A Ferro-Silicon-Aluminum Composite Alloy Powder and Its Preparation Method
By preparing a composite iron-silicon-aluminum alloy powder of flake powder and spherical powder, the problem of balancing performance and processability in high-frequency scenarios in existing technologies has been solved. This achieves a combination of high permeability, low loss and good flowability, making it suitable for high-frequency magnetic devices in modern electronic and power fields.
Patent Information
- Application Number
- CN202611445343.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-17
- Publication Date
- 2026-11-10
AI Technical Summary
Existing single-form iron-silicon-aluminum powders are difficult to balance high permeability, low loss and good processing performance in high-frequency scenarios, resulting in high preparation costs and difficult processes, which cannot meet the diversified and high-performance requirements of modern electronic and power fields.
A composite method of flake powder and spherical powder was adopted. By adjusting the mechanical ball milling parameters and combining ultrasonic oscillation and transverse magnetic field heat treatment, an iron-silicon-aluminum alloy powder with a composite structure of flake powder and spherical powder was prepared, and its soft magnetic properties were optimized.
It achieves synergistic optimization of performance and processability, expands the application range of iron-silicon-aluminum materials, reduces preparation costs, simplifies the process flow, and is suitable for industrial mass production.
Smart Images

Figure CN123072869A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of soft magnetic powder core technology, specifically relating to a method for preparing iron-silicon-aluminum composite alloy powder. Background Technology
[0002] Driven by the rapid iteration in modern electronic and power fields such as new energy vehicles, 5G communications, and smart grids, magnetic components are developing rapidly towards higher frequencies, smaller sizes, and lower losses. This poses stringent challenges to the comprehensive performance of core soft magnetic materials. Iron-silicon-aluminum (Fe-Si-Al) alloy powder, due to its advantages of low coercivity, excellent DC superposition characteristics, good temperature stability, and low cost, has become a core material for the preparation of key components such as medium- and high-frequency inductors and filter cores. It is widely used in critical scenarios such as switching power supplies, pulse transformers, and electromagnetic compatibility filters, and its performance directly determines the energy efficiency and reliability of terminal equipment.
[0003] Currently, mainstream industrial solutions for preparing iron-silicon-aluminum alloy powders still focus on the production of single-form powders. Among them, gas-atomized spherical iron-silicon-aluminum powder, with its mature preparation process, high particle sphericity, and good surface finish, exhibits excellent flowability and bulk density, significantly reducing the difficulty of molding and processing. Therefore, it dominates the mass production of low- and medium-frequency magnetic devices. However, the isotropic structure of spherical particles limits the improvement of their permeability. Furthermore, at high frequencies (1MHz and above), the current skin effect is significant, easily generating a large amount of eddy current loss inside the particles. This leads to excessively high device temperature rise and reduced energy efficiency, making it difficult to meet the low-loss requirements of high-end applications such as 5G communication and high-frequency switching power supplies. This defect has become a core bottleneck restricting its expansion into the high-frequency field.
[0004] To address high-frequency loss issues, mechanically ground flake-shaped iron-silicon-aluminum powder has become a research hotspot. The flake structure imparts significant shape anisotropy to the material, not only overcoming the Snoek limit of spherical particles and improving high-frequency permeability stability, but also reducing the effective particle thickness below the skin depth, significantly suppressing the skin effect and eddy current loss, making it an ideal soft magnetic material for high-frequency applications. However, flake-shaped iron-silicon-aluminum powder has inherent drawbacks: firstly, the flake particles have poor flowability and low bulk density, easily leading to agglomeration and uneven distribution during molding, resulting in insufficient core density and large performance fluctuations; secondly, its strong anisotropy makes its magnetic properties dependent on directional alignment processes, and traditional high-pressure molding easily causes flake particle breakage, further deteriorating magnetic properties. Furthermore, the additional orientation process significantly increases production complexity and cost, limiting its industrial application. In summary, existing single-form iron-silicon-aluminum powder cannot simultaneously achieve high-frequency low-loss performance and excellent processability, failing to meet the diversified and high-performance demands of modern electronic and power fields for soft magnetic materials. Therefore, there is an urgent need to develop a composite iron-silicon-aluminum powder preparation technology that combines performance advantages with processing feasibility. Summary of the Invention
[0005] This invention addresses the problem that existing single-form iron-silicon-aluminum powders cannot simultaneously meet the requirements of high magnetic permeability, low loss, good processing performance, and isotropy in high-frequency scenarios, resulting in high preparation costs and difficult processes. It provides a method for preparing iron-silicon-aluminum alloy powder composed of flake powder and spherical powder, achieving synergistic optimization of performance and processability.
