Composite surface treatment methods to improve the corrosion resistance of stainless steel sheets

By performing zonal testing and nonlinear polymerization on the surface of stainless steel sheets, local weak points are identified and eliminated, thereby improving the corrosion resistance of stainless steel sheets and solving the problem that existing technologies cannot effectively improve overall corrosion resistance.

CN123063764APending Publication Date: 2026-11-10ZHEJIANG YILI METAL MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611194394.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-07
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing composite surface treatment solutions cannot identify and eliminate weak points where pitting corrosion begins in stainless steel sheets, resulting in the overall corrosion resistance of the sheet being limited to the worst local area and thus unable to be effectively improved.

Method used

The surface of the stainless steel sheet is divided into multiple zones, and parameters such as passivation film thickness, film density, and surface roughness are collected for each zone. The energy of passivation and sealing process compensation is calculated for each zone through maximum-dominated nonlinear aggregation, thereby achieving differentiated compensation treatment for each zone.

Benefits of technology

It improves the overall corrosion resistance of the board and reduces the possibility of local pitting corrosion. By using zoned sensing and precise allocation of compensation resources, it solves the problem of limited overall performance caused by the "weakest link" effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123063764A_ABST
    Figure CN123063764A_ABST
Patent Text Reader

Abstract

This application relates to the field of stainless steel surface treatment technology, and particularly to a composite surface treatment method for improving the corrosion resistance of stainless steel sheets. The method includes: dividing the surface of the stainless steel sheet to be treated into multiple surface partitions and obtaining surface state parameters for each partition; calculating film thickness degradation components, density degradation components, and roughness degradation components based on the surface state parameters and corresponding process target values; performing maximum-dominated nonlinear aggregation on the film thickness degradation components and density degradation components to obtain passivation channel degradation risk factors, and determining closed channel degradation risk factors based on the roughness degradation components; determining the passivation process compensation treatment energy, determining the closed process compensation treatment energy, performing passivation compensation treatment according to the passivation process compensation treatment energy, and performing closed compensation treatment according to the closed process compensation treatment energy. This method is beneficial for improving the overall pitting corrosion resistance of the sheet and reducing the possibility of local pitting corrosion initiation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of stainless steel surface treatment technology, and particularly relates to a composite surface treatment method for improving the corrosion resistance of stainless steel sheets. Background Technology

[0002] The corrosion resistance of stainless steel sheets depends on the integrity and density of their surface passivation film. In corrosive environments containing chloride ions, pitting corrosion easily initiates at weak points in the passivation film. Once pitting occurs, it rapidly propagates into the substrate, often causing premature failure of the sheet material and even the entire equipment. To improve corrosion resistance, industrial processes commonly employ composite surface treatments for stainless steel sheets. This involves first strengthening the passivation film through a passivation process, followed by a sealing process to form a sealing film on top of the passivation film, creating a composite film layer that synergistically resists corrosive media. However, in actual production, due to fluctuations in preceding processes such as rolling, annealing, and pickling, the initial state of the surface of stainless steel sheets is not uniform across different regions: the passivation film thickness, film density, and surface roughness vary in different areas. The overall pitting corrosion resistance of the sheet material follows the "weakest link" effect, determined by the worst-performing local area, rather than by the average state. If even one area has a thinner passivation film, lower density, or higher roughness, that area becomes a weak point for pitting corrosion, significantly shortening the corrosion resistance life of the entire sheet.

[0003] In the existing technology, the control scheme of the existing composite surface treatment uses a mean-type single parameter as feedback and a uniform overall roller pressure / speed adjustment as the execution method. In the process of averaging, the feedback quantity systematically dilutes the local extreme deterioration. Moreover, its execution mechanism is a uniform overall adjustment throughout the line and does not have the physical ability to implement differentiated compensation for specific areas. Therefore, it cannot identify or eliminate the weak points of pitting corrosion on the stainless steel plate, resulting in the overall corrosion resistance of the plate being limited to the worst local area and unable to be effectively improved. Summary of the Invention

[0004] This application provides a composite surface treatment method to improve the corrosion resistance of stainless steel sheets, which can improve the problem that existing control schemes cannot identify and eliminate weak points where local pitting corrosion begins to occur in the sheet.

[0005] In a first aspect, embodiments of this application provide a composite surface treatment method for improving the corrosion resistance of stainless steel sheets, applied to a composite surface treatment equipment for stainless steel sheets. The equipment includes a control device, a zone detection unit, a passivation zone execution mechanism for a passivation process, and a sealing zone execution mechanism for a sealing process. The control device is electrically connected to the zone detection unit, the passivation zone execution mechanism, and the sealing zone execution mechanism, respectively. The method includes: The surface of the stainless steel sheet to be treated is divided into multiple surface partitions, and the control device controls the partition detection unit to acquire the surface state parameters of each surface partition; wherein, the surface state parameters include passivation film thickness characterization parameters, film density characterization parameters, and surface roughness parameters; Based on the surface state parameters of each surface partition and the corresponding process target value, the film thickness degradation component, density degradation component and roughness degradation component of each surface partition are calculated. The film thickness degradation component and the density degradation component of each surface partition are subjected to maximum-dominant nonlinear aggregation to obtain the passivation channel degradation risk factor of each surface partition, and the closed channel degradation risk factor of each surface partition is determined according to the roughness degradation component. The passivation process compensation energy for each surface partition is determined based on the passivation channel degradation risk factor, and the sealing process compensation energy for each surface partition is determined based on the sealing channel degradation risk factor. The control device controls the passivation partition execution mechanism to perform partition-differentiated passivation compensation processing according to the passivation process compensation energy for each surface partition, and controls the sealing partition execution mechanism to perform partition-differentiated sealing compensation processing according to the sealing process compensation energy for each surface partition.

[0006] The technical solutions described in this application embodiment have at least the following technical effects: The composite surface treatment method for improving the corrosion resistance of stainless steel sheets provided in this application divides the surface to be treated into multiple surface partitions and collects three heterogeneous state parameters—passivation film thickness, film density, and surface roughness—for each partition. This ensures that the state of any local area on the sheet that may become a pitting corrosion weak point is independently perceived, eliminating the information loss caused by mean-based indicators for local extreme degradation. The partitioned collection of these three heterogeneous parameters allows for the independent quantification of the film thickness, density, and roughness state of each local area that may become a pitting corrosion weak point, providing a complete data foundation for subsequent partition-based assessment of degradation risk and implementation of differentiated compensation. Then, a maximum-dominated nonlinear aggregation is performed on the film thickness and density degradation components of each surface partition to obtain a passivation channel degradation risk factor. A closed channel degradation risk factor is determined based on the roughness degradation component. The maximum-dominated nonlinear aggregation uses the most severe degradation component as the dominant term of the risk factor and a weighted term of the sum of degradation components as a secondary correction term. This ensures that when extreme degradation occurs in any dimension of any partition, the risk factor of that partition will inevitably become prominent and trigger compensation. The compensation method eliminates mean dilution from a mathematical structure perspective. This aggregation method is isomorphic to the physical law of the "barrel effect" in pitting corrosion initiation, which is not present in mean-based feedback or weighted average risk coefficients. Then, based on the passivation channel degradation risk factor and the closed channel degradation risk factor, the compensation energy for the passivation process and the compensation energy for the closed process are determined respectively. The control device controls the passivation partition execution mechanism and the closed partition execution mechanism to perform the compensation process in a differentiated manner. The decoupling mapping between the degradation component and the process channel allows the film thickness and density degradation to be compensated by the passivation process, while the roughness degradation is compensated by the closed process. Process compensation, with compensation energy corresponding one-to-one with the physical causes of degradation, reduces the cross-interference caused by a single energy index driving two processes and also reduces the over-processing of irrelevant processes. This application solidifies the identification of the weakest link and the targeted allocation of compensation resources on a mathematical structure through partitioned heterogeneous perception, maximum value-dominated nonlinear aggregation, and dual-channel decoupling. This allows the compensation energy to be accurately positioned according to the causes and degrees of degradation, thus resolving the dilemma where the overall corrosion resistance of the board is determined by the worst local area. This is beneficial to improving the overall pitting corrosion resistance of the board and reducing the possibility of local pitting corrosion initiation.

[0007] Secondly, embodiments of this application provide a composite surface treatment system for improving the corrosion resistance of stainless steel sheets, applied to a composite surface treatment equipment for stainless steel sheets. The composite surface treatment equipment includes a control device, a zone detection unit, a passivation zone execution mechanism for the passivation process, and a sealing zone execution mechanism for the sealing process. The control device is electrically connected to the zone detection unit, the passivation zone execution mechanism, and the sealing zone execution mechanism, respectively. The system includes: The acquisition module is used to divide the surface of the stainless steel sheet to be treated into multiple surface partitions. The control device controls the partition detection unit to acquire the surface state parameters of each surface partition. The surface state parameters include passivation film thickness characterization parameters, film density characterization parameters, and surface roughness parameters. The calculation module is used to calculate the film thickness degradation component, density degradation component and roughness degradation component of each surface partition based on the surface state parameters of each surface partition and the corresponding process target value. The determination module is used to perform maximum-dominant nonlinear aggregation on the film thickness degradation component and the density degradation component of each surface partition to obtain the passivation channel degradation risk factor of each surface partition, and to determine the closed channel degradation risk factor of each surface partition based on the roughness degradation component. An execution module is used to determine the passivation process compensation processing energy of each surface partition based on the passivation channel degradation risk factor, and to determine the sealing process compensation processing energy of each surface partition based on the sealing channel degradation risk factor. The control device controls the passivation partition execution mechanism to perform partition-differentiated passivation compensation processing according to the passivation process compensation processing energy of each surface partition, and controls the sealing partition execution mechanism to perform partition-differentiated sealing compensation processing according to the sealing process compensation processing energy of each surface partition.

