldback micro-mixing channel in two separate streams and mixed evenly to obtain a mixed solution; (2) The mixed solution was subjected to low-temperature nucleation and medium-temperature dense growth in sequence; (3) During the growth of microsphere gel, it enters the embedded multi-level cleaning channel simultaneously to complete the replacement of organic residues with ethanol, the rinsing of water-soluble impurities with pure water, and the removal of weak acid metal ions through complexation. Growth and purification are completed simultaneously. (4) Under an inert atmosphere, the monodisperse high-density silica microspheres were obtained by sequentially performing constant temperature curing, gradient drying, and segmented low-temperature sintering.

2. The method for preparing monodisperse high-density silica microspheres according to claim 1, characterized in that, In step (1), the structure of the multi-stage foldback micro-hybrid channel includes T-type, Y-type, cross-type, and laminar flow focusing microfluidic chips, with a channel width between 50μm and 500μm.

3. The method for preparing monodisperse high-density silica microspheres according to claim 1, characterized in that, In step (1), the flow rate ratio of the silicon source precursor solution to the alkaline catalytic solution is 1:(0.8~2).

4. The method for preparing monodisperse high-density silica microspheres according to claim 1, characterized in that, In step (1), the silicon source precursor solution includes any one of tetraethyl orthosilicate, methyl orthosilicate, tetramethoxysilane, and modified organosilicon sol; and / or the alkaline catalytic solution includes any one of ammonia, triethylamine, and ethanolamine.

5. The method for preparing monodisperse high-density silica microspheres according to claim 1, characterized in that, In step (2), the temperature for low-temperature nucleation is controlled at 20℃~30℃, and the temperature for medium-temperature densification is controlled at 40℃~65℃.

6. The method for preparing monodisperse high-density silica microspheres according to claim 1, characterized in that, After step (3), a functionalization modification step is added: the purified highly active microsphere sol enters the modification channel, and the silane coupling agent is uniformly and directionally grafted under a steady-state laminar flow field to obtain multifunctional modified microspheres.

7. The method for preparing monodisperse high-density silica microspheres according to claim 6, characterized in that, The silane coupling agent includes any one of epoxy silane coupling agents, amino silane coupling agents, alkyl silane coupling agents, phenyl silane coupling agents, and vinyl silane coupling agents.

8. The method for preparing monodisperse high-density silica microspheres according to claim 1, characterized in that, In step (4), the temperature during segmented low-temperature sintering is controlled at 600℃~850℃, the heating rate is controlled at 1℃ / min~3℃ / min, and the holding time is controlled at 1h~4h.

9. A monodisperse, highly dense silica microsphere, characterized in that, It is prepared by the preparation method described in any one of claims 1 to 8.

10. The monodisperse, highly dense silica microspheres according to claim 9, characterized in that, The silica microspheres have a particle size of 300 nm to 1.0 μm.

Citation Information

Patent Citations

  • Preparation method of continuous controllable monodispersed silica microspheres

    CN104003408A

  • High-throughput preparation method of monodisperse silicon dioxide microspheres

    CN112811431A

  • Silicon dioxide aerogel based on microchannel technology and preparation method and device thereof

    CN118515288A