Method for manufacturing semiconductor structure, semiconductor structure and display device

By employing a substrate selective epitaxial growth method in MicroLED display technology, the thickness of the quantum well growth auxiliary layer is controlled to regulate the indium content of the quantum well layer, thus solving the problem of monolithic multicolor integration in existing technologies. This achieves efficient and simple multicolor integrated MicroLED displays, improving device performance and display accuracy.

CN123076083APending Publication Date: 2026-11-10JINAN GOERTEK VISUAL DISPLAY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611316119.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-27
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing MicroLED display technology suffers from problems such as high process complexity, low yield, high cost, and large size of optomechanical system in monolithic multicolor integration, making it difficult to achieve efficient and simple monolithic multicolor integration and limiting the improvement of device performance and display accuracy.

Method used

By using a substrate, buffer layer and mask layer stacked on a substrate, light-emitting devices of different colors can be formed by selective area epitaxial growth. The indium content of the quantum well layer can be controlled by adjusting the thickness of the quantum well growth auxiliary layer, thereby achieving precise control of light-emitting devices of different colors, simplifying the fabrication process and improving the yield.

Benefits of technology

This technology enables efficient and simple monolithic multicolor integrated MicroLED displays, reducing manufacturing costs, improving device yield and display accuracy, reducing the complexity and size of the optomechanical system, and enhancing the display effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123076083A_ABST
    Figure CN123076083A_ABST
Patent Text Reader

Abstract

The application provides a preparation method of a semiconductor structure, a semiconductor structure and a display device. In the preparation method, a quantum well growth auxiliary layer, a quantum well layer and a semiconductor structure of a second conduction type are respectively prepared on a side of a semiconductor structure of a first conduction type away from a substrate for forming light-emitting devices of different colors. The thicknesses of the quantum well growth auxiliary layers are different in the light-emitting devices of different colors, the indium content of the corresponding quantum well layers can be adjusted through the thicknesses of the quantum well growth auxiliary layers, the light-emitting wavelength of the light-emitting devices of different colors can be precisely adjusted, the preparation efficiency of the multi-color light-emitting devices is improved, and the semiconductor structure with full-color display can be favorably manufactured on a large scale. In addition, the selected-area growth method can reduce the damage to the light-emitting devices and improve the preparation yield compared with the etching preparation method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of semiconductor device manufacturing technology, and more specifically, to a method for preparing a semiconductor structure, a semiconductor structure, and a display device. Background Technology

[0002] With the continuous and rapid development of micro-display technology, it has become a core technology in high-end display fields such as augmented reality (AR), virtual reality (VR), near-eye displays, and micro-projection. MicroLED micro-display technology, with its advantages of high brightness, low power consumption, long lifespan, high refresh rate, wide color gamut, and excellent environmental adaptability, is widely recognized as one of the most promising next-generation display technologies, with broad application prospects in consumer electronics, automotive displays, and smart wearables. However, MicroLED display technology still faces many technical bottlenecks in its industrialization process. Among them, monolithic multi-color integrated display is the core challenge restricting its performance improvement and miniaturization. Current mainstream multi-color integration schemes mostly adopt a discrete fabrication method for red, green, and blue primary color chips, requiring components such as color-combining prisms and complex optical modules to achieve color mixing and light output. This not only significantly increases manufacturing costs and assembly complexity but also greatly increases the size of the optomechanical system, making miniaturization difficult and severely limiting further improvements in pixel density, resolution, and display accuracy of micro-display chips. In addition, MicroLED still faces many technical challenges in key process aspects such as epitaxial growth uniformity, heterogeneous bonding reliability, and backplane driving compatibility, which directly lead to unstable device performance and low yield, seriously hindering the large-scale development of multi-color integrated MicroLED display technology.

[0003] To overcome the limitations of existing technologies, the industry is gradually exploring new technological routes, aiming to achieve highly efficient, simple, and highly integrated monolithic multi-color integrated MicroLED displays. Currently, while novel solutions such as quantum dot color conversion and vertical stacking multi-color integration possess the theoretical feasibility of monolithic integration, they still face significant technological barriers. Specifically, quantum dot color conversion suffers from low conversion efficiency, poor stability, and limited color gamut. Vertical stacking solutions, on the other hand, face drawbacks such as high process complexity, numerous interlayer interface defects, extremely low yield, and high manufacturing costs; the overall process route is not yet mature and cannot meet the requirements of industrial mass production. Therefore, there is an urgent need to develop a monolithic multi-color integrated MicroLED display technology that is simple to process, highly integrated, cost-controllable, and has excellent yield, effectively breaking through existing technological bottlenecks and solving core problems such as the difficulty of multi-color integration, large system size, and limited performance. Summary of the Invention

[0004] In order to overcome the technical problems mentioned in the above background, this application provides a method for preparing a semiconductor structure, a semiconductor structure, and a display device to solve the above technical problems.

[0005] A first aspect of this application provides a method for fabricating a semiconductor structure, the method comprising: A substrate is provided, wherein the substrate includes a substrate, a buffer layer and a mask layer stacked together, and the mask layer has a plurality of mask openings that expose the buffer layer; A plurality of semiconductor structures of the first conductivity type are formed on the substrate at the corresponding mask opening positions; A quantum well growth auxiliary layer, a quantum well layer, and a second conductivity type semiconductor structure are sequentially fabricated on the side of a first conductivity type semiconductor structure used to form light-emitting devices of different colors away from the substrate. The light-emitting device is formed by the stacked first conductivity type semiconductor structure, the quantum well growth auxiliary layer, the quantum well layer, and the second conductivity type semiconductor structure. The quantum well growth auxiliary layer includes a first surface in contact with the first conductivity type semiconductor structure and a second surface in contact with the quantum well layer. The area of ​​the second surface is smaller than the area of ​​the first surface. In light-emitting devices with different emission colors, the thickness of each quantum well growth auxiliary layer is different. The thicker the quantum well growth auxiliary layer, the smaller the area of ​​the second surface, and the higher the indium content of the corresponding quantum well layer.