[0008] Thirdly, embodiments of this application provide a composite surface treatment device for improving the corrosion resistance of stainless steel sheets, including a control device, a partition detection unit, a passivation partition execution mechanism for a passivation process, and a sealing partition execution mechanism for a sealing process. The partition detection unit includes an electrochemical probe and a laser roughness meter. The control device is electrically connected to the partition detection unit, the passivation partition execution mechanism, and the sealing partition execution mechanism, respectively. The control device includes a memory, a processor, and a computer program stored in the memory and executable on the processor. When the processor executes the computer program, it implements the method described in the first aspect above.

[0009] Fourthly, embodiments of this application provide a computer-readable storage medium storing a computer program that, when executed by a processor, implements the method described in the first aspect above.

[0010] Fifthly, embodiments of this application provide a computer program product that, when running on a composite surface treatment device for improving the corrosion resistance of stainless steel sheets, causes the composite surface treatment device for improving the corrosion resistance of stainless steel sheets to perform the composite surface treatment method for improving the corrosion resistance of stainless steel sheets described in the first aspect.

[0011] It is understood that the beneficial effects of the second to fifth aspects mentioned above can be found in the relevant descriptions in the first aspect mentioned above, and will not be repeated here. Attached Figure Description

[0012] To more clearly illustrate the technical solutions in the embodiments of this application, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0013] Figure 1 This is a schematic flowchart of a composite surface treatment method for improving the corrosion resistance of stainless steel sheets provided in an embodiment of this application. Figure 2 This is a schematic diagram comparing the characteristics of maximum value-dominated nonlinear aggregation and mean-value-based aggregation provided in the embodiments of this application; Figure 3 This is a schematic diagram of the limiting characteristic curve of the compensation processing energy as a function of the degradation risk factor, provided in the embodiments of this application. Figure 4 This is a schematic diagram illustrating the convergence process of the retest risk factor with the number of iterations in various scenarios provided in the embodiments of this application; Figure 5 This is a schematic diagram of the composite surface treatment system for improving the corrosion resistance of stainless steel sheets provided in the embodiments of this application; Figure 6 This is a schematic diagram of the control device of the composite surface treatment equipment for improving the corrosion resistance of stainless steel sheets provided in the embodiments of this application. Detailed Implementation

[0014] In the following description, specific details such as particular system architectures and techniques are set forth for illustrative purposes and not for limitation, in order to provide a thorough understanding of the embodiments of this application. However, those skilled in the art will understand that this application may also be implemented in other embodiments without these specific details. In other instances, detailed descriptions of well-known systems, apparatuses, circuits, and methods have been omitted so as not to obscure the description of this application with unnecessary detail.

[0015] It should be understood that, when used in this application specification and the appended claims, the term "comprising" indicates the presence of the described features, integrals, steps, operations, elements and / or components, but does not exclude the presence or addition of one or more other features, integrals, steps, operations, elements, components and / or a collection thereof.

[0016] Related technologies provide a closed-loop control scheme for the passivation film on the strip surface. This scheme uses an online thickness gauge to detect the passivation film thickness in real time, calculates the average film thickness over a certain length or time period, subtracts the target value from the average film thickness to obtain the deviation, and then sequentially adjusts process parameters such as the coating roller pressure, the pressure difference between the feed roller and the coating roller, and the speed difference based on the deviation to bring the average film thickness back to the target range. The fundamental drawbacks of this scheme are: firstly, the feedback quantity is the average film thickness across the entire line, a single-parameter indicator of average value. Severe localized degradation in individual areas is diluted by the data from a large number of normal areas during the averaging process, and the control system may not be able to detect or eliminate weak points where pitting corrosion begins to occur; secondly, it only collects the single parameter of film thickness, while pitting corrosion initiation is also affected by film density and surface roughness. Areas with acceptable film thickness but insufficient density or excessive roughness remain weak points; thirdly, its execution method is uniform adjustment of roller pressure and speed across the entire line. Even if local anomalies are detected in the detection process, it may not have the ability to implement differentiated compensation for specific areas.

[0017] Another related technology provides a composite surface treatment solution for stainless steel. This method involves determining the protection potential and passivation potential through anodic polarization, electrochemically passivating the entire stainless steel within the potential window defined by these two parameters, and then coating it with a self-assembled molecular film to form a composite protection. This type of solution performs a one-size-fits-all treatment on the entire surface: the entire surface receives the same passivation potential and the same treatment time. It neither perceives the state differences between regions nor provides a quantitative convergence determination after treatment. Locally weak areas may still remain after the overall treatment, and this remains undetected.

[0018] Therefore, the technical problem that the existing technology urgently needs to solve is that the existing control schemes for composite surface treatment use average single parameters as feedback and overall uniformity as the execution method. They cannot identify and eliminate local pitting corrosion initiation weak points on stainless steel plates, resulting in the overall corrosion resistance of the plate being limited to the worst local area and unable to be effectively improved.

[0019] To address the aforementioned problems, this application provides a composite surface treatment method for improving the corrosion resistance of stainless steel sheets. This method divides the surface to be treated into multiple surface partitions and collects three heterogeneous state parameters—passivation film thickness, film density, and surface roughness—for each partition. This ensures that the state of any local area on the board that could potentially become a pitting corrosion weak point is independently perceived, eliminating the information loss caused by mean-based indicators for local extreme degradation. The partitioned collection of these three heterogeneous parameters allows for the independent quantification of the film thickness, density, and roughness state of each local area that could potentially become a pitting corrosion weak point, providing a complete data foundation for subsequent partition-based degradation risk assessment and differentiated compensation. Then, a maximum-dominated nonlinear aggregation is performed on the film thickness and density degradation components of each surface partition to obtain the passivation channel degradation risk factor. The closed channel degradation risk factor is determined based on the roughness degradation component. The maximum-dominated nonlinear aggregation uses the most severe degradation component as the dominant term of the risk factor and the weighted term of the sum of degradation components as the secondary correction term. This ensures that when extreme degradation occurs in any dimension of any partition, the risk factor of that partition will inevitably become prominent and trigger compensation, mathematically eliminating the possibility of extreme degradation. Mean dilution, this polymerization method is isomorphic to the physical law of the "barrel effect" initiation of pitting corrosion, which is not present in mean-based feedback or weighted average risk coefficients. Then, based on the passivation channel degradation risk factor and the closed channel degradation risk factor, the compensation energy for the passivation process and the compensation energy for the closed process are determined respectively. The control device controls the passivation partition execution mechanism and the closed partition execution mechanism to perform compensation processes in a differentiated manner in each partition. The decoupling mapping between the degradation component and the process channel allows the passivation process to compensate for film thickness and density degradation, while the closed process compensates for roughness degradation. The compensation energy corresponds one-to-one with the physical causes of degradation, which reduces the cross-interference caused by the single energy index driving the two processes and also reduces the over-processing of irrelevant processes. This application solidifies the identification of the weakest link and the targeted allocation of compensation resources on the mathematical structure through partitioned heterogeneous perception, maximum value-dominated nonlinear aggregation and dual-channel decoupling. This allows the compensation energy to be accurately positioned according to the causes and degree of degradation, thus resolving the dilemma that the overall corrosion resistance of the board is determined by the worst local area. This is conducive to improving the overall pitting corrosion resistance of the board and reducing the possibility of local pitting corrosion initiation.

[0020] The composite surface treatment method for improving the corrosion resistance of stainless steel sheets provided in this application embodiment can be applied to a composite surface treatment device for improving the corrosion resistance of stainless steel sheets. In this case, the composite surface treatment device for improving the corrosion resistance of stainless steel sheets is the subject of execution of the composite surface treatment method for improving the corrosion resistance of stainless steel sheets provided in this application embodiment. This application embodiment does not impose any restrictions on the specific type of composite surface treatment device for improving the corrosion resistance of stainless steel sheets.

