Porous sustained-release eco-friendly drag reducer and its preparation method
By preparing a porous carrier to support conductive carbon materials and hygroscopic salts, combined with a semi-permeable sustained-release membrane, the conductivity and environmental friendliness issues of existing drag-reducing agents were solved, achieving long-lasting sustained release and adaptive response drag-reducing effects.
Patent Information
- Application Number
- CN202611301604.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-26
- Publication Date
- 2026-11-10
AI Technical Summary
Existing drag-reducing agents cannot simultaneously achieve long-lasting sustained release, high conductivity, and environmental friendliness, and suffer from problems such as rapid loss of conductive components, uneven release, and environmental pollution.
By preparing a porous support, loading conductive carbon materials, hygroscopic inorganic salts and corrosion inhibitors, a semi-permeable slow-release membrane layer is formed, constructing a multi-level porous network structure to achieve synergistic conductivity of conductive ions and electrons. In a humid environment, it moderately swells to form hydrated ion channels, and in a dry environment, it becomes dense to slow down water evaporation and ion loss.
It achieves long-term sustained release of drag-reducing agents, has low volume resistivity, is environmentally friendly, avoids the rapid loss and environmental pollution of traditional drag-reducing agents, and has adaptive response capabilities.
Abstract
Description
Technical Field
[0001] This invention relates to the field of drag-reducing agent preparation technology, and in particular to a porous slow-release eco-friendly drag-reducing agent and its preparation method. Background Technology
[0002] Grounding resistance is a crucial indicator of a grounding system's current-carrying capacity. In power transmission and transformation projects, wind power foundations, and communication base stations, reducing grounding resistance is essential for ensuring equipment and personnel safety. In areas with high soil resistivity (such as mountainous regions, rocky strata, and permafrost areas), the natural soil resistivity often reaches hundreds or even thousands of ohm-meters, making it difficult to meet grounding resistance design requirements. In engineering projects, artificial resistance-reducing agents are typically added to improve the conductivity of the soil around the grounding electrode. Currently, commonly used resistance-reducing agents mainly include inorganic salts, bentonite-based agents, and conductive cement-based agents. However, while inorganic salt-based resistance-reducing agents have good conductivity, they contain Cl⁻ and SO₄²⁻. 2- Plasma is easily lost with rainwater, causing its resistance-reducing effect to decay rapidly. Furthermore, the large amount of lost ions negatively impacts groundwater sources and surrounding vegetation. Bentonite-based resistance-reducing agents have strong water retention but insufficient conductivity, and are prone to shrinkage and cracking after drying, leading to a rebound in grounding resistance. While conductive cement-based resistance-reducing agents possess certain strength and conductivity after curing, they lack sustained moisture absorption and slow-release capabilities, resulting in a significant decrease in resistance-reducing effect during dry seasons. Therefore, developing a resistance-reducing agent that combines long-lasting resistance reduction, environmental friendliness, and adaptive adjustment capabilities has become a pressing technical challenge in the field of grounding technology.
[0003] In recent years, researchers have attempted to extend the shelf life of drag-reducing agents by adsorbing conductive components onto porous carriers or by coating them with slow-release membranes, but many shortcomings remain. For example, while directly loading conductive salts into porous materials can delay release, the release rate of the salts is difficult to control. Excessive initial release leads to waste and environmental pollution, while insufficient release in the later stages results in drag-reducing failure. Although using a single coating membrane can slow down the release rate, excessively dense membranes can hinder water permeation and ion migration, affecting conductivity. If the porous carrier lacks sufficient mechanical strength, it is prone to breakage under construction, landfill, or soil stress, leading to pore structure collapse and increased channels for conductive component loss. Summary of the Invention
[0004] The purpose of this invention is to provide a porous, slow-release, eco-friendly drag-reducing agent and its preparation method, aiming to solve the problem that existing drag-reducing agents cannot simultaneously achieve long-lasting slow release, high conductivity, and environmental friendliness.
[0005] In a first aspect, the present invention provides a method for preparing a porous, sustained-release, eco-friendly drag-reducing agent, comprising the following steps:
[0006] S1. Inorganic mineral raw materials are mixed with pore-forming agents and binders and granulated, then dried and sintered at high temperature to obtain a porous carrier;
[0007] S2. The porous carrier is immersed in a mixed slurry containing conductive carbon material, hygroscopic inorganic salt and corrosion inhibitor, and then vacuum infiltrated and dried to load the conductive active components into the pores and surface of the porous carrier, thereby obtaining a loaded carrier.