[0006] In one possible implementation, the light-emitting device includes a first light-emitting device, a second light-emitting device, and a third light-emitting device of different colors. The step of sequentially fabricating a quantum well growth auxiliary layer, a quantum well layer, and a second conductivity type semiconductor structure on the side of the first conductivity type semiconductor structure used to form the light-emitting devices of different colors away from the substrate includes: A first barrier layer is formed on the side of the first conductivity type semiconductor structure away from the substrate, and the first barrier layer is patterned to form a first window, wherein the first window only exposes the first conductivity type semiconductor structure used to form the first light-emitting device. A first quantum well growth auxiliary layer, a first quantum well layer, and a second conductive type semiconductor structure are sequentially fabricated on the first conductive type semiconductor structure exposed by the first window. The first light-emitting device is composed of the stacked first conductive type semiconductor structure, the first quantum well growth auxiliary layer, the first quantum well layer, and the second conductive type semiconductor structure. A second barrier layer is formed on the side of the first quantum well layer and the first barrier layer away from the substrate, and the first barrier layer and the second barrier layer are patterned to form a second window, wherein the second window only exposes the first conductivity type semiconductor structure used to form the second light-emitting device; A second quantum well growth auxiliary layer, a second quantum well layer, and a second conductive type semiconductor structure are sequentially fabricated on the first conductive type semiconductor structure exposed in the second window. The second light-emitting device is composed of the stacked first conductive type semiconductor structure, the second quantum well growth auxiliary layer, the second quantum well layer, and the second conductive type semiconductor structure. A third barrier layer is fabricated on the side of the second quantum well layer and the second barrier layer away from the substrate, and the first barrier layer, the second barrier layer and the third barrier layer are patterned to form a third window, wherein the third window only exposes the first conductivity type semiconductor structure used to form the third light-emitting device; A third quantum well growth auxiliary layer, a third quantum well layer, and a second conductive type semiconductor structure are sequentially fabricated on the first conductive type semiconductor structure exposed by the third window. The third light-emitting device is composed of the stacked first conductive type semiconductor structure, the third quantum well growth auxiliary layer, the third quantum well layer, and the second conductive type semiconductor structure.

[0007] In one possible implementation, the wavelengths of the light emitted by the first light-emitting device, the second light-emitting device, and the third light-emitting device decrease sequentially. In the step of sequentially fabricating a quantum well growth auxiliary layer, a quantum well layer, and a second conductivity type semiconductor structure on the side of the first conductivity type semiconductor structure used to form different color light-emitting devices away from the substrate: The first quantum well growth auxiliary layer is grown using a first epitaxial growth time, the second quantum well growth auxiliary layer is grown using a second epitaxial growth time, and the third quantum well growth auxiliary layer is grown using a third epitaxial growth time. The epitaxial growth time of the first epitaxial growth time, the epitaxial growth time of the second epitaxial growth time, and the epitaxial growth time of the third epitaxial growth time decrease sequentially.

[0008] A second aspect of this application provides a semiconductor structure, the semiconductor structure including a substrate and a plurality of light-emitting devices of different light-emitting colors grown on the substrate; In the direction away from the substrate, each of the light-emitting devices includes a first conductivity type semiconductor structure, a quantum well growth auxiliary layer, a quantum well layer, and a second conductivity type semiconductor structure stacked together. The quantum well growth auxiliary layer includes a first surface in contact with the first conductivity type semiconductor structure and a second surface in contact with the quantum well layer, wherein the area of ​​the second surface is smaller than the area of ​​the first surface. In light-emitting devices with different emission colors, the thickness of each quantum well growth auxiliary layer is different in the plane direction perpendicular to the substrate. The thicker the quantum well growth auxiliary layer, the smaller the area of ​​the second surface, and the higher the indium content of the corresponding quantum well layer.

[0009] In one possible implementation, in light-emitting devices with different emission colors, each of the quantum well growth auxiliary layers has a first surface of the same area, and each of the quantum well growth auxiliary layers has a second surface of different areas.

[0010] In one possible implementation, the greater the thickness of the quantum well growth auxiliary layer in the plane perpendicular to the substrate, the longer the wavelength of the light emitted by the corresponding color-emitting device. In another possible implementation, in light-emitting devices with different emitting colors, the thickness of each quantum well layer is the same in the plane perpendicular to the substrate. The thickness of the quantum well layer is greater than or equal to 2 nanometers and less than or equal to 10 nanometers.

[0011] In one possible implementation, the light-emitting device includes a first light-emitting device, a second light-emitting device, and a third light-emitting device with different light-emitting colors, wherein the wavelengths of the light emitted by the first light-emitting device, the second light-emitting device, and the third light-emitting device decrease sequentially. The first light-emitting device includes a first quantum well growth auxiliary layer, the second light-emitting device includes a second quantum well growth auxiliary layer, and the third light-emitting device includes a third quantum well growth auxiliary layer.

[0012] The areas of the second surface of the first quantum well growth auxiliary layer, the second surface of the second quantum well growth auxiliary layer, and the second surface of the third quantum well growth auxiliary layer increase sequentially.

[0013] In one possible implementation, the first quantum well growth auxiliary layer has a first thickness, the second quantum well growth auxiliary layer has a second thickness, and the third quantum well growth auxiliary layer has a third thickness in a plane direction perpendicular to the substrate. The first thickness, the second thickness, and the third thickness decrease sequentially. The first thickness is greater than or equal to 120 nanometers and less than or equal to 200 nanometers, the second thickness is greater than or equal to 80 nanometers and less than 120 nanometers, and the third thickness is greater than or equal to 5 nanometers and less than 80 nanometers.

[0014] In one possible implementation, the first light-emitting device further includes a first quantum well layer, the second light-emitting device further includes a second quantum well layer, and the third light-emitting device further includes a third quantum well layer. The first quantum well layer has a first indium concentration, the second quantum well layer has a second indium concentration, and the third quantum well layer has a third indium concentration, wherein the first indium concentration, the second indium concentration, and the third indium concentration decrease sequentially. The first indium concentration is greater than or equal to 30% and less than or equal to 40%, the second indium concentration is greater than or equal to 18% and less than or equal to 25%, and the third indium concentration is greater than or equal to 8% and less than or equal to 15%.

[0015] In one possible implementation, the roughness of the first surface is greater than the roughness of the second surface.

[0016] In one possible implementation, the substrate includes a substrate, a buffer layer, and a mask layer stacked together, wherein the first conductivity type semiconductor structure is at least partially located on the side of the mask layer away from the substrate, and wherein the mask layer includes a mask opening that exposes the buffer layer. The first conductivity type semiconductor structure includes a seed layer and a first conductivity type semiconductor body covering the seed layer. The seed layer fills the mask opening and forms a cone on the side of the mask layer away from the substrate. The cone is located within the first conductivity type semiconductor body. The seed layer is made of GaN, InGaN, or AlGaN, the first conductivity type semiconductor body is made of N-type InGaN, and the second conductivity type semiconductor structure is made of P-type GaN.