[0021] For example, a composite surface treatment device for improving the corrosion resistance of stainless steel sheets may include a control device, a partition detection unit, a passivation partition execution mechanism for the passivation process, and a sealing partition execution mechanism for the sealing process. The partition detection unit includes an electrochemical probe and a laser roughness meter. The control device is electrically connected to the partition detection unit, the passivation partition execution mechanism, and the sealing partition execution mechanism, respectively. The electrochemical probe is a sensor used for in-situ measurement of the electrochemical parameters of the passivation film on the metal surface. It obtains two types of parameters: the equivalent capacitance of the passivation film and the passivation current density, by applying a small AC perturbation to the surface being measured or extracting the equivalent capacitance from the impedance response and applying a potentiodynamic scan to obtain the polarization curve. In one specific implementation, the electrochemical probes are arranged in a probe array in corresponding positions on each surface partition. Multiple probe units correspond one-to-one with each surface partition along the width of the plate. Each probe unit is controlled by a multiplexer or scanning mechanism to be connected in turn to the excitation source and the impedance analysis circuit. The impedance analysis circuit sends the response signal back to the data acquisition module of the control device through a signal conditioning circuit. The electrochemical probe and the laser roughness meter together constitute the partition detection unit, realizing the in-situ acquisition of three types of heterogeneous state parameters. The electrochemical probe operates using a parallel-plate capacitance model: the passivation film appears as a uniform dielectric layer sandwiched between the metal substrate and the electrolyte, and its equivalent capacitance is inversely proportional to the film thickness; the film thickness can be inverted by measuring the equivalent capacitance. The passivation current density is read from the polarization curve obtained by potentiodynamic scanning within the passivation plateau region. Both types of electrochemical parameters are acquired by the same probe unit at the same measurement location, ensuring spatial consistency between the film thickness and density parameters.

[0022] A laser roughness meter is an instrument that measures the microscopic geometric undulations of a surface using a non-contact optical method. It performs a line scan along the diagonal direction of each surface partition, and takes the arithmetic mean deviation of the profile along the scan line as the surface roughness parameter of that partition. In one specific implementation, the laser roughness meter includes a laser displacement sensor and a scanning axis or follower mechanism that drives it to reciprocate along the width of the plate. This scanning axis or follower mechanism is synchronized with the positioning signal of the conveyor rollers, ensuring that the roughness line scan falls within the corresponding surface partition. The laser roughness meter, as claimed, is the detection instrument for acquiring surface roughness parameters. Its non-contact measurement and electrochemical detection are performed in parallel, without additional time commitment during the detection cycle.

[0023] It can be understood that the passivation partitioning actuator is a hardware unit driven by a control device and independently adjusts the passivation processing energy input according to partition. Its partitioned passivation electrode group applies electrochemical passivation energy to the corresponding surface partition. In a specific implementation, the partitioned passivation electrode group consists of several electrode pairs and a partition switching matrix. Under the command of the control device, the partition switching matrix connects the controllable power supply to the electrode pairs of the corresponding partition as needed.

[0024] The zoned sealing actuator is a hardware unit driven by a control device that independently adjusts the sealing energy input for each zone. Its zoned sealant spraying valve assembly sprays sealant independently for each zone, and its zoned heating unit independently controls the curing temperature for each zone. Together, they achieve the filling and leveling of surface valleys by the zoned sealing film. In one specific implementation, the zoned sealant spraying valve assembly consists of spraying valves, spraying manifolds, and a paint supply device corresponding to each zone. The opening degree of the spraying valves is controlled by the zoned sealant spraying quantity command, and the sealant is sprayed independently to the corresponding zone through the spraying manifold. The zoned heating unit consists of heating elements corresponding to each zone and a temperature feedback loop. The heating elements apply curing heating energy to the corresponding zone, and the temperature sensor collects the surface temperature of the zone in real time and transmits it back to the control device to form a temperature control closed loop, allowing the sealing film to cure at a controlled temperature. The zoned sealing actuator is communicatively connected to the control device and receives compensation energy commands calculated based on the degradation risk factor of the zoned sealing channel.

[0025] The control device can be a programmable logic controller or an industrial control computer, etc. The data acquisition module of the control device is electrically connected to the partition detection unit via a signal conditioning circuit, forming a detection signal upload link from the detection unit to the control device; the communication interface module of the control device is electrically connected to the passivation partition actuator and the closure partition actuator via a fieldbus or industrial Ethernet, forming a control command link from the control device to the actuator; the passivation partition actuator and the closure partition actuator are respectively directed towards the stainless steel plate in the direction of action, applying passivation and closure compensation to the corresponding partitions.

[0026] To better understand the composite surface treatment method for improving the corrosion resistance of stainless steel sheets provided in the embodiments of this application, the specific implementation process of the composite surface treatment method for improving the corrosion resistance of stainless steel sheets provided in the embodiments of this application will be described by way of example below.

[0027] Figure 1 A schematic flowchart of a composite surface treatment method for improving the corrosion resistance of stainless steel sheets, provided in an embodiment of this application, is shown. The composite surface treatment method for improving the corrosion resistance of stainless steel sheets includes: S100 divides the surface of the stainless steel sheet to be treated into multiple surface partitions, and the control device controls the partition detection unit to obtain the surface state parameters of each surface partition; among which, the surface state parameters include passivation film thickness characterization parameters, film density characterization parameters, and surface roughness parameters.

[0028] It can be understood that surface partitioning refers to dividing the surface to be treated into several rectangular sub-regions along the width and length directions of the stainless steel sheet. Each surface partition is the smallest control unit for subsequent state perception, risk assessment and compensation execution. The passivation film thickness characterization parameter is a quantity that reflects the thickness of the passivation film in the partition. The film density characterization parameter is a quantity that reflects the density of the passivation film in the partition, i.e., the number of defects. The surface roughness parameter is a quantity that reflects the degree of micro-undulation of the surface in the partition. The three correspond to the three types of physical causes of pitting corrosion initiation, namely, insufficient film barrier in thin areas, dense ion channels in sparse areas, and retention of corrosive media in rough areas.

[0029] For example, film thickness and density parameters can be obtained in situ and non-destructively using electrochemical probes arranged in zones, and surface roughness parameters can be obtained using a laser roughness meter, so that the three types of heterogeneous state parameters can be collected synchronously at the same zone location; alternatively, the three types of parameters can be obtained by integrating the electrochemical probe and the laser probe into the same follow-up detection mechanism and scanning the plate zone by zone along the direction of travel, etc., but not limited to these.

[0030] In this embodiment, the surface to be treated is divided into multiple surface partitions and three types of heterogeneous state parameters are collected for each partition. This allows the state of any local area on the board that may become a pitting corrosion weak point to be independently perceived, providing a complete data foundation for subsequent assessment of degradation risk by partition and implementation of differentiated compensation.

[0031] In one possible implementation, S100, the control device controls the partition detection unit to acquire surface state parameters of each surface partition, including: S110, the control device controls the electrochemical probes arranged in the control zones to collect the equivalent capacitance of the passivation film in each surface zone.

[0032] It can be understood that the passivation film equivalent capacitance is the equivalent capacitance value exhibited by the passivation film in the electrochemical measurement system. Its magnitude is inversely proportional to the passivation film thickness and is an intermediate measurement for inverting film thickness. Electrochemical probes are arranged in sections at corresponding positions on each surface section. Small AC perturbations are applied under unified control by the control device to extract the equivalent capacitance from the impedance response.

[0033] In this embodiment, the equivalent capacitance is used as an intermediate quantity for film thickness inversion, so that film thickness detection and density detection share the same set of partitioned electrochemical probes, reducing the types of detection hardware and allowing the two types of parameters to be obtained at the same measurement location.

[0034] S120, based on the equivalent capacitance of the passivation film, the passivation film thickness characterization parameters of each surface partition are obtained.

[0035] It can be understood that the passivation film thickness parameter is a quantity that reflects the actual thickness of the passivation film in a given region, derived from the equivalent capacitance of the passivation film. The passivation film can be approximated as a uniform dielectric layer sandwiched between the metal substrate and the electrolyte. Its equivalent capacitance is directly proportional to the dielectric constant and area, and inversely proportional to the thickness. Therefore, the thickness can be derived from the capacitance.

[0036] In this embodiment, the calibrated relative permittivity is used for conversion, so that the film thickness inversion of different batches of plates has a consistent benchmark.

[0037] In one possible implementation, S120, the passivation film thickness characterization parameters for each surface partition are calculated based on the equivalent capacitance of the passivation film, including: S121, the product of the passivation film relative permittivity, the vacuum permittivity, and the effective measurement area of ​​the electrochemical probe is divided by the equivalent capacitance of the passivation film in each surface partition to obtain the passivation film thickness characterization parameter for each surface partition; where the passivation film relative permittivity is the relative permittivity of the passivation film material, the vacuum permittivity is the permittivity in a vacuum, and the effective measurement area of ​​the electrochemical probe is the effective measurement area in contact between the probe and the surface being measured.

[0038] This conversion can be understood as a direct inversion of the parallel-plate capacitor model, and its mathematical expression is as follows: in, The passivation film thickness characterization parameter for the i-th surface region is derived from the measured equivalent capacitance of the i-th surface region in this step. The inversion yields; The relative permittivity of the passivation film is 15.6. For the passivation film mainly composed of chromium oxide on the surface of stainless steel, this value can be taken as 15.6. This value is obtained by calibrating the film thickness and capacitance by combining the actual measurements of the standard sample of the same grade. The vacuum permittivity is taken as 8.854 × 10⁻⁶. -12 F / m; A is the effective measurement area of ​​the electrochemical probe, which is determined by the probe's structural dimensions.