[0008] S3. The load carrier is immersed in a film-forming solution, and after being removed, it is cross-linked and cured to form a semi-permeable slow-release film layer on the outer surface of the load carrier. After drying, a porous slow-release eco-friendly drag-reducing agent is obtained.
[0009] In some embodiments, in step S1, the inorganic mineral raw material includes at least one of diatomite, zeolite, bentonite, and kaolin.
[0010] The pore-forming agent is selected from at least one of ammonium bicarbonate, ammonium carbonate, polymethyl methacrylate microspheres, and sawdust.
[0011] The binder is selected from at least one of polyvinyl alcohol, dextrin, and starch;
[0012] The mass ratio of the inorganic mineral raw material, the pore-forming agent, and the binder is (60~85):(5~30):(5~15).
[0013] In some embodiments, in step S1, the particle size of the granules obtained after granulation is 2mm to 20mm; the drying temperature is 60℃ to 120℃, and the drying time is 2h to 8h; the high-temperature sintering temperature is 800℃ to 1200℃, the heating rate is 2℃ / min to 10℃ / min, and the holding time is 1h to 4h.
[0014] In some embodiments, the porous carrier in step S1 has an apparent porosity of 30% to 65%, an average pore size of 0.5 μm to 20 μm, and a compressive strength ≥ 5 MPa.
[0015] In some embodiments, in step S2, the conductive carbon material is selected from at least one of graphite powder, conductive carbon black, and carbon nanotubes;
[0016] The hygroscopic inorganic salt is selected from at least one of sodium chloride, potassium chloride, calcium chloride, magnesium sulfate, and sodium nitrate.
[0017] The corrosion inhibitor is selected from at least one of sodium molybdate, zinc phosphate, sodium gluconate, and benzotriazole;
[0018] The mass ratio of the conductive carbon material, the hygroscopic inorganic salt, and the corrosion inhibitor is (5~15):(60~80):(1~5).
[0019] In some embodiments, in step S2, the solid content of the mixed slurry is 20% to 50%, the vacuum degree of the vacuum permeation is -0.08 MPa to -0.1 MPa, the pressure holding time is 10 min to 60 min, the drying temperature is 60℃ to 120℃, and the drying time is 2 h to 12 h.
[0020] In some embodiments, in step S2, the mass ratio of the porous carrier to the mixed slurry is 1:(2~5), and the impregnation time is 30min~120min.
[0021] In some embodiments, in step S3, the film-forming solution is any one of polyvinyl alcohol aqueous solution, sodium carboxymethyl cellulose aqueous solution, or chitosan acetate solution, and the mass concentration of the film-forming solution is 0.5% to 5%.
[0022] The cross-linking and curing process uses at least one of glutaraldehyde, epichlorohydrin, or calcium ion solution as a cross-linking agent, and the cross-linking and curing time is 5 min to 60 min.
[0023] In some embodiments, in step S3, the thickness of the semi-permeable sustained-release membrane layer is 10 μm to 100 μm, and the water vapor permeability is 50 g / (m²). 2 ·24h)~500g / (m 2 • 24h), swelling degree is 50%~200%;
[0024] The drying temperature is 40℃~80℃, and the drying time is 1h~6h.
[0025] Secondly, the present invention provides a porous sustained-release eco-drag reducer prepared according to the above-described method for preparing a porous sustained-release eco-drag reducer.
[0026] Compared with the prior art, the present invention has the following advantages:
[0027] 1. This invention prepares an inorganic mineral-based porous carrier by high-temperature sintering. It utilizes the dual effects of pore-forming agent decomposition and liquid-phase sintering between mineral particles to form a multi-level pore network structure spanning micropores, mesopores, and macropores. The apparent porosity reaches 30%~65%, the pore size distribution is 0.5μm~20μm, and the compressive strength is ≥5MPa. It takes into account the contradictory requirements of high porosity and high strength, and provides sufficient loading space and stable structural support for conductive active components.