[0017] In one possible implementation, the light-emitting device further includes an electron blocking layer located between the quantum well layer and the second conductivity type semiconductor structure.

[0018] A third aspect of this application also provides a display device, the display device comprising a semiconductor structure prepared by a preparation method provided in any possible implementation of the first aspect, or a semiconductor structure provided in any possible implementation of the second aspect.

[0019] This application provides a method for fabricating a semiconductor structure, the semiconductor structure itself, and a display device. In the semiconductor structure fabrication method, a quantum well growth auxiliary layer, a quantum well layer, and a second conductivity type semiconductor structure are fabricated on the side of a first conductivity type semiconductor structure used to form different color light-emitting devices, away from the substrate. In light-emitting devices of different colors, the thickness of each quantum well growth auxiliary layer is different. The indium content of the corresponding quantum well layer can be controlled by adjusting the thickness of the quantum well growth auxiliary layer, achieving precise control of the emission wavelength of different color light-emitting devices, improving the fabrication efficiency of multi-color light-emitting devices, and facilitating the large-scale manufacturing of semiconductor structures with full-color displays. Furthermore, selective growth, compared to etching, reduces damage to the light-emitting devices and improves the fabrication yield. Attached Figure Description

[0020] To more clearly illustrate the technical solutions of the embodiments of this application, the accompanying drawings required in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of this application and should not be regarded as a limitation of the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.

[0021] Figure 1 A schematic flowchart illustrating the semiconductor structure fabrication method provided in this embodiment is illustrated. Figure 2a and Figure 2b Example Figure 1 Corresponding process flow chart; Figure 3 An example of implementation is provided. Figure 1 Process diagram for step S12; Figure 4 An example of implementation is provided. Figure 1 A flowchart illustrating step S13; Figure 5a and Figure 5b Example Figure 4 Corresponding process flow chart; Figure 6 A schematic diagram of a semiconductor structure provided in this embodiment is illustrated. Figure 7 Another schematic diagram of the semiconductor structure provided in this embodiment is illustrated.

[0022] Icons: 1-Semiconductor structure; 11-Substrate; 111-Substrate; 112-Buffer layer; 113-Mask layer; 1131-Mask opening; 12-First conductivity type semiconductor structure; 121-Seed layer; 122-First conductivity type semiconductor body; 13-Quantum well growth auxiliary layer; 131-First quantum well growth auxiliary layer; 132-Second quantum well growth auxiliary layer; 133-Third quantum well growth auxiliary layer; 13A-First surface; 13B-Second surface; 14-Quantum well layer; 141 142-First quantum well layer; 143-Second quantum well layer; 15-Second conductivity type semiconductor structure; 16-Protective layer; 171-First barrier layer; 172-Second barrier layer; 173-Third barrier layer; 1711-First window; 1712-Second window; 1713-Third window; 18-Electron barrier layer; 10-Light emission device; 10a-First light emission device; 10b-Second light emission device; 10c-Third light emission device; 20-First conductivity type semiconductor layer. Detailed Implementation

[0023] To make the objectives, technical solutions, and advantages of the embodiments of this application clearer, the technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. The components of the embodiments of this application described and shown in the accompanying drawings can generally be arranged and designed in various different configurations.

[0024] Therefore, the following detailed description of the embodiments of this application provided in the accompanying drawings is not intended to limit the scope of the claimed application, but merely to illustrate selected embodiments of the application. All other embodiments obtained by those skilled in the art based on the embodiments of this application without inventive effort are within the scope of protection of this application.

[0025] It should be noted that similar labels and letters in the following figures indicate similar items. Therefore, once an item is defined in one figure, it does not need to be further defined and explained in subsequent figures.

[0026] In the description of this application, it should be noted that the terms "upper," "lower," etc., indicating the orientation or positional relationship are based on the orientation or positional relationship shown in the accompanying drawings, or the orientation or positional relationship commonly used when the product is in use. They are used only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation on this application. In addition, the terms "first," "second," etc., are used only to distinguish descriptions and should not be construed as indicating or implying relative importance.

[0027] It should be noted that, where there is no conflict, different features in the embodiments of this application can be combined with each other.

[0028] To address the technical problems mentioned in the background section, the inventors have innovatively designed the following technical solutions, which will be described in detail below with reference to the accompanying drawings. It should be noted that the deficiencies in the solutions of related technologies are the result of the inventors' practical experience and careful research. Therefore, the discovery process of the aforementioned technical problems and the solutions proposed in the embodiments of this application below should be considered contributions made by the inventors during the invention process, and should not be construed as technical content known to those skilled in the art.

[0029] Please refer to Figure 1 , Figure 2a and Figure 2b , Figure 1 This embodiment illustrates a flowchart of a method for fabricating a semiconductor structure. Figure 2a and Figure 2b Example Figure 1 The corresponding process flow diagram is shown below. Figure 1 , Figure 2a and Figure 2b The method for fabricating the semiconductor structure provided in this embodiment will be described in detail. In this embodiment, the method for fabricating the semiconductor structure includes the following steps.

[0030] Step S11: Provide a substrate 11.

[0031] In this embodiment, the substrate 11 includes a substrate 111, a buffer layer 112, and a mask layer 113 stacked together. The mask layer 113 has a plurality of mask openings 1131 that expose the buffer layer 112.

[0032] The substrate 111 can be a silicon substrate or a sapphire substrate. The buffer layer 112 can be a single-layer structure or a multi-layer structure grown on the substrate 111. The buffer layer 112 is used to suppress dislocation propagation, release interface stress, and improve the lattice mismatch problem between the epitaxial material and the substrate 111.

[0033] A mask layer 113 is grown on the side of the buffer layer 112 away from the substrate 111, and multiple mask openings 1131 are opened to expose the buffer layer 112 through patterning. The area where the mask openings 1131 are located serves as the growth area for subsequent film layers. This growth area can define the position of the fabricated light-emitting device 10. Specifically, corresponding mask openings 1131 can be formed on the mask layer 113 according to the arrangement of the light-emitting device 10 to be fabricated.

[0034] Step S12: A plurality of first conductivity type semiconductor structures 12 are formed on the substrate 11 at the corresponding mask opening 1131 position.