[0039] In this embodiment, a calibrated relative permittivity is used for conversion, ensuring a consistent benchmark for film thickness inversion and preventing the calculation of film thickness degradation components from being affected by individual probe differences. Capacitance-based film thickness inversion achieves in-situ, non-destructive quantitative analysis of nanoscale passivation films. Compared to offline sampling methods, this approach allows for zone-by-zone film thickness acquisition without interrupting production line operations, providing real-time data for zone-specific compensation.

[0040] S130, the control device controls the electrochemical probe to collect the passivation current density of each surface partition in the potentiodynamic scanning mode, and uses the passivation current density as a parameter to characterize the film density.

[0041] It can be understood that passivation current density refers to the current density required to maintain the dynamic equilibrium of the passivation film when the metal is in a passivated state. The denser the passivation film, the fewer the ion migration channels in the film and the smaller the current required to maintain the passivation state. Therefore, passivation current density is an electrochemical characterization of film density, and the larger the value, the worse the density.

[0042] In this embodiment, the passivation current density is used as a parameter to characterize the film density, transforming the density of microscopic defects in the film, which is difficult to measure directly, into a macroscopic electrochemical quantity that can be obtained online, thus bringing the key initiation factor of density-induced corrosion into the sensing range of closed-loop control.

[0043] In one possible implementation, S130, the control device controls the electrochemical probe to acquire the passivation current density of each surface partition in a potentiodynamic scanning manner, including: S131, the control device controls the electrochemical probe to perform potentiodynamic scanning at a preset scanning rate within a preset potential range to obtain the polarization curves of each surface partition; based on the polarization curves, the passivation plateau range where the current density changes with potential less than a preset fluctuation limit is determined, and the current density corresponding to the midpoint potential of the passivation plateau range is determined as the passivation current density of the corresponding surface partition.

[0044] It can be understood that the electrochemical probe acquires this parameter using a potentiodynamic scanning method, that is, controlling the probe to continuously change the potential applied to the surface under test at a constant rate and simultaneously recording the current response. The resulting potential-current density relationship is the polarization curve. The passivation plateau is a flat section on the polarization curve where the current density is insensitive to potential changes, corresponding to the potential range in which the passivation film is in a stable passivation state. The preset scan rate can be 2mV / s, and the preset potential range can be -0.1V to +0.6V relative to a saturated calomel electrode, covering the typical passivation region of austenitic stainless steel in neutral and weakly acidic media. The preset fluctuation limit can be set to a current density change of no more than 10% within every 100mV potential change. The longest continuous potential range that meets this condition is determined as the passivation plateau range. Using the current density corresponding to the midpoint potential of the passivation plateau range as the passivation current density can avoid reading distortion when transitioning from the plateau ends to the activation region or the over-passivation region.

[0045] In this embodiment, the electrochemical probes of each surface partition perform scanning in parallel, with each scan taking approximately 350 seconds. All partitions are completed in parallel at once, ensuring that the detection cycle matches the production line cycle. Using the reading at the midpoint of the platform interval as the passivation current density ensures that the density characterization quantity of different partitions and different batches has a strictly consistent reading caliber, eliminating the randomness caused by manual point selection. Hidden weak partitions with adequate film thickness but insufficient density no longer escape from the control system.

[0046] S140, the control device controls the laser roughness meter to collect surface roughness parameters of each surface zone.

[0047] It is understandable that surface roughness is a parameter describing the microscopic geometric undulations of a surface, which can be characterized by the arithmetic mean deviation of the profile. The greater the roughness, the deeper the surface micro-valve, and the easier it is for corrosive media to remain in the valleys, forming a local occlusion environment, which becomes a geometric inducement for pitting corrosion. At the same time, excessive roughness also makes it difficult for sealants to completely cover the surface. The laser roughness meter performs a line scan along the diagonal direction of each surface partition in a non-contact manner, and takes the arithmetic mean deviation of the profile on the scan line as the surface roughness parameter of that partition. The scanning process is performed in parallel with electrochemical detection without occupying additional detection cycles.

[0048] In this embodiment, the degradation cause of roughness (geometric dimension) is included in the partitioned state profile along with the degradation causes of film thickness and density (film layer dimensions). The three heterogeneous parameters together constitute a complete perception of the risk of pitting corrosion initiation.

[0049] S200 calculates the film thickness degradation component, density degradation component, and roughness degradation component of each surface partition based on the surface state parameters of each surface partition and the corresponding process target value.

[0050] It can be understood that the degradation component refers to a dimensionless quantity obtained by normalizing the deviation of a certain surface condition parameter from its process target value to the range of 0 to 1, where 0 represents no degradation and 1 represents the most severe degradation defined by the normalization benchmark. The film thickness degradation component, density degradation component, and roughness degradation component correspond to the degree of degradation of the three types of parameters, respectively. The process target values ​​include the passivation film thickness process target value, the film density process target value, and the surface roughness process target value, which are determined according to the corrosion resistance design requirements of the plate grade and the service environment.

[0051] For example, the film thickness, density, and roughness can be calculated by using the process target value corresponding to each surface state parameter as a benchmark and normalizing the deviation between the measured value and the target value to a preset range, so that the degradation of each dimension is measured by its own acceptance standard; or an independently set normalized benchmark value can be introduced to each state parameter for normalization calculation, etc., but not limited to this.

[0052] In this embodiment of the application, the normalization benchmark adopts the process target value of each parameter or the independently set normalization benchmark value, rather than the average value of the whole board, so that normal process differences between intervals will not be misjudged as degradation.

[0053] In one possible implementation, S200, based on the surface state parameters of each surface partition and the corresponding process target values, calculates the film thickness degradation component, density degradation component, and roughness degradation component of each surface partition, including: S210, based on the passivation film thickness characterization parameters and the passivation film thickness process target value of each surface partition, calculate the film thickness degradation component of each surface partition.

[0054] It is understandable that the direction of film thickness degradation is that the thinner the film, the more dangerous it is. Therefore, it is normalized by subtracting the measured value from the process target value and then dividing by the process target value. The mathematical expression of the film thickness degradation component is as follows: Among them, δ d,i d represents the film thickness degradation component of the i-th surface partition; i The passivation film thickness characterization parameter for the i-th surface partition obtained in step S120; d tar is the target value for the passivation film thickness process; clip[·] is a limiting function that restricts the input value to between 0 and 1, outputting 0 when the input is less than 0 and 1 when it is greater than 1. The degradation component is 0 when the measured film thickness equals the target value, and the degradation component tends to 1 when the measured film thickness approaches 0.

[0055] In this embodiment, a film thickness exceeding the process target value is considered as no degradation rather than negative degradation. An excessively thick passivation film does not constitute a cause of pitting corrosion. Allowing negative values ​​to participate in subsequent polymerization would incorrectly compensate for actual degradation in other dimensions. Directional normalization by subtracting the measured value from the target ensures that any degree of thinning in the film thickness dimension is positively vectorized as degradation, reducing the problem of mean-based indicators canceling out thicker and thinner regions.

[0056] S220, based on the film density characterization parameters and film density process target values ​​of each surface partition, calculates the density degradation component of each surface partition.

[0057] It is understandable that the direction of density degradation is that the higher the passivation current density, the more porous and dangerous the film layer becomes. Therefore, normalization is performed by subtracting the process target value from the measured value. The mathematical expression of the density degradation component is: Among them, δ j,i Let j be the density degradation component of the i-th surface partition; i The passivation current density of the i-th surface region acquired in step S130; j tar The target value for film density is determined by the statistical distribution of qualified samples of the same grade; j ref The density normalization reference value is obtained by calibrating the difference between the upper limit of the passivation current density distribution of qualified samples and the pitting corrosion sensitivity threshold.

[0058] In this embodiment of the application, j ref Independent of j tar The setting allows the sensitivity of the density degradation component to be individually tuned based on the pitting sensitivity of the grade, with a smaller j value selected for grades sensitive to pitting. ref This can improve the response sensitivity to density degradation.

[0059] S230, based on the surface roughness parameters and surface roughness process target values ​​of each surface partition, calculates the roughness degradation component of each surface partition.

[0060] It is understandable that the direction of roughness degradation is that the greater the roughness, the more dangerous it is, and the normalized form is consistent with the density degradation component. The mathematical expression of the roughness degradation component is as follows: .in, Let be the roughness degradation component of the i-th surface partition; is the surface roughness parameter of the i-th surface partition collected in step S140; is the target value of the surface roughness process, which is determined by the sealing agent's ability to completely cover the surface and the medium retention sensitivity of the service environment; The roughness normalization reference value is obtained by taking the difference between the upper limit of the roughness that can be effectively leveled by the closed process and the process target value.

[0061] In this embodiment, the roughness degradation component constitutes the degradation risk factor of the closed channel independently and does not participate in the aggregation of the passivation channel. This is because the energy input of the passivation process acts on the growth and densification of the film layer and has almost no effect on the surface geometry. Roughness degradation can only be compensated by the sealing process by filling the valleys with a sealant.

[0062] S300 performs maximum-dominant nonlinear aggregation on the film thickness degradation component and density degradation component of each surface partition to obtain the passivation channel degradation risk factor of each surface partition, and determines the closed channel degradation risk factor of each surface partition based on the roughness degradation component.