[0006] Specifically, the following steps are included: The first step involves preparing iron-silicon-aluminum alloy powder (chemical composition: Si: 9.0-10.0 wt%, Al: 5.0-6.0 wt%). The powder (wt%, Fe balance, impurity content Cr≤wt0.01%, O≤0.16wt%) and stainless steel grinding balls are placed in a stainless steel ball mill jar at a mass ratio of 1:15~35. Anhydrous ethanol is added at a mass ratio of 0.6~1.2:1 with the iron-silicon-aluminum alloy powder as a protective agent and antioxidant before ball milling. The grinding balls have a diameter of 2-12mm and a multi-size grinding ball mixture ratio (2mm:5mm:12mm=3:5:2). The ball milling speed is 300~500r / min and the ball milling time is 2~24h. After ball milling, the powder is vacuum dried in an oven at a drying temperature of 95-115℃ for 30min-1h to obtain a composite powder containing some flake powder and spherical powder. The particle size of the flake powder in the powder is 8~120μm and the particle size of the spherical powder is 20-30μm.
[0007] The second step involves stress-relief annealing of the dried powder in a tube furnace at a temperature of 5000-800℃ for 1.5-3 hours. The furnace atmosphere is a nitrogen-argon mixture (volume ratio 7:3), with a heating rate of 5℃ / min and furnace-cooled cooling to eliminate internal stress generated during ball milling and optimize magnetic properties.
[0008] The third step is to dissolve the silicone resin in acetone and stir it for 1-2 hours. Then, pour the completely dissolved solution into the annealed powder and mix the coating material and the iron-silicon-aluminum alloy powder at a mass ratio of 1.5-3:100. Stir the coating material at a speed of 30 r / min for 30 min. After coating, bake it in an oven to allow the solvent to evaporate completely at a temperature of 55-65℃.
[0009] The fourth step involves loading the coated iron-silicon-aluminum alloy powder into a pressing mold and using ultrasonic-assisted oscillation treatment at a frequency of 40kHz for 30-80s. Through oscillation and gravity, the flake powder is arranged along the horizontal plane and then cold-pressed. The pressing pressure is 5-35 tons and the holding time is 1 minute to ensure that the powder is dense and uniform.
[0010] In the fifth step, the magnetic ring is subjected to transverse magnetic field heat treatment, the baking temperature of the magnetic ring is 170-190°C (preferably 180°C), and the baking time is 1h, which further optimizes the directional arrangement effect of the flaky powder. After baking, the Fe-Si-Al magnetic ring with a composite structure of flaky powder and spherical powder is obtained.
[0011] Compared with the prior art, the present invention has the following advantages: (1) The content of the flaky powder (15%~90%) can be precisely regulated by adjusting parameters such as the rotation speed and time of mechanical ball milling, so that the composite powder exhibits tunable soft magnetic properties, adapts to the requirements of different high-frequency and medium-high frequency application scenarios, and expands the application range of Fe-Si-Al materials; (2) Through the combination of spherical powder and flaky powder, the present invention synergistically exerts the processing advantages of spherical Fe-Si-Al powder with good fluidity, isotropy and high apparent density, as well as the performance advantages of flaky Fe-Si-Al powder with high magnetic permeability and low high-frequency eddy current loss, solves the performance shortboard of single-form powder, and obtains composite powder with more excellent comprehensive properties; (3) The preparation process adopts the combination of ultrasonic oscillation orientation and transverse magnetic field-assisted heat treatment, which avoids the deformation and fragmentation defects generated during the traditional high-pressure compaction process of flaky powder, simplifies the orientation arrangement process, reduces the preparation cost, and the process is simple and easy to operate, has good repeatability, and is suitable for industrial mass production. Brief Description of the Drawings
[0012] Figure 1 is a 300-times magnified SEM image of the Fe-Si-Al alloy powder prepared at a rotation speed of 300r / min and ball milling for 4h according to the present invention; Figure 2 is a 300-times magnified SEM image of the Fe-Si-Al alloy powder prepared at a rotation speed of 300r / min and ball milling for 8h according to the present invention; Figure 3 is a 300-times magnified SEM image of the Fe-Si-Al alloy powder prepared at a rotation speed of 300r / min and ball milling for 12h according to the present invention; Figure 4 is a 300-times magnified SEM image of the Fe-Si-Al alloy powder prepared at a rotation speed of 500r / min and ball milling for 4h according to the present invention; Figure 5 is a 300-times magnified SEM image of the Fe-Si-Al alloy powder prepared at a rotation speed of 500r / min and ball milling for 8h according to the present invention. Detailed Description of the Embodiments
[0013] The technical solutions in the embodiments of the present invention will be clearly and completely described below with reference to the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by a person of ordinary skill in the art without creative work shall fall within the protection scope of the present invention.