[0035] In this embodiment, the first conductivity type semiconductor structure 12 has a top surface on the side away from the substrate 11, which can be used to grow subsequent film layers.

[0036] The orthographic projection of the top surface of the first conductivity type semiconductor structure 12 on the substrate 11 away from the substrate 11, and the orthographic projection of the bottom surface of the first conductivity type semiconductor structure 12 on the substrate 11 facing the substrate 11.

[0037] The shape of the top surface of the first conductivity type semiconductor structure 12 on the side away from the substrate 11, projected onto the substrate 11, is the same as the shape of the top surface of the first conductivity type semiconductor structure 12 on the side away from the substrate 11, projected onto the substrate 11.

[0038] In this step, the first conductivity type semiconductor structures 12 used to form different color light-emitting devices 10 are completely identical and can be fabricated simultaneously using a unified process method, which simplifies the process and improves process efficiency.

[0039] In this step, a seed layer 121 is first epitaxially grown in the region where the mask opening 1131 is located; then, multiple spaced first conductivity type semiconductor structures 12 are epitaxially grown on the basis of the seed layer 121. One seed layer 121 corresponds to one first conductivity type semiconductor structure 12.

[0040] In step S13, a quantum well growth auxiliary layer 13, a quantum well layer 14, and a second conductivity type semiconductor structure 15 are sequentially fabricated on the side of the first conductivity type semiconductor structure 12 used to form different color light-emitting devices 10 away from the substrate 11.

[0041] In this embodiment, depending on the color of the fabricated light-emitting device 10, a quantum well growth auxiliary layer 13, a quantum well layer 14, and a second conductivity type semiconductor structure 15 can be fabricated on the side of the corresponding first conductivity type semiconductor structure 12 away from the substrate 11.

[0042] For example, the light-emitting device 10 includes a first light-emitting device 10a, a second light-emitting device 10b, and a third light-emitting device 10c. In this step, a first quantum well growth auxiliary layer 131, a first quantum well layer 141, and a second conductive semiconductor structure 15 can be sequentially fabricated on the side of the first conductive semiconductor structure 12 away from the substrate 11 corresponding to the first light-emitting device 10a; then, a second quantum well growth auxiliary layer 132, a second quantum well layer 142, and a second conductive semiconductor structure 15 can be sequentially fabricated on the side of the first conductive semiconductor structure 12 away from the substrate 11 corresponding to the second light-emitting device 10b; and then, a third quantum well growth auxiliary layer 133, a third quantum well layer 143, and a second conductive semiconductor structure 15 can be sequentially fabricated on the side of the first conductive semiconductor structure 12 away from the substrate 11 corresponding to the third light-emitting device 10c. It is understood that the above is only an example, and the order of fabricating the quantum well growth auxiliary layer 13 and the quantum well layer 14 can also be different from the above description. In this embodiment, the specific order is not limited.

[0043] A light-emitting device 10 is formed by a first conductivity type semiconductor structure 12, a quantum well growth auxiliary layer 13, a quantum well layer 14, and a second conductivity type semiconductor structure 15 stacked together. Specifically, a first light-emitting device 10a is formed by a first conductivity type semiconductor structure 12, a first quantum well growth auxiliary layer 131, a first quantum well layer 141, and a second conductivity type semiconductor structure 15 stacked together. A second light-emitting device 10b is formed by a first conductivity type semiconductor structure 12, a second quantum well growth auxiliary layer 132, a second quantum well layer 142, and a second conductivity type semiconductor structure 15 stacked together. A third light-emitting device 10c is formed by a first conductivity type semiconductor structure 12, a third quantum well growth auxiliary layer 133, a third quantum well layer 143, and a second conductivity type semiconductor structure 15 stacked together.

[0044] In this embodiment, light-emitting devices 10 of different colors can be arranged in any way according to the related technology to form pixel units in order to achieve full-color display.

[0045] For example, the light-emitting device 10 includes a red light-emitting device, a green light-emitting device and a blue light-emitting device. The light-emitting devices 10 of different colors can be arranged in Real, Pentile, diamond or tripod arrangement, etc.

[0046] In this embodiment, the quantum well growth auxiliary layer 13 includes a first surface 13A in contact with the first conductivity type semiconductor structure 12 and a second surface 13B in contact with the quantum well layer 14. The area of ​​the second surface 13B is smaller than the area of ​​the first surface 13A. In the direction away from the substrate 11, the cross-section of the first conductivity type semiconductor structure 12 gradually decreases in the direction parallel to the substrate 11. For example, the shape of the first conductivity type semiconductor structure 12 can be frustum-shaped.

[0047] In the light-emitting devices 10 with different emission colors, the thickness of each quantum well growth auxiliary layer 13 varies in the direction perpendicular to the plane of the substrate 11. Specifically, the thicker the quantum well growth auxiliary layer 13, the smaller the area of ​​its second surface 13B, and consequently, the higher the indium content of the corresponding quantum well layer 14. Under the same or similar epitaxial growth conditions, a smaller growth surface area encourages the accumulation of more indium atoms, thereby increasing the indium content in the corresponding quantum well layer 14.

[0048] The above method involves fabricating a quantum well growth auxiliary layer 13, a quantum well layer 14, and a second conductivity type semiconductor structure 15 on the side of the first conductivity type semiconductor structure 12 used to form different colored light-emitting devices 10 away from the substrate 11. In light-emitting devices 10 with different emission colors, the thickness of each quantum well growth auxiliary layer 13 is different. The indium content of the corresponding quantum well layer 14 can be controlled by adjusting the thickness of the quantum well growth auxiliary layer 13, thereby achieving precise control of the emission wavelength of different colored light-emitting devices 10, improving the fabrication efficiency of multi-color light-emitting devices 10, and facilitating the large-scale manufacturing of semiconductor structures with full-color displays. Furthermore, compared to etching fabrication, selective growth reduces damage to the light-emitting device 10 and improves the fabrication yield.

[0049] In one possible implementation, such as Figure 3 As shown, in step S12, in order to prevent the first conductivity type semiconductor structure 12 from being damaged or stripped during the top removal process, in this embodiment, a protective layer 16 can be deposited or epitaxially grown around the first conductivity type semiconductor layer 20. The protective layer 16 includes, but is not limited to, SiO2, Al2O3, TiN, Si3N4, etc.