[0063] It can be understood that maximum-dominated nonlinear aggregation refers to an aggregation method in which the maximum value among each degradation component is used as the dominant term of the aggregation result, and the weighted term of the sum of each degradation component is used as the secondary correction term. The passivation channel degradation risk factor and the closed channel degradation risk factor are the partition-level risk quantities that drive the compensation of the passivation process and the compensation of the closed process, respectively. The film thickness degradation component and the density degradation component both belong to the degradation of the passivation film itself and enter the passivation channel after aggregation; the roughness degradation component belongs to the degradation of the surface geometry and enters the closed channel separately. The division between the two channels is based on the correspondence between the physical cause of the degradation and the process that can compensate for the degradation.

[0064] For example, the most severe degradation among the film thickness degradation component and the density degradation component can be retained as the dominant term for aggregation, and the concurrent degradation of the two components can be superimposed as a secondary correction term with a preset weight between 0 and 1. This allows the aggregation result to be determined by the worst dimension and reflect the multidimensional concurrent hazards, thereby obtaining the degradation risk factor of the passivation channel, and mapping the roughness dimension separately as the degradation risk factor of the closed channel. Alternatively, the same aggregation behavior can be approximated by the generalized p-norm or the soft maximum function, so that the aggregation result does not decrease monotonically with the larger of the two components, and an upward buoyancy is added when both components are high, etc., but not limited to these.

[0065] In this embodiment, the normalization reference adopts the process target value of each parameter or the independently set normalization reference value, rather than the average value of the whole board. The film thickness and density degradation components enter the passivation channel after aggregation, while the roughness degradation component enters the closed channel separately, so that the compensation resources are deployed in a targeted manner according to the physical causes.

[0066] In one possible implementation, S300, the thickness degradation component and density degradation component of each surface partition are subjected to maximum-dominated nonlinear aggregation to obtain the passivation channel degradation risk factor of each surface partition, and the closed channel degradation risk factor of each surface partition is determined based on the roughness degradation component, including: S310, for each surface partition, take the larger of the film thickness degradation component and the density degradation component as the dominant term.

[0067] It is understandable that the dominant factor is the film thickness degradation component. With density degradation component The larger of the two is denoted as max( , This larger value directly reflects the most severe degradation of the partition in terms of passivation film quality, and is the lower bound of the risk factor.

[0068] In this embodiment, a larger value is used as the dominant term, ensuring that extreme deterioration in any dimension is fully transmitted to the risk factor, thus structurally eliminating mean dilution.

[0069] S320 uses the product of the polymerization correction factor and the sum of the film thickness degradation component and the density degradation component as the correction term; wherein the polymerization correction factor is greater than 0 and less than 1.

[0070] It is understandable that the correction term is the aggregate correction coefficient. The product of the film thickness degradation component and the density degradation component is denoted as: ·( + Aggregate correction factor The weight of the cumulative effect term relative to the dominant term is determined. If the value is too large, the aggregation will degenerate into an approximately linear weighted average, thus reintroducing the risk of dilution. If the value is too small, it will not be able to reflect the cumulative harm of multidimensional concurrent degradation. The value can be adjusted in the range of 0.2 to 0.4 based on the two-factor degradation ratio of historical pitting failure samples. In the embodiment of this application, the value is 0.3.

[0071] In the embodiments of this application, the correction term is applied to the dominant term only when there is concurrent degradation in multiple dimensions, reflecting the superposition effect of pitting corrosion risk when film thickness and density deteriorate simultaneously.

[0072] S330, add the dominant term and the correction term to obtain the passivation channel degradation risk factor of the surface partition; directly determine the roughness degradation component as the closed channel degradation risk factor of the surface partition.

[0073] It is understandable that the mathematical expression of the passivation channel degradation risk factor is as follows: .in, The passivation channel degradation risk factor for the i-th surface partition; The film thickness degradation component obtained in step S210; The density degradation component obtained in step S220; The aggregation correction coefficient determined in step S320. Closed-channel degradation risk factor. Directly take the roughness degradation component (From step S230) Since the closed channel only corresponds to a single dimension of roughness degradation, aggregation is not required.

[0074] In the embodiments of this application, The lower bound of the value is the most severe degradation component itself, and the upper bound is (1+2α) times the unit degradation. The magnitude relationship between the dominant term and the correction term remains stable throughout the entire value range, and the risk ranking will not be reversed due to the correction term.

[0075] This application employs maximum-dominant nonlinear aggregation instead of arithmetic average or weighted average aggregation because pitting corrosion initiation follows the "barrel effect," where the actual risk of a partition is determined by the most severe degradation dimension. If mean-based aggregation is used, for a partition with a film thickness degradation component as high as 0.9, the aggregation value is lowered to below 0.5 as long as another component is close to 0, systematically diluting extreme degradation. However, the result of maximum-dominant aggregation is always no less than the most severe degradation component itself, and the weighted summation term only applies superposition correction when multiple dimensions of concurrent degradation occur. This mathematical structure is strictly isomorphic to the physical law of the barrel effect, a feature lacking in mean-based feedback and weighted average risk coefficients in related technologies. Compared to related technologies that use the average film thickness across the entire line as feedback, the lower bound of the risk factor in this application is the most severe degradation component, while mean-based indicators divide it by the total number of partitions. Figure 2As shown, the maximum value-dominated aggregation in this application, compared with the mean-type aggregation and the weighted average-type aggregation, gives the risk expression of the same weak partition as annihilation, decay, and aggravation respectively. The mathematical structure and physical law of this application are uniquely isomorphic.

[0076] S400: The passivation process compensation energy for each surface partition is determined based on the passivation channel degradation risk factor, and the sealing process compensation energy for each surface partition is determined based on the sealing channel degradation risk factor. The control device controls the passivation partition execution mechanism to perform partition-differentiated passivation compensation processing according to the passivation process compensation energy of each surface partition, and controls the sealing partition execution mechanism to perform partition-differentiated sealing compensation processing according to the sealing process compensation energy of each surface partition.

[0077] It can be understood that compensation processing energy refers to the processing energy input by the process execution mechanism to a unit area surface. For the passivation process, it is manifested as the combination of electrochemical energy input of the zoned passivation electrode and the amount of passivation liquid sprayed, which increases and promotes the thickening and densification of the passivation film. For the sealing process, it is manifested as the combination of the amount of zoned sealant sprayed and the curing energy of the zoned heating unit, which increases and enhances the sealant's ability to fill and level surface valleys. Zoned differentiated execution means that the execution mechanism of each surface zone operates according to its own independently calculated compensation processing energy, without mutual interference.

[0078] In this embodiment, the compensation processing energy of the passivation channel and the closed channel are calculated, limited, and executed independently, and the physical destination of the compensation energy corresponds strictly to the cause of degradation.

[0079] For example, the differentiated compensation processing energy for each process can be determined by using the baseline processing energy of each process as the base, the product of the risk factor and the corresponding process compensation gain coefficient as the amplification ratio, and limiting the resulting energy to the upper limit of the processing energy of that process; or the risk factor can be mapped to the compensation processing energy by looking up a table and then truncated by the upper limit of the energy, etc., but not limited to these.

[0080] In one possible implementation, S400, the passivation process compensation processing energy for each surface partition is determined based on the passivation channel degradation risk factor, and the sealing process compensation processing energy for each surface partition is determined based on the sealing channel degradation risk factor, including: S410: Using the passivation process reference processing energy as the base, and the product of the passivation channel compensation gain coefficient and the passivation channel degradation risk factor as the amplification ratio, the increase corresponding to multiplying the passivation process reference processing energy by the amplification ratio is superimposed on the base, and the resulting energy is limited within the upper limit of the passivation process processing energy to obtain the passivation process compensation processing energy for each surface partition; wherein, the passivation process reference processing energy is the conventional passivation processing energy performed when the passivation channel degradation risk factor is 0, the passivation channel compensation gain coefficient is the passivation process energy increase caused by a unit passivation channel degradation risk factor, and the upper limit of the passivation process processing energy is the process safety boundary of the passivation processing energy.

[0081] It can be understood that the mathematical expression for the energy compensation process in the passivation step is as follows: .in, For the first The passivation process for each surface partition compensates for processing energy. Derived from step S330; The reference processing energy for the passivation process is determined by the standard passivation process specification for qualified plates, and is taken as 100kJ / m² in this embodiment. The passivation channel compensation gain coefficient determines the energy increase caused by a unit risk factor. It is calibrated by the measured response relationship between the passivation energy increment and the increase in film thickness and the decrease in passivation current density. In the embodiments of this application, it is taken as 0.5. The upper limit of the energy for the passivation process is determined by the process safety boundary of stress cracking of the film layer or over-corrosion of the substrate caused by excessive passivation. In the embodiments of this application, it is taken as 160kJ / m².

[0082] In this embodiment, the limiting function ensures that even if the risk factor reaches its theoretical limit under extreme degradation, the output energy will not exceed the process safety boundary. The formula outputs physically achievable energy values ​​across the entire input domain. The proportional compensation law with saturation protection ensures that the compensation energy increases smoothly and boundedly with degradation risk, achieving on-demand compensation while eliminating secondary process risks caused by over-processing from the formula structure.