[0028] 2. This invention uses vacuum permeation to compound conductive carbon material, hygroscopic inorganic salt, and corrosion inhibitor in a mass ratio of (5~15):(60~80):(1~5) and load them inside a porous carrier. The hygroscopic inorganic salt absorbs environmental moisture to form a conductive ionic solution, the conductive carbon material constructs a stable electron transport framework, and the corrosion inhibitor inhibits the corrosion of the grounding electrode by corrosive ions. The three work together to achieve a mixed conductivity mechanism of "ionic conductivity + electronic conductivity", making the volume resistivity of the drag-reducing agent ≤5Ω·m. At the same time, the leachate is neutral to weakly alkaline, avoiding the pollution of soil and groundwater by traditional drag-reducing agents.
[0029] 3. This invention modifies the semi-permeable slow-release membrane layer through cross-linking, achieving a water vapor permeability of 50~500 g / (m²). 2 With a swelling degree of 50%~200% (24h), the film layer swells moderately in a humid environment to form hydrated ion channels to ensure the effective release of conductive ions, and shrinks and densifies in a dry environment to slow down water evaporation and ion loss. This gives the drag-reducing agent an adaptive response capability of "absorbing moisture and conducting electricity when it comes into contact with water, and locking in slow release when it loses water", which effectively solves the technical problem of traditional drag-reducing agents releasing too quickly in the early stage and not releasing enough in the later stage, leading to drag reduction failure. Detailed Implementation
[0030] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Unless otherwise defined, the technical or scientific terms used herein should have the ordinary meaning understood by those skilled in the art. The terms "comprising" and similar expressions used herein mean that the element or object preceding the word covers the element or object listed after the word and its equivalents, but does not exclude other elements or objects.
[0031] Example 1
[0032] This embodiment provides a method for preparing a porous, sustained-release, eco-friendly drag-reducing agent, comprising the following steps:
[0033] Step S1: Weigh diatomaceous earth (inorganic mineral raw material), ammonium bicarbonate (pore-forming agent), and polyvinyl alcohol (binder) in a mass ratio of 75:15:10. Mix the three ingredients thoroughly in a mixer, then granulate the mixture in a granulator, screening out particles with a diameter of 5mm~10mm. Place the resulting particles in a drying oven and dry at 80℃ for 4 hours to remove free moisture. Place the dried particles in a high-temperature sintering furnace and heat to 1000℃ at a rate of 5℃ / min, holding for 2 hours for sintering. Cool to room temperature with the furnace to obtain a porous carrier.
[0034] The porous carrier obtained in this embodiment has an apparent porosity of 52%, an average pore size of 8 μm, and a compressive strength of 12 MPa, according to the test results.
[0035] Step S2: Weigh conductive carbon black (conductive carbon material), calcium chloride (hygroscopic inorganic salt), and sodium molybdate (corrosion inhibitor) at a mass ratio of 10:75:3, add them to deionized water, and stir to prepare a mixed slurry with a solid content of 35%. Mix the porous carrier obtained in step S1 with the mixed slurry at a mass ratio of 1:3, place it in a vacuum impregnation tank, evacuate to -0.09 MPa, and maintain the pressure for 30 minutes to allow the mixed slurry to fully penetrate into the pores of the porous carrier under negative pressure. After the pressure maintenance is completed, restore the pressure to normal and continue impregnation for 60 minutes. Remove the impregnated particles and place them in a forced-air drying oven to dry at 80°C for 8 hours, so that the conductive active components are loaded into the pores and surface of the porous carrier, obtaining the loaded carrier.
[0036] Step S3: Prepare a 2% (w / w) polyvinyl alcohol aqueous solution as a film-forming solution. Immerse the loading carrier obtained in step S2 into the film-forming solution for 10 minutes, then remove it and drain off excess solution from the surface. Place the impregnated particles in a 0.5% (w / w) glutaraldehyde solution for cross-linking and curing treatment for 30 minutes, forming a semi-permeable slow-release film layer on the outer surface of the loading carrier. After cross-linking is complete, remove the particles and place them in a drying oven at 60°C for 3 hours to obtain the porous slow-release eco-friendly drag-reducing agent.