[0014] Example 1 A method for preparing an iron-silicon-aluminum composite alloy powder, comprising the following steps: The first step involves placing iron-silicon-aluminum alloy powder and stainless steel grinding balls in a stainless steel ball mill jar at a mass ratio of 1:20. Anhydrous ethanol at a mass ratio of 0.8:1 to the iron-silicon-aluminum alloy powder is added as a protective agent before ball milling. The grinding ball diameter is 2mm:5mm:12mm = 3:5:2, the milling speed is 300 r / min, and the milling time is 4 hours. After milling, the powder is vacuum dried in an oven at 100℃ for 30 minutes. This yields a composite powder containing some flake and spherical powder, with the flake powder content being approximately 25% and the particle size of the flake powder being 10~60μm. The powder after 4 hours of milling is as follows: Figure 1 As shown, from Figure 1 As can be seen, a small amount of flaky powder begins to appear in the spherical powder matrix, and it is evenly distributed.
[0015] The second step involves stress-relief annealing of the dried powder in a tube furnace at a temperature of 700℃ for 2 hours. The furnace atmosphere is a nitrogen-argon mixture (volume ratio 7:3), with a heating rate of 5℃ / min and furnace cooling.
[0016] The third step is to dissolve the silicone resin in acetone and stir it for 1 hour. Then, pour the completely dissolved solution into the annealed powder and mix the coating material and the iron-silicon-aluminum alloy powder at a mass ratio of 2:100. Stir the coating material at a speed of 30 r / min for 30 min. After stirring, bake it in an oven to allow the solvent to evaporate completely at a temperature of 60°C.
[0017] The fourth step involves loading the coated iron-silicon-aluminum alloy powder into a pressing mold and treating it with ultrasonic-assisted oscillation at a frequency of 40 kHz for 60 seconds. Subsequently, cold pressing is performed at a pressure of 20 tons for 1 minute.
[0018] The fifth step is to perform transverse magnetic field heat treatment on the magnetic ring. The baking temperature of the magnetic ring is 180℃ and the baking time is 1h to further optimize the directional arrangement effect of the flake powder. After baking, an iron-silicon-aluminum magnetic ring with a composite structure of flake powder and spherical powder is obtained.
[0019] Example 2 A method for preparing an iron-silicon-aluminum composite alloy powder, comprising the following steps: The first step involves placing iron-silicon-aluminum alloy powder and stainless steel grinding balls in a stainless steel ball mill jar at a mass ratio of 1:20. Anhydrous ethanol at a mass ratio of 0.8:1 to the iron-silicon-aluminum alloy powder is added as a protective agent before ball milling. The grinding ball diameter is 2mm:5mm:12mm = 3:5:2, the milling speed is 300 r / min, and the milling time is 8 hours. After milling, the powder is vacuum dried in an oven at 100℃ for 30 minutes. This yields a composite powder containing some flake and spherical powder, with the flake powder content approximately 59% and a particle size of 10-100 μm. The powder after 8 hours of milling is as follows: Figure 2 As shown, from Figure 2 As can be seen, a small amount of flaky powder begins to appear in the spherical powder matrix, and it is evenly distributed.