[0083] S420 uses the baseline processing energy of the closed process as the base, and the product of the closed channel compensation gain coefficient and the closed channel degradation risk factor as the amplification ratio. The increase corresponding to multiplying the baseline processing energy of the closed process by the amplification ratio is superimposed on the base, and the resulting energy is limited within the upper limit of the closed process processing energy to obtain the closed process compensation processing energy of each surface partition. Among them, the baseline processing energy of the closed process is the normal closed process energy executed when the closed channel degradation risk factor is 0, the closed channel compensation gain coefficient is the increase in closed process energy caused by a unit of closed channel degradation risk factor, and the upper limit of closed process processing energy is the process safety boundary of the closed process energy.

[0084] It can be understood that the mathematical expression for the energy compensation of a closed process is as follows: .in, For the first i The energy is compensated for by the sealing process of each surface partition; The risk factors for the deterioration of the closed channel are directly determined in step S330. The baseline processing energy for the closed-loop process is 100 kJ / m² in this embodiment. The gain coefficient for closed-channel compensation is determined by the measured response relationship between the closed-channel energy increment and the roughness leveling amount. In this embodiment, it is taken as 0.6. The upper limit of the energy for the sealing process is determined by the process boundary of uncontrolled film thickening and incomplete curing caused by excessive sealing agent. In the embodiments of this application, it is taken as 150kJ / m².

[0085] In this embodiment, the gain coefficients and energy limits of the two channels are independently tuned. The compensation strengths of the passivation channel and the closed channel can be adapted to the physical response characteristics of their respective processes. Adjusting the parameters of one channel does not affect the compensation behavior of the other channel. Figure 3 As shown, the limiting characteristic curve of the compensation processing energy of this application as a function of the degradation risk factor rises smoothly as the risk factor increases and saturates at the upper limit of the energy, thus reducing overprocessing.

[0086] In one possible implementation, the method further includes: S500 compares the film thickness degradation component, density degradation component, and roughness degradation component of each surface partition with their corresponding trigger thresholds. If any degradation component of any surface partition is greater than the corresponding trigger threshold, the surface partition is determined to be a partition to be compensated, and compensation processing is performed on the partition to be compensated. If the degradation components of all surface partitions are not greater than the corresponding trigger thresholds, the surface condition of the stainless steel sheet is determined to be normal, and the passivation partition execution mechanism and the closed partition execution mechanism are controlled to perform processing according to the baseline processing energy.

[0087] It is understood that the trigger threshold is a criterion for determining whether a degradation component constitutes substantial degradation requiring compensation, and it is set individually for each degradation component. The trigger criterion is implemented through item-by-item comparison at the component level, rather than through comparison of aggregated risk factors. Therefore, any substantial degradation in any single dimension can independently trigger compensation, and there is no possibility of it being smoothed out by aggregation operations. In the embodiments of this application, the trigger threshold for all three degradation components can be set to 0.1, that is, if any parameter deviates from the process target value by 10% of the normalized baseline, the compensation process for that partition is triggered.

[0088] In this embodiment, the typical value of the degradation component of a normal board material under a qualified preceding process does not exceed 0.05. After substituting into the criterion, all zones are judged as normal, and the system performs conventional processing according to the baseline processing energy. The compensation mechanism is in a standby state with zero overhead. The trigger caliber is set to be determined item by item at the component level, so that the control system operates with the lowest overhead under normal operating conditions, and any substantial degradation in any single dimension under abnormal operating conditions deterministically enters the compensation process, thus balancing sensitivity and economy.

[0089] In one possible implementation, after calculating the film thickness degradation component, density degradation component, and roughness degradation component of each of the surface partitions, and before controlling the passivation partitioning execution mechanism and the closing partitioning execution mechanism to perform compensation processing, the method further includes: S600: Retest the electrochemical state parameters of each surface partition. The electrochemical state parameters include the passivation film thickness characterization parameter and the film density characterization parameter. Calculate the retest risk factor for each surface partition based on the electrochemical state parameters. If the retest risk factor for each surface partition is less than or equal to the convergence threshold, the composite surface treatment of the stainless steel sheet is determined to be complete. Otherwise, repeat the compensation process and retest for surface partitions with retest risk factors greater than the convergence threshold until the retest risk factor for that surface partition is less than or equal to the convergence threshold, or the number of iterations reaches the preset maximum number of iterations. If the number of iterations reaches the preset maximum number of iterations and there are still surface partitions with retest risk factors greater than the convergence threshold, output an abnormal prompt message and mark the corresponding surface partition.

[0090] It is understood that retesting refers to re-performing electrochemical detection on the surface partition after the compensation treatment is completed; the retesting risk factor is the risk amount calculated by normalizing the film thickness characterization parameter and the film density characterization parameter obtained from the retesting according to the same normalization and maximum value-dominated aggregation method as the passivation channel, that is, first calculate the film thickness degradation component and density degradation component with the retesting value according to the formulas in steps S210 and S220, and then aggregate according to the formula in step S330; the convergence threshold is the threshold for determining that the partition protection state has entered the equilibrium range, which is 0.15 in this embodiment; the preset maximum number of iterations is the upper limit of the number of times the same partition can be repeatedly compensated, which constitutes the deadlock exit of the iteration process, which is 3 times in this embodiment. The risk factor for retesting consists only of electrochemical dual parameters and does not include a roughness component. This is because the sealing process improves the effective protection state of the surface by filling with a sealant, but the geometric roughness reading after filling does not decrease proportionally. If the roughness component is included in the convergence criterion, a mathematical inversion will occur where the protection state has been met but the criterion is never satisfied. The equivalent film thickness and equivalent passivation current density measured by the electrochemical dual parameters under the cover of the sealing film precisely reflect the true protection capability after the passivation film and the sealing film are superimposed, and are the correct criteria for convergence judgment.

[0091] In this embodiment, the convergence threshold ε is set to 0.15, and the preset maximum number of iterations is 3. The retest is performed using electrochemical dual parameters characterizing the overall protective state of the composite film layer, ensuring that the final protective state of each partition is quantitatively verified and converges to the equilibrium range. The closed-loop structure of iterative compensation and retest convergence ensures that the final protective state of each surface partition is quantitatively verified, and the overall pitting corrosion resistance of the substrate no longer depends on the unverified worst-case scenario. The deadlock exit ensures that individual partitions that cannot be salvaged by surface treatment due to substrate defects are explicitly marked and transferred to manual handling. The control process terminates within a finite number of steps under any input, avoiding infinite loops. Figure 4 As shown, the retest risk factor in each scenario gradually decreases with the number of iterations and converges to below the convergence threshold. Partitions that do not reach convergence are marked with a deadlock exit after reaching the preset maximum number of iterations.

[0092] The following is a complete numerical example illustrating the execution process of the above method.

[0093] Please see Figure 3 and 4 A certain austenitic stainless steel sheet is divided into 20 surface zones, consisting of 4 columns along the width and 5 rows along the length. The process parameters are set as follows: passivation film thickness target value. =3.0nm, target value for film density process =0.5μA / cm², normalized reference quantity for density =2.0μA / cm², surface roughness target value =0.4μm, roughness normalized reference value =0.8μm, polymerization correction factor =0.3, trigger thresholds are all 0.1, and the passivation process baseline processing energy is... =100kJ / m², compensation gain coefficient =0.5, upper limit of energy =160kJ / m², baseline processing energy for closed-loop processes =100kJ / m², compensation gain coefficient =0.6, Energy Limit =150kJ / m², convergence threshold ε=0.15, preset maximum number of iterations 3.

[0094] Scenario 1 (Normal Partition): A partition's measured d=3.0nm, j=0.5μA / cm², Ra=0.4μm. Calculations yield... =clip[(3.0−3.0) / 3.0]=0, =clip[(0.5−0.5) / 2.0]=0, =clip[(0.4−0.4) / 0.8]=0; All three components are not greater than the trigger threshold of 0.1, so the operation is considered normal and will proceed according to the baseline energy. =100kJ / m², =100kJ / m².

[0095] Scenario 2 (Slightly Degraded Partition): Actual Test of a Certain Partition , , Calculated , , All three components are greater than 0.1, triggering compensation. Passivation channel: , Closed passage: , Post-compensation retest: Characterization parameters of equivalent film thickness of composite film layer. Equivalent passivation current density Retesting the deterioration component , Retesting risk factors Convergence is determined in the first iteration.

[0096] Scenario 3 (Severely Degraded Partition): Actual Test of a Certain Partition , , Calculated , , This triggers compensation. Passivation channel: , If the limit is reached, the energy limit will be applied; the channel will be closed. , Retest after the first round of compensation If convergence fails, perform a second round of compensation and a second round of retesting on the partition. The convergence was determined.

[0097] Scenario 4 (Deadlock Exit): If a certain partition has a matrix inclusion defect and the risk factor is still 0.35 > 0.15 after 3 rounds of iteration, and the number of iterations reaches the preset maximum number of iterations, the control device outputs an abnormal prompt message and marks the board surface coordinates of the partition, and the board is transferred to the manual re-inspection process.