[0050] In this embodiment, the side of the protective layer 16 furthest from the substrate 11 can be used as the cut surface of the first conductivity type semiconductor structure 12 at a uniform height for top removal processing of the first conductivity type semiconductor layer 20. Top removal processing methods include, but are not limited to, chemical etching, thermal annealing, and chemical mechanical polishing.

[0051] In one possible implementation, the light-emitting device 10 includes a first light-emitting device 10a, a second light-emitting device 10b, and a third light-emitting device 10c. Please refer to... Figure 4 , Figure 5a and Figure 5b Step S13 can be achieved in the following way.

[0052] In step S131, a first barrier layer 171 is formed on the side of the first conductivity type semiconductor structure 12 away from the substrate 11, and the first barrier layer 171 is patterned to form a first window 1711.

[0053] In this embodiment, a first barrier layer 171 can be deposited or grown on the entire side of the first conductivity type semiconductor structure 12 away from the substrate 11. The first barrier layer 171 is patterned to form a first window 1711. The first window 1711 exposes only the first conductivity type semiconductor structure 12 that forms the first light-emitting device 10a. The material of the first barrier layer 171 includes, but is not limited to, SiO2, Al2O3, TiN, Si3N4, etc.

[0054] In step S132, a first quantum well growth auxiliary layer 131, a first quantum well layer 141, and a second conductivity type semiconductor structure 15 are sequentially fabricated on the first conductivity type semiconductor structure 12 exposed in the first window 1711.

[0055] In this embodiment, a first quantum well growth auxiliary layer 131, a first quantum well layer 141, and a second conductivity type semiconductor structure 15 can be sequentially fabricated by epitaxial growth. The first light-emitting device 10a is formed by the stacked first conductivity type semiconductor structure 12, the first quantum well growth auxiliary layer 131, the first quantum well layer 141, and the second conductivity type semiconductor structure 15.

[0056] In this step, the first quantum well growth auxiliary layer 131 is grown using the first epitaxial growth time.

[0057] In step S133, a second barrier layer 172 is formed on the side of the first quantum well layer 141 and the first barrier layer 171 away from the substrate 11, and the first barrier layer 171 and the second barrier layer 172 are patterned to form a second window 1712.

[0058] In this embodiment, a second barrier layer 172 can be fabricated on the entire side of the first quantum well layer 141 and the first barrier layer 171 away from the substrate 11 by deposition or growth. The first barrier layer 171 and the second barrier layer 172 are patterned to form a second window 1712. The second window 1712 exposes only the first conductivity type semiconductor structure 12 forming the second light-emitting device 10b. The material of the second barrier layer 172 includes, but is not limited to, SiO2, Al2O3, TiN, Si3N4, etc.

[0059] In step S134, a second quantum well growth auxiliary layer 132, a second quantum well layer 142, and a second conductivity type semiconductor structure 15 are sequentially fabricated on the first conductivity type semiconductor structure 12 exposed by the second window 1712.

[0060] In this embodiment, the second quantum well growth auxiliary layer 132, the second quantum well layer 142, and the second conductivity type semiconductor structure 15 can be sequentially fabricated by epitaxial growth. The second light-emitting device 10b is formed by the stacked first conductivity type semiconductor structure 12, the second quantum well growth auxiliary layer 132, the second quantum well layer 142, and the second conductivity type semiconductor structure 15.

[0061] In this step, the second quantum well growth auxiliary layer 132 is grown using the second epitaxial growth time.

[0062] In step S135, a third barrier layer 173 is formed on the side of the second quantum well layer 142 and the second barrier layer 172 away from the substrate 11, and the first barrier layer 171, the second barrier layer 172 and the third barrier layer 173 are patterned to form a third window 1713.

[0063] In this embodiment, a third barrier layer 173 can be fabricated on the entire side of the second quantum well layer 142 and the second barrier layer 172 away from the substrate 11 by deposition or growth. The first barrier layer 171, the second barrier layer 172, and the third barrier layer 173 are patterned to form a third window 1713. The third window 1713 exposes only the first conductivity type semiconductor structure 12 forming the third light-emitting device 10c. The material of the third barrier layer 173 includes, but is not limited to, SiO2, Al2O3, TiN, Si3N4, etc.

[0064] In step S136, a third quantum well growth auxiliary layer 133, a third quantum well layer 143, and a second conductivity type semiconductor structure 15 are sequentially fabricated on the first conductivity type semiconductor structure 12 exposed in the third window 1713.

[0065] In this embodiment, the third quantum well growth auxiliary layer 133, the third quantum well layer 143, and the second conductivity type semiconductor structure 15 can be sequentially fabricated by epitaxial growth. The third light-emitting device 10c is formed by the stacked first conductivity type semiconductor structure 12, the third quantum well growth auxiliary layer 133, the third quantum well layer 143, and the second conductivity type semiconductor structure 15.

[0066] In this step, the third quantum well growth auxiliary layer 133 is grown using the third epitaxial growth time.

[0067] In one possible implementation, the wavelengths of the light emitted by the first light-emitting device 10a, the second light-emitting device 10b, and the third light-emitting device 10c decrease sequentially. For example, the first light-emitting device 10a can be a red light-emitting device, the second light-emitting device 10b can be a green light-emitting device, and the third light-emitting device 10c can be a blue light-emitting device.

[0068] The epitaxial growth time for the first, second, and third epitaxial growth periods decreases sequentially. The longer the epitaxial growth time, the thicker the grown film. That is, in this embodiment, the thicknesses of the first quantum well growth auxiliary layer 131, the second quantum well growth auxiliary layer 132, and the third quantum well growth auxiliary layer 133 decrease sequentially.

[0069] The different growth parameters control the thickness of the quantum well growth auxiliary layer 13 for growing different colored light-emitting devices 10, and the indium content in the quantum well layer 14 can be precisely controlled by adjusting the thickness of the quantum well growth auxiliary layer 13.

[0070] In this embodiment, in the plane direction perpendicular to the substrate 11, the first quantum well growth auxiliary layer 131 has a first thickness, the second quantum well growth auxiliary layer 132 has a second thickness, and the third quantum well growth auxiliary layer 133 has a third thickness.

[0071] The first thickness is greater than or equal to 120 nanometers and less than or equal to 200 nanometers, the second thickness is greater than or equal to 80 nanometers and less than 120 nanometers, and the third thickness is greater than or equal to 5 nanometers and less than 80 nanometers.