[0037] Testing showed that the thickness of the semi-permeable sustained-release membrane layer prepared in this embodiment was 50 μm, and the water vapor permeability was 280 g / (m²). 2 The swelling degree is 130% (24h); the volume resistivity of the finished drag-reducing agent is 2.8Ω·m, and the pH value of the leachate is 7.8.
[0038] Example 2
[0039] This embodiment provides a method for preparing a porous, sustained-release, eco-friendly drag-reducing agent, comprising the following steps:
[0040] Step S1: Weigh zeolite (inorganic mineral raw material), polymethyl methacrylate microspheres (pore-forming agent, average particle size 10 μm), and dextrin (binder) at a mass ratio of 70:20:10. Mix the three components thoroughly in a mixer, then granulate the mixture in a granulator, screening out particles with a diameter of 8 mm to 15 mm. Place the resulting particles in a drying oven and dry at 100°C for 3 hours. Place the dried particles in a high-temperature sintering furnace, heating to 1100°C at a rate of 3°C / min, holding at that temperature for 3 hours for sintering. Cool to room temperature with the furnace to obtain a porous carrier.
[0041] The porous carrier obtained in this embodiment has an apparent porosity of 48%, an average pore size of 12 μm, and a compressive strength of 15 MPa, according to the test results.
[0042] Step S2: Weigh graphite powder (conductive carbon material), magnesium sulfate (hygroscopic inorganic salt), and sodium gluconate (corrosion inhibitor) at a mass ratio of 8:72:5, add them to deionized water, and stir to prepare a mixed slurry with a solid content of 40%. Mix the porous carrier obtained in step S1 with the mixed slurry at a mass ratio of 1:4, place it in a vacuum impregnation tank, evacuate to -0.095 MPa, and hold the pressure for 20 minutes. After the pressure holding is completed, restore the pressure to normal and continue impregnation for 90 minutes. Remove the impregnated particles and place them in a forced-air drying oven to dry at 100°C for 6 hours to obtain the supported carrier.
[0043] Step S3: Prepare a 1.5% (w / w) sodium carboxymethyl cellulose aqueous solution as the film-forming solution. Immerse the loading carrier obtained in step S2 into the film-forming solution for 15 minutes, then remove it and drain off excess solution from the surface. Place the impregnated particles in a 0.3% (w / w) epichlorohydrin solution for crosslinking and curing treatment for 45 minutes. After crosslinking, remove the particles and place them in a drying oven at 50°C for 4 hours to obtain the porous slow-release eco-friendly drag-reducing agent.
[0044] Testing showed that the thickness of the semi-permeable sustained-release membrane layer prepared in this embodiment was 70 μm, and the water vapor permeability was 210 g / (m²). 2 The swelling degree is 160% (24h); the volume resistivity of the finished drag-reducing agent is 3.5Ω·m, and the pH value of the leachate is 8.2.
[0045] Example 3
[0046] This embodiment provides a method for preparing a porous, sustained-release, eco-friendly drag-reducing agent, comprising the following steps:
[0047] Step S1: Weigh bentonite (inorganic mineral raw material), sawdust (pore-forming agent), and starch (binder) in a mass ratio of 80:10:10. Mix the three ingredients thoroughly in a mixer, then granulate the mixture in a granulator, screening out particles with a diameter of 2mm to 8mm. Place the resulting particles in a drying oven and dry at 60℃ for 6 hours. Place the dried particles in a high-temperature sintering furnace, heating to 900℃ at a rate of 8℃ / min, holding at that temperature for 4 hours for sintering. Cool to room temperature with the furnace to obtain a porous carrier.
[0048] The porous carrier obtained in this embodiment has an apparent porosity of 58%, an average pore size of 15 μm, and a compressive strength of 8 MPa, according to the test results.
[0049] Step S2: Weigh carbon nanotubes (conductive carbon material), potassium chloride (hygroscopic inorganic salt), and benzotriazole (corrosion inhibitor) at a mass ratio of 12:78:2, add them to deionized water, and stir to prepare a mixed slurry with a solid content of 30%. Mix the porous support obtained in step S1 with the mixed slurry at a mass ratio of 1:5, place it in a vacuum impregnation tank, evacuate to -0.085 MPa, and maintain the pressure for 45 min. After the pressure maintenance is completed, restore the pressure to normal and continue impregnation for 120 min. Remove the impregnated particles and place them in a forced-air drying oven to dry at 70℃ for 10 h to obtain the supported support.