[0098] To illustrate the differences between the aggregate structure of this application and related technologies, a comparative analysis is conducted using data from scenario three: the three degradation components of this partition are 0.9, 0.35, and 0.625. If a mean-based index is used, the arithmetic mean of the three components is (0.9 + 0.35 + 0.625) / 3 ≈ 0.625. The extreme degradation with a film thickness dimension as high as 0.9 is diluted to 0.625, and under the averaging of all 20 partitions on the entire plate, it will be further diluted to less than 0.05 and completely obscured. If a weighted average risk coefficient is used, weighting the two film layer components with weights of 0.8 and 0.2 yields 0.8 × 0.9 + 0.2 × 0.35 = 0.79, which is still lower than the extreme components themselves. Meanwhile, the passivation channel risk factor of this application... =1.275, which not only fully preserves the extreme degradation of 0.9, but also exacerbates the harm of concurrent degradation through superimposed correction terms, directly driving the capping level compensation energy.

[0099] It should be understood that the sequence number of each step in the above embodiments does not imply the order of execution. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of this application.

[0100] Corresponding to the composite surface treatment method for improving the corrosion resistance of stainless steel sheets described in the above embodiments, this application also provides a composite surface treatment system for improving the corrosion resistance of stainless steel sheets. Each module of this device can realize each step of the composite surface treatment method for improving the corrosion resistance of stainless steel sheets. Figure 5 The diagram shows a structural block diagram of a composite surface treatment system for improving the corrosion resistance of stainless steel sheets according to an embodiment of this application. For ease of explanation, only the parts related to the embodiments of this application are shown.

[0101] Reference Figure 5 This composite surface treatment system for improving the corrosion resistance of stainless steel sheets includes: The acquisition module is used to divide the surface of the stainless steel sheet to be treated into multiple surface partitions, and the control device controls the partition detection unit to acquire the surface state parameters of each surface partition; among which, the surface state parameters include passivation film thickness characterization parameters, film density characterization parameters, and surface roughness parameters; The calculation module is used to calculate the film thickness degradation component, density degradation component and roughness degradation component of each surface partition based on the surface state parameters of each surface partition and the corresponding process target value. The determination module is used to perform maximum-dominated nonlinear aggregation of the film thickness degradation component and density degradation component of each surface partition to obtain the passivation channel degradation risk factor of each surface partition, and determine the closed channel degradation risk factor of each surface partition based on the roughness degradation component. The execution module is used to determine the passivation process compensation energy of each surface partition based on the passivation channel degradation risk factor, and to determine the sealing process compensation energy of each surface partition based on the sealing channel degradation risk factor. The control device controls the passivation partition execution mechanism to perform partition-differentiated passivation compensation processing according to the passivation process compensation energy of each surface partition, and controls the sealing partition execution mechanism to perform partition-differentiated sealing compensation processing according to the sealing process compensation energy of each surface partition.

[0102] It should be noted that the information interaction and execution process between the above modules are based on the same concept as the method embodiments of this application. For details on their specific functions and technical effects, please refer to the method embodiments section, which will not be repeated here.

[0103] Those skilled in the art will understand that, for the sake of convenience and brevity, the above-described module division is merely an example. In practical applications, the above functions can be assigned to different modules as needed, that is, the internal structure of the system can be divided into different modules to complete all or part of the functions described above. The modules in the embodiments can be integrated into one processing unit, or each module can exist physically separately, or two or more modules can be integrated into one unit. The integrated unit can be implemented in hardware or as a software functional unit. Furthermore, the specific names of the modules are only for easy differentiation and are not intended to limit the scope of protection of this application. The specific working process of the modules in the above system can be referred to the corresponding process in the foregoing method embodiments, and will not be repeated here.

[0104] This application also provides a composite surface treatment device for improving the corrosion resistance of stainless steel sheets, including a control device, a partition detection unit, a passivation partition execution mechanism for the passivation process, and a sealing partition execution mechanism for the sealing process. The partition detection unit includes an electrochemical probe and a laser roughness meter. The control device is electrically connected to the partition detection unit, the passivation partition execution mechanism, and the sealing partition execution mechanism, respectively. Figure 6 This is a schematic diagram of the structure of a control device 6 provided in an embodiment of this application. Figure 6 As shown, the control device 6 in this embodiment includes: at least one processor 60 ( Figure 6 Only one is shown in the image), at least one memory 61 ( Figure 6 (Only one is shown in the image) and a computer program 62 stored in the at least one memory 61 and executable on the at least one processor 60, wherein when the processor 60 executes the computer program 62, it causes the control device 6 to perform the steps in any of the above embodiments of the composite surface treatment method for improving the corrosion resistance of stainless steel sheets, or causes the control device 6 to perform the functions of each module in the above embodiments of the device.

[0105] For example, the computer program 62 may be divided into one or more modules / units, which are stored in the memory 61 and executed by the processor 60 to complete this application. The one or more modules / units may be a series of computer program instruction segments capable of performing a specific function, which describe the execution process of the computer program 62 in the control device 6.

[0106] The control device 6 can be a desktop computer, laptop, handheld computer, or cloud server, etc. This composite surface treatment equipment for improving the corrosion resistance of stainless steel sheets may include, but is not limited to, a processor 60 and a memory 61. Those skilled in the art will understand that... Figure 6 This is merely an example of control device 6 and does not constitute a limitation on control device 6. It may include more or fewer components than shown, or combine certain components, or different components, such as input / output devices, network access devices, buses, etc.

[0107] The processor 60 can be a Central Processing Unit (CPU), or it can be other general-purpose processors, digital signal processors (DSPs), application-specific integrated circuits (ASICs), field-programmable gate arrays (FPGAs), or other programmable logic devices, discrete gate or transistor logic devices, discrete hardware components, etc. The general-purpose processor can be a microprocessor or any conventional processor.

[0108] In some embodiments, the memory 61 may be an internal storage unit of the control device 6, such as a hard disk or memory of the control device 6. In other embodiments, the memory 61 may be an external storage device of the control device 6, such as a plug-in hard disk, smart media card (SMC), secure digital (SD) card, flash card, etc., equipped on the control device 6. Furthermore, the memory 61 may include both internal storage units and external storage devices of the control device 6. The memory 61 is used to store operating systems, applications, bootloaders, data, and other programs, such as the program code of computer programs. The memory 61 can also be used to temporarily store data that has been output or will be output.

[0109] This application also provides a computer-readable storage medium storing a computer program that, when executed by a processor, implements the steps in any of the above method embodiments.

[0110] This application provides a computer program product that, when run on a composite surface treatment device for improving the corrosion resistance of stainless steel sheets, enables the device to perform the steps described in any of the above method embodiments.

[0111] If the integrated unit is implemented as a software functional unit and sold or used as an independent product, it can be stored in a computer-readable storage medium. Based on this understanding, all or part of the processes in the methods of the above embodiments of this application can be implemented by a computer program instructing related hardware. The computer program can be stored in a computer-readable storage medium, and when executed by a processor, it can implement the steps of the various method embodiments described above. The computer program includes computer program code, which can be in the form of source code, object code, executable files, or certain intermediate forms. The computer-readable medium can include at least: any entity or device capable of carrying the computer program code to a composite surface treatment device for improving the corrosion resistance of stainless steel sheets, a recording medium, a computer memory, a read-only memory (ROM), a random access memory (RAM), an electrical carrier signal, a telecommunication signal, and a software distribution medium. Examples include USB flash drives, portable hard drives, magnetic disks, or optical disks.

[0112] In the above embodiments, the descriptions of each embodiment have different focuses. For parts that are not described in detail or recorded in a certain embodiment, please refer to the relevant descriptions of other embodiments.

[0113] Those skilled in the art will recognize that the units and algorithm steps of the various examples described in conjunction with the embodiments disclosed herein can be implemented in electronic hardware, or a combination of computer software and electronic hardware. Whether these functions are implemented in hardware or software depends on the specific application and design constraints of the technical solution. Those skilled in the art can use different methods to implement the described functions for each specific application, but such implementation should not be considered beyond the scope of this application.

[0114] In the embodiments provided in this application, it should be understood that the disclosed composite surface treatment equipment and method for improving the corrosion resistance of stainless steel sheets can be implemented in other ways. For example, the embodiments of the composite surface treatment equipment for improving the corrosion resistance of stainless steel sheets described above are merely illustrative. For instance, the division of modules is only a logical functional division, and in actual implementation, there may be other division methods. For example, multiple modules may be combined or integrated into another system, or some features may be ignored or not executed. Furthermore, the coupling or direct coupling or communication connection shown or discussed may be indirect coupling or communication connection through some interfaces, devices, or modules, and may be electrical, mechanical, or other forms.

[0115] The modules described as separate components may or may not be physically separate. The components shown as modules may or may not be physical modules; that is, they may be located in one place or distributed across multiple network units. Some or all of the modules can be selected to achieve the purpose of this embodiment according to actual needs.

[0116] The above-described embodiments are only used to illustrate the technical solutions of this application, and are not intended to limit them. Although this application has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of this application, and should all be included within the protection scope of this application.