[0072] In this embodiment, among the light-emitting devices 10 with different emission colors, the thickness of each quantum well layer 14 is the same in the plane direction perpendicular to the substrate 11. Exemplarily, the thickness of the well layers is greater than or equal to 2 nanometers and less than or equal to 10 nanometers.

[0073] In one possible implementation, the first quantum well layer 141 has a first indium content, the second quantum well layer 142 has a second indium content, and the third quantum well layer 143 has a third indium content. The first indium content, the second indium content, and the third indium content decrease sequentially.

[0074] The first indium content is greater than or equal to 30% and less than or equal to 40%, the second indium content is greater than or equal to 18% and less than or equal to 25%, and the third indium content is greater than or equal to 8% and less than or equal to 15%.

[0075] In one possible implementation, after step S13, the preparation method provided in this embodiment further includes sequentially removing the third barrier layer 173, the second barrier layer 172, the first barrier layer 171, and the protective layer 16 to obtain... Figure 6 Semiconductor structure 1 is shown.

[0076] Based on the same inventive concept, this application also provides a semiconductor device 1 prepared by the above-described preparation method, such as... Figure 6 As shown, the semiconductor device 1 includes a substrate 11 and a plurality of light-emitting devices 10 with different light-emitting colors grown on the substrate 11.

[0077] In the direction away from the substrate 11 (Z direction in the figure), each light-emitting device 10 includes a first conductivity type semiconductor structure 12, a quantum well growth auxiliary layer 13, a quantum well layer 14 and a second conductivity type semiconductor structure 15 stacked together.

[0078] In this embodiment, the quantum well growth auxiliary layer 13 includes a first surface 13A in contact with the first conductivity type semiconductor structure 12 and a second surface 13B in contact with the quantum well layer 14. The area of ​​the second surface 13B is smaller than the area of ​​the first surface 13A. In the direction away from the substrate 11, the cross-section of the first conductivity type semiconductor structure 12 gradually decreases in the direction parallel to the substrate 11. For example, the first conductivity type semiconductor structure 12 can be truncated pyramidal in shape.

[0079] In the light-emitting devices 10 with different emission colors, the thickness of each quantum well growth auxiliary layer 13 varies in the direction perpendicular to the plane of the substrate 11. Specifically, the thicker the quantum well growth auxiliary layer 13, the smaller the area of ​​its second surface 13B, and consequently, the higher the indium content of the corresponding quantum well layer 14. Under the same or similar epitaxial growth conditions, a smaller growth surface area encourages the accumulation of more indium atoms, thereby increasing the indium content in the corresponding quantum well layer 14.

[0080] In the above structure, the indium content of the quantum well layer 14 can be precisely controlled by adjusting the thickness of the quantum well growth auxiliary layer 13, allowing for the fabrication of light-emitting devices 10 of different colors on the same substrate 11 to achieve color mixing and light emission. This eliminates the need for optical components such as color-combining prisms, reducing the complexity and size of the entire optomechanical system. Furthermore, compared to schemes requiring optical components for light mixing, this effectively avoids drawbacks such as low color conversion efficiency, insufficient luminous stability, color gamut attenuation, and poor reliability, thereby improving the luminous efficiency, color consistency, and lifespan of multi-color displays. Simultaneously, the spacing between the epitaxially grown light-emitting devices 10 can improve display resolution and enhance the display effect.

[0081] In one possible implementation, in light-emitting devices 10 with different emission colors, each quantum well growth auxiliary layer 13 has a first surface 13A of the same area, and each quantum well growth auxiliary layer 13 has a second surface 13B of different areas.

[0082] In this embodiment, the greater the thickness of the quantum well growth auxiliary layer 13 in the direction perpendicular to the plane of the substrate 11, the smaller the corresponding second surface 13B. When the quantum well layer 14 is epitaxially grown on the second surface 13B, the higher the indium content in the quantum well layer 14, the longer the wavelength of the light emitted by the formed light-emitting device 10.

[0083] In one possible implementation, in light-emitting devices 10 with different emission colors, the thickness of each quantum well layer 14 is the same in the plane direction perpendicular to the substrate 11 (Z direction in the figure).

[0084] Different color light-emitting devices 10 have quantum well layers 14 of the same thickness and quantum well growth auxiliary layers 13 of different thicknesses. By using quantum well growth auxiliary layers 13 of different thicknesses, the indium content in the quantum well layers 14 of the same thickness can be controlled, so as to achieve precise control of the emission wavelength of different color light-emitting devices 10.

[0085] In this embodiment, the thickness of the quantum well layer 14 is greater than or equal to 2 nanometers and less than or equal to 10 nanometers. Exemplarily, the thickness of the quantum well layer 14 includes 2 nanometers, 2.5 nanometers, 3.4 nanometers, 5 nanometers, 6.3 nanometers, 8.1 nanometers, 9.1 nanometers, or 10 nanometers, etc.

[0086] In one possible implementation, the light-emitting device 10 includes a first light-emitting device 10a, a second light-emitting device 10b, and a third light-emitting device 10c of different emitting colors, wherein the wavelengths of the light emitted by the first light-emitting device 10a, the second light-emitting device 10b, and the third light-emitting device 10c decrease sequentially. For example, the first light-emitting device 10a is a red light-emitting device, the second light-emitting device 10b is a green light-emitting device, and the third light-emitting device 10c is a blue light-emitting device.

[0087] In this embodiment, the first light-emitting device 10a includes a first quantum well growth auxiliary layer 131, the second light-emitting device 10b includes a second quantum well growth auxiliary layer 132, and the third light-emitting device 10c includes a third quantum well growth auxiliary layer 133. The areas of the second surface 13B of the first quantum well growth auxiliary layer 131, the second surface 13B of the second quantum well growth auxiliary layer 132, and the second surface 13B of the third quantum well growth auxiliary layer 133 increase sequentially.

[0088] The greater the thickness of the quantum well growth auxiliary layer 13, the smaller the corresponding second surface 13B. In the plane perpendicular to the substrate 11, the first quantum well growth auxiliary layer 131 has a first thickness, the second quantum well growth auxiliary layer 132 has a second thickness, and the third quantum well growth auxiliary layer 133 has a third thickness. The first thickness, the second thickness, and the third thickness decrease sequentially.