[0050] Step S3: Prepare a 3% (w / w) chitosan-acetic acid solution as the film-forming solution (chitosan is dissolved in a 1% (v / v) aqueous acetic acid solution). Immerse the loading carrier obtained in step S2 into the film-forming solution for 20 minutes, then remove it and drain off excess solution. Place the impregnated particles in a 2% (w / w) calcium ion solution for crosslinking and curing for 50 minutes. After crosslinking, remove the particles and place them in a drying oven at 45°C for 5 hours to obtain the porous, slow-release, eco-friendly drag-reducing agent.
[0051] Testing showed that the thickness of the semi-permeable sustained-release membrane layer prepared in this embodiment was 80 μm, and the water vapor permeability was 150 g / (m²). 2 The swelling degree is 180% (24h); the volume resistivity of the finished drag-reducing agent is 4.2Ω·m, and the pH value of the leachate is 8.5.
[0052] Comparative Example 1
[0053] This comparative example is basically the same as Example 1, except that no pore-forming agent was added in step S1. Instead, the inorganic mineral raw material (diatomaceous earth) and the binder (polyvinyl alcohol) were directly mixed, granulated, dried, and sintered at a mass ratio of 85:15. The remaining steps are the same as in Example 1.
[0054] Comparative Example 2
[0055] This comparative example is basically the same as Example 1, except that vacuum infiltration was not used in step S2. Instead, the porous carrier was impregnated in the mixed slurry under normal pressure, and the impregnation time was extended to 4 hours. The remaining steps are the same as in Example 1.
[0056] Comparative Example 3
[0057] This comparative example is basically the same as Example 1, except that no crosslinking curing treatment was performed in step S3; instead, the support carrier was immersed in the film-forming solution and then directly removed and dried. The remaining steps are the same as in Example 1.
[0058] The performance testing process for the drag-reducing agents prepared in the above embodiments and comparative examples is as follows:
[0059] (1) Volume resistivity test: Refer to DL / T 887-2004 standard, load the resistance reducing agent sample into the standard test mold, and use the four-electrode method to determine its volume resistivity.
[0060] (2) Test of the loss rate of conductive components: The resistance reducing agent sample was soaked in deionized water for 30 days (simulating long-term rain erosion), and the deionized water was changed every 5 days. After soaking, the mass fraction of the remaining conductive components in the sample was measured and the loss rate was calculated.
[0061] (3) pH test: Take the drag-reducing agent sample and add it to deionized water at a mass ratio of 1:10. After stirring, let it stand for 24 hours and measure the pH value of the supernatant.
[0062] (4) Compressive strength test: The compressive strength of a single particle of porous carrier is determined by a universal testing machine in accordance with GB / T 5072 standard.
[0063] In summary, Comparative Example 1, without the addition of a pore-forming agent, resulted in a carrier porosity of only 22%, insufficient loading of conductive components, and a volume resistivity as high as 18.6 Ω·m, far exceeding the 2.8 Ω·m of Example 1. Comparative Example 2, without vacuum infiltration, had conductive components loaded only on the particle surface, resulting in a loss rate as high as 35.4%, far exceeding the 8.2% of Example 1. Comparative Example 3, without cross-linking and curing, saw the membrane rapidly swell and disintegrate in water immersion, with a loss rate as high as 52.7%, essentially losing its slow-release function. Comparative Example 4, although using a commercially available resistance-reducing agent with acceptable initial conductivity, had a loss rate as high as 78.5%, and the leachate was acidic (pH=6.2), adversely affecting both the metal grounding electrode and the soil environment. The results of these comparative examples fully demonstrate the synergistic contribution and irreplaceable nature of the addition of pore-forming agents, vacuum infiltration, and cross-linking curing treatments in each step of this invention to the overall performance of the final product.
[0064] While embodiments of the present invention have been described in detail above, it will be apparent to those skilled in the art that various modifications and variations can be made to these embodiments. However, it should be understood that such modifications and variations fall within the scope and spirit of the invention as set forth in the claims. Furthermore, the invention described herein may have other embodiments and can be implemented or carried out in various ways.