Claims

1. A composite surface treatment method for improving the corrosion resistance of stainless steel sheets, characterized in that, An application is made in a stainless steel sheet composite surface treatment equipment, the stainless steel sheet composite surface treatment equipment including a control device, a zone detection unit, a passivation zone execution mechanism for the passivation process, and a sealing zone execution mechanism for the sealing process, the control device being electrically connected to the zone detection unit, the passivation zone execution mechanism, and the sealing zone execution mechanism respectively, the method including: The surface of the stainless steel sheet to be treated is divided into multiple surface partitions, and the control device controls the partition detection unit to acquire the surface state parameters of each surface partition; wherein, the surface state parameters include passivation film thickness characterization parameters, film density characterization parameters, and surface roughness parameters; Based on the surface state parameters of each surface partition and the corresponding process target value, the film thickness degradation component, density degradation component and roughness degradation component of each surface partition are calculated. The film thickness degradation component and the density degradation component of each surface partition are subjected to maximum-dominant nonlinear aggregation to obtain the passivation channel degradation risk factor of each surface partition, and the closed channel degradation risk factor of each surface partition is determined according to the roughness degradation component. The passivation process compensation energy for each surface partition is determined based on the passivation channel degradation risk factor, and the sealing process compensation energy for each surface partition is determined based on the sealing channel degradation risk factor. The control device controls the passivation partition execution mechanism to perform partition-differentiated passivation compensation processing according to the passivation process compensation energy for each surface partition, and controls the sealing partition execution mechanism to perform partition-differentiated sealing compensation processing according to the sealing process compensation energy for each surface partition.

2. The composite surface treatment method for improving the corrosion resistance of stainless steel sheets as described in claim 1, characterized in that, The calculation of the film thickness degradation component, density degradation component, and roughness degradation component for each surface partition based on the surface state parameters and corresponding process target values ​​of each surface partition includes: Based on the passivation film thickness characterization parameters and passivation film thickness process target values ​​of each of the surface partitions, the film thickness degradation component of each of the surface partitions is calculated. Based on the film density characterization parameters and film density process target values ​​of each of the surface partitions, the density degradation component of each of the surface partitions is calculated. Based on the surface roughness parameters and surface roughness process target values ​​of each surface partition, the roughness degradation component of each surface partition is calculated.

3. The composite surface treatment method for improving the corrosion resistance of stainless steel sheets as described in claim 1, characterized in that, The partition detection unit includes an electrochemical probe and a laser roughness meter. The control device controls the partition detection unit to acquire surface state parameters of each surface partition, including: The control device controls the electrochemical probes arranged in the control zones to collect the passivation film equivalent capacitance of each of the surface zones; The passivation film thickness characterization parameters for each of the surface partitions are obtained based on the equivalent capacitance of the passivation film. The control device controls the electrochemical probe to collect the passivation current density of each surface partition in a potentiodynamic scanning manner, and uses the passivation current density as a parameter to characterize the film density. The control device controls the laser roughness meter to collect surface roughness parameters of each of the surface partitions.

4. The composite surface treatment method for improving the corrosion resistance of stainless steel sheets as described in claim 3, characterized in that, The passivation film thickness characterization parameters for each surface partition, calculated based on the equivalent capacitance of the passivation film, include: The passivation film thickness characterization parameter for each surface partition is obtained by dividing the product of the passivation film relative permittivity, the vacuum permittivity, and the effective measurement area of ​​the electrochemical probe by the equivalent capacitance of the passivation film in each of the surface partitions; wherein, the passivation film relative permittivity is the relative permittivity of the passivation film material, the vacuum permittivity is the permittivity in a vacuum, and the effective measurement area of ​​the electrochemical probe is the effective measurement area in contact between the probe and the surface being measured.

5. The composite surface treatment method for improving the corrosion resistance of stainless steel sheets as described in claim 3, characterized in that, The control device controls the electrochemical probe to acquire the passivation current density of each surface partition in a potentiodynamic scanning manner, including: The control device controls the electrochemical probe to perform potentiodynamic scanning at a preset scanning rate within a preset potential range to obtain the polarization curves of each surface partition. Based on the polarization curve, a passivation plateau range is determined where the current density changes with potential at a rate less than a preset fluctuation limit. The current density corresponding to the midpoint potential of the passivation plateau range is then determined as the passivation current density of the corresponding surface partition.

6. The composite surface treatment method for improving the corrosion resistance of stainless steel sheets as described in claim 1, characterized in that, The step of performing maximum-dominated nonlinear aggregation on the film thickness degradation component and the density degradation component of each surface partition to obtain the passivation channel degradation risk factor of each surface partition, and determining the closed channel degradation risk factor of each surface partition based on the roughness degradation component, includes: For each of the surface partitions, the larger of the film thickness degradation component and the density degradation component is taken as the dominant term; The product of the polymerization correction factor and the sum of the film thickness degradation component and the density degradation component is used as the correction term; wherein the polymerization correction factor is greater than 0 and less than 1. The dominant term and the correction term are added together to obtain the passivation channel degradation risk factor of the surface partition; the roughness degradation component is directly determined as the closed channel degradation risk factor of the surface partition.

7. The composite surface treatment method for improving the corrosion resistance of stainless steel sheets as described in claim 1, characterized in that, The step of determining the passivation process compensation processing energy for each of the surface partitions based on the passivation channel degradation risk factor, and determining the sealing process compensation processing energy for each of the surface partitions based on the sealing channel degradation risk factor, includes: Using the passivation process baseline processing energy as the base, and the product of the passivation channel compensation gain coefficient and the passivation channel degradation risk factor as the amplification ratio, the passivation process baseline processing energy multiplied by the amplification ratio is superimposed onto the base, and the resulting energy is limited within the upper limit of the passivation process processing energy to obtain the passivation process compensation processing energy for each of the surface partitions; wherein, the passivation process baseline processing energy is the conventional passivation processing energy performed when the passivation channel degradation risk factor is 0, the passivation channel compensation gain coefficient is the passivation process energy increase caused by a unit passivation channel degradation risk factor, and the upper limit of the passivation process processing energy is the process safety boundary of the passivation processing energy; Using the baseline processing energy of the closed process as the base, and the product of the closed channel compensation gain coefficient and the closed channel degradation risk factor as the amplification ratio, the increase corresponding to multiplying the baseline processing energy of the closed process by the amplification ratio is superimposed on the base, and the resulting energy is limited within the upper limit of the closed process processing energy to obtain the closed process compensation processing energy for each of the surface partitions; wherein, the baseline processing energy of the closed process is the normal closed process energy executed when the closed channel degradation risk factor is 0, the closed channel compensation gain coefficient is the increase in closed process energy caused by a unit of closed channel degradation risk factor, and the upper limit of the closed process processing energy is the process safety boundary of the closed process energy.

8. The composite surface treatment method for improving the corrosion resistance of stainless steel sheets as described in claim 1, characterized in that, After calculating the film thickness degradation component, density degradation component, and roughness degradation component of each of the surface partitions, and before controlling the passivation partition execution mechanism and the closing partition execution mechanism to perform compensation processing, the method further includes: The film thickness degradation component, density degradation component, and roughness degradation component of each of the surface partitions are compared with their respective trigger thresholds. When any degradation component of any of the surface partitions is greater than the corresponding trigger threshold, the surface partition is determined to be a partition to be compensated, and compensation processing is performed on the partition to be compensated; when the degradation components of all the surface partitions are not greater than the corresponding trigger threshold, the surface condition of the stainless steel plate is determined to be normal, and the passivation partition execution mechanism and the closed partition execution mechanism are controlled to perform processing according to the baseline processing energy.

9. The composite surface treatment method for improving the corrosion resistance of stainless steel sheets as described in claim 1, characterized in that, After calculating the film thickness degradation component, density degradation component, and roughness degradation component of each of the surface partitions, and before controlling the passivation partitioning actuator and the closing partitioning actuator to perform compensation processing, the method further includes: The electrochemical state parameters of each of the surface partitions were remeasured, including the passivation film thickness characterization parameters and the film density characterization parameters; The retest risk factor of each surface partition is calculated based on the electrochemical state parameters. When the retest risk factor of each surface partition is less than or equal to the convergence threshold, the composite surface treatment of the stainless steel sheet is determined to be complete. Otherwise, the compensation process and retest are repeated for the surface partitions whose retest risk factor is greater than the convergence threshold until the retest risk factor of the surface partition is less than or equal to the convergence threshold, or the number of iterations reaches the preset maximum number of iterations. When the number of iterations reaches the preset maximum number of iterations and there are still surface partitions whose retest risk factor is greater than the convergence threshold, an abnormal prompt message is output and the corresponding surface partition is marked.

10. A composite surface treatment device for improving the corrosion resistance of stainless steel sheets, characterized in that, The method includes a control device, a partition detection unit, a passivation partition execution mechanism for a passivation process, and a sealing partition execution mechanism for a sealing process. The partition detection unit includes an electrochemical probe and a laser roughness meter. The control device is electrically connected to the partition detection unit, the passivation partition execution mechanism, and the sealing partition execution mechanism, respectively. The control device includes a memory, a processor, and a computer program stored in the memory and executable on the processor. When the processor executes the computer program, it implements the method as described in any one of claims 1 to 9.