[0089] Specifically, the first thickness is greater than or equal to 120 nanometers and less than or equal to 200 nanometers, the second thickness is greater than or equal to 80 nanometers and less than 120 nanometers, and the third thickness is greater than or equal to 5 nanometers and less than 80 nanometers. For example, the first thickness includes 120 nanometers, 135 nanometers, 150 nanometers, 185 nanometers, or 200 nanometers, the second thickness includes 80 nanometers, 85 nanometers, 96 nanometers, 103 nanometers, or 112 nanometers, and the third thickness includes 5 nanometers, 10 nanometers, 20 nanometers, 40 nanometers, or 60 nanometers, etc.

[0090] In this embodiment, the first light-emitting device 10a further includes a first quantum well layer 141, the second light-emitting device 10b further includes a second quantum well layer 142, and the third light-emitting device 10c further includes a third quantum well layer 143. The first quantum well layer 141 has a first indium concentration, the second quantum well layer 142 has a second indium concentration, and the third quantum well layer 143 has a third indium concentration. The first indium concentration, the second indium concentration, and the third indium concentration decrease sequentially.

[0091] Specifically, the first indium concentration is greater than or equal to 30% and less than or equal to 40%, the second indium concentration is greater than or equal to 18% and less than or equal to 25%, and the third indium concentration is greater than or equal to 8% and less than or equal to 15%. For example, the first indium concentration is 30%, 30.5%, 34%, 37.6%, or 40%, etc.; the second indium concentration is 18%, 19.5%, 21.5%, 23.8%, or 25%, etc.; and the third indium concentration is 8%, 9.5%, 11.2%, 13.5%, or 15%, etc.

[0092] In one possible implementation, the roughness of the first surface 13A is greater than that of the second surface 13B, that is, the surface of the second surface 13B is smoother than the surface of the first surface 13A, which can improve the film quality of the quantum well layer 14 on the second surface 13B.

[0093] In one possible implementation, such as Figure 6 As shown, the first conductivity type semiconductor structure 12 includes a seed layer 121 and a first conductivity type semiconductor body 122 covering the seed layer 121.

[0094] The seed layer 121 fills the mask opening 1131 and forms a cone on the side of the mask layer 113 away from the substrate 11. A first conductivity type semiconductor body 122 covers the seed layer 121 and is frustum-shaped. The shape of the first conductivity type semiconductor body 122 is related to the shape of the seed layer 121. For example, when the shape of the seed layer 121 is a square pyramid, the shape of the first conductivity type semiconductor body 122 is a frustum.

[0095] In this embodiment, the seed layer 121 is made of GaN, InGaN or AlGaN, the first conductivity type semiconductor body 122 is an N-type InGaN layer, and the second conductivity type semiconductor structure 15 is a P-type GaN layer.

[0096] Further, please refer to Figure 7 The light-emitting device 10 also includes an electron blocking layer 18 located between the quantum well layer 14 and the second conductivity type semiconductor structure 15. The electron blocking layer 18 can block electrons from entering the second conductivity type semiconductor structure 15, thereby preventing the lifespan of the light-emitting device 10 from being shortened due to electrons entering the second conductivity type semiconductor structure 15.

[0097] Based on the same inventive concept, embodiments of this application also provide a display device, which includes a display panel prepared by the preparation method in the preceding embodiments, or a display panel described in the preceding embodiments. The display device includes an AR display device and / or a VR display device.

[0098] In summary, this application provides a method for fabricating a semiconductor structure, a semiconductor structure, and a display device. In the method for fabricating the semiconductor structure, a quantum well growth auxiliary layer, a quantum well layer, and a second conductivity type semiconductor structure are fabricated on the side of a first conductivity type semiconductor structure used to form different color light-emitting devices, away from the substrate. In light-emitting devices of different colors, the thickness of each quantum well growth auxiliary layer is different. The indium content of the corresponding quantum well layer can be controlled by adjusting the thickness of the quantum well growth auxiliary layer, thereby achieving precise control of the emission wavelength of different color light-emitting devices, improving the fabrication efficiency of multi-color light-emitting devices, and facilitating the large-scale manufacturing of semiconductor structures with full-color displays. Furthermore, selective growth, compared to etching, reduces damage to the light-emitting device and improves the fabrication yield.

[0099] The above description is merely a preferred embodiment of this application and is not intended to limit this application. Various modifications and variations can be made to this application by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the protection scope of this application.

Claims

1. A method for fabricating a semiconductor structure, characterized in that, The method includes: A substrate is provided, wherein the substrate includes a substrate, a buffer layer and a mask layer stacked together, and the mask layer has a plurality of mask openings that expose the buffer layer; A plurality of semiconductor structures of the first conductivity type are formed on the substrate at the corresponding mask opening positions; A quantum well growth auxiliary layer, a quantum well layer, and a second conductivity type semiconductor structure are sequentially fabricated on the side of a first conductivity type semiconductor structure used to form light-emitting devices of different colors away from the substrate. The light-emitting device is formed by the stacked first conductivity type semiconductor structure, the quantum well growth auxiliary layer, the quantum well layer, and the second conductivity type semiconductor structure. The quantum well growth auxiliary layer includes a first surface in contact with the first conductivity type semiconductor structure and a second surface in contact with the quantum well layer. The area of ​​the second surface is smaller than the area of ​​the first surface. In light-emitting devices with different emission colors, the thickness of each quantum well growth auxiliary layer is different. The thicker the quantum well growth auxiliary layer, the smaller the area of ​​the second surface, and the higher the indium content of the corresponding quantum well layer.

2. The method for preparing the semiconductor structure according to claim 1, characterized in that, The light-emitting device includes a first light-emitting device, a second light-emitting device, and a third light-emitting device with different emission colors. The step of sequentially fabricating a quantum well growth auxiliary layer, a quantum well layer, and a second conductivity type semiconductor structure on the side of the first conductivity type semiconductor structure used to form the light-emitting devices of different colors away from the substrate includes: A first barrier layer is formed on the side of the first conductivity type semiconductor structure away from the substrate, and the first barrier layer is patterned to form a first window, wherein the first window only exposes the first conductivity type semiconductor structure used to form the first light-emitting device. A first quantum well growth auxiliary layer, a first quantum well layer, and a second conductive type semiconductor structure are sequentially fabricated on the first conductive type semiconductor structure exposed by the first window. The first light-emitting device is composed of the stacked first conductive type semiconductor structure, the first quantum well growth auxiliary layer, the first quantum well layer, and the second conductive type semiconductor structure. A second barrier layer is formed on the side of the first quantum well layer and the first barrier layer away from the substrate, and the first barrier layer and the second barrier layer are patterned to form a second window, wherein the second window only exposes the first conductivity type semiconductor structure used to form the second light-emitting device; A second quantum well growth auxiliary layer, a second quantum well layer, and a second conductive type semiconductor structure are sequentially fabricated on the first conductive type semiconductor structure exposed in the second window. The second light-emitting device is composed of the stacked first conductive type semiconductor structure, the second quantum well growth auxiliary layer, the second quantum well layer, and the second conductive type semiconductor structure. A third barrier layer is fabricated on the side of the second quantum well layer and the second barrier layer away from the substrate, and the first barrier layer, the second barrier layer and the third barrier layer are patterned to form a third window, wherein the third window only exposes the first conductivity type semiconductor structure used to form the third light-emitting device; A third quantum well growth auxiliary layer, a third quantum well layer, and a second conductive type semiconductor structure are sequentially fabricated on the first conductive type semiconductor structure exposed by the third window. The third light-emitting device is composed of the stacked first conductive type semiconductor structure, the third quantum well growth auxiliary layer, the third quantum well layer, and the second conductive type semiconductor structure.