[0020] The second step involves stress-relief annealing of the dried powder in a tube furnace at a temperature of 700℃ for 2 hours. The furnace atmosphere is a nitrogen-argon mixture (volume ratio 7:3), with a heating rate of 5℃ / min and furnace cooling.
[0021] The third step is to dissolve the silicone resin in acetone and stir it for 1 hour. Then, pour the completely dissolved solution into the annealed powder and mix the coating material and the iron-silicon-aluminum alloy powder at a mass ratio of 2:100. Stir the coating material at a speed of 30 r / min for 30 min. After stirring, bake it in an oven to allow the solvent to evaporate completely at a temperature of 60°C.
[0022] The fourth step involves loading the coated iron-silicon-aluminum alloy powder into a pressing mold and treating it with ultrasonic-assisted oscillation at a frequency of 40 kHz for 60 seconds. Subsequently, cold pressing is performed at a pressure of 20 tons for 1 minute.
[0023] The fifth step is to perform transverse magnetic field heat treatment on the magnetic ring. The baking temperature of the magnetic ring is 180℃ and the baking time is 1h to further optimize the directional arrangement effect of the flake powder. After baking, an iron-silicon-aluminum magnetic ring with a composite structure of flake powder and spherical powder is obtained.
[0024] Example 3 A method for preparing an iron-silicon-aluminum composite alloy powder, comprising the following steps: The first step involves placing iron-silicon-aluminum alloy powder and stainless steel grinding balls in a stainless steel ball mill jar at a mass ratio of 1:20. Anhydrous ethanol at a mass ratio of 0.8:1 to the iron-silicon-aluminum alloy powder is added as a protective agent before ball milling. The grinding ball diameter is 2mm:5mm:12mm = 3:5:2, the milling speed is 300 r / min, and the milling time is 12 hours. After milling, the powder is vacuum dried in an oven at 100℃ for 30 minutes. This yields a composite powder containing both flaky and spherical powders, with the flaky powder content approximately 86% and a particle size of 6-130 μm. The powder after 12 hours of milling is as follows: Figure 3 As shown, from Figure 3 As can be seen, a small amount of flaky powder begins to appear in the spherical powder matrix, and it is evenly distributed.
[0025] The second step involves stress-relief annealing of the dried powder in a tube furnace at a temperature of 700℃ for 2 hours. The furnace atmosphere is a nitrogen-argon mixture (volume ratio 7:3), with a heating rate of 5℃ / min and furnace cooling.
[0026] The third step is to dissolve the silicone resin in acetone and stir it for 1 hour. Then, pour the completely dissolved solution into the annealed powder and mix the coating material and the iron-silicon-aluminum alloy powder at a mass ratio of 2:100. Stir the coating material at a speed of 30 r / min for 30 min. After stirring, bake it in an oven to allow the solvent to evaporate completely at a temperature of 60°C.
[0027] The fourth step involves loading the coated iron-silicon-aluminum alloy powder into a pressing mold and treating it with ultrasonic-assisted oscillation at a frequency of 40 kHz for 60 seconds. Subsequently, cold pressing is performed at a pressure of 20 tons for 1 minute.
[0028] The fifth step is to perform transverse magnetic field heat treatment on the magnetic ring. The baking temperature of the magnetic ring is 180℃ and the baking time is 1h to further optimize the directional arrangement effect of the flake powder. After baking, an iron-silicon-aluminum magnetic ring with a composite structure of flake powder and spherical powder is obtained.
[0029] Example 4 A method for preparing an iron-silicon-aluminum composite alloy powder, comprising the following steps: The first step involves placing iron-silicon-aluminum alloy powder and stainless steel grinding balls in a stainless steel ball mill jar at a mass ratio of 1:20. Anhydrous ethanol at a mass ratio of 0.8:1 to the iron-silicon-aluminum alloy powder is added as a protective agent before ball milling. The grinding ball diameter is 2mm:5mm:12mm = 3:5:2, the milling speed is 500 r / min, and the milling time is 4 hours. After milling, the powder is vacuum dried in an oven at 100℃ for 30 minutes. This yields a composite powder containing some flake and spherical powder, with the flake powder content approximately 54% and a particle size of 20~70μm. The powder after 4 hours of milling is as follows: Figure 4 As shown, from Figure 4 As can be seen, a small amount of flaky powder begins to appear in the spherical powder matrix, and it is evenly distributed.