Claims
1. A method for preparing a porous, sustained-release, eco-friendly drag-reducing agent, characterized in that, Includes the following steps: S1. Inorganic mineral raw materials are mixed with pore-forming agents and binders and granulated, then dried and sintered at high temperature to obtain a porous carrier; S2. The porous carrier is immersed in a mixed slurry containing conductive carbon material, hygroscopic inorganic salt and corrosion inhibitor, and then vacuum infiltrated and dried to load the conductive active components into the pores and surface of the porous carrier, thereby obtaining a loaded carrier. S3. The load carrier is immersed in a film-forming solution, and after being removed, it is cross-linked and cured to form a semi-permeable slow-release film layer on the outer surface of the load carrier. After drying, a porous slow-release eco-friendly drag-reducing agent is obtained.
2. The preparation method of the porous slow-release eco-friendly drag-reducing agent according to claim 1, characterized in that, In step S1, the inorganic mineral raw material includes at least one of diatomite, zeolite, bentonite, and kaolin. The pore-forming agent is selected from at least one of ammonium bicarbonate, ammonium carbonate, polymethyl methacrylate microspheres, and sawdust. The binder is selected from at least one of polyvinyl alcohol, dextrin, and starch; The mass ratio of the inorganic mineral raw material, the pore-forming agent and the binder is (60~85):(5~30):(5~15).
3. The preparation method of the porous slow-release ecological drag-reducing agent according to claim 1, characterized in that, In step S1, the particle size of the granulated particles is 2mm to 20mm, the drying temperature is 60℃ to 120℃, the drying time is 2h to 8h, the high-temperature sintering temperature is 800℃ to 1200℃, the heating rate is 2℃ / min to 10℃ / min, and the holding time is 1h to 4h.
4. The preparation method of the porous slow-release ecological drag-reducing agent according to claim 1, characterized in that, The porous carrier obtained in step S1 has an apparent porosity of 30%~65%, an average pore size of 0.5μm~20μm, and a compressive strength ≥5MPa.
5. The preparation method of the porous slow-release eco-friendly drag-reducing agent according to claim 1, characterized in that, In step S2, the conductive carbon material is selected from at least one of graphite powder, conductive carbon black, and carbon nanotubes. The hygroscopic inorganic salt is selected from at least one of sodium chloride, potassium chloride, calcium chloride, magnesium sulfate, and sodium nitrate. The corrosion inhibitor is selected from at least one of sodium molybdate, zinc phosphate, sodium gluconate, and benzotriazole; The mass ratio of the conductive carbon material, the hygroscopic inorganic salt, and the corrosion inhibitor is (5~15):(60~80):(1~5).
6. The preparation method of the porous slow-release ecological drag-reducing agent according to claim 1, characterized in that, In step S2, the solid content of the mixed slurry is 20%~50%, the vacuum degree of the vacuum permeation is -0.08MPa~-0.1MPa, the pressure holding time is 10min~60min, the drying temperature is 60℃~120℃, and the drying time is 2h~12h.
7. The preparation method of the porous slow-release eco-friendly drag-reducing agent according to claim 1, characterized in that, In step S2, the mass ratio of the porous carrier to the mixed slurry is 1:(2~5), and the impregnation time is 30min~120min.
8. The preparation method of the porous slow-release eco-friendly drag-reducing agent according to claim 1, characterized in that, In step S3, the film-forming solution is any one of polyvinyl alcohol aqueous solution, sodium carboxymethyl cellulose aqueous solution, or chitosan acetate solution, and the mass concentration of the film-forming solution is 0.5%~5%. The cross-linking and curing process uses at least one of glutaraldehyde, epichlorohydrin, or calcium ion solution as a cross-linking agent, and the cross-linking and curing time is 5 min to 60 min.
9. The preparation method of the porous slow-release ecological drag-reducing agent according to claim 1, characterized in that, In step S3, the thickness of the semi-permeable sustained-release membrane layer is 10 μm to 100 μm, and the water vapor permeability is 50 g / (m²). 2 ·24h)~500g / (m 2 • 24h), swelling degree is 50%~200%; The drying temperature is 40℃~80℃, and the drying time is 1h~6h.
10. A porous sustained-release eco-friendly drag-reducing agent prepared by the method of any one of claims 1-9.