3. The method for preparing the semiconductor structure as described in claim 2, characterized in that, The wavelengths of the light emitted by the first light-emitting device, the second light-emitting device, and the third light-emitting device decrease sequentially. In the step of sequentially fabricating a quantum well growth auxiliary layer, a quantum well layer, and a second conductivity type semiconductor structure on the side of the first conductivity type semiconductor structure used to form different color light-emitting devices away from the substrate: The first quantum well growth auxiliary layer is grown using a first epitaxial growth time, the second quantum well growth auxiliary layer is grown using a second epitaxial growth time, and the third quantum well growth auxiliary layer is grown using a third epitaxial growth time. The epitaxial growth time of the first epitaxial growth time, the epitaxial growth time of the second epitaxial growth time, and the epitaxial growth time of the third epitaxial growth time decrease sequentially.

4. A semiconductor structure, characterized in that, The semiconductor structure includes a substrate and multiple light-emitting devices of different colors grown on the substrate. In the direction away from the substrate, each of the light-emitting devices includes a first conductivity type semiconductor structure, a quantum well growth auxiliary layer, a quantum well layer, and a second conductivity type semiconductor structure stacked together. The quantum well growth auxiliary layer includes a first surface in contact with the first conductivity type semiconductor structure and a second surface in contact with the quantum well layer, wherein the area of ​​the second surface is smaller than the area of ​​the first surface. In light-emitting devices with different emission colors, the thickness of each quantum well growth auxiliary layer is different in the plane direction perpendicular to the substrate. The thicker the quantum well growth auxiliary layer, the smaller the area of ​​the second surface, and the higher the indium content of the corresponding quantum well layer.

5. The semiconductor structure as described in claim 4, characterized in that, In light-emitting devices with different emission colors, each of the quantum well growth auxiliary layers has a first surface of the same area, and each of the quantum well growth auxiliary layers has a second surface of different areas.

6. The semiconductor structure as described in claim 4, characterized in that, In the plane perpendicular to the substrate, the thicker the quantum well growth auxiliary layer, the longer the wavelength of the light emitted by the corresponding color light-emitting device.

7. The semiconductor structure as described in claim 4, characterized in that, In light-emitting devices with different emission colors, the thickness of each quantum well layer is the same in the plane direction perpendicular to the substrate. The thickness of the quantum well layer is greater than or equal to 2 nanometers and less than or equal to 10 nanometers.

8. The semiconductor structure as described in claim 4, characterized in that, The light-emitting device includes a first light-emitting device, a second light-emitting device, and a third light-emitting device with different light-emitting colors, wherein the wavelengths of the light emitted by the first light-emitting device, the second light-emitting device, and the third light-emitting device decrease sequentially. The first light-emitting device includes a first quantum well growth auxiliary layer, the second light-emitting device includes a second quantum well growth auxiliary layer, and the third light-emitting device includes a third quantum well growth auxiliary layer; The areas of the second surface of the first quantum well growth auxiliary layer, the second surface of the second quantum well growth auxiliary layer, and the second surface of the third quantum well growth auxiliary layer increase sequentially.

9. The semiconductor structure as described in claim 8, characterized in that, In a plane direction perpendicular to the substrate, the first quantum well growth auxiliary layer has a first thickness, the second quantum well growth auxiliary layer has a second thickness, and the third quantum well growth auxiliary layer has a third thickness; The first thickness, the second thickness, and the third thickness decrease sequentially. The first thickness is greater than or equal to 120 nanometers and less than or equal to 200 nanometers, the second thickness is greater than or equal to 80 nanometers and less than 120 nanometers, and the third thickness is greater than or equal to 5 nanometers and less than 80 nanometers.

10. The semiconductor structure as described in claim 8, characterized in that, The first light-emitting device further includes a first quantum well layer, the second light-emitting device further includes a second quantum well layer, and the third light-emitting device further includes a third quantum well layer; The first quantum well layer has a first indium concentration, the second quantum well layer has a second indium concentration, and the third quantum well layer has a third indium concentration, wherein the first indium concentration, the second indium concentration, and the third indium concentration decrease sequentially. The first indium concentration is greater than or equal to 30% and less than or equal to 40%, the second indium concentration is greater than or equal to 18% and less than or equal to 25%, and the third indium concentration is greater than or equal to 8% and less than or equal to 15%.

11. The semiconductor structure according to any one of claims 4-10, characterized in that, The roughness of the first surface is greater than the roughness of the second surface.

12. The semiconductor structure according to any one of claims 4-10, characterized in that, The substrate includes a substrate, a buffer layer, and a mask layer stacked together, wherein the first conductivity type semiconductor structure is at least partially located on the side of the mask layer away from the substrate, and wherein the mask layer includes a mask opening that exposes the buffer layer; The first conductivity type semiconductor structure includes a seed layer and a first conductivity type semiconductor body covering the seed layer. The seed layer fills the mask opening and forms a cone on the side of the mask layer away from the substrate. The cone is located within the first conductivity type semiconductor body. The seed layer is made of GaN, InGaN, or AlGaN, the first conductivity type semiconductor body is made of N-type InGaN, and the second conductivity type semiconductor structure is made of P-type GaN.

13. A display device, characterized in that, The display device includes a semiconductor structure prepared by the method of preparing the semiconductor structure according to any one of claims 1-3, or a semiconductor structure according to any one of claims 4-12.