[0030] The second step involves stress-relief annealing of the dried powder in a tube furnace at a temperature of 700℃ for 2 hours. The furnace atmosphere is a nitrogen-argon mixture (volume ratio 7:3), with a heating rate of 5℃ / min and furnace cooling.
[0031] The third step is to dissolve the silicone resin in acetone and stir it for 1 hour. Then, pour the completely dissolved solution into the annealed powder and mix the coating material and the iron-silicon-aluminum alloy powder at a mass ratio of 2:100. Stir the coating material at a speed of 30 r / min for 30 min. After stirring, bake it in an oven to allow the solvent to evaporate completely at a temperature of 60°C.
[0032] The fourth step involves loading the coated iron-silicon-aluminum alloy powder into a pressing mold and treating it with ultrasonic-assisted oscillation at a frequency of 40 kHz for 60 seconds. Subsequently, cold pressing is performed at a pressure of 20 tons for 1 minute.
[0033] The fifth step is to perform transverse magnetic field heat treatment on the magnetic ring. The baking temperature of the magnetic ring is 180℃ and the baking time is 1h to further optimize the directional arrangement effect of the flake powder. After baking, an iron-silicon-aluminum magnetic ring with a composite structure of flake powder and spherical powder is obtained.
[0034] Example 5 A method for preparing an iron-silicon-aluminum composite alloy powder, comprising the following steps: The first step involves placing iron-silicon-aluminum alloy powder and stainless steel grinding balls in a stainless steel ball mill jar at a mass ratio of 1:20. Anhydrous ethanol at a mass ratio of 0.8:1 to the iron-silicon-aluminum alloy powder is added as a protective agent before ball milling. The grinding ball diameter is 2mm:5mm:12mm = 3:5:2, the milling speed is 500 r / min, and the milling time is 8 hours. After milling, the powder is vacuum dried in an oven at 100℃ for 30 minutes. This yields a composite powder containing both flake and spherical powders, with the flake powder content approximately 90% and a particle size of 20~100μm. The powder after 8 hours of milling is as follows: Figure 5 As shown, from Figure 5 As can be seen, a small amount of flaky powder begins to appear in the spherical powder matrix, and it is evenly distributed.
[0035] The second step involves stress-relief annealing of the dried powder in a tube furnace at a temperature of 700℃ for 2 hours. The furnace atmosphere is a nitrogen-argon mixture (volume ratio 7:3), with a heating rate of 5℃ / min and furnace cooling.
[0036] The third step is to dissolve the silicone resin in acetone and stir it for 1 hour. Then, pour the completely dissolved solution into the annealed powder and mix the coating material and the iron-silicon-aluminum alloy powder at a mass ratio of 2:100. Stir the coating material at a speed of 30 r / min for 30 min. After stirring, bake it in an oven to allow the solvent to evaporate completely at a temperature of 60°C.
[0037] The fourth step involves loading the coated iron-silicon-aluminum alloy powder into a pressing mold and treating it with ultrasonic-assisted oscillation at a frequency of 40 kHz for 60 seconds. Subsequently, cold pressing is performed at a pressure of 20 tons for 1 minute.
[0038] The fifth step is to perform transverse magnetic field heat treatment on the magnetic ring. The baking temperature of the magnetic ring is 180℃ and the baking time is 1h to further optimize the directional arrangement effect of the flake powder. After baking, an iron-silicon-aluminum magnetic ring with a composite structure of flake powder and spherical powder is obtained.
[0039] The magnetic rings prepared in Examples 1-5 were tested, and the test results are as follows: Testing items Detection methods Magnetic ring 1 Magnetic ring 2 Magnetic ring 3 Magnetic ring 4 Magnetic ring 5 magnetic permeability LCR tester @1MHz 58.3 65.4 77.6 62.5 77.2 Saturation magnetic induction VSM 0.98T 0.99T 1.00T 0.99T 1.01T Coercivity BH Analyzer @1M, 15mT 10.1A / m 12.5A / m 13.1A / m 11.6A / m 13.4A / m Eddy current loss BH Analyzer @1M, 15mT 231kW / m³ 208kW / m³ 186kW / m³ 227kW / m³ 201kW / m³ Liquidity Hall effect current meter 53s 55s 58s 53s 56s isotropic magnetic permeability anisotropy 0.26 0.29 0.31 0.27 0.32 Loose packing density Songzhong Analyzer 3.7g / cm³ 3.9g / cm³ 4.1g / cm³ 3.9g / cm³ 4.2g / cm³ As demonstrated in the above embodiments, composite iron-silicon-aluminum alloy powders with varying flake powder contents can be obtained by adjusting the ball milling time and speed. The soft magnetic properties exhibit a regular variability: as the flake powder content increases, the permeability gradually increases, eddy current losses continuously decrease, while maintaining good flowability and isotropy. The preparation process of this invention is simple and easy to operate, with controllable costs. The prepared composite powder exhibits excellent comprehensive performance and can be widely used in high-frequency magnetic devices in fields such as 5G communication, the Internet of Things, and switching power supplies, meeting the performance requirements of different scenarios.
[0040] The embodiments of the present invention have been described in detail above. Specific examples have been used to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only for the purpose of helping to understand the method and core ideas of the present invention. At the same time, for those skilled in the art, there will be changes in the specific implementation methods and application scope based on the ideas of the present invention. Therefore, the content of this specification should not be construed as a limitation of the present invention.
Claims
1. A method for preparing an iron-silicon-aluminum composite alloy powder, characterized in that, The preparation method includes the following steps: The first step involves placing iron-silicon-aluminum alloy powder and stainless steel grinding balls into a grinding jar at a mass ratio of 1:15~35, adding anhydrous ethanol at a mass ratio of 0.6~1.2:1 to the iron-silicon-aluminum alloy powder, and then ball milling. The grinding ball diameter is 2-12 mm, the ball milling speed is 300~500 r / min, and the ball milling time is 2~24 h. After ball milling, the powder is dried at a temperature of 95-115℃ for 30 min-1 h to obtain a composite powder containing some flake powder and spherical powder. The second step involves stress-relief annealing of the dried powder at a temperature of 5000~800℃ for 1.5~3 h in a nitrogen-argon mixed atmosphere in the annealing furnace. The third step is to dissolve the silicone resin in acetone to obtain a mixed coating material; The mixed coating material is then poured into the annealed powder. The mass ratio of the mixed coating material to the iron-silicon-aluminum alloy powder is 1.5~3:100, and the mixture is stirred. After coating, the mixture is placed in an oven to bake until the solvent is completely evaporated. The baking temperature is 55-65℃. The fourth step is to load the coated iron-silicon-aluminum alloy powder into a pressing mold and use ultrasonic-assisted vibration treatment. Through vibration and gravity, the flake powder is arranged along the horizontal plane and then cold-pressed. The pressing pressure is 5 to 35 tons. The fifth step is to perform transverse magnetic field heat treatment on the magnetic ring. The baking temperature of the magnetic ring is 170-190℃. After baking, an iron-silicon-aluminum magnetic ring with a composite structure of flake powder and spherical powder is obtained.
2. The method for preparing an iron-silicon-aluminum composite alloy powder as described in claim 1, characterized in that, The chemical composition of the iron-silicon-aluminum alloy powder is: Si 9.0-10.0%, Al 5.0-6.0%, Fe balance.
3. The method for preparing an iron-silicon-aluminum composite alloy powder as described in claim 1, characterized in that, The ratio of different grinding ball sizes is 2mm:5mm:12mm = 3:5:
2.
4. The method for preparing an iron-silicon-aluminum composite alloy powder as described in claim 1, characterized in that, The annealing furnace atmosphere is a nitrogen-argon mixture with a volume ratio of 7:
3.
5. The method for preparing an iron-silicon-aluminum composite alloy powder as described in claim 1, characterized in that, The heating rate for annealing is controlled at 5℃ / min, and the cooling method is furnace cooling.
6. The method for preparing an iron-silicon-aluminum composite alloy powder as described in claim 1, characterized in that, The fourth step involves an oscillation frequency of 40kHz and an oscillation time of 30-80s.
7. A type of iron-silicon-aluminum composite alloy powder, characterized in that, The iron-silicon-aluminum composite alloy powder is prepared by the preparation method described in any one of claims 1